Color vision correction resin lens
Enhance spectral color purity and the dimensions of color vision vector space by using acrylate/spiropyran/transition metal oxide nano-microsphere three-layer composite core-shell structure in color blind correction glasses , solves the problem that traditional correction glasses cannot increase the color vision dimension, and achieves effective correction and visual health protection for patients with color blindness.
Patent Information
- Application Number
- CN202111244248.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-25
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-10-25
AI Technical Summary
Traditional color blindness correction glasses cannot increase the dimension of the color vision vector space, causing patients to rely on different brightness to distinguish colors. Long-term wearing may lead to visual distortion and visual health problems, and at the same time, the appearance effect is poor, affecting the aesthetics.
Using organic/inorganic nanocomposite microsphere light-visual materials, including acrylate/spiropyran/transition metal oxide nanosphere three-layer composite core-shell structure, the lens enhances spectral color purity and the dimensions of color vision vector space indoors, correcting The color perception is abnormal, the shell is acrylate, and the spiropyran color discoloration compound is located between the core and the shell, and can quickly fade into light or colorless after ultraviolet rays.
It improves the color discrimination ability of color blind patients, corrects color abnormalities, ensures the real vision, has high color saturation and good color complementation effect, and is comfortable to wear, and is suitable for patients with weak red and green and secondary red and green blindness.
Smart Images

Figure CN114035342B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ophthalmic optics, and in particular relates to a color vision correction ophthalmic lens. Background Art
[0002] Color vision is one of the important visual functions of the eye. The seven colors of the visible spectrum in sunlight can be attributed to the three primary colors, namely red, green and blue. The retinal cone cells contain red, green and blue pigments. The human eye can recognize about 100 different colors. Congenital color vision abnormalities are caused by abnormal lack of color pigments in cone cells. It can usually be divided into total color blindness, red-green color blindness and red-green color weakness. Monochromatic vision with only one color pigment is total color blindness; those with two color pigments are dichromatic vision, and those who lack red or green pigments are red-green color blindness; those with normal color pigments in cone cells but less color pigments are trichromatic vision, that is, red-green color weakness. According to human color vision physiology and physics, the color vision characteristics of normal people are three-dimensional vector space, and the three basis vectors correspond to the three primary colors of red, green and blue respectively. Each color can be represented as a point or a vector in this vector space. When the dimension of this vector space of a color-blind person is smaller than that of a normal person and the difference in brightness is not obvious (the color-blindness test chart is based on this principle), the color-blind person cannot distinguish between the two colors.
[0003] Traditional color blindness correction glasses cannot increase the dimension of this vector space, but change the difference in brightness between the two colors. After wearing traditional color blindness correction glasses, color blind patients rely on the difference in brightness to distinguish the two "colors". However, wearing such glasses for a long time will cause visual distortion, which is not good for visual health. In addition, the disadvantages of the existing technology are poor appearance, and the lenses are obviously abnormal colors, such as bright red and dark blue, which many patients have concerns about and affect the appearance. Some color blind glasses, while correcting color vision abnormalities, greatly attenuate the amount of normal light transmitted, making them unusable in dim light, interfering with the normal part of vision, and long-term wearing will lead to decreased vision.
[0004] Traditional color blindness correction glasses cannot increase the dimension of this vector space, but change the difference in brightness between the two colors. After wearing traditional color blindness correction glasses, color blind patients rely on the difference in brightness to distinguish the two "colors". However, in this way, some people who can distinguish "colors" by the difference in brightness when not wearing traditional color blindness correction glasses cannot distinguish them when wearing these color blindness correction glasses. Not only that, the overall vision of people wearing traditional color blindness correction glasses will always decline, and the bright red and bright blue appearance is also difficult to accept. Summary of the invention
[0005] The purpose of the present invention is to provide a color vision correction resin lens, which contains an organic / inorganic nano-composite microsphere optometry material, which is a three-layer composite core-shell structure of acrylate / spiropyran / transition metal oxide nano-microspheres, wherein the core is oxide nanoparticles, the shell is coated with acrylate, and the spiropyran color-changing compound is in the middle layer between the core and the shell, forming a composite multi-layer core-shell structure. The optometry material plays a role of filtering and color complementation in the lens. Under normal indoor light, the lens has a darker color, can automatically enhance the color purity of a certain band spectrum and the dimension of the color vision vector space, improve the color discrimination ability of color blind patients, correct color vision abnormalities, especially patients with red-green color deficiency and secondary severe red-green color blindness, and after returning to the outdoors (ultraviolet irradiation), it can quickly fade to light color or colorless, ensuring that the patient sees things realistically and maintains visual health, and has the advantages of high color saturation, good color complementation effect, and comfortable wearing.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A color vision correction resin lens, comprising a lens resin substrate and an organic / inorganic nanocomposite microsphere optometry material, wherein the material is a three-layer composite core-shell structure of acrylate / spiropyran / transition metal oxide nanospheres, wherein the core is a transition metal oxide nanosphere, the microspheres are coated with a spiropyran compound shown in formula I, and the shell is acrylate; wherein the mass ratio of the transition metal oxide nanospheres, the spiropyran, and the acrylate is (2-4):(2-3):(1-2); and the mass ratio of the organic / inorganic nanocomposite microsphere optometry material to the lens resin substrate is 1:(30-200);
[0008]
[0009] In the color vision correction lens as described above, preferably, the acrylic ester is polymerized from acrylic ester monomers, and the acrylic ester monomers are selected from at least one of methyl acrylate, ethyl acrylate, 2-methyl methacrylate and 2-ethyl methacrylate.
[0010] In the color vision correction lens as described above, preferably, the transition metal oxide is selected from one or more of titanium oxide, iron oxide, copper oxide and cobalt oxide.
[0011] As mentioned above, the color vision correction lens, preferably, the lens base material is methyl methacrylate.
[0012] The color vision correction lens as described above, preferably, the mass ratio of the organic / inorganic nanocomposite microsphere optical material to the lens resin substrate is 1: (55-75);
[0013] For the color vision correction lens as described above, preferably, the organic / inorganic nanocomposite microsphere optical material is prepared by the following method:
[0014] I. Adding purified water and an emulsifier to a reaction kettle, and after complete dissolution, adding transition metal oxide nanoparticles, wherein the concentration of the transition metal oxide nanoparticles in water is 1.5-5.0 wt %; dropping a saturated aqueous solution of sodium acetate into the system, wherein the mass ratio of sodium acetate to the oxide nanoparticles is 1:0.5-1.0; and agglomerating the transition metal oxide nanoparticles into nanoscale clusters with uniform particles;
[0015] II. Add a crosslinking agent to the reaction system, introduce nitrogen, add a spiropyran compound solution represented by formula I, the mass ratio of spiropyran to transition metal oxide nanospheres is (2-3): (2-4), and the spiropyran particles are adsorbed on the surface of the oxide clusters;
[0016] III. Add acrylate monomer to the reaction system, the mass ratio of acrylate monomer to transition metal oxide nanospheres is (1-2): (2-4), and obtain an O / W type emulsion after stirring. After stirring and heating to 65-90°C, add an initiator, keep warm and polymerize for 12-18 hours, and generate an acrylate shell outside the particles formed in step II; obtain the organic / inorganic nanocomposite microsphere optical material by filtering, washing and drying.
[0017] In the color vision correction lens as described above, preferably, the particle size of the transition metal oxide nanoparticles is 2-12 nm.
[0018] For the color vision correction lens as described above, preferably, the solvent of the spiropyran compound solution is at least one of chloroform, acetone, propyl acetate, butyl acetate, ethyl acetate, dibutyl phthalate, and petroleum ether, and the mass ratio of the spiropyran compound to the solvent is 1:(2-3).
[0019] In the color vision correction lens as described above, preferably, the cross-linking agent is butyl methacrylate or diallyl phthalate, and the amount used is 0.5-2% of the mass of the acrylate monomer.
[0020] In the color vision correction lens as described above, preferably, the emulsifier is at least one of RF-345, polyvinyl pyrrolidone or sodium dodecylbenzene sulfonate, and the amount used is 2-6 g / L.
[0021] In the color vision correction lens as described above, preferably, the initiator is at least one of dibenzoyl peroxide, diisopropyl peroxydicarbonate, ammonium persulfate and sodium persulfate, and the amount used is 0.2-0.4% of the amount of the acrylate monomer used.
[0022] The spiropyran compound (I) of the present invention can be synthesized by the following method, but is not limited to the following method.
[0023] Synthesis of spiropyran compounds shown in formula I:
[0024] I. 1-6 g of 3,3-dimethyl-1′-methyl-2-methyleneindole is slowly added dropwise to 3-10 mL of concentrated H2SO4, and the temperature is controlled at 1-10°C in an ice-water bath; 0.1-0.6 g of fuming HNO3 is slowly added dropwise to 1-3 mL of concentrated H2SO4, and the temperature is controlled at 1-10°C in an ice-water bath; the mixed acid is added dropwise to a sulfuric acid solution containing 3,3-dimethyl-1′-methyl-2-methyleneindole, and the reaction temperature is controlled to be below 10°C. After stirring for 2-3 hours, the mixture is allowed to stand at 1-5°C and then refrigerated for 9-12 hours. A concentrated NaOH solution is added dropwise to alkalize the mixture, and a red solid is precipitated. The mixture is filtered, washed with water, and dried to obtain nitro-3,3-dimethyl-1′-methyl-2-methyleneindole (PS01).
[0025] II. Take 0.2-1 g of PS01 and 2-6 g of SnCl2 in 15-20 mL of 37% hydrochloric acid, heat to reflux for 1.5-2.5 h, cool in an ice-water bath to obtain a clear solution, add concentrated sodium hydroxide solution dropwise to alkalize, stop adding after a large amount of white granular solid appears, extract with ether, wash with water, filter, and remove the solvent by rotary evaporation to obtain amino-3,3-dimethyl-1′-methyl-2-methyleneindole (PS02).
[0026]
[0027] III. Dissolve 0.2-1 g of PS02 in 1-3 mL of CH2Cl2 under nitrogen protection and cool in an ice-water bath; dissolve 0.03-0.1 g of glutaric acid chloride in 1-3 mL of CH2Cl2, add glutaric acid chloride solution dropwise to the PS02 solution, add 0.5-3 mL of triethylamine, stir at room temperature for 2-3 h, filter, wash with water, and evaporate the organic layer to remove the solvent to obtain a white solid containing 2-1,3,3-trimethyl-2-methyleneindole-diamide (PS03).
[0028]
[0029] IV. Under nitrogen protection, take 0.02-0.1 g of PS03 and 0.01-0.06 g of 5-nitrosalicylicylaldehyde, dissolve in 15-35 mL of anhydrous ethanol, heat in a water bath at 30-50° C. for 12-20 h; after cooling to room temperature, solid crystals precipitate, filter and dry to obtain a purple-red spiropyran compound powder.
[0030]
[0031] The beneficial effects of the present invention are as follows:
[0032] 1. In view of the color rendering requirements of color blindness correction glasses under weak indoor light, the present invention studies the application of photochromic compounds as color vision correction optometry materials. The photochromic spiropyran compounds are colorless or light-colored closed ring bodies under light, and are colored (dark) open ring bodies in the dark. Among the numerous spiropyran photochromic compounds, it is found that the compound of formula (I) combined with transition metal oxide nanoparticles has a satisfactory color correction effect.
[0033] 2. The organic / inorganic nanocomposite microsphere optical material used as a filter color-compensating material of the present invention is a three-layer composite core-shell structure of acrylate / spiropyran / transition metal oxide nano-microspheres. Spiropyran is located between the outer shell and the inner core, i.e., the middle layer, as a color-changing compound. The transition metal oxide clusters of the inner core provide a certain color for the optical material and serve as a carrier of the spiropyran compound. In the preferred preparation method, the prepared inner core transition metal oxide clusters have a mesoporous nanostructure, which can increase the van der Waals area of the color-changing molecules adsorbed on the surface, increase the conjugated system, and increase the gaps between molecules, thereby greatly increasing the space for the molecules to undergo isomerization reactions, reducing conversion barriers, enhancing the activity of the color-changing body, and making the spectral response more sensitive. Under different lighting conditions, the filter characteristics in different band spectral regions can be changed to improve the vividness of the color. The acrylate outer shell has good rigidity, protects the color-changing compound from the influence of the external environment, and is also conducive to combining with the resin material matrix when preparing the optical material.
[0034] 3. In the process of preparing organic / inorganic nanocomposite microspheres for optical materials, the reaction conditions are controlled to generate three-layer composite core-shell nanospheres with uniform and accurate size. Sodium acetate plays an important role in the reaction process. On the one hand, it makes the oxide nanocrystals gradually aggregate into nuclei, and on the other hand, it effectively prevents a large number of particles from agglomerating into nuclei. The composite microspheres prepared by this method have an outer diameter of 35-90nm, wherein the diameter of the oxide nanospheres is 15-40nm, the thickness of the middle layer is 5-15nm, and the thickness of the outer shell is 5-10nm.
[0035] 4. The color blindness correction lens of the present invention maintains a darker color under normal indoor light, can automatically enhance the color purity of a certain band of the spectrum and the dimension of the color vision vector space, improve the color discrimination ability of color blind patients, and correct color vision abnormalities, especially for patients with red-green color deficiency, secondary severe red-green color deficiency, and blue color deficiency. After returning to the outdoors (under ultraviolet irradiation), it can gradually fade into a light color or colorless, ensuring that the patient sees objects realistically and maintains visual health. It has the advantages of high color saturation, good color complementation effect, and comfortable wearing. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a transmission electron microscope photograph of the acrylate / spiropyran / iron oxide nanocomposite microspheres prepared in Example 1.
[0037] Figure 2 This is a transmission electron microscope photograph of the acrylate / spiropyran / copper oxide nanocomposite microspheres prepared in Example 2.
[0038] Figure 3 This is a transmission electron microscope photograph of the acrylate / spiropyran / cobalt oxide nanocomposite microspheres prepared in Example 3.
[0039] Figure 4 This is a transmission electron microscope photograph of the acrylate / spiropyran / titanium oxide nanocomposite microspheres prepared in Example 4.
[0040] Figure 5 This is the absorption spectrum curve of spiropyran compound (I).
[0041] Figure 6 This is the infrared spectrum of the acrylate / spiropyran / iron oxide nanocomposite microspheres prepared in Example 1.
[0042] Figure 7 This is a transmittance spectrum of the color vision correction lens prepared in Example 1.
[0043] Figure 8 This is the infrared spectrum of the acrylate / spiropyran / copper oxide nanocomposite microspheres prepared in Example 2.
[0044] Fig. 9 This is a transmittance spectrum of the color vision correction lens prepared in Example 2.
[0045] Fig.10 This is a transmittance spectrum of the color vision correction lens prepared in Example 3.
[0046] Fig.11 This is a transmittance spectrum of the color vision correction lens prepared in Example 4.
[0047] FIG. 12 is a graph showing N2 adsorption-desorption isotherms and pore size distribution curves of the nanocomposite microsphere samples prepared in Examples 1-4.
[0048] Fig.13 This is a comparison chart of the effects of the color vision correction lens prepared in Example 1 before wearing (13-1) and after wearing (13-2).
[0049] Fig.14 This is a comparison chart of the effects of the color vision correction lens prepared in Example 2 before wearing (14-1) and after wearing (14-2).
[0050] Fig.15 This is a comparison chart of the effects of the color vision correction lens prepared in Example 3 before wearing (15-1) and after wearing (15-2).
[0051] Fig.16This is a comparison chart of the effects of the color vision correction lens prepared in Example 4 before wearing (16-1) and after wearing (16-2).
[0052] Fig.17 The figures are photos of nanocomposite microspheres prepared in the examples, wherein 17-1, 17-2, 17-3 and 17-4 are photos of microsphere products prepared by the methods of Example 1, Example 2, Example 3 and Example 4, respectively. DETAILED DESCRIPTION
[0053] The present invention is further described below by means of specific examples, but this is not intended to limit the protection scope of the present invention.
[0054] The spiropyran compounds in the following examples and comparative examples were prepared by the following method:
[0055] Preparation of spiropyran compounds shown in formula I:
[0056] A. Slowly drop 1.8 g of 3,3-dimethyl-1′-methyl-2-methyleneindole into 4 mL of 85% H2SO4, and cool in an ice-water bath to control the temperature at 4°C; slowly drop 0.35 g of 98% HNO3 into 1.6 mL of 85% H2SO4, drop the mixed acid into the sulfuric acid solution containing 3,3-dimethyl-1′-methyl-2-methyleneindole, control the reaction temperature at 5°C, stir for 3.5 h, let stand at 5°C for 10 h, drop 37% NaOH solution for alkalization, and a red solid precipitates. Filter, wash with water, and dry to obtain nitro-3,3-dimethyl-1′-methyl-2-methyleneindole (PS01)
[0057] B. Take 0.5 g of PS01 and 3.5 g of SnCl2 in 16 mL of 37% hydrochloric acid and heat to reflux for 2 h. Cool in an ice-water bath to obtain a clear solution. Add 35% sodium hydroxide solution dropwise to alkalize the solution. After a large amount of white granular solid appears, extract with ether, wash with water, filter, and rotary evaporate to obtain amino-3,3-dimethyl-1′-methyl-2-methyleneindole (PS02) as a white solid.
[0058] C. Dissolve 0.2 g of PS02 in 3 mL of CH2Cl2, protect with nitrogen, and cool to 5°C in an ice-water bath; dissolve 0.06 g of glutaric acid chloride in 2.2 mL of CH2Cl2, add the glutaric acid chloride solution dropwise to the PS02 solution, add 1.2 mL of triethylamine, stir at room temperature for 2 h, filter, wash with water, and evaporate the organic layer to remove the solvent to obtain a white solid containing 2-1,3,3-trimethyl-2-methyleneindole-diamide (PS03).
[0059] D. Under nitrogen protection, 0.06 g of PS03 and 0.04 g of 5-nitrosalicylic aldehyde were dissolved in 25 mL of anhydrous ethanol and heated in a water bath at 30-50° C. for 18 h. After cooling to room temperature, crystalline particles appeared, which were filtered and dried to obtain a purple-red spiropyran compound powder (I).
[0060] The spiropyran compound (I) prepared in the above step was dissolved in tetrahydrofuran and divided into multiple glass test tubes. After marking, the solution was irradiated at room temperature for 15 min. The solution was colorless under light and gradually turned red after being moved to a dark place for 12 seconds. The solution could be recycled multiple times. The solution had a broad absorption peak at 245 nm to 350 nm. For details, see Figure 5 shown.
[0061] Elemental Analysis C 43 H 42 % N6O8 found (calculated): C 66.94 (67.00); H 5.44 (5.49); N 10.95 (10.90).
[0062] Example 1: Preparation of organic / inorganic nanocomposite microspheres and color vision correction lenses
[0063] (I) Preparation of organic / inorganic nanocomposite microspheres:
[0064] (1) Take 3g of emulsifier RF-345 and add it to 1200g of pure water. After it is completely dissolved, add 35g of nano iron oxide, add 150g of saturated sodium acetate aqueous solution dropwise within 70min, and then add 20g of crosslinking agent DAP; introduce nitrogen into the reaction kettle, add 150g of dichloromethane solvent containing spiropyran compound (Formula I) (115g of solvent for 35g of spiropyran), add 18g of methyl acrylate monomer and 10g of ethyl acrylate monomer, stir and heat to 65°C, add 0.1g of initiator ammonium persulfate, keep warm for 18h, filter, wash and dry to obtain acrylate / spiropyran / iron oxide deep red nanospheres. The yield is 85%.
[0065] (2) The product prepared in step (1) was observed using a JEM-2100 transmission electron microscope. Figure 1As shown, it can be seen that the appearance is spherical, wherein the dark-colored core is composed of many uniform-sized, monodispersed iron oxide nanospheres, the middle layer is a spiropyran compound, and the transparent layer is an acrylic ester shell. It can be seen that the iron oxide nanospheres with a large specific surface area and pore volume adsorb the spiropyran compound material and are coated with acrylic ester to form a core-shell structure composite microsphere. Since the acrylic ester outer shell is a colorless and transparent material, a white outline is displayed in the transmission electron microscope photo. The average crystal size of iron oxide and the diameter of the nanocomposite microspheres are obtained by Scherrer formula (D = K / βcos θ) and Zeta potential analysis and calculation, wherein the iron oxide nanocrystal diameter is about 4nm, the thickness of the spiropyran color-changing material and the acrylic ester coating shell is about 15nm, the core of the iron oxide nanosphere is about 31nm, and the diameter of the entire composite microsphere is about 61nm.
[0066] (3) The product prepared in step (1) was tested by Fourier transform infrared spectroscopy (FT-IR). Figure 6 The analysis of the middle curve shows that at 3408cm -1 and 1220cm -1 The absorption peaks at 2961cm are caused by the stretching and bending vibrations of the amino group, indicating the presence of spiropyran compounds; -1 The absorption peak at 1730 cm is caused by the stretching vibration of methylene. -1 1610cm -1 1089cm -1 The strong peak at 591 cm is due to the vibration of C=O, which is the characteristic absorption peak of MMA (acrylate). -1 The absorption peak at 400 nm changes from a narrow shoulder peak to a sharp peak, indicating the presence of Fe-O. This indicates that the nanocomposite microspheres prepared in Example 1 are not a single iron oxide substance, but also contain spiropyran compounds and acrylate substances.
[0067] (4) Appearance photos of the product prepared in step (1) Figure 17-1 shown.
[0068] (ii) Preparation of color vision correction lenses: 20.0 g of acrylate / spiropyran / iron oxide nanospheres prepared in step (1) are added to a reaction vessel containing 1200 g of methyl methacrylate monomer (acrylic), 15 g of dichloromethane is added for thorough mixing, and then 3.5 g of dibenzoyl peroxide (BPO) is added to the monomer, and the mixture is stirred at a low speed of 200 r / min, and the polymerization reaction is controlled at 80° C. for 3 hours to complete the prepolymerization; the prepolymerized mixture is filtered and degassed, and then injected into a mold, and the temperature is raised from room temperature to 85° C. in a curing furnace over 20 hours to complete the primary curing; after the primary curing is completed, the mold is opened and cleaned, and the temperature is maintained at 105° C. in a precision-controlled curing furnace for 2 hours to complete the secondary curing to obtain a color vision correction lens.
[0069] The light transmittance of the color vision correction lens prepared in step (ii) was tested using the UV-8000 ultraviolet-visible bi-photometer produced by Shanghai Yuanxi Instrument Co., Ltd. The test results are detailed in Figure 7 ,from Figure 7 It can be seen from the spectrum that the transmittance of the sample is 0 for ultraviolet light, purple light, blue light and green light below 530nm, and it maintains a high transmittance for red light in the range of 605-700nm. This shows that the lens has a high resolution for red and can be used as a red weak correction lens.
[0070] Example 2: Preparation of organic / inorganic nanocomposite microspheres and color vision correction lenses
[0071] (I) Preparation of organic / inorganic nanocomposite microspheres:
[0072] 1. Take 2.5g of emulsifier RF-345 and add it to 1100g of pure water. After it is completely dissolved, add 30g of nano copper oxide, add 120g of saturated sodium acetate aqueous solution dropwise within 70min, and then add 20g of crosslinking agent DAP; introduce nitrogen into the reactor, add 145g of dichloromethane solvent containing spiropyran compound (Formula I) (spiropyran 35g solvent 110g), add methyl acrylate monomer 18g and ethyl acrylate monomer 10g, stir and heat to 65°C, add initiator ammonium persulfate 0.1g, keep warm for 16h, filter, wash and dry to obtain acrylate / spiropyran / copper oxide nanospheres. The yield is 82%.
[0073] 2. The product prepared in step 1 was observed by transmission electron microscopy. Figure 2 As shown, it can be seen that the appearance is spherical, wherein the dark-colored core is a nanosphere composed of copper oxide grains, the middle layer is a spiropyran compound, and the transparent layer is an acrylic shell. After analysis and calculation, the diameter of the copper oxide nanocrystal is about 4.5nm, the thickness of the spiropyran color-changing material and the acrylic coating shell is about 19nm, the core of the copper oxide nanosphere is about 41nm, and the diameter of the entire composite microsphere is about 79nm.
[0074] 3. The samples prepared in step 1 were tested by Fourier transform infrared spectroscopy (FT-IR). Figure 8 The analysis of the curve shows that the product has obvious characteristic absorption peaks of spiropyran and acrylate, and has the same characteristics as the product prepared in Example 1, except that at 591 cm -1 and 524cm -1 There is an obvious absorption peak at 500cm -1 Nearby is the Cu-O stretching vibration, proving the presence of copper oxide in the sample.
[0075] 4. The appearance photo of the product prepared in step 1 is as follows Figure 17-2 shown.
[0076] (II) Preparation of color vision correction lenses:
[0077] 18.0 g of acrylate / spiropyran / copper oxide nanospheres prepared in step 1 were added to a reaction vessel containing 1200 g of methyl methacrylate monomer (acrylic), 12 g of dichloromethane was added for thorough mixing, and then 3.5 g of BPO was added to the monomer, and the mixture was stirred at a low speed of 200 r / min, and the polymerization reaction was controlled at 80° C. for 3 hours to complete the prepolymerization; the prepolymerized mixture was filtered and degassed, and then injected into the mold, and the temperature was raised from room temperature to 85° C. in a curing furnace over 18 hours to complete the primary curing; after the primary curing was completed, the mold was opened and cleaned, and the temperature was kept at 105° C. in a precision-controlled curing furnace for 2 hours to complete the secondary curing to obtain a color vision correction lens.
[0078] The color vision correction lens prepared in step (ii) was tested for transmittance. The test results are detailed in Fig. 9 ,from Fig. 9 The spectrum shows that the sample has a low transmittance for ultraviolet light below 380nm and a high transmittance for blue light within 500nm, which means that the lens has a high resolution for blue light and can be used as a blue weak correction lens.
[0079] Example 3: Preparation of organic / inorganic nanocomposite microspheres and color vision correction lenses
[0080] (I) Preparation of organic / inorganic nanocomposite microspheres:
[0081] a. Take 2.4g of sodium dodecylbenzene sulfonate, an emulsifier, and add it to 1000g of pure water. After it is completely dissolved, add 30g of nano cobalt oxide, add 140g of saturated aqueous sodium acetate solution dropwise within 70min, and then add 20g of crosslinking agent butyl acrylate; introduce nitrogen into the reactor, add 145g of dichloromethane solvent containing spiropyran compound (Formula I) (105g of spiropyran 40g solvent), add 28g of methyl acrylate monomer, stir and heat to 65°C, add 0.1g of sodium persulfate initiator, keep warm for 16h, filter, wash and dry to obtain acrylate / spiropyran / cobalt oxide nanospheres. The yield is 80%.
[0082] b. The product prepared in step a is observed by transmission electron microscopy, such as Figure 3 As shown, it can be seen that the appearance is spherical, wherein the dark-colored inner core is a nanosphere composed of cobalt oxide grains, the middle layer is a spiropyran compound, and the transparent layer is an acrylate shell. After analysis and calculation, the particle size of the cobalt oxide nanocrystal is about 4.1nm, the thickness of the spiropyran color-changing material and the acrylate coating shell is about 14nm, the inner core of the cobalt oxide nanosphere is about 32nm, and the diameter of the entire composite microsphere is about 60nm.
[0083] c. The sample prepared in step a was tested by Fourier transform infrared spectroscopy (FT-IR) and had absorption characteristic peaks similar to those of the sample prepared in Example 1, wherein the absorption peak at 593 cm-1 was related to the Co-0 stretching vibration, proving the presence of cobalt oxide in the sample.
[0084] d. The appearance photo of the product prepared in step a is as follows Figure 17-3 shown.
[0085] (II) Preparation of color vision correction lenses:
[0086] 22.0 g of acrylate / spiropyran / cobalt oxide nanospheres prepared in step a are added to a reaction container containing 1300 g of methyl methacrylate monomer (acrylic), 12 g of dichloromethane is added for thorough mixing and stirring, and then 3.3 g of BPO is added to the monomer, and the mixture is stirred at a low speed of 200 r / min, and the polymerization reaction is controlled at 80° C. for 3 hours to complete the prepolymerization; the prepolymerized mixture is filtered and degassed, and then injected into a mold, and the temperature is raised from room temperature to 80° C. in a curing furnace over 20 hours to complete the primary curing; after the primary curing is completed, the mold is opened and cleaned, and the temperature is maintained at 105° C. in a precision-controlled curing furnace for 2.5 hours to complete the secondary curing to obtain a color vision correction lens.
[0087] The color vision correction lens prepared in step (ii) was tested for transmittance. The test results are detailed in Fig.10 ,from Fig.10 The spectrum shows that the sample has a transmittance of 0 for ultraviolet light below 380nm, a certain transmittance for blue light in the 480nm range, and a relatively high transmittance for red light in the 650-700nm range. This means that the lens has a certain resolution for both blue and red light, and can be used as a lens for red color blindness correction.
[0088] Example 4: Preparation of organic / inorganic nanocomposite microspheres and color vision correction lenses
[0089] (I) Preparation of organic / inorganic nanocomposite microspheres:
[0090] i. Take 2g of sodium dodecylbenzene sulfonate, an emulsifier, and add it to 1000g of pure water. After it is completely dissolved, add 26g of nano titanium oxide, add 140g of saturated aqueous sodium acetate solution dropwise within 70min, and then add 20g of crosslinking agent butyl acrylate; introduce nitrogen into the reactor, add 130g of dichloromethane solvent containing spiropyran compound (Formula I) (spiropyran 30g solvent 100g), add 26g of ethyl acrylate monomer, stir and heat to 70°C, add 0.1g of sodium persulfate initiator, keep warm for 16h, filter, wash and dry to obtain acrylate / spiropyran / titanium oxide nanospheres. The yield is 78%.
[0091] ii. The product prepared in step (i) is observed by transmission electron microscopy, such as Figure 4 As shown, it can be seen that the appearance is spherical, wherein the inner core is a nanosphere composed of white titanium oxide crystals, the middle layer is a spiropyran compound, and the transparent layer is an acrylic ester shell. After analysis and calculation, the particle size of the titanium oxide nanocrystal is about 4.2nm, the thickness of the spiropyran color-changing material and the acrylic ester coating shell is about 13nm, the inner core of the titanium oxide nanosphere is about 25nm, and the diameter of the entire composite microsphere is about 51nm.
[0092] iii. The sample prepared in step (i) was subjected to Fourier transform infrared spectroscopy (FT-IR) testing and had similar absorption characteristic peaks to those of the sample prepared in Example 1, except that at 506 cm -1 、601cm -1 and 700cm -1 The absorption peak at is consistent with the characteristic absorption peak of Ti-O, proving the presence of titanium oxide in the sample.
[0093] iv. Appearance photos of the product prepared in step (i) Figure 17-4 shown.
[0094] (II) Preparation of color vision correction lenses:
[0095] 16.0 g of acrylate / spiropyran / titanium oxide nanospheres prepared in step (i) were added to a reaction vessel containing 1000 g of methyl methacrylate monomer (acrylic), 10 g of dichloromethane was added for thorough mixing, and then 3.0 g of BPO was added to the monomer, and the mixture was stirred at a low speed of 200 r / min, and the polymerization reaction was controlled at 80° C. for 3 hours to complete the prepolymerization; the prepolymerized mixture was filtered and degassed, and then injected into a mold, and the temperature was raised from room temperature to 80° C. in a curing furnace over 20 hours to complete the primary curing; after the primary curing was completed, the mold was opened and cleaned, and the temperature was kept at 105° C. in a precision-controlled curing furnace for 2.5 hours to complete the secondary curing to obtain a color vision correction lens.
[0096] The color vision correction lens prepared in step (ii) was tested for transmittance. The test results are detailed in Fig.11 ,from Fig.11 It can be seen from the spectrum that the sample has a transmittance of 0 for ultraviolet light below 410nm, a certain transmittance for blue light within 500nm, and a relatively high transmittance for red light within 630nm. This means that the lens has a certain resolution for both blue and red light and can be used as a red-green color weak correction lens.
[0097] Example 5: Preparation of color vision correction lenses
[0098] 12.0 g of acrylate / spiropyran / copper oxide nanospheres prepared in Example 2 and 8.0 g of acrylate / spiropyran / titanium oxide nanospheres prepared in Example 4 were added to a reaction container containing 1400 g of methyl methacrylate monomer (acrylic), 13 g of dichloromethane was added for thorough mixing, and then 3.5 g of BPO was added to the monomers. The mixture was stirred at a low speed of 200 r / min and the polymerization reaction was controlled at 80° C. for 3 hours to complete the prepolymerization. The prepolymerized mixture was filtered and degassed and then injected into a mold. The temperature was raised from room temperature to 85° C. in a curing furnace over 18 hours to complete the primary curing. After the primary curing was completed, the mold was opened and cleaned, and the temperature was kept at 105° C. in a precision-controlled curing furnace for 2 hours to complete the secondary curing to obtain a color vision correction lens.
[0099] Example 6: Preparation of color vision correction lenses
[0100] 12.5 g of acrylate / spiropyran / cobalt oxide nanospheres prepared in Example 3 and 7.5 g of acrylate / spiropyran / titanium oxide nanospheres prepared in Example 4 were added to a reaction container containing 1400 g of methyl methacrylate monomer (acrylic), 13 g of dichloromethane was added for thorough mixing, and then 3.5 g of BPO was added to the monomers. The mixture was stirred at a low speed of 200 r / min and the polymerization reaction was controlled at 80° C. for 3 hours to complete the prepolymerization. The prepolymerized mixture was filtered and degassed and then injected into a mold. The temperature was raised from room temperature to 85° C. in a curing furnace over 18 hours to complete the primary curing. After the primary curing was completed, the mold was opened and cleaned, and the temperature was kept at 105° C. in a precision-controlled curing furnace for 2 hours to complete the secondary curing to obtain a color vision correction lens.
[0101] Example 7: Preparation of color vision correction lenses
[0102] 15 g of acrylate / spiropyran / iron oxide nanospheres prepared in Example 1 and 7.0 g of acrylate / spiropyran / titanium oxide nanospheres prepared in Example 4 were added to a reaction container containing 1400 g of methyl methacrylate monomer (acrylic), 13 g of dichloromethane was added for thorough mixing, and then 3.5 g of BPO was added to the monomers. The mixture was stirred at a low speed of 200 r / min and the polymerization reaction was controlled at 80° C. for 3 hours to complete the prepolymerization. The prepolymerized mixture was filtered and degassed and then injected into a mold. The temperature was raised from room temperature to 85° C. in a curing furnace over 18 hours to complete the primary curing. After the primary curing was completed, the mold was opened and cleaned, and the temperature was kept constant at 105° C. for 2 hours in a precision-controlled curing furnace to complete the secondary curing to obtain a color vision correction lens.
[0103] Example 8: Structural analysis of nanocomposite microspheres prepared in Examples 1-4
[0104] The nanocomposite microsphere samples prepared in Examples 1-4 were subjected to N2 adsorption-desorption isotherm detection to analyze the structural characteristics of the nanocomposite microspheres. The results are shown in FIG12 . P1, P2, P3, and P4 represent the nanocomposite microsphere samples prepared in Examples 1-4, respectively. Fig.12a It is the N2 adsorption-desorption isotherm. The isotherm type of the sample with 10h hydrothermal reaction time is type IV, and there is a hysteresis loop at P / P0 of 0.4-1.0, indicating the existence of mesopores. Figure 12b The pore size distribution curve shows that there is an obvious convex peak at 3nm, but no convex peak after 5nm, indicating that the pore size is small, about 3nm, and the mesopores in the sample are formed by the aggregation of nanoparticles. All these results are consistent with the SEM images of the nanocomposite microspheres observed previously.
[0105] Example 9: Optical performance test of the color vision correction lenses prepared in Examples 1-7
[0106] (I) Backlight color change performance test:
[0107] Testing steps: Put one copy of the marked lenses prepared in Examples 1-7 into a sunlight simulation box for irradiation testing. Irradiate for 6 minutes at room temperature. The distance between the lens and the light source is 20CM. The radiation amount hv=2Eg. Record the lens conditions before and after irradiation. The test results are shown in Table 1.
[0108] Table 1 Lens color change in backlight
[0109]
[0110] Conclusion: The above results show that the samples prepared in this example exhibit a reverse light color change effect, which is exactly the opposite of the performance of most pyran compounds, that is, they are colorless or light-colored closed-ring bodies under light, and they are colored (dark) open-ring bodies in the dark. And the color change speed is relatively fast.
[0111] (II) Color purity (color saturation) detection:
[0112] Testing steps: The color vision correction lenses prepared in Examples 1-7 were marked and inserted into trial frames for color purity testing on a computer ophthalmometer. The straight-line distance between the human eye and the color picture was 3.5 m. The testers tested the white film and the color vision correction lenses for the tested persons in groups and recorded the results, as shown in Table 2. The color detector was used for testing and recording. The test results are shown in Table 2.
[0113] Table 2 Color purity (color saturation) detection
[0114]
[0115] Conclusion: The lens prepared in this example enhances the color discrimination ability of the eyes and the color saturation of the objects seen is high.
[0116] (III) Color blindness picture recognition test:
[0117] According to the examination results of the "Color Blindness Examination Chart", the type and degree of color vision abnormality were determined. Referring to the mixed color scale value of the TZ-1 color vision tester and the effect of the patient trying on the color blindness correction lens, the lenses prepared in Examples 1 to 7 were tested respectively, and the color discrimination correction effect was recorded, as shown in Tables 3 and Figure 13-16 The participants in the test could identify at least 29 pictures and at most 39 pictures, thus judging that the color blindness correction lenses prepared in Examples 1-7 are suitable for patients with red-green color deficiency, tritanopia, secondary red-green color deficiency, red-green color deficiency and red-green-tritanopia, respectively.
[0118] Table 3 Chromaticity Correction
[0119] Chroma Correction Color identification before wearing Color identification after wearing Corrective effect Example 1 Red is hard to tell See red clearly Correction of red color deficiency Example 2 Weaker blue Blue clear Correction of blue color deficiency Example 3 Red is weaker Red clear Corrected red-eye blindness Example 4 Red and green are weak See red and green clearly Correction of weak red and green levels Example 5 Weak green See blue and green Correction of weak red, blue and green levels Example 6 Red is weaker Red is effective Correction of red color weakness Example 7 Red and blue are weaker See red, blue and green clearly Correction of weak red, blue and green levels
Claims
1. A color vision correction resin lens, characterized in that: The lens comprises a lens resin substrate and an organic / inorganic nanocomposite microsphere optometry material. The material is a three-layer composite core-shell structure of acrylate / spiropyran / transition metal oxide nanospheres, wherein the core is a transition metal oxide nanosphere, the microsphere is coated with a spiropyran compound shown in formula I, and the shell is acrylate; wherein the mass ratio of the transition metal oxide nanosphere, the spiropyran, and the acrylate is (2-4): (2-3): (1-2); and the mass ratio of the organic / inorganic nanocomposite microsphere optometry material to the lens resin substrate is 1: (30-200); (I) The transition metal oxide is selected from one or more of titanium oxide, iron oxide, copper oxide and cobalt oxide.
2. The color vision correction resin lens according to claim 1, characterized in that: The acrylic ester is polymerized from acrylic ester monomers, and the acrylic ester monomers are selected from at least one of methyl acrylate, ethyl acrylate, 2-methyl methacrylate and 2-ethyl methacrylate.
3. The color vision correction resin lens according to claim 1, characterized in that: The lens matrix material is methyl methacrylate.
4. The color vision correction resin lens according to claim 1 or 3, characterized in that: The mass ratio of the organic / inorganic nanocomposite microsphere optical material to the lens resin substrate is 1:(55~75).
5. The color vision correction resin lens according to any one of claims 1 to 3, characterized in that: The organic / inorganic nanocomposite microsphere optical material is prepared by the following method: I. Adding purified water and an emulsifier to a reaction kettle, and after the mixture is completely dissolved, adding transition metal oxide nanoparticles, wherein the concentration of the transition metal oxide nanoparticles in water is 1.5-5.0 wt %; dropping a saturated aqueous solution of sodium acetate into the system, wherein the mass ratio of sodium acetate to the oxide nanoparticles is 1:0.5-1.0; and agglomerating the transition metal oxide nanoparticles into nanoscale clusters with uniform particles; II. adding a crosslinking agent to the reaction system, introducing nitrogen, adding a spiropyran compound solution represented by formula I, wherein the mass ratio of spiropyran to transition metal oxide nanospheres is (2-3): (2-4), and the spiropyran particles are adsorbed on the surface of the oxide clusters; III. Adding acrylate monomer to the reaction system, the mass ratio of acrylate monomer to transition metal oxide nanospheres is (1-2): (2-4), stirring to obtain an O / W type emulsion, stirring and heating to 65-90°C, adding an initiator, and heat-preserving and polymerizing for 12-18 hours to form an acrylate shell outside the particles formed in step II; filtering, washing, and drying to obtain the organic / inorganic nanocomposite microsphere optical material.
6. The color vision correction resin lens according to claim 5, characterized in that: The particle size of the transition metal oxide nanoparticles is 2-12 nm.
7. The color vision correction resin lens according to claim 5, characterized in that: The solvent of the spiropyran compound solution is at least one of chloroform, acetone, propyl acetate, butyl acetate, ethyl acetate, dibutyl phthalate, and petroleum ether, and the mass ratio of the spiropyran compound to the solvent is 1:(2-3).
8. The color vision correction resin lens according to claim 5, characterized in that: The crosslinking agent is butyl methacrylate or diallyl phthalate, and the amount used is 0.5-2% of the mass of the acrylate monomer.
9. The color vision correction resin lens according to claim 5, characterized in that: The emulsifier is at least one of RF-345, polyvinyl pyrrolidone or sodium dodecylbenzene sulfonate, and the amount used is 2-6 g / L.
10. The color vision correction resin lens according to claim 5, characterized in that: The initiator is at least one of dibenzoyl peroxide, diisopropyl peroxydicarbonate, ammonium persulfate and sodium persulfate, and the amount used is 0.2-0.4% of the amount of the acrylate monomer.