A method for preparing a semiconductor passivation structure
Through the combined structure of multi-layer films and photoresist protective layers, the problem of performance changes of the passivation layer of semiconductor devices under external stress is solved, achieving high density, resistance to moisture and heat, and resistance to impurity ions, and improving the stability of the device. performance and reliability.
Patent Information
- Application Number
- CN202111155172.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-09-29
AI Technical Summary
The passivation layer structure in existing semiconductor devices can easily cause changes in interface performance under external stresses such as moisture, high temperature, voltage and current, leading to instability and degradation of device parameters. Moreover, the passivation structure of a single-layer film has poor adhesion and compactness. Low, it is difficult to meet the requirements of water resistance, water decomposition and anti-ion penetration at the same time.
A passivation structure composed of multi-layer films, including a silicon dioxide film with optimized refractive index and stress reduction and a silicon nitride film with increasing refractive index and stress, is formed through a photoresist protective layer to form an overlapping structure to improve adhesion. and stability.
It can effectively reduce the residual stress of the passivation layer, improve the density and resistance to moisture and heat, enhance the protection ability against impurity ions, and improve the stability and reliability of the device.
Smart Images

Figure CN114038761B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor devices, and in particular to a method for preparing a semiconductor passivation structure. Background Art
[0002] The failure of semiconductor devices is usually related to the electrical, thermal, physical and chemical effects occurring at various interfaces within the device structure. Semiconductor devices can be regarded as a series or series-parallel system composed of multiple components or multiple materials. In this system, there are many solid phase interfaces, such as semiconductor / insulator interface (such as GaAs / SiO2), metal / insulator interface (such as Au / SiO2), metal / semiconductor interface (such as Au / GaAs), metal-metal interface (such as Au / Cu / Ge / Au), etc. Under the influence of external stresses such as humidity, high temperature, voltage and current, solid / solid diffusion, ion charge migration, hot electron injection, electrochemical corrosion, and even cracks may occur between the above interfaces, resulting in slow changes in the electrical, thermal and mechanical properties of the interface, thereby causing instability and degradation of device parameters, and even complete failure. The research on the mechanism and process of passivation is essentially a study on interface effects, which helps to optimize the structure of semiconductor devices and improve the reliability of semiconductor devices.
[0003] In the field of compound semiconductor chip manufacturing, the passivation layer can effectively reduce and stabilize the surface state of compound semiconductor materials, prevent the chip surface from being infiltrated by water vapor, ion penetration and chemical corrosion, improve the chip's resistance to moisture and heat, and can also serve as a structural support layer to avoid mechanical damage. The passivation layer is widely used in the field of compound semiconductor chip manufacturing. It can not only enhance the stability and reliability of compound semiconductor devices, but also improve the device's packaging and testing yield. In addition, compound semiconductor materials such as gallium arsenide (GaAs), indium phosphide (InP), indium arsenide (InAs), etc., have differences in Young's modulus and thermal expansion coefficient between passivation layer materials such as silicon dioxide (SiO2) and silicon nitride (SiN). Therefore, in the chip manufacturing process, stress changes will occur due to temperature changes during the process, which may cause cracks, wrinkles, or even fall off in the film on the surface of the chip, causing the chip to fail.
[0004] Conventional passivation layer materials mainly include silicon dioxide and silicon nitride. The material type, structure and process parameters of the passivation layer are different, and the film parameters of the passivation layer (refractive index, density, film stress, etc.) and their effects on the chip surface are also different.
[0005] In the prior art, the passivation layer usually adopts a single-layer structure, such as a single-layer silicon dioxide film or a single-layer silicon nitride film, which is usually formed by a plasma enhanced chemical vapor deposition (PECVD) process. Figure 1The passivation layer A4 is usually a silicon dioxide film or a silicon nitride film, which fills the gap between the metal layer A3, the material layer A2 and the substrate A1 on the surface of the chip. However, the passivation structure of a single-layer film is prone to poor adhesion between the film and the substrate material, or the residual stress of the film is large, the film density is low, or it cannot simultaneously meet the performance requirements of good water resistance, good water hydrolysis resistance, good ion penetration resistance, and high breakdown voltage. For the passivation structure of two or more layers of thin films, if the residual stress, density, surface state treatment effect of each layer of the film and the stability of the electrical properties between each interface are not fully considered, the electrical, thermal and mechanical properties between the interfaces such as the semiconductor and passivation layer interface, the metal and passivation layer interface, etc. inside the device may change slowly under the influence of external factors such as temperature, humidity, voltage, and current, causing device failure. Summary of the invention
[0006] In view of the above problems existing in the prior art, a method for preparing a semiconductor passivation structure is now provided.
[0007] The specific technical solutions are as follows:
[0008] A method for preparing a semiconductor passivation structure, comprising: sequentially preparing a functional layer and a first metal layer on a substrate, wherein a middle portion of the first metal layer has a first notch to expose the functional layer, and further comprising:
[0009] Step S1: forming a first passivation layer on the substrate, wherein the first passivation layer wraps the functional layer and the first metal layer;
[0010] Step S2: removing the first passivation layer to retain the first passivation layer in the first notch and protruding from the first notch;
[0011] Step S3: forming a first photoresist layer on the first passivation layer, wherein the first photoresist layer partially covers the first passivation layer;
[0012] Step S4: forming a second metal layer on the first metal layer and wrapping the first passivation layer, and then removing the first photoresist layer to form a second notch on the second metal layer, wherein the second notch is located in a partial area above the first passivation layer;
[0013] Step S5: forming a second passivation layer on the first passivation layer and covering the upper surface of the second metal layer;
[0014] Step S6: partially removing the second passivation layer covering the upper surface of the second metal layer;
[0015] Step S7: forming a protective layer on the second passivation layer, wherein the protective layer wraps the second passivation layer.
[0016] Preferably, the first passivation layer comprises:
[0017] At least two layers of silicon dioxide film, the refractive index of the multi-layer silicon dioxide film decreases from bottom to top, the stress of the multi-layer silicon dioxide film decreases from bottom to top, and the process temperature of the multi-layer silicon dioxide film decreases from bottom to top;
[0018] The stress of the silicon dioxide film is compressive stress;
[0019] The refractive index of the silicon dioxide film located at the bottom layer is greater than 1.5;
[0020] The refractive index of the silicon dioxide film is in the range of 1.45-1.55; the stress range of the silicon dioxide film is -200MPa-0MPa;
[0021] The BHF etching rate of the silicon dioxide film ranges from 100 nm / min to 1000 nm / min;
[0022] The process temperature range of the silicon dioxide film is 300°C-350°C;
[0023] The thickness of the silicon dioxide film ranges from 10 nm to 1000 nm.
[0024] Preferably, the second passivation layer comprises:
[0025] At least two layers of silicon nitride film, the refractive index of the multi-layer silicon nitride film increases from bottom to top, the stress of the multi-layer silicon nitride film increases from bottom to top, and the process temperature of the multi-layer silicon nitride film decreases from bottom to top;
[0026] The stress of the silicon nitride film is tensile stress;
[0027] The refractive index of the silicon nitride film is in the range of 1.9-2.2;
[0028] The stress range of the silicon nitride film is 0-200MPa;
[0029] The BHF etching rate of the silicon nitride film is in the range of 20nm / min-1000nm / min; the process temperature of the silicon nitride film is in the range of 250°C-300°C;
[0030] The thickness of the silicon nitride film ranges from 100 nm to 1 μm.
[0031] Preferably, the step S2 comprises:
[0032] Step S21: coating a photoresist on the first passivation layer;
[0033] Step S22: removing the photoresist above the first metal layer to expose a portion of the first passivation layer above the first metal layer;
[0034] Step S23: etching and opening a portion of the first passivation layer above the first metal layer;
[0035] Step S24: removing the photoresist and the first passivation layer above the substrate to retain the first passivation layer in the first notch and protruding from the first notch.
[0036] Preferably, step S6 comprises:
[0037] Step S61: coating a photoresist on the second passivation layer;
[0038] Step S62: removing a portion of the photoresist above the second metal layer to expose a portion of the second passivation layer;
[0039] Step S63: etching the exposed second passivation layer to make an opening, so that a portion of the second metal layer is exposed;
[0040] Step S64: removing the photoresist.
[0041] Preferably, step S7 comprises:
[0042] Step S71: coating a photoresist on the second passivation layer, wherein the photoresist covers the second metal layer;
[0043] Step S72: exposing a portion of the second metal layer through photolithography and developer etching processes;
[0044] Step S73: curing the photoresist through a baking process to form the protective layer.
[0045] Preferably, the thickness of the first metal layer and the second metal layer is 0.2 μm to 2 μm.
[0046] Preferably, the length of the portion where the second metal layer overlaps the first passivation layer is between 5 μm and 100 μm.
[0047] Preferably, the length of the overlapping portion of the second metal layer and the second passivation layer is between 5 μm and 100 μm.
[0048] Preferably, the first passivation layer and the second passivation layer are formed by a plasma chemical vapor deposition process.
[0049] The above technical solution has the following advantages or beneficial effects: by setting a passivation layer composed of multiple layers of thin films, the residual stress of the passivation layer is effectively reduced, and at the same time, it has excellent density, moisture and heat resistance, resistance to impurity ion entry, high breakdown voltage, and strong adhesion, so that the passivation layer has a stronger suppression effect on the surface state of compound semiconductors, and the device performance parameters and stability are better; the edges of the passivation layer and the metal layer overlap with each other to avoid impurity ion contamination and thermal ion injection at the interface between the metal layer and the passivation layer, so that the chip performance is stable and the subsequent packaged device is stable; the top layer of the device uses photoresist as the top protective layer, which can improve the reliability of device performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] The embodiments of the present invention will be described more fully with reference to the attached drawings, which are provided for illustration and description only and are not intended to limit the scope of the present invention.
[0051] Figure 1 is an overall schematic diagram of an embodiment of the present invention;
[0052] Figure 2 is a flow chart of a method according to a first embodiment of the present invention;
[0053] Figure 3 A schematic diagram of a device having a first passivation layer in a first embodiment of the present invention;
[0054] Figure 4 It is a schematic diagram of a device after the opening process in the first embodiment of the present invention;
[0055] Figure 5 It is a schematic diagram of a device after a first photoresist layer is generated in the first embodiment of the present invention;
[0056] Figure 6 It is a schematic diagram of a device after the second metal layer is prepared in the first embodiment of the present invention;
[0057] Figure 7 It is a schematic diagram of a device after preparing the second passivation layer in the first embodiment of the present invention;
[0058] Figure 8 It is a schematic diagram of a device after the second passivation layer is opened in the first embodiment of the present invention;
[0059] Fig. 9 It is a schematic diagram of a device for coating photoresist in the first embodiment of the present invention;
[0060] Fig.10 A schematic diagram of a device for generating a protective layer in a first embodiment of the present invention;
[0061] Fig.11 This is a schematic diagram of sub-steps of step S2 in the first embodiment of the present invention;
[0062] Fig.12 This is a schematic diagram of sub-steps of step S6 in the first embodiment of the present invention;
[0063] Fig.13 This is a schematic diagram of sub-steps of step S7 in the first embodiment of the present invention;
[0064] Fig.14 A schematic diagram of forming the first and second silicon dioxide films in the second embodiment of the present invention;
[0065] Fig.15 A schematic diagram of forming a second metal layer in a second embodiment of the present invention;
[0066] Fig.16 A schematic diagram of forming the first and second silicon nitride films in the second embodiment of the present invention;
[0067] Fig.17 A schematic diagram of forming a photoresist layer in the second embodiment of the present invention;
[0068] Fig.18 This is a schematic diagram showing the completion of the preparation of the passivation structure in the third embodiment of the present invention;
[0069] Fig.19 This is a schematic diagram showing the completion of the preparation in the third embodiment of the present invention. DETAILED DESCRIPTION
[0070] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0071] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0072] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but they are not intended to limit the present invention.
[0073] In response to many problems existing in the prior art, the present invention aims to optimize the residual stress of the passivation structure on the chip surface, improve the ability of the passivation structure to isolate water molecules and impurity ions, and improve the compound semiconductor device's resistance to moisture and heat, voltage and current, and resistance to impurity ion penetration, ultimately making the device parameters stable in a variety of harsh application scenarios.
[0074] The passivation structure disclosed in the present invention includes a multi-layer passivation film, a two-layer metal layer structure and a photoresist protection layer, which is suitable for various compound semiconductor chips and can effectively improve the moisture and heat resistance of various compound semiconductor chips and improve the stability of the chip.
[0075] The multilayer film in the present invention is a multilayer passivation film composed of silicon dioxide and silicon nitride. By optimizing the process parameters of each passivation layer, the refractive index, thickness, density and stress of each layer are controlled within different types and numerical ranges, and finally the stress level of the overall structure of the passivation layer is controllable and has high density, which can effectively resist the invasion of impurity ions and improve the reliability of compound semiconductor devices.
[0076] The details are as follows:
[0077] Embodiment 1:
[0078] A method for preparing a semiconductor passivation structure, wherein a functional layer 2 and a first metal layer 3 are sequentially prepared on a substrate 1, wherein a middle portion of the first metal layer 3 has a first notch to expose the functional layer 2, as shown by convex 2, and the preparation method further comprises:
[0079] Step S1: Figure 3 As shown, a first passivation layer 4 is formed on the substrate 1, and the first passivation layer 4 wraps the functional layer 2 and the first metal layer 3;
[0080] Step S2: removing the first passivation layer 4 to retain the first passivation layer 4 in the first notch and protruding from the first notch. The result is as follows: Figure 4 As shown;
[0081] Specifically, the first metal layer 3 needs to be connected to the second metal layer 5 so that the entire device has a good conduction effect.
[0082] Step S3: Form a first photoresist layer 4.1 on the first passivation layer 4. Figure 5 As shown, the first photoresist layer 4.1 partially covers the first passivation layer 4;
[0083] Step S4: Form a second metal layer 5 on the first metal layer 3 and wrap the first passivation layer 4, then remove the first photoresist layer 4.1, so that a second notch is formed on the second metal layer 5, and the second notch is located in a partial area above the first passivation layer 4. The result is as follows: Figure 6 As shown;
[0084] Specifically, after the first passivation layer 4 is prepared, a wet etching process is used to open the first passivation layer 4 to expose the first metal layer 3. Then, the second metal layer 5 is selectively prepared on the first metal layer 3 by photolithography, and the second metal layer 5 is characterized in that a part of the second metal layer 5 covers the edge of the first passivation layer 4, presenting an overlapping structure.
[0085] Since the first passivation layer 4 adopts a wet etching opening process to expose the first metal layer 3, the wet etching process itself is anisotropic. After the first passivation layer is corroded, it is very likely to cause gaps or holes at the interface between the first passivation layer 4 and the first metal layer 3. The second metal layer 5 is prepared to form an overlapping structure, which can further optimize the interface between the metal layer and the passivation layer and improve the ability to resist the entry of water molecules and impurity ions.
[0086] Step S5: Form a second passivation layer 6 on the first passivation layer 4 and cover the upper surface of the second metal layer 5. Figure 7 As shown;
[0087] Step S6: Partially remove the second passivation layer 6 covering the upper surface of the second metal layer 5. The result is as follows: Figure 8 As shown;
[0088] Specifically, after the second passivation layer 6 is prepared, a wet etching process is used to open the second metal layer 5. By means of photolithography, the second passivation layer 6 is selectively etched on the second metal layer 5 so that the second metal layer 5 can be exposed outside the second passivation layer 6, and is used to serve as a metal electrode after the protective layer 7 is formed. The characteristic is that the second passivation layer 6 should partially cover the edge of the second metal layer 5, presenting an overlapping structure. The interface between the metal layer and the passivation layer can be further optimized to improve the ability to resist the entry of water molecules and impurity ions.
[0089] Step S7: Fig. 9 and Fig.10 As shown, a protective layer 7 is formed on the second passivation layer 6 , and the protective layer 7 wraps the second passivation layer 6 .
[0090] Specifically, since photoresist is a soft material, its impact resistance and pressure resistance are better than those of hard materials such as silicon dioxide and silicon nitride, so photoresist is finally used as the material of the protective layer 7.
[0091] The photoresist in the present invention preferably has the characteristics of high dielectric constant, low stress, low thermal expansion coefficient and low water absorption, and finally the activity of the photoresist is reduced by high temperature baking, so that it can be used as the outermost protective layer 7 of the chip.
[0092] As an optional implementation, the first metal layer 3 and the second metal layer 5 are Au—Ge—Ni—Au structures or Ti—Cu—Ti—Au structures, and the first metal layer 3 and the second metal layer 5 have the same structure.
[0093] Specifically, by providing the first metal layer 3 and the second metal layer 5 with different structures, the overall electrical properties of the compound semiconductor device can be effectively adjusted, so that the compound semiconductor device is more adaptable to the design indicators.
[0094] In a preferred embodiment, the first passivation layer 4 includes:
[0095] At least two layers of silicon dioxide film, the refractive index of the multi-layer silicon dioxide film decreases from bottom to top, the refractive index of the multi-layer silicon dioxide film decreases from bottom to top, the stress of the multi-layer silicon dioxide film decreases from bottom to top, and the process temperature of the multi-layer silicon dioxide film decreases from bottom to top;
[0096] The stress of silicon dioxide film is compressive stress;
[0097] The refractive index of the silicon dioxide film at the bottom layer is greater than 1.5;
[0098] The refractive index of silicon dioxide film ranges from 1.45 to 1.55; the stress range of silicon dioxide film is -200MPa–0MPa;
[0099] The BHF etching rate of silicon dioxide film ranges from 100nm / min to 1000nm / min;
[0100] The process temperature range of silicon dioxide film is 300℃-350℃;
[0101] The thickness of the silicon dioxide film ranges from 10nm to 1000nm.
[0102] Specifically, by controlling parameters such as the refractive index and the processing rate, a multilayer silicon dioxide film with different compactness and stress can be generated. In the first passivation layer 4, the bottom layer combined with the substrate 1 needs to use a silicon dioxide film with the largest refractive index (such as a refractive index of 1.55), the highest density, and the largest stress, and then follow the law of decreasing refractive index, decreasing compactness, and decreasing stress, so that the overall stress of the first passivation layer 4 is low, and it has excellent compactness, and can form a good step structure with the second metal layer 5 to achieve a good sealing effect.
[0103] In a preferred embodiment, the second passivation layer 6 includes:
[0104] At least two layers of silicon nitride film, the refractive index of the multi-layer silicon nitride film increases from bottom to top, the refractive index of the multi-layer silicon nitride film increases from bottom to top, the stress of the multi-layer silicon nitride film increases from bottom to top, and the process temperature of the multi-layer silicon nitride film decreases from bottom to top;
[0105] The stress of silicon nitride film is tensile stress;
[0106] The refractive index of silicon nitride films ranges from 1.9 to 2.2;
[0107] The stress range of silicon nitride films is 0-200MPa;
[0108] The BHF etching rate of silicon nitride film ranges from 20nm / min to 1000nm / min; the process temperature range of silicon nitride film is 250℃-300℃;
[0109] The thickness of silicon nitride film ranges from 100nm to 1μm.
[0110] Specifically, by controlling parameters such as the refractive index and processing rate, a multilayer silicon nitride film with different densities and stresses can be generated. In the second passivation layer 6, the bottom layer needs to use a silicon nitride film with the smallest refractive index (such as a refractive index of 1.9), a low density, and a small stress, and then follows the law of increasing refractive index, increasing density, and increasing stress, so that the overall stress of the second passivation layer 6 is low and has excellent density.
[0111] In a preferred embodiment, Fig.11 As shown, step S2 includes:
[0112] Step S21: coating a photoresist on the first passivation layer 4;
[0113] Step S22: removing the photoresist above the first metal layer 3 to expose a portion of the first passivation layer 4 above the first metal layer 3;
[0114] Step S23: etching and opening a portion of the first passivation layer 4 above the first metal layer 3;
[0115] Step S24: removing the photoresist and the first passivation layer 4 on the substrate 1 to retain the first passivation layer 4 in the first notch and protruding from the first notch.
[0116] Specifically, after step S1, a device in which the first passivation layer 4 is prepared by a PECVD process is Figure 3As shown, the first passivation layer will wrap around the outside of the substrate 1, the functional layer 2 and the first metal layer 3, so the excess first passivation layer 4 needs to be removed for subsequent preparation processes. In this technical solution, a photolithography process is used to remove the excess passivation layer. The first passivation layer 4 is selectively coated with photoresist and then photolithography is performed. The first passivation layer 4 above the first metal layer 3 can be exposed after being etched by the developer. Then, a wet etching process is used to etch the first passivation layer 4 to finally form an opening as shown in the figure. Figure 4 The structure shown.
[0117] In a preferred embodiment, Fig.12 As shown, step S6 includes:
[0118] Step S61: coating a photoresist on the second passivation layer 6;
[0119] Step S62: removing a portion of the photoresist on the second metal layer 5 to expose a portion of the second passivation layer 6;
[0120] Step S63: etching the exposed second passivation layer 6 to make an opening, so that a portion of the second metal layer 5 is exposed;
[0121] Step S64: removing the photoresist.
[0122] Specifically, the device in which the second passivation layer 6 is prepared by the PECVD process in step S5 is as follows: Figure 7 As shown, the second passivation layer 6 completely covers the second metal layer 5 and the first passivation layer 4. Therefore, it is necessary to remove the excess second passivation layer 6 for subsequent preparation processes. In the present technical solution, a photolithography process is used to remove the excess passivation layer. The second passivation layer 6 is selectively coated with photoresist and then photolithography is performed. The second passivation layer 6 above the second metal layer 5 can be exposed after being etched by the developer. At this time, it should be noted that in order to achieve the overlapping part of the second passivation layer 6 and the second metal layer, the area where the second passivation layer 6 is exposed by the developer should be controlled to achieve the effect of a 5μm to 100μm interface area between the second passivation layer 6 and the second metal layer 5. Subsequently, a wet etching process is used to etch the second passivation layer 6 to form an opening as shown in the figure. Figure 8 The structure shown.
[0123] In a preferred embodiment, Fig.13 As shown, step S7 includes:
[0124] Step S71: coating a photoresist on the second passivation layer 6, the photoresist covering the second metal layer 5;
[0125] Step S72: a photolithography and developer etching process is performed to expose a portion of the second metal layer 5;
[0126] Step S73: curing the photoresist through a baking process to form a protective layer 7.
[0127] Specifically, in order to achieve better device surface flatness, when coating photoresist, the effect is often as follows Fig. 9 As shown, it is necessary to remove part of the redundant photoresist above the second metal layer 5 so as to expose the second metal layer 5 so that it can be used as a metal electrode. In the process of etching the photoresist, the lateral boundary of the protective layer 7 should be controlled to be between the lateral boundary of the second passivation layer 6 and the lateral boundary of the second metal layer 5, so as to achieve the wrapping effect of the protective layer 7 on the second passivation layer 6, so that the interface between the second passivation layer 6 and the second metal layer 5 is not directly exposed outside the device, thereby improving the protection performance of the chip.
[0128] In a preferred embodiment, the thickness of the first metal layer 3 and the second metal layer 5 is 0.2 μm to 2 μm.
[0129] In a preferred embodiment, the length of the overlapping portion of the second metal layer 5 and the first passivation layer 4 is between 5 μm and 100 μm, so as to form a step-like structure and achieve a better sealing effect.
[0130] In a preferred embodiment, the length of the overlapping portion of the second metal layer 5 and the second passivation layer 6 is between 5 μm and 100 μm, so as to form a step-like structure and achieve a better sealing effect.
[0131] In a preferred embodiment, the first passivation layer 4 and the second passivation layer 6 are formed by a plasma chemical vapor deposition process.
[0132] Embodiment 2:
[0133] A gallium arsenide Hall element chip passivation structure is used to implement the preparation method in Example 1, such as Fig.14As shown, after the GaAs Hall element chip generates a substrate B1, a functional layer B2 and a first metal layer B3, a first passivation layer is prepared on the substrate, and the first passivation layer includes a first silicon dioxide film B4 and a second silicon dioxide film B5. Among them, the first metal layer B3 is prepared by a physical vapor deposition (PVD) process, which adopts a Ti-Cu-Ti-Au metal structure, and the cumulative thickness is about 300-400nm. The first silicon dioxide film B4 and the second silicon dioxide film B5 are both prepared by a plasma enhanced chemical vapor deposition process (PECVD). The refractive index of the first silicon dioxide film B4 should be greater than the refractive index of the second silicon dioxide film B5, the stress of the first silicon dioxide film B4 should be greater than the stress of the second silicon dioxide film B5, the BHF corrosion rate of the first silicon dioxide film B4 should be less than the corrosion rate of the second silicon dioxide film B5, and the process temperature of the first silicon dioxide film B4 should be greater than the process temperature of the second silicon dioxide film B5. The specific parameters are shown in Table 1 below. By forming the first silicon dioxide film B4 and the second silicon dioxide film B5 to form the first passivation layer together, the first passivation layer can have lower internal stress and excellent compactness, thereby improving its ability to resist moisture and heat.
[0134]
[0135] Table 1
[0136] After the first silicon dioxide film B4 and the second silicon dioxide film B5 are prepared, the effect is as follows: Fig.15 As shown, a second metal layer B6 is prepared on the first metal layer B3 and the second silicon dioxide film B5 by a physical vapor deposition process; the second metal layer B6 adopts a Ti-Cu-Ti-Au metal structure with a cumulative thickness of about 300 to 400 nm, and its edge overlaps above the second silicon dioxide film B5 with an overlapping scale of 10 μm. By setting the second metal layer B6 whose edge overlaps with the first passivation layer, the junction between the first passivation layer and the first metal layer B3 can be effectively covered, thereby preventing water vapor and impurities from passing through the junction between the first passivation layer and the first metal layer B3 and entering the functional layer B2 below, thereby effectively improving the device's resistance to moisture and heat.
[0137] Subsequently, a plasma enhanced chemical vapor deposition process (PECVD) is used to sequentially prepare a first silicon nitride film B7 and a second silicon nitride film B8 on top of the second silicon dioxide film B5 and the second metal layer B6 to form a second passivation layer, wherein the refractive index of the first silicon nitride film B7 should be smaller than the refractive index of the second silicon nitride film B8, the stress of the first silicon nitride film B7 should be smaller than the stress of the second silicon nitride film B8, the BHF etching rate of the first silicon nitride film B7 should be greater than the etching rate of the second silicon nitride film B8, and the process temperature of the first silicon nitride film B7 should be greater than the process temperature of the second silicon nitride film B8. The specific parameters of the first silicon nitride film B7 and the second silicon nitride film B8 are shown in Table 2. This results in a 10μm overlapping area between the first silicon nitride film B7 and the second metal layer B6. The final effect is as follows. Fig.16 shown.
[0138]
[0139] Table 2
[0140] Finally, a photoresist is coated on the second metal layer B6 and the second silicon nitride film B8 and then baked and cured to form a protective layer B9. The effect is as follows: Fig.17 The photoresist used to form the protective layer B9 should be selected from photoresists having the characteristics of high dielectric constant, low stress, low thermal expansion coefficient and low water absorption to achieve a good protective effect.
[0141] The gallium arsenide Hall element with the above passivation structure formed in this embodiment is less affected by the environment, and the voltage drift caused is also less than that in the prior art, as shown below:
[0142] The passivation structure disclosed in the present invention and the passivation structure in the prior art are respectively prepared for the same type of gallium arsenide Hall element, and moisture and heat resistance tests are performed on them to verify that the passivation structure disclosed in the present invention has better moisture and heat resistance than the passivation structure in the prior art.
[0143] (1) Sample Introduction
[0144] Sample A: GaAs Hall element, the surface of which is prepared with the passivation structure of the above-mentioned Example 2
[0145] Sample B: Gallium arsenide Hall element, the surface of which is passivated using existing technology (single-layer passivation film, single-layer metal layer, no photoresist protective layer)
[0146] The above-mentioned gallium arsenide Hall element samples are all made after the Hall element chip is packaged, and the packaging structure and packaging process are consistent, and the packaging test method is consistent.
[0147] (2) Experimental conditions
[0148] ①Test principle:
[0149] When the GaAs Hall element is in high temperature and high humidity conditions, if there are material defects on the surface of its packaging structure, moisture and impurities will invade the material defective part of the packaging structure, thereby affecting the electrical and structural performance of the device.
[0150] ②Purpose of the test:
[0151] Evaluate the product's ability to maintain its original performance after long-term exposure to humidity stress and temperature stress.
[0152] ③Testing instruments:
[0153] Constant temperature and humidity environmental test chamber.
[0154] ④Operational specifications:
[0155] Ⅰ. Carry out initial value test on the samples to be tested and record their initial values one by one;
[0156] Ⅱ. Place the sample in an environmental test chamber with specified temperature and humidity;
[0157] III. After a specified period of wet heat storage (the standard time intervals are usually: 168hr, 504hr, 1000hr, and 168 hours was selected as the test time interval in this test);
[0158] IV. Take the sample out of the test chamber and let it stand at room temperature for 2 to 24 hours. Complete parameter testing and record within 48 hours of the end of the test.
[0159] Ⅴ. Compare and analyze the data before and after the test to determine whether the test has any impact on the product.
[0160] ⑤Test conditions and criteria:
[0161] Typical test conditions: test temperature T = 85 ± 3 ° C, test humidity RH = 85 ± 5%, the number of samples is 22, and the test time is 168 hours.
[0162] (3) Data comparison:
[0163] The above-mentioned damp heat test was performed on sample A and sample B according to the above-mentioned test conditions and operation procedures. After 168 hours of testing, 5mA constant current drive and 6V constant voltage drive were used. Then, it was determined whether the unbalanced voltage of sample A or sample B drifted, and the number of samples with unbalanced voltage drift was counted.
[0164] According to statistics, the number of devices with unbalanced voltage drift among the 22 tested samples A is 18, and the number of devices with unbalanced voltage drift among the 22 tested samples B is 0, indicating that the gallium arsenide Hall element with a passivation structure prepared based on Example 2 has better resistance to moisture and heat.
[0165] Embodiment three:
[0166] The difference between this embodiment and the above technical solution is that it has only one metal layer, thereby simplifying the passivation layer structure. However, by setting silicon nitride films with different refractive indices, stress types, stress values and BHF etching rates, a better anti-humidity and heat effect than the prior art can be achieved.
[0167] Specifically, Fig.18 As shown, a first silicon dioxide film C4, a second silicon dioxide film C5, a first silicon nitride film C6, and a second silicon nitride film C7 are sequentially prepared on a gallium arsenide Hall element having a substrate C1 and a functional layer C2 by a plasma chemical vapor deposition process (PECVD). At the same time, a metal layer C3 is formed on the substrate C1 and the functional layer C2 by a physical vapor deposition process (PVD), and the cumulative thickness thereof is about 1000 to 2000 nm, and the upper surface of the metal layer C3 is lower than the height of the second silicon nitride film C7.
[0168] The structure composed of the first silicon dioxide film C4 and the second silicon dioxide film C5 corresponds to the first passivation layer described in the above preparation method. At the same time, the refractive index of the first silicon dioxide film C4 should be greater than the refractive index of the second silicon dioxide film C5, the stress of the first silicon dioxide film C4 should be greater than the stress of the second silicon dioxide film C5, and the BHF etching rate of the first silicon dioxide film C4 should be less than the etching rate of the second silicon dioxide film C5. The process temperature of the first silicon dioxide film C4 should be greater than the process temperature of the second silicon dioxide film C5.
[0169] In addition, the structure composed of the first silicon nitride film C6 and the second silicon nitride film C7 corresponds to the second passivation layer described in the above preparation method. At the same time, the refractive index of the first silicon nitride film C6 should be smaller than the refractive index of the second silicon nitride film C7, the stress of the first silicon nitride film C6 should be smaller than the stress of the second silicon nitride film C7, and the BHF etching rate of the first silicon nitride film C6 should be greater than the etching rate of the second silicon nitride film C7. The process temperature of the first silicon nitride film C6 should be greater than the process temperature of the second silicon nitride film C7.
[0170]
[0171] Table 3
[0172] Subsequently, a photoresist is coated on the metal layer C3 and the second silicon nitride film C7, and the metal layer C3 is exposed after development, and then baked and cured to form a protective layer C8 to protect the chip surface. The metal layer C3 is exposed on both sides of the protective layer C8 to be used as a metal electrode. The photoresist used to form the protective layer C8 should be selected from photoresists with high dielectric constant, low stress, low thermal expansion coefficient and low water absorption to achieve a good protection effect.
[0173] The gallium arsenide Hall element with the above passivation structure formed in this embodiment is less affected by the environment, and the voltage drift caused is also less than that in the prior art, as shown below:
[0174] The passivation structure disclosed in the present invention and the passivation structure in the prior art are respectively prepared for the same type of gallium arsenide Hall element, and moisture and heat resistance tests are performed on them to verify that the passivation structure disclosed in the present invention has better moisture and heat resistance than the passivation structure in the prior art.
[0175] (1) Sample Introduction
[0176] Sample A: GaAs Hall element, the surface of which is prepared with the passivation structure of the above-mentioned embodiment 3
[0177] Sample B: a gallium arsenide Hall element, the surface of which has a passivation structure prepared by the existing technology (a single-layer passivation film, a single-layer metal layer, and no photoresist protective layer);
[0178] The above-mentioned gallium arsenide Hall element samples are all made after the Hall element chip is packaged, and their packaging structure and packaging process are consistent, and the packaging test method is consistent.
[0179] (4) Experimental conditions
[0180] ①Test principle:
[0181] When the GaAs Hall element is in high temperature and high humidity conditions, if there are material defects on the surface of its packaging structure, moisture and impurities will invade the material defective part of the packaging structure, thereby affecting the electrical and structural performance of the device.
[0182] ②Purpose of the test:
[0183] Evaluate the product's ability to maintain its original performance after long-term exposure to humidity stress and temperature stress.
[0184] ③Testing instruments:
[0185] Constant temperature and humidity environmental test chamber;
[0186] ④Operational specifications:
[0187] Ⅰ. Carry out initial value test on the samples to be tested and record them one by one;
[0188] Ⅱ. Place the sample in an environmental test chamber with specified temperature and humidity;
[0189] III. After a specified period of wet heat storage (the standard time intervals are usually: 168hr, 504hr, 1000hr, and 168 hours was selected as the test time interval in this test);
[0190] IV. Take the sample out of the test chamber and let it stand at room temperature for 2 to 24 hours. Complete parameter testing and record within 48 hours of the end of the test.
[0191] Ⅴ. Compare and analyze the data before and after the test to determine whether the test has any impact on the product.
[0192] ⑤Test conditions and criteria:
[0193] Typical test conditions: test temperature T = 85 ± 3 ° C, test humidity RH = 85 ± 5%, the number of samples is 22, and the test time is 168 hours.
[0194] (5) Data comparison
[0195] The above-mentioned damp heat test was performed on sample A and sample B according to the above-mentioned test conditions and operation procedures. After 168 hours of testing, 5mA constant current drive and 6V constant voltage drive were used. Then, it was determined whether the unbalanced voltage of sample A or sample B drifted, and the number of samples with unbalanced voltage drift was counted.
[0196] According to statistics, the number of devices with unbalanced voltage drift among the 22 tested samples A is 10, and the number of devices with unbalanced voltage drift among the 22 tested samples B is 0, indicating that the gallium arsenide Hall element with a passivation structure prepared based on Example 2 has better resistance to moisture and heat.
[0197] The beneficial effects of the present invention are as follows: by setting a passivation layer composed of a multi-layer thin film, the residual stress of the passivation layer is effectively reduced, and at the same time, it has excellent compactness, moisture and heat resistance, resistance to impurity ion entry, high breakdown voltage, and strong adhesion, so that the passivation layer has a stronger suppression effect on the surface state of the compound semiconductor, and the device performance parameters and stability are better; the edges of the passivation layer and the metal layer overlap with each other, avoiding impurity ion contamination and hot ion injection at the interface between the metal layer and the passivation layer, so that the chip performance is stable and the subsequent packaged device is stable; the top layer of the device uses photoresist as the top protective layer, which can improve the reliability of the device performance.
[0198] The above are only preferred embodiments of the present invention, and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the description and illustrations of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a semiconductor passivation structure, characterized in that: A functional layer and a first metal layer are sequentially prepared on a substrate, wherein a middle portion of the first metal layer has a first notch to expose the functional layer, and further comprising: Step S1: forming a first passivation layer on the substrate, wherein the first passivation layer wraps the functional layer and the first metal layer; Step S2: removing the first passivation layer to retain the first passivation layer in the first notch and protruding from the first notch; Step S3: forming a first photoresist layer on the first passivation layer, wherein the first photoresist layer partially covers the first passivation layer; Step S4: forming a second metal layer on the first metal layer and wrapping the first passivation layer, and then removing the first photoresist layer to form a second notch on the second metal layer, wherein the second notch is located in a partial area above the first passivation layer; Step S5: forming a second passivation layer on the first passivation layer and covering the upper surface of the second metal layer; Step S6: partially removing the second passivation layer covering the upper surface of the second metal layer; Step S7: forming a protective layer on the second passivation layer, wherein the protective layer wraps the second passivation layer; The first passivation layer comprises: At least two layers of silicon dioxide film, the refractive index of the multi-layer silicon dioxide film decreases from bottom to top, the stress of the multi-layer silicon dioxide film decreases from bottom to top, and the process temperature of the multi-layer silicon dioxide film decreases from bottom to top; The second passivation layer comprises: There are at least two layers of silicon nitride film, the refractive index of the multi-layer silicon nitride film increases from bottom to top, the stress of the multi-layer silicon nitride film increases from bottom to top, and the process temperature of the multi-layer silicon nitride film decreases from bottom to top.
2. The preparation method according to claim 1, characterized in that: In the first passivation layer: The stress of the silicon dioxide film is compressive stress; The refractive index of the silicon dioxide film located at the bottom layer is greater than 1.5; The refractive index of the silicon dioxide film is in the range of 1.45-1.55; the stress range of the silicon dioxide film is -200MPa-0MPa; The BHF etching rate of the silicon dioxide film ranges from 100 nm / min to 1000 nm / min; The process temperature range of the silicon dioxide film is 300°C-350°C; The thickness of the silicon dioxide film ranges from 10 nm to 1000 nm.
3. The preparation method according to claim 1, characterized in that: In the second passivation layer: The stress of the silicon nitride film is tensile stress; The refractive index of the silicon nitride film is in the range of 1.9-2.2; The stress range of the silicon nitride film is 0-200MPa; The BHF etching rate of the silicon nitride film is in the range of 20nm / min-1000nm / min; the process temperature of the silicon nitride film is in the range of 250°C-300°C; The thickness of the silicon nitride film ranges from 100 nm to 1 μm.
4. The preparation method according to claim 1, characterized in that: The step S2 comprises: Step S21: coating a photoresist on the first passivation layer; Step S22: removing the photoresist above the first metal layer to expose a portion of the first passivation layer above the first metal layer; Step S23: etching and opening a portion of the first passivation layer above the first metal layer; Step S24: removing the photoresist and the first passivation layer above the substrate to retain the first passivation layer in the first notch and protruding from the first notch.
5. The preparation method according to claim 1, characterized in that: The step S6 comprises: Step S61: coating a photoresist on the second passivation layer; Step S62: removing a portion of the photoresist above the second metal layer to expose a portion of the second passivation layer; Step S63: etching the exposed second passivation layer to make an opening, so that a portion of the second metal layer is exposed; Step S64: removing the photoresist.
6. The preparation method according to claim 1, characterized in that: The step S7 comprises: Step S71: coating a photoresist on the second passivation layer, wherein the photoresist covers the second metal layer; Step S72: exposing a portion of the second metal layer through photolithography and developer etching processes; Step S73: curing the photoresist through a baking process to form the protective layer.
7. The preparation method according to claim 1, characterized in that: The thickness of the first metal layer and the second metal layer is 0.2 μm to 2 μm.
8. The preparation method according to claim 1, characterized in that: The length of the portion where the second metal layer overlaps the first passivation layer is between 5 μm and 100 μm.
9. The preparation method according to claim 1, characterized in that: The length of the overlapping portion of the second metal layer and the second passivation layer is between 5 μm and 100 μm.
10. The preparation method according to claim 1, characterized in that: The first passivation layer and the second passivation layer are formed by a plasma chemical vapor deposition process.