A nanocomposite cellulose acetate forward osmosis membrane and preparation method thereof

By introducing ZIFs nanomaterials into cellulose acetate membranes and growing zeolite imidazole skeletons using in situ reverse diffusion technology to form a high-performance positive permeability membrane, the problem of taking into account both water flux and retention rate of existing membranes and improving mechanical properties , suitable for a variety of water treatment applications.

CN114028946BActive Publication Date: 2024-12-06ZHEJIANG UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111242024.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-25
Publication Date
2024-12-06
Estimated Expiration
2041-10-25

AI Technical Summary

Technical Problem

The existing positive permeability membranes are difficult to take into account both the increase in water flux and the intercept rate, and the internal concentration difference polarization has a great impact, which reduces the effective osmotic pressure of the separation layer.

Method used

By introducing ZIFs nanomaterials into cellulose acetate membranes, zeolite imidazole skeleton materials are grown in dense separation layers using in situ reverse diffusion technology to form a high-performance nanocomposite cellulose acetate positive permeability membrane.

Benefits of technology

It achieves a balance of high water flux and high retention rate, while improving the mechanical strength, solvent resistance and pollution resistance of the membrane. It is suitable for first aid water bags, juice concentration, seawater desalination and industrial wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003319859280000011
    Figure HDA0003319859280000011
  • Figure HDA0003319859280000012
    Figure HDA0003319859280000012
  • Figure HDA0003319859280000021
    Figure HDA0003319859280000021
Patent Text Reader

Abstract

The present invention discloses a nano composite cellulose acetate forward osmosis membrane and a preparation method thereof. The forward osmosis membrane comprises: a porous support layer and a cellulose acetate dense separation layer containing ZIFs nano material. The present invention also provides a membrane making technology, i.e., nano particles are added to the membrane by an in-situ reverse diffusion method while forming the membrane by non-solvent induced phase separation. The nano particles provide more water channels for the forward osmosis membrane, reduce the mass transfer resistance and tortuosity, solve the problem that the existing forward osmosis membrane cannot have both high water flux and high retention rate, and provide the forward osmosis membrane with certain pressure resistance. The forward osmosis membrane of the present invention can be used in the fields of emergency water bags, fruit juice concentration, seawater desalination, industrial wastewater treatment, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of membrane separation, and in particular to a cellulose acetate forward osmosis membrane modified by introducing ZIFs nanomaterials through in-situ reverse diffusion technology, and a preparation method of the forward osmosis membrane. Background Art

[0002] In recent years, with the global population growth, rapid industrialization and the continuous destruction of available freshwater resources, water shortage has become a serious global problem. Membrane technology has attracted much attention in wastewater treatment and seawater desalination. Forward osmosis is an emerging membrane separation technology that uses the osmotic pressure difference of the solutions on both sides of the membrane (feed liquid and draw liquid) as a driving force to transfer water from the low osmotic pressure area to the high osmotic pressure area through the semipermeable membrane, thereby achieving dehydration and concentration of the feed liquid. Due to its low energy consumption, low membrane pollution, and low requirements for the structural stability of membrane materials, it has gradually become the mainstream of future membrane technology applications. However, the existence of concentration polarization greatly weakens the actual osmotic pressure on both sides of the forward osmosis membrane separation layer, limiting the performance of forward osmosis technology. Among them, compared with external concentration polarization, internal concentration polarization has a greater impact on the performance of forward osmosis, greatly reducing the effective osmotic pressure on both sides of the separation layer. Since the internal concentration polarization is generated in the porous support layer of the membrane, and the solutes in the draw liquid in the porous support layer mainly exist in the form of molecular diffusion, it is less affected by the external hydraulic conditions of the membrane support layer and is extremely difficult to eliminate.

[0003] With the development of nanotechnology, many new functional nanomaterials have been applied to forward osmosis membranes to improve the forward osmosis performance of the membranes. Metal organic frameworks (MOFs) are a new type of porous materials with ultra-large specific surface area and high pore volume formed by the coordination of metal ions and organic ligands. Zeolite imidazole frameworks (ZIFs) are a subclass of microporous metal organic frameworks (MOFs) composed of divalent transition metal cations and organic imidazole linkers. Compared with inorganic fillers, ZIFs have a stronger affinity with organic polymers. It is precisely because of the good compatibility between the two phases that the introduction of ZIFs nanomaterials can improve water flux and other properties without losing the selectivity of the membrane. The uniform loading of nanofillers on the membrane can increase the water flux of the membrane and reduce the internal concentration polarization. Therefore, it is an important research direction to increase the forward osmosis performance of forward osmosis membranes by introducing nanoparticles. Summary of the invention

[0004] The purpose of the present invention is to provide a novel nanocomposite cellulose acetate forward osmosis membrane and its preparation method and application. The main problem that the existing forward osmosis membrane cannot have both high water flux and high rejection rate is solved. The present invention aims to modify the dense separation layer structure, and a novel forward osmosis membrane is prepared by growing zeolite imidazole framework materials (ZIFs) by in-situ reverse diffusion technology while generating a dense separation layer by non-solvent induced phase separation.

[0005] The high-performance nanocomposite cellulose acetate forward osmosis membrane of the present invention not only ensures high water flux and good salt rejection rate, but also has certain mechanical strength, solvent resistance and pollution resistance, and can be used in the fields of emergency water bags, juice concentration, seawater desalination or industrial wastewater treatment.

[0006] The technical solution of the present invention is as follows:

[0007] A nano-composite cellulose acetate forward osmosis membrane, comprising: a porous support layer, a cellulose acetate dense separation layer doped with ZIFs nanomaterials;

[0008] The porous support layer is a fiber nonwoven fabric or a textile material composed of one or more polymers such as polyester, polyamide, polyethersulfone or polyolefin;

[0009] The dense separation layer of cellulose acetate doped with ZIFs nanomaterials is formed by non-solvent induced phase separation and in-situ reverse diffusion technology;

[0010] The polymer used in the cellulose acetate dense separation layer includes: any one of cellulose acetate, cellulose diacetate, and cellulose triacetate, or a mixture of two of them in a mass ratio of 1:1 to 1:4;

[0011] The ZIFs nanomaterial includes one or more ZIFs materials such as ZIF-5, ZIF-7, ZIF-8, ZIF-11, ZIF-67, and ZIF-90.

[0012] A method for preparing a nano-composite cellulose acetate forward osmosis membrane comprises the following steps:

[0013] (1) adding cellulose acetate to a casting solution solvent consisting of 1,4-dioxane, methanol, acetone and L-lactic acid, stirring and dissolving at 40 to 80° C., then subjecting the mixture to ultrasonic treatment and standing for degassing (for more than 3 hours) to obtain a casting solution for later use;

[0014] The mass ratio of each component in the casting solution solvent is: 40-70 parts of 1,4-dioxane, 5-15 parts of methanol, 12-24 parts of acetone, and 2-10 parts of L-lactic acid;

[0015] The mass percentage of the cellulose acetate in the casting solution is 5 to 11%;

[0016] (2) soaking the porous support layer in a metal salt solution, then taking it out and drying it for later use;

[0017] The soaking temperature is 20 to 50°C and the soaking time is 1 minute to 24 hours;

[0018] The concentration of the metal salt solution is 0.1-20 g / 100 mL, the solvent is deionized water, and the metal salt is selected from: one or more of zinc nitrate hexahydrate, zinc chloride, zinc sulfate, zinc acetate, cobalt nitrate hexahydrate, cobalt chloride hexahydrate, and cobalt sulfate heptahydrate;

[0019] The drying temperature is 30-60°C;

[0020] (3) uniformly coating the casting solution obtained in step (1) on the porous support layer prepared in step (2), and after standing in air (0 to 60 seconds), immersing the porous support layer coated with the casting solution in an organic ligand solution, and then taking it out and subjecting it to heat treatment to obtain the nanocomposite cellulose acetate forward osmosis membrane;

[0021] The coating thickness of the casting solution is 0.03 to 0.5 mm;

[0022] The concentration of the organic ligand solution is 0.1-10 g / 100 mL, the solvent is deionized water, and the organic ligand is selected from one of 2-methylimidazole, benzimidazole, 2-aminobenzimidazole, and imidazole-2-carboxaldehyde, or a mixture of any two of them in a mass ratio of 1:1 to 1:4;

[0023] The temperature of immersion in the organic ligand solution is 20 to 50°C for 1 minute to 24 hours, and non-solvent-induced phase separation is performed to form a membrane, and ZIFs nanoparticles are generated by in-situ reverse diffusion in the dense separation layer.

[0024] The heat treatment temperature is 30-80° C. and the time is 3-60 min.

[0025] The nano composite cellulose acetate forward osmosis membrane prepared by the invention includes flat membrane, hollow fiber homogeneous membrane or hollow composite membrane and tubular membrane.

[0026] The nano composite cellulose acetate forward osmosis membrane prepared by the invention can be applied to the fields of emergency water bags, fruit juice concentration, seawater desalination or industrial wastewater treatment.

[0027] The beneficial effects of the present invention are:

[0028] The high-performance forward osmosis membrane of the present invention introduces nanoparticles at the defects on the membrane surface through in-situ reverse diffusion technology to construct more water channels, and combines a dense separation layer of cellulose acetate containing a large number of hydrophilic groups prepared by a phase inversion method to ensure high water flux and high retention rate. It also has high mechanical strength, solvent resistance, and pollution resistance, and can be used in the fields of emergency water bags, juice concentration, seawater desalination, or industrial wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 : Scanning electron micrograph of a control forward osmosis membrane (comparative example) prepared from blank nonwoven fabric.

[0030] Figure 2 : Scanning electron microscope image of the high-performance nanocomposite cellulose acetate forward osmosis membrane prepared in Example 4.

[0031] Figure 3 : Comparison chart of water flux and reverse solute flux data of the control forward osmosis membrane prepared from blank non-woven fabric (comparative example) and the forward osmosis membranes prepared from Example 1, Example 2, and Example 4. DETAILED DESCRIPTION

[0032] After extensive and in-depth research, the inventor of the present application has developed a high-performance nanocomposite cellulose acetate forward osmosis membrane prepared by reverse diffusion self-sealing technology, including a non-woven fabric support layer and a cellulose acetate separation layer doped with nanomaterials. Among them, the nanocomposite forward osmosis membrane is formed by phase inversion and simultaneous in-situ reverse diffusion, which increases the water channel and selectivity of the forward osmosis membrane and improves the forward osmosis performance of the membrane. On this basis, the present invention was completed.

[0033] The following is a further description of the method for preparing a nanocomposite cellulose acetate forward osmosis membrane by reverse diffusion self-sealing technology according to the present invention through specific examples. It should be understood that the following examples are only for specific illustration and do not limit the protection scope of the present invention. At the same time, obvious changes and modifications made by those skilled in the art according to the present invention are also included in the protection scope of the present invention.

[0034] Comparative Example

[0035] The cellulose acetate forward osmosis membrane was prepared by non-solvent induced phase separation method. 3.5g of cellulose acetate, 3.634g of methanol reagent, 7.25g of acetone, 4.5g of L-lactic acid, and 29.5g of 1,4-dioxane were accurately weighed and placed in a clean and dry round-bottom flask, stirred for 15h in an oil bath at 50℃, and then allowed to stand for degassing for more than 10h; the clean non-woven fabric was dried and placed on a film scraping machine for film scraping, with the film scraping speed set to 120cm / min and the film scraping thickness set to 150um; the film was placed in a fume hood for solvent evaporation for 45s and then placed in deionized water at room temperature for phase inversion for 3min, and then placed in deionized water at 40℃ and 80℃ for finalization, each for 3min; after the phase inversion of the forward osmosis membrane was completed, it was placed in an oven at 80℃ for drying for 30min and stored for testing.

[0036] The thickness of a cellulose acetate forward osmosis membrane prepared in the comparative example is 240±10um, and the water flux is 2.67L / (m 2 ·h), the reverse solute flux is 0.0305 mol / (m 2 h).

[0037] Example 1

[0038] Preparation of nanocomposite cellulose acetate forward osmosis membrane using in situ reverse diffusion technology. Accurately weigh 4.5g of cellulose acetate, 3.634g of methanol reagent, 7.25g of acetone, 5.8g of L-lactic acid, and 29.5g of 1,4-dioxane into a clean and dry round-bottom flask, stir for 15h in an oil bath at 50℃, and then stand for degassing for more than 10h; prepare 1.9g / 100ml of zinc nitrate hexahydrate aqueous solution, soak the clean non-woven fabric in the 40℃ zinc aqueous solution for 3min, dry it, and place it on a film scraper to scrape the film. The scraping speed of the film scraper is set to 120cm / min, and the film thickness is 150um; evaporate the solvent of the scraped film in a fume hood for 45s, and then place it in a 2.6g / 100ml 2-methylimidazole aqueous solution at 40℃ for phase transformation and reverse diffusion growth of ZIF-8; the forward osmosis membrane is phase transformed in the aqueous solution for 3min, then placed in an oven at 80℃ for drying for 30min, and stored for testing.

[0039] The thickness of the novel nanocomposite cellulose acetate forward osmosis membrane prepared in Example 1 is 240±10 um, and the water flux is 3.99 L / (m 2 ·h), the reverse solute flux is 0.0806mol / (m 2 h).

[0040] Example 2

[0041] Nanocomposite cellulose acetate forward osmosis membrane was prepared by in-situ reverse diffusion technology. 5.5g of cellulose acetate, 3.634g of methanol reagent, 7.25g of acetone, 7.1g of L-lactic acid, and 29.5g of 1,4-dioxane were accurately weighed and placed in a clean and dry round-bottom flask, stirred for 15h in an oil bath at 50℃, and then left to degas for more than 10h; 1.9g / 100ml of zinc nitrate hexahydrate aqueous solution was prepared, and the clean non-woven fabric was soaked in the 40℃ zinc nitrate aqueous solution for 3min, and then placed on a film scraper for film scraping after drying. The film scraping speed was set to 120cm / min and the film thickness was 150um; the film was placed in a 2.6g / 100ml 2-methylimidazole aqueous solution at 40℃ for phase transformation and reverse diffusion growth of ZIF-8 in the evaporation of solvent in a fume hood for 45s; the forward osmosis membrane was placed in an 80℃ oven for drying for 30min after phase transformation in the imidazole aqueous solution for 3min, and then stored for testing.

[0042] The thickness of a novel nanocomposite cellulose acetate forward osmosis membrane prepared in Example 2 is 240±10 um, and the water flux is 5.16 L / (m 2 ·h), the reverse solute flux is 0.0502mol / (m 2 h).

[0043] Example 3

[0044] Preparation of nanocomposite cellulose acetate forward osmosis membrane using in situ reverse diffusion technology. Accurately weigh 5.5g of cellulose acetate, 3.634g of methanol reagent, 7.25g of acetone, 3.23g of L-lactic acid, and 29.5g of 1,4-dioxane into a clean and dry round-bottom flask, stir for 15h in a 50℃ oil bath, and then stand for degassing for more than 10h; prepare a 2.0g / 100ml aqueous solution of cobalt chloride hexahydrate, soak a clean non-woven fabric in a 40℃ aqueous solution of cobalt zinc chloride hexahydrate for 3min, dry it, and place it on a film scraper for film scraping. The film scraping speed is set to 120cm / min and the film scraping thickness is 200um; after the solvent of the scraped film evaporates in a fume hood for 45s, it is placed in a 40℃ 2.76g / 100ml 2-methylimidazole aqueous solution for phase transformation and reverse diffusion growth of ZIF-67; after the forward osmosis membrane is phase transformed in the imidazole aqueous solution for 3min, it is placed in an 80℃ oven for drying for 30min and stored for testing.

[0045] A novel nano-composite cellulose acetate forward osmosis membrane prepared in Example 3.

[0046] Example 4

[0047] Nanocomposite cellulose acetate forward osmosis membrane was prepared by in-situ reverse diffusion technology. 3.5g of cellulose acetate, 3.634g of methanol reagent, 7.25g of acetone, 4.5g of L-lactic acid, and 29.5g of 1,4-dioxane were accurately weighed and placed in a clean and dry round-bottom flask, stirred for 15h in an oil bath at 50℃, and then left to degas for more than 10h; 1.9g / 100ml of zinc nitrate hexahydrate aqueous solution was prepared, and the clean non-woven fabric was soaked in the 40℃ zinc nitrate aqueous solution for 3min, and then dried and placed on a film scraper for film scraping. The film scraping speed was set to 120cm / min and the film thickness was 150um; the scraped film was placed in a 2.6g / 100ml 2-methylimidazole aqueous solution at 40℃ for phase transformation and reverse diffusion growth of ZIF-8 in the evaporation of solvent in a fume hood for 45s; the forward osmosis membrane was placed in an 80℃ oven for drying for 30min after the phase transformation in the imidazole aqueous solution for 3min, and then stored for testing.

[0048] The thickness of a novel nanocomposite cellulose acetate forward osmosis membrane prepared in Example 4 is 240±10 um, and the water flux is 5.94 L / (m 2 ·h), the reverse solute flux is 0.0749 mol / (m 2 h).

[0049] Note: The polyethylene terephthalate (PET) nonwoven fabric used in the examples was purchased from Hangzhou Water Treatment Center. Water flux and reverse solute flux test conditions: temperature 25±1°C, 1M NaCl as the draw solution, and deionized water as the feed solution.

[0050] The above test results show that the high-performance nano-composite cellulose acetate forward osmosis membrane prepared by the present invention has good forward osmosis performance, and has excellent promotion and application prospects and industrialization value.

Claims

1. A nanocomposite cellulose acetate forward osmosis membrane, It is characterized in that include: A porous support layer and a dense separation layer of cellulose acetate doped with ZIFs nanomaterials; The porous support layer is a fiber nonwoven fabric or a textile material composed of one or more of polyester, polyamide, polyethersulfone or polyolefin; The polymer in the cellulose acetate dense separation layer is any one of cellulose acetate, cellulose diacetate, and cellulose triacetate, or a mixture of two of them in a mass ratio of 1:1 to 1:4; The ZIFs nanomaterial is one or more of ZIF-5, ZIF-7, ZIF-8, ZIF-11, ZIF-67, and ZIF-90; The preparation method of the nanocomposite cellulose acetate forward osmosis membrane comprises the following steps: (1) adding cellulose acetate to a casting solution solvent consisting of 1,4-dioxane, methanol, acetone and L-lactic acid, stirring and dissolving at 40 to 80° C., then subjecting to ultrasonic treatment and standing for degassing to obtain a casting solution for later use; (2) soaking the porous support layer in a metal salt solution, then taking it out and drying it for later use; The metal salt is selected from: one or more of zinc nitrate hexahydrate, zinc chloride, zinc sulfate, zinc acetate, cobalt nitrate hexahydrate, cobalt chloride hexahydrate, and cobalt sulfate heptahydrate; The concentration of the metal salt solution is 0.1-20 g / 100 mL, and the solvent is deionized water; The soaking temperature is 20 to 50°C and the soaking time is 1 minute to 24 hours; (3) uniformly coating the casting solution obtained in step (1) on the porous support layer prepared in step (2), and after standing in the air, immersing the porous support layer coated with the casting solution in an organic ligand solution to phase-invert and simultaneously reversely diffuse and grow ZIFs, and then taking out and heat-treating it to obtain the nanocomposite cellulose acetate forward osmosis membrane; The coating thickness of the casting solution is 0.03 to 0.5 mm; The organic ligand is selected from one of 2-methylimidazole, benzimidazole, 2-aminobenzimidazole, imidazole-2-carboxaldehyde, or a mixture of any two of them in a mass ratio of 1:1 to 1:4; The concentration of the organic ligand solution is 0.1-10 g / 100 mL, and the solvent is deionized water; The temperature for immersion in the organic ligand solution is 20 to 50°C, and the time is 1 minute to 24 hours; The heat treatment temperature is 30-80° C. and the time is 3-60 min.

2. The nanocomposite cellulose acetate forward osmosis membrane according to claim 1, It is characterized in that The mass ratio of the components in the casting solution solvent of the preparation method step (1) is: 40-70 parts of 1,4-dioxane, 5-15 parts of methanol, 12-24 parts of acetone, and 2-10 parts of L-lactic acid.

3. The nanocomposite cellulose acetate forward osmosis membrane according to claim 1, It is characterized in that In step (1) of the preparation method, the mass percentage of cellulose acetate in the casting solution is 5-11%.

4. Application of the nanocomposite cellulose acetate forward osmosis membrane as claimed in claim 1 in emergency water bags, juice concentration, seawater desalination or industrial wastewater treatment.

Citation Information

Patent Citations

  • Cellulose acetate forward osmotic membrane and preparation method thereof

    CN103537200A

  • Flat type mixed substrate forward osmosis membrane based on metal-organic frameworks ZIF-8 and preparation method thereof

    CN107837690A

  • In Situ Fabrication of Metal-Organic Framework Films and Mixed-Matrix Membranes

    US20210053015A1