A preparation method of excess sludge composite nano zero-valent iron

By coating nano zero-valent iron in sludge, the problem of easy agglomeration of zero-valent iron nanoparticles and difficulty in sludge treatment is solved, efficient removal of heavy metals and simple sludge recycling are achieved, and the adsorption capacity of nano-zero-valent iron is enhanced. , avoiding secondary pollution of the environment.

CN114012104BActive Publication Date: 2024-10-18HARBIN INST OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202111307691.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-05
Publication Date
2024-10-18
Estimated Expiration
2041-11-05

AI Technical Summary

Technical Problem

Existing zero-valent iron nanoparticles are prone to agglomeration, resulting in an increase in particle size and loss of nano-characteristics, affecting their application value. At the same time, it is difficult to effectively recover the remaining sludge after treatment, and it is easy to cause secondary environmental pollution.

Method used

The preparation method of the remaining sludge composite nano-zero-valent iron is adopted, by mixing FeCl3·6H2O and NaBH4 aqueous solutions with the sludge, performing a reduction reaction and using magnets to separate, coating the nano-zero-valent iron on the surface of the sludge to enhance its dispersion and adsorption capacity and avoid oxidation through vacuum drying.

Benefits of technology

It improves the dispersion and adsorption efficiency of nano zero-valent iron, achieves efficient removal of heavy metals, has magnetic separation characteristics, simplifies the separation and recovery of adsorbents, avoids secondary pollution, and provides an efficient treatment and treatment of sludge. Recycling methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114012104B_ABST
    Figure CN114012104B_ABST
Patent Text Reader

Abstract

A method for preparing excess sludge composite nano zero-valent iron relates to a method for preparing composite nano zero-valent iron. In order to solve the problem that zero-valent iron nanoparticles are easy to agglomerate and excess sludge produces secondary pollution to the environment. Method: Take excess sludge from the secondary sedimentation tank of a sewage treatment plant, let it settle to obtain settled sludge, add distilled water to the settled sludge, use nitrogen aeration, add FeCl 3 6H 2 O, then add NaBH 4 The aqueous solution is stirred under nitrogen protection, the solid product is separated by a magnet and washed with anhydrous ethanol, and finally the solid product is dried to obtain residual sludge composite nano zero-valent iron. The present invention uses sludge to encapsulate nano zero-valent iron. The addition of nano zero-valent iron can enhance the removal effect of heavy metals such as Sb and As, increase the dispersibility of nano zero-valent iron, have high reduction and adsorption efficiency, and avoid secondary pollution. The present invention is suitable for preparing residual sludge composite nano zero-valent iron.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing composite nanometer zero-valent iron. Background Art

[0002] The rapid development of industry and agriculture in recent years has led to an increase in heavy metal emissions from more and more industries such as mining, electroplating, chemical industry, and leather making. The increased use of pesticides and fertilizers has also led to frequent heavy metal pollution incidents. Heavy metals cannot be biodegraded and are easily accumulated in large quantities in organisms. Trace amounts of heavy metals in environmental media can be enriched in organisms to hundreds or even hundreds of thousands of times, and then poison the human body through the food chain. Therefore, how to effectively control heavy metal pollution has become one of the issues to be solved in the field of environmental protection.

[0003] Municipal sewage treatment plants produce a large amount of excess sludge every day. If this excess sludge cannot be effectively recycled and treated, it will act on the environment again to cause secondary pollution. However, sludge treatment of heavy metal wastewater is difficult to separate from wastewater after treatment, the speed is slow, and the separation cost is high.

[0004] Zero-valent iron nanoparticles have a small particle size and a large surface energy. In order to reduce their own surface energy, zero-valent iron nanoparticles tend to agglomerate. Agglomeration will cause the size of zero-valent iron nanoparticles to become larger and lose many nano properties based on small size, thereby reducing the reaction sites and affecting their practical application value. Summary of the invention

[0005] In order to solve the problems that existing zero-valent iron nanoparticles are easy to agglomerate and residual sludge produces secondary pollution to the environment, the present invention provides a preparation method of residual sludge composite nano zero-valent iron.

[0006] The preparation method of the excess sludge composite nano zero-valent iron of the present invention is carried out according to the following steps:

[0007] The residual sludge from the secondary sedimentation tank of the sewage treatment plant was taken and allowed to settle. The supernatant was removed to obtain the settled sludge. Distilled water was added to the settled sludge and nitrogen was used for aeration. Then FeCl3·6H2O was added, and then NaBH4 aqueous solution was added. The dissolved NaBH4 was added to achieve Fe 3+ The mixture is stirred under nitrogen protection, the solid product is separated by a magnet and washed with anhydrous ethanol, and finally the solid product is dried to obtain residual sludge composite nano zero-valent iron;

[0008] The ratio of the mass of the settled sludge to the volume of the distilled water is 1 g: (4-6) mL;

[0009] The mass ratio of the sedimentation sludge to FeCl3·6H2O is (39-41):3;

[0010] The drying process is: drying in a vacuum drying oven at 35°C for 22 to 26 hours; drying in the vacuum drying oven is to isolate the air to prevent zero-valent iron from being passivated by oxygen during the drying process, and 35°C is to prevent excessively high temperatures from denaturing substances such as polysaccharides in the sludge.

[0011] The concentration of the NaBH4 aqueous solution is 0.16 g / mL; a higher concentration of the NaBH4 aqueous solution will cause the reaction to be too intense and the reaction solution will easily overflow; a lower concentration of the NaBH4 aqueous solution requires more water. In addition to NaBH4, hydrated hydrazine and polyols can also reduce Fe 3+ The advantage of NaBH4 is that it reacts quickly and conveniently.

[0012] The NaBH4 aqueous solution contains BH4 - With FeCl3·6H2O 3+ The molar ratio is 3.

[0013] The principles and beneficial effects of the present invention are:

[0014] In the present invention, the complexation, adsorption, coprecipitation and other reactions that occur when nano zero-valent iron treats heavy metal wastewater effectively remove heavy metals; nano zero-valent iron has strong reducing properties and can be used to reduce high-valent heavy metal ions to low-valent heavy metals with lower toxicity or lower mobility, and has high reduction and adsorption efficiency. The residual sludge actually contains a large number of microorganisms and their extracellular secretions. These are macromolecular polymers composed of polysaccharides and proteins, etc., which contain a large number of functional groups and can complex with heavy metal ions to remove heavy metal ions in water. The present invention uses sludge to wrap nano zero-valent iron. The addition of nano zero-valent iron can enhance the removal effect of heavy metals such as Sb and As; the present invention uses a coating method to wrap the sludge on the surface of nano zero-valent iron, increase the dispersibility of nano zero-valent iron, thereby increasing the adsorption sites in contact with heavy metals, and then improve the adsorption efficiency. The present invention is based on nano zero-valent iron and residual sludge to prepare residual sludge composite nano zero-valent iron, which not only retains the advantages of residual sludge being highly efficient and suitable for treating low-concentration heavy metal wastewater, but also has the unique magnetic separation characteristics and high adsorption characteristics of nano zero-valent iron. When used as an adsorbent, the residual adsorbent and the adsorbed product can be separated and recovered simply and quickly through an external magnetic field, with high flocculation efficiency and high reduction adsorption efficiency, avoiding secondary pollution. Moreover, the preparation process is simple, easy to recycle, and easy to scale up; the present invention recycles and reuses residual sludge, providing a new idea for the treatment and disposal of residual sludge. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a transmission electron microscope image of nano-zero-valent iron;

[0016] Figure 2This is a transmission electron microscope image of the excess sludge composite nano-zero-valent iron prepared in Example 1;

[0017] Figure 3 This is a graph showing the unit adsorption capacity of antimony and arsenic by nano zero-valent iron and residual sludge composite nano zero-valent iron prepared in Example 1. DETAILED DESCRIPTION

[0018] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.

[0019] Specific implementation method 1: The preparation method of excess sludge composite nano zero-valent iron in this implementation method is carried out according to the following steps:

[0020] The residual sludge from the secondary sedimentation tank of the sewage treatment plant was taken and allowed to settle. The supernatant was removed to obtain the settled sludge. Distilled water was added to the settled sludge and nitrogen was used for aeration. Then FeCl3·6H2O was added, and then NaBH4 aqueous solution was added. The dissolved NaBH4 was added to achieve Fe 3+ The mixture is stirred under nitrogen protection, the solid product is separated by a magnet and washed with anhydrous ethanol, and finally the solid product is dried to obtain residual sludge composite nano zero-valent iron;

[0021] The ratio of the mass of the settled sludge to the volume of the distilled water is 1 g: (4-6) mL;

[0022] The mass ratio of the sedimentation sludge to FeCl3·6H2O is (39-41):3;

[0023] The drying process is: drying in a vacuum drying oven at 35°C for 22 to 26 hours; drying in the vacuum drying oven is to isolate the air to prevent zero-valent iron from being passivated by oxygen during the drying process, and 35°C is to prevent excessively high temperatures from denaturing substances such as polysaccharides in the sludge.

[0024] The concentration of the NaBH4 aqueous solution is 0.16 g / mL; a higher concentration of the NaBH4 aqueous solution will cause the reaction to be too intense and the reaction solution will easily overflow; a lower concentration of the NaBH4 aqueous solution requires more water. In addition to NaBH4, hydrated hydrazine and polyols can also reduce Fe 3+ The advantage of NaBH4 is that it reacts quickly and conveniently.

[0025] The NaBH4 aqueous solution contains BH4 - With FeCl3·6H2O 3+ The molar ratio is 3.

[0026] In this embodiment, the complexation, adsorption, coprecipitation and other reactions that occur when nano zero-valent iron treats heavy metal wastewater effectively remove heavy metals; nano zero-valent iron has strong reducing properties and can be used to reduce high-valent heavy metal ions to low-valent heavy metals with lower toxicity or lower mobility, and has high reduction and adsorption efficiency. The residual sludge actually contains a large number of microorganisms and their extracellular secretions. These are macromolecular polymers composed of polysaccharides and proteins, etc., which contain a large number of functional groups and can complex with heavy metal ions to remove heavy metal ions in water. This embodiment uses sludge to wrap nano zero-valent iron. The addition of nano zero-valent iron can enhance the removal effect of heavy metals such as Sb and As; this embodiment uses a coating method to wrap sludge on the surface of nano zero-valent iron, increase the dispersibility of nano zero-valent iron, thereby increasing the adsorption sites in contact with heavy metals, and then improve the adsorption efficiency. This embodiment is based on nano zero-valent iron and residual sludge to prepare residual sludge composite nano zero-valent iron, which not only retains the advantages of residual sludge being efficient and suitable for treating low-concentration heavy metal wastewater, but also has the unique magnetic separation characteristics and high adsorption characteristics of nano zero-valent iron. When used as an adsorbent, the residual adsorbent and the adsorbed product can be separated and recovered simply and quickly through an external magnetic field, with high flocculation efficiency and high reduction adsorption efficiency, avoiding secondary pollution. Moreover, the preparation process is simple, easy to recycle, and easy to scale up; this embodiment recycles and reuses residual sludge, providing a new idea for the treatment and disposal of residual sludge.

[0027] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the nitrogen aeration time is 30 to 35 minutes.

[0028] Specific implementation method three: This implementation method is different from specific implementation method two in that: the nitrogen aeration time is 32 minutes.

[0029] Specific implementation method 4: This implementation method is different from any one of specific implementation methods 1 to 3 in that: the ratio of the mass of the settled sludge to the volume of distilled water is 1 g: (5-6) mL.

[0030] Specific implementation mode 5: This implementation mode is different from specific implementation mode 4 in that the ratio of the mass of the settled sludge to the volume of the distilled water is 1 g:5 mL.

[0031] Specific implementation method six: This implementation method is different from any one of specific implementation methods one to five in that the mass ratio of the settled sludge to FeCl3·6H2O is (40-41):3.

[0032] Specific implementation method seven: This implementation method is different from specific implementation method six in that the mass ratio of the settled sludge to FeCl3·6H2O is 40:3.

[0033] Specific implementation eight: This implementation differs from any one of specific implementations one to seven in that: the drying process is: drying in a vacuum drying oven at 35° C. for 22 to 26 hours.

[0034] Specific implementation method 9: This implementation method is different from any one of specific implementation methods 1 to 8 in that: the stirring is performed for 29 to 31 minutes under nitrogen protection.

[0035] Specific implementation method ten: This implementation method is different from specific implementation method nine in that: the stirring is performed for 30 minutes under nitrogen protection.

[0036] Embodiment 1:

[0037] The preparation method of excess sludge composite nano zero-valent iron in this embodiment is carried out according to the following steps:

[0038] The residual sludge from the secondary sedimentation tank of the sewage treatment plant was taken and allowed to settle. The supernatant was removed to obtain the settled sludge. Distilled water was added to the settled sludge and nitrogen was used for aeration. Then FeCl3·6H2O was added, and then NaBH4 aqueous solution was added. The dissolved NaBH4 was added to achieve Fe 3+ The mixture is reduced to zero-valent iron, stirred under nitrogen protection, the solid product is separated by a magnet and washed with anhydrous ethanol, and finally the solid product is dried to obtain residual sludge composite nano-zero-valent iron.

[0039] The nitrogen aeration time is 30 to 35 minutes; the ratio of the mass of the sedimentation sludge to the volume of distilled water is 1g:5mL; the mass ratio of the sedimentation sludge to FeCl3·6H2O is 40:3; the drying process is: drying at 35°C in a vacuum drying oven for 24 hours; the concentration of the NaBH4 aqueous solution is 0.16g / mL; the BH4 in the NaBH4 aqueous solution is 0.16g / mL; - with Fe 3+ The molar ratio is 3; the mixture is stirred for 30 minutes under nitrogen protection.

[0040] Figure 1 This is a transmission electron microscope image of nano-zero-valent iron; Figure 2 This is a transmission electron microscope image of the excess sludge composite nano-zero-valent iron prepared in Example 1; Figure 1 and Figure 2 It can be seen that Figure 1 The nano-zero-valent iron in the medium has a certain degree of aggregation, while the residual sludge composite nano-zero-valent iron prepared in Example 1 has higher dispersibility. Before the transmission electron microscopy test, the residual sludge composite nano-zero-valent iron and the nano-zero-valent iron were ultrasonically dispersed in anhydrous ethanol, and the obtained dispersion was dropped onto a copper mesh and dried.

[0041] Figure 3Graph showing the unit adsorption of antimony and arsenic by nano zero-valent iron and residual sludge composite nano zero-valent iron prepared in Example 1; wherein a corresponds to the unit metal (antimony) system, wherein the concentration of Sb before adsorption is 0.4 mmol / L; b corresponds to the unit metal (arsenic) system, wherein the concentration of As before adsorption is 0.4 mmol / L; c corresponds to Sb in the binary metal system, wherein the concentration of Sb before adsorption in the binary metal system is 0.4 mmol / L; d corresponds to As in the binary metal system, wherein the concentration of As before adsorption in the binary metal system is 0.4 mmol / L; in the above system, the addition amount of nano zero-valent iron / composite material is 0.5 g / L, and the addition amount of nano zero-valent iron is 0.5 g / L. Figure 3 It can be seen that the adsorption capacity of the residual sludge composite nano zero-valent iron prepared in Example 1 for antimony or arsenic is higher than that of nano zero-valent iron.

Claims

1. A method for preparing excess sludge composite nano zero-valent iron, characterized in that: The preparation method of excess sludge composite nano zero-valent iron is carried out according to the following steps: The residual sludge from the secondary sedimentation tank of the sewage treatment plant was taken and allowed to settle. The supernatant was removed to obtain the settled sludge. Distilled water was added to the settled sludge and nitrogen was used for aeration. Then FeCl3·6H2O was added, and then NaBH4 aqueous solution was added. The dissolved NaBH4 was added to achieve Fe 3+ The mixture is stirred under nitrogen protection, the solid product is separated by a magnet and washed with anhydrous ethanol, and finally the solid product is dried to obtain residual sludge composite nano zero-valent iron; The ratio of the mass of the settled sludge to the volume of the distilled water is 1 g: (4-6) mL; The mass ratio of the sedimentation sludge to FeCl3·6H2O is (39-41):3; The drying process is as follows: drying in a vacuum drying oven at 35°C for 22 to 26 hours; The concentration of the NaBH4 aqueous solution is 0.16 g / mL; The NaBH4 aqueous solution contains BH4 - With FeCl3·6H2O 3+ The molar ratio is 3; The residual sludge composite nano-zero-valent iron contains a large number of microorganisms and their extracellular secretions, and contains a large number of functional groups, which can complex with heavy metal ions to remove heavy metal ions in water; The sludge is wrapped on the surface of nano zero-valent iron by a coating method to increase the dispersibility of nano zero-valent iron, thereby increasing the adsorption sites in contact with heavy metals and subsequently improving the adsorption efficiency.

2. The method for preparing excess sludge composite nano zero-valent iron according to claim 1, characterized in that: The nitrogen aeration time is 30 to 35 minutes.

3. The method for preparing excess sludge composite nano zero-valent iron according to claim 2, characterized in that: The nitrogen aeration time was 32 minutes.

4. The method for preparing excess sludge composite nano zero-valent iron according to claim 1, characterized in that: The ratio of the mass of the settled sludge to the volume of the distilled water is 1 g: (5-6) mL.

5. The method for preparing excess sludge composite nano zero-valent iron according to claim 4, characterized in that: The ratio of the mass of the settled sludge to the volume of distilled water is 1 g:5 mL.

6. The method for preparing excess sludge composite nano zero-valent iron according to claim 1, characterized in that: The mass ratio of the settled sludge to FeCl3·6H2O is (40-41):

3.

7. The method for preparing excess sludge composite nano zero-valent iron according to claim 6, characterized in that: The mass ratio of the settled sludge to FeCl3·6H2O is 40:

3.

8. The method for preparing excess sludge composite nano zero-valent iron according to claim 1, characterized in that: The drying process is: drying in a vacuum drying oven at 35° C. for 22 to 26 hours.

9. The method for preparing excess sludge composite nano zero-valent iron according to claim 1, characterized in that: The mixture was stirred for 29 to 31 minutes under nitrogen protection.

10. The method for preparing excess sludge composite nano zero-valent iron according to claim 9, characterized in that: The mixture was stirred for 30 minutes under nitrogen protection.

Citation Information

Patent Citations

  • Modified water purification sludge-loaded nano zero-valent iron material as well as preparation method and application thereof