Film capacitors
By arranging a metal layer on the surface of the dielectric resin film of the film capacitor and designing a specific recessed structure, the problem in the prior art that the resin film is not easily thermally decomposed during a short circuit is solved, and a film capacitor with good self-healing properties is realized.
Patent Information
- Application Number
- CN202080046218.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-02-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-02-25
AI Technical Summary
The dielectric resin film of existing film capacitors is not easily decomposed thermally during a short circuit, resulting in insufficient self-repairability.
A metal layer is provided on the surface of the dielectric resin film, and a specific recess structure is present on the surface to ensure that there are more than 25 and less than 125 recesses with a long diameter of 30 nm or more and 800 nm or less per 5 μm × 5 μm area to improve the Thermal decomposition of resin films.
A film capacitor with good self-repairability and easy thermal decomposition of the dielectric resin film during a short circuit is realized, and the insulation recovery ability is improved.
Smart Images

Figure CN114040938B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a film capacitor and a film for the film capacitor. Background Art
[0002] As one type of capacitor, there is a film capacitor having the following structure, that is, a flexible resin film is used as a dielectric, and a first opposing electrode and a second opposing electrode are arranged opposite to each other via the resin film. Such a film capacitor is produced, for example, by winding or stacking a resin film having the first opposing electrode and a resin film having the second opposing electrode.
[0003] For example, Patent Document 1 discloses a thin film capacitor comprising: dielectric resin films arranged to overlap each other; a first opposing electrode and a second opposing electrode arranged to oppose each other via the dielectric resin film; and a first terminal electrode and a second terminal electrode electrically connected to the first opposing electrode and the second opposing electrode, respectively, wherein the surface roughness Ra of at least one main surface of the dielectric resin film is greater than or equal to 3 nm and less than or equal to 1000 nm, the dielectric resin film is configured to have a thermosetting resin with a glass transition point of greater than or equal to 130° C. as a resin component, and when the thermogravimetric change rate of the resin component is measured at a heating rate of 10° C. / min in nitrogen, the weight of a thermal decomposition residue at 500° C. is less than or equal to 40% by weight.
[0004] Prior Art Literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2013 / 069485 Summary of the invention
[0007] Problems to be solved by the invention
[0008] In the film capacitor described in Patent Document 1, the surface roughness Ra of the dielectric resin film is set to be greater than 3 nm and less than 1000 nm, so that when the dielectric resin film is wound or stacked, a small gap is formed between the overlapping films. Therefore, the decomposed gas becomes easy to fly out from the inside of the film capacitor, and the self-healing function works well.
[0009] However, since the dielectric resin film has high heat resistance, the dielectric resin film may not be thermally decomposed during a short circuit, and decomposition gas may not be dispersed. Therefore, it can be said that there is still room for improvement in self-healing properties.
[0010] The present invention is made to solve the above-mentioned problems, and its purpose is to provide a film capacitor in which a dielectric resin film is easily thermally decomposed and has good self-healing properties when a short circuit occurs. The present invention also aims to provide a film for a film capacitor used as the dielectric resin film of the above-mentioned film capacitor.
[0011] Technical solutions to solve problems
[0012] Regarding the film capacitor of the present invention, in a first embodiment, it comprises: a dielectric resin film having a first surface and a second surface opposite to each other in a thickness direction; and a metal layer provided on the first surface of the dielectric resin film, wherein on the surface of the first surface of the dielectric resin film, there are 25 or more and 125 or less first depressions having a major diameter of 30 nm or more and 800 nm or less per an area of 5 μm×5 μm.
[0013] Regarding the film capacitor of the present invention, in a second embodiment, it comprises: a dielectric resin film having a first surface and a second surface opposite to each other in the thickness direction; and a metal layer provided on the first surface of the dielectric resin film, wherein a first depression exists on the surface of the first surface of the dielectric resin film, and on the surface of the metal layer, following the first depression, there are more than 25 and less than 125 third depressions with a major diameter of more than 30 nm and less than 800 nm per an area of 5 μm×5 μm.
[0014] The film for a film capacitor of the present invention is composed of a dielectric resin film having a first surface and a second surface opposite to each other in the thickness direction, and on the surface of the first surface of the dielectric resin film, there are more than 25 and less than 125 first depressions with a long diameter of more than 30 nm and less than 800 nm per an area of 5 μm×5 μm.
[0015] Effects of the Invention
[0016] According to the present invention, it is possible to provide a film capacitor in which a dielectric resin film is easily thermally decomposed during a short circuit and which has excellent self-healing properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 FIG. 1 is a cross-sectional view schematically showing an example of a thin film capacitor of the present invention.
[0018] Figure 2 This is a cross-sectional view schematically showing an example of the film for a film capacitor of the present invention.
[0019] Figure 3 This is an example of a SEM photograph taken of the first surface of the dielectric resin film constituting the film for the film capacitor of the present invention.
[0020] Figure 4 This is an example of a SEM photograph taken of the first surface of a dielectric resin film constituting a conventional film for a film capacitor.
[0021] Figure 5 It is a top view schematically showing a method of measuring the major diameter of a depression.
[0022] Figure 6 FIG. 1 is a cross-sectional view schematically showing another example of the film for a film capacitor of the present invention.
[0023] Figure 7 This is an example of a SEM photograph taken of the second surface of the dielectric resin film constituting the film for the film capacitor of the present invention.
[0024] Figure 8 FIG. 1 is a cross-sectional view schematically showing an example of a metallized film constituting the film capacitor of the present invention.
[0025] Fig. 9 FIG. 1 is a cross-sectional view schematically showing another example of the metallized film constituting the film capacitor of the present invention.
[0026] Fig.10 FIG. 1 is a plan view schematically showing another example of the metallized film constituting the film capacitor of the present invention.
[0027] Fig.11A , Fig. 11B , Fig. 11C as well as Fig.11D It is schematically shown Figure 2 FIG. 2 is a process diagram showing an example of a method for manufacturing the film 1 for a film capacitor.
[0028] Fig. 12A , Fig. 12B as well as Fig. 12C It is schematically shown Figure 6 FIG. 2 is a process diagram showing an example of a method for manufacturing the thin film 1A for a thin film capacitor.
[0029] Fig.13A , Fig. 13B as well as Fig. 13C It is schematically shown Figure 6 FIG. 2 is a process diagram showing an example of a method for manufacturing the thin film 1A for a thin film capacitor.
[0030] Fig.14 This is a schematic diagram for explaining a method of measuring the frictional force when thin films are overlapped. DETAILED DESCRIPTION
[0031] Hereinafter, the film capacitor and the film for the film capacitor of the present invention will be described.
[0032] However, the present invention is not limited to the following configurations, and can be applied with appropriate changes within the scope of the present invention.
[0033] A combination of two or more of the preferred structures of the present invention described below also constitutes the present invention.
[0034] [Film capacitors]
[0035] A film capacitor of the present invention comprises: a dielectric resin film having a first surface and a second surface facing each other in a thickness direction; and a metal layer provided on the first surface of the dielectric resin film.
[0036] Hereinafter, as one embodiment of the film capacitor of the present invention, a wound film capacitor is described as an example, wherein a first dielectric resin film having a first metal layer and a second dielectric resin film having a second metal layer are wound in a stacked state. The film capacitor of the present invention may also be a stacked film capacitor, etc., in which a first dielectric resin film having a first metal layer and a second dielectric resin film having a second metal layer are stacked.
[0037] Figure 1 FIG. 1 is a cross-sectional view schematically showing an example of a thin film capacitor of the present invention.
[0038] Figure 1 The film capacitor 100 shown is a wound film capacitor, which is formed by winding a first metalized film 130 having a first metal layer (counter electrode) 120 provided on one surface of a first dielectric resin film 110 and a second metalized film 160 having a second metal layer (counter electrode) 150 provided on one surface of a second dielectric resin film 140. The film capacitor 100 further includes a first external terminal electrode 170 electrically connected to the first metal layer 120 and a second external terminal electrode 180 electrically connected to the second metal layer 150.
[0039] First metal layer 120 is formed to reach one side edge of first metalized film 130 but not to reach the other side edge. On the other hand, second metal layer 150 is formed to reach the other side edge but not to reach one side edge of second metalized film 160. First metal layer 120 and second metal layer 150 include, for example, aluminum, zinc, or the like.
[0040] The first metalized film 130 and the second metalized film 160 are wound and stacked. Figure 1As shown, the first metallized film 130 and the second metallized film 160 are offset from each other in the width direction, so that the end of the first metal layer 120 on the side reaching the side edge of the first metallized film 130 and the end of the second metal layer 150 on the side reaching the side edge of the second metallized film 160 are exposed.
[0041] exist Figure 1 In the illustrated film capacitor 100 , first metallized film 130 is wound outside second metallized film 160 , and first metal layer 120 and second metal layer 150 are respectively oriented inward in each of first metallized film 130 and second metallized film 160 .
[0042] The first external terminal electrode 170 and the second external terminal electrode 180 are formed by thermally spraying, for example, zinc, on each end surface of the capacitor body obtained as described above. The first external terminal electrode 170 is in contact with the exposed end portion of the first metal layer 120, thereby being electrically connected to the first metal layer 120. On the other hand, the second external terminal electrode 180 is in contact with the exposed end portion of the second metal layer 150, thereby being electrically connected to the second metal layer 150.
[0043] The film capacitor of the present invention is preferably pressed into a flat shape such as an ellipse or an oblong cross-sectional shape, thereby being set to a more compact shape than when the cross-sectional shape is a perfect circle. The film capacitor of the present invention may also have a cylindrical winding shaft. The winding shaft is arranged on the central axis of the wound metallized film and becomes the winding shaft when the metallized film is wound.
[0044] In the film capacitor of the present invention, the film for film capacitor of the present invention is used as the dielectric resin film. Figure 1 In the illustrated film capacitor 100 , the film for a film capacitor of the present invention may be used for both the first dielectric resin film 110 and the second dielectric resin film 140 , or may be used for only one of them.
[0045] [Film for film capacitors]
[0046] Figure 2 This is a cross-sectional view schematically showing an example of the film for a film capacitor of the present invention.
[0047] Figure 2 The film 1 for film capacitor shown is composed of a dielectric resin film 10. The dielectric resin film 10 has a first surface 11 and a second surface 12 which are opposite to each other in the thickness direction. On the surface of the first surface 11 of the dielectric resin film 10, there is a depression 41 as a first depression. On the other hand, on the surface of the second surface 12 of the dielectric resin film 10, there is no depression 41.
[0048] The depressions present on the first surface of the dielectric resin film can be confirmed by observing the first surface of the dielectric resin film using a scanning electron microscope (SEM). In the SEM photograph, the black-looking portions are judged to be depressions.
[0049] Figure 3 This is an example of a SEM photograph taken of the first surface of the dielectric resin film constituting the film for the film capacitor of the present invention.
[0050] exist Figure 3 In FIG. 1 , it can be confirmed that the depression 41 exists on the first surface 11 of the dielectric resin film 10 .
[0051] Figure 4 This is an example of a SEM photograph taken of the first surface of a dielectric resin film constituting a conventional film for a film capacitor.
[0052] exist Figure 4 In the figure, it can be confirmed that there is no depression 41 on the first surface 11 of the dielectric resin film 10a.
[0053] The film for a film capacitor of the present invention is characterized in that among the depressions existing on the surface of the first surface of the dielectric resin film, there are 25 or more and 125 or less first depressions having a major diameter of 30 nm to 800 nm per an area of 5 μm×5 μm.
[0054] The number of first depressions can be obtained by observing random positions on the surface of the first surface of the dielectric resin film with a SEM at a magnification of 30,000 times and counting the number of depressions having a major diameter of 30 nm to 800 nm in an observation field of 5 μm×5 μm.
[0055] Figure 5 It is a top view schematically showing a method of measuring the major diameter of a depression.
[0056] like Figure 5 As shown in FIG. 1 , when the depression 41 is observed in the thickness direction of the dielectric resin film, the length of the most diagonally spaced portion is defined as the major diameter D of the depression 41. The same applies to the measurement of the major diameters of other depressions described later.
[0057] Figure 6 FIG. 1 is a cross-sectional view schematically showing another example of the film for a film capacitor of the present invention.
[0058] Figure 6The film capacitor film 1A shown is composed of a dielectric resin film 10A. A first depression 41A exists on the first surface 11 of the dielectric resin film 10A as a first depression. On the other hand, a depression 42 exists on the second surface 12 of the dielectric resin film 10A as a second depression.
[0059] Regarding the recess 41A, in addition to Figure 2 In addition to the depressions of the same size as the depression 41 shown, there are also depressions of the same size as the depression 42. In addition, on the surface of the first surface 11 of the dielectric resin film 10A, there may be a first depression Figure 2 The depression 41 is shown.
[0060] The depressions present on the second surface of the dielectric resin film can be confirmed by observing the second surface of the dielectric resin film using a scanning electron microscope (SEM). In the SEM photograph, the black-looking portions are judged to be depressions.
[0061] Figure 7 This is an example of a SEM photograph taken of the second surface of the dielectric resin film constituting the film for the film capacitor of the present invention.
[0062] exist Figure 7 In FIG. 1 , it can be confirmed that the depression 42 exists on the second surface 12 of the dielectric resin film 10A.
[0063] In the film capacitor film of the present invention, preferably, among the depressions existing on the second surface of the dielectric resin film, there are 3 or more and 11 or less second depressions having a major diameter of 100 nm to 800 nm per an area of 13 μm×13 μm.
[0064] The number of the second depressions can be obtained by observing random positions on the surface of the second surface of the dielectric resin film with a SEM at a magnification of 10,000 times and counting the number of depressions having a major axis of 100 nm to 800 nm in an observation field of 13 μm×13 μm.
[0065] In the film for a film capacitor of the present invention, the glass transition point of the dielectric resin film is preferably 160° C. or higher and 190° C. or lower. In this case, the heat resistance of the film capacitor can be improved.
[0066] In this specification, the glass transition point of a dielectric resin film means the temperature at which the loss tangent (tanδ) expressed as loss modulus / storage modulus shows a maximum peak when the storage modulus and loss modulus are measured by a dynamic viscoelasticity measuring apparatus (DMA).
[0067] In the film for film capacitors of the present invention, the weight of thermal decomposition residue when the dielectric resin film is heated to 500° C. in a nitrogen atmosphere (hereinafter, also referred to as the thermal decomposition residue weight of the dielectric resin film) is preferably less than 20% by weight. In this case, the dielectric resin film is easily thermally decomposed, and thus can be used as a film capacitor with good self-healing properties. More preferably, the thermal decomposition residue weight of the dielectric resin film is less than 10% by weight.
[0068] In this specification, the so-called thermal decomposition residue weight of the dielectric resin film means the residue weight (%) at 500°C measured by heating the dielectric resin film from room temperature to 600°C at a heating rate of 5°C / min in a nitrogen atmosphere using a differential thermal gravimetric analysis device (TG-DTA).
[0069] In the film for a film capacitor of the present invention, the dielectric resin film preferably contains a curable resin as a main component.
[0070] In this specification, the term "main component" means a component with the largest weight percentage, preferably a component with a weight percentage exceeding 50% by weight. Therefore, the dielectric resin film may contain additives such as silicone resin, uncured portions of starting materials such as the first organic material and the second organic material described later, as components other than the main component.
[0071] The curable resin may be a thermosetting resin or a photocurable resin.
[0072] In this specification, the so-called thermosetting resin means a resin that can be cured by heat, and the curing method is not limited. Therefore, as long as it is a resin that can be cured by heat, a resin that is cured by methods other than heat (for example, light, electron beam, etc.) is also included in the thermosetting resin. In addition, depending on the material, there is a situation where the reaction begins due to the reactivity of the material itself, and for materials that do not necessarily need to be provided with heat or light from the outside to promote curing, they are also considered thermosetting resins. The same is true for photocurable resins, and the curing method is not limited.
[0073] The curable resin preferably includes a cured product of the first organic material and the second organic material. For example, a cured product obtained by reaction between a hydroxyl group (OH group) of the first organic material and an isocyanate group (NCO group) of the second organic material can be mentioned.
[0074] When a cured product is obtained by the above-mentioned reaction, there may be a case where an uncured portion of the starting material remains in the film. For example, the dielectric resin film may also contain at least one of a hydroxyl group and an isocyanate group. In this case, the dielectric resin film may contain either a hydroxyl group or an isocyanate group, or both of them.
[0075] In addition, the presence of a hydroxyl group and / or an isocyanate group can be confirmed by Fourier transform infrared spectrophotometer (FT-IR).
[0076] The first organic material preferably includes a phenoxy resin.
[0077] The second organic material preferably includes diphenylmethane diisocyanate, a modified diphenylmethane diisocyanate, or a mixture thereof, and preferably includes 4,4′-diphenylmethane diisocyanate, a modified 4,4′-diphenylmethane diisocyanate, or a mixture thereof.
[0078] The dielectric resin film may also contain additives for adding other functions. For example, smoothness can be imparted by adding a leveling agent. The additive is more preferably a material having a functional group that reacts with a hydroxyl group and / or an isocyanate group, forming a part of the cross-linked structure of the cured product. As such a material, for example, a resin having at least one functional group selected from the group consisting of a hydroxyl group, an epoxy group, a silanol group, and a carboxyl group can be cited.
[0079] The thickness of the dielectric resin film is not particularly limited, but is preferably 1 μm or more and 5 μm or less.
[0080] The thickness of the dielectric resin film referred to here means the thickness measured at a position where no depression exists on the surface.
[0081] In addition, the thickness of the dielectric resin film can be measured using an optical film thickness meter.
[0082] The film for a film capacitor of the present invention is formed into a metalized film by providing a metal layer on the first surface of a dielectric resin film, thereby constituting the film capacitor of the present invention.
[0083] Figure 8 FIG. 1 is a cross-sectional view schematically showing an example of a metallized film constituting the film capacitor of the present invention.
[0084] Figure 8 The metallized film 30 shown has Figure 2The dielectric resin film 10 shown in FIG. 1 and the metal layer 20 provided on the first surface of the dielectric resin film 10. As described above, the first surface 11 of the dielectric resin film 10 has a depression 41 as a first depression. On the other hand, the second surface 12 of the dielectric resin film 10 does not have the depression 41. Furthermore, the depression 43 as a third depression exists on the surface of the metal layer 20 following the depression 41.
[0085] The depressions present on the surface of the metal layer can be confirmed by observing the surface of the first surface of the dielectric resin film with a scanning electron microscope (SEM) in a state where the metal layer is provided.
[0086] In the film capacitor of the present invention, in the first mode, it is characterized in that among the depressions existing on the surface of the first surface of the dielectric resin film, there are 25 or more and 125 or less first depressions having a major diameter of 30 nm to 800 nm per an area of 5 μm×5 μm.
[0087] Since the first depression having a long diameter of 30 nm or more and 800 nm or less exists on the surface of the first surface of the dielectric resin film, the dielectric resin film becomes easy to be thermally decomposed when heat is applied to the dielectric resin film. When insulation breakdown occurs at a certain point of the dielectric resin film during use of the film capacitor, the dielectric resin film generates heat due to the current flowing through the portion. If the dielectric resin film is easy to be thermally decomposed, the dielectric resin film is thermally decomposed due to the heat generated by the current, thereby the portion of insulation breakdown disappears and the insulation of the dielectric resin film is restored. Therefore, it can be set as a film capacitor with good self-healing properties.
[0088] In the thin film capacitor of the present invention, in the first aspect, preferably, on the surface of the metal layer, following the first depressions, 25 or more and 125 or less third depressions having a major diameter of 30 nm to 800 nm are present per an area of 5 μm×5 μm.
[0089] In addition, in the film capacitor of the present invention, in the second mode, it is characterized in that there is a first depression on the surface of the first surface of the dielectric resin film, and on the surface of the metal layer, following the first depression, there are more than 25 and less than 125 third depressions with a long diameter of more than 30nm and less than 800nm per area of 5μm×5μm.
[0090] Since the third depression having a major diameter of 30 nm to 800 nm exists on the surface of the metal layer following the first depression, the dielectric resin film is easily thermally decomposed when heat is applied to the dielectric resin film, thereby providing a film capacitor with excellent self-healing properties.
[0091] The number of the third depressions can be obtained by observing random positions on the surface of the first surface of the dielectric resin film at a magnification of 30,000 times using an SEM in a state where a metal layer is provided, and counting the number of depressions having a major diameter of greater than 30 nm and less than 800 nm in an observation field of view of 5 μm×5 μm.
[0092] Hereinafter, when the first embodiment and the second embodiment are not particularly distinguished, they are simply referred to as “film capacitors of the present invention”.
[0093] Fig. 9 FIG. 1 is a cross-sectional view schematically showing another example of the metallized film constituting the film capacitor of the present invention.
[0094] Fig. 9 The metallized film 30A shown has Figure 6 1 and a metal layer 20A provided on the first surface of the dielectric resin film 10A. As described above, the first surface 11 of the dielectric resin film 10A has a depression 41A as a first depression. On the other hand, the second surface 12 of the dielectric resin film 10A has a depression 42 as a second depression. Furthermore, the surface of the metal layer 20A has a depression 43A as a third depression following the depression 41A.
[0095] In addition, the surface of the first surface 11 of the dielectric resin film 10A may also be Figure 8 Similarly, the depression 41 exists as the first depression. In this case, a depression 43 exists as the third depression following the depression 41 on the surface of the metal layer 20A.
[0096] In the film capacitor of the present invention, preferably, among the depressions existing on the second surface of the dielectric resin film, there are 3 or more and 11 or less second depressions having a major diameter of 100 nm to 800 nm per an area of 13 μm×13 μm.
[0097] By providing the second depressions having a major diameter of 100 nm or more and 800 nm or less on the second surface of the dielectric resin film, the surface of the dielectric resin film is provided with depressions and projections, and the friction coefficient is reduced, thereby improving the sliding property of the dielectric resin film. As a result, compared with a case where the surface of the dielectric resin film is smooth, the operability of the film in conveying and winding is improved.
[0098] In the film capacitor of the present invention, a fuse portion is preferably provided in the metal layer.
[0099] The so-called fuse part means a portion where the electrode part and the electrode part are connected by dividing the metal layer that will become the opposing electrode into a plurality of electrodes. The pattern of the metal layer having the fuse part is not particularly limited, and for example, the electrode patterns disclosed in Japanese Patent Publication No. 2004-363431 and Japanese Patent Publication No. 5-251266 can be used.
[0100] Fig.10 FIG. 1 is a plan view schematically showing another example of the metallized film constituting the film capacitor of the present invention.
[0101] exist Fig.10 In the illustrated metalized film 30B, a fuse portion 21 a in which a portion of an electrode is thinned and divided electrodes 21 c divided by insulating slits 21 b are provided on a metal layer 20B provided on one surface of a dielectric resin film 10B.
[0102] In the film capacitor of the present invention, the fuse portion preferably overlaps with the third recess in the thickness direction.
[0103] Since the third recess is provided at a position overlapping with the fuse portion of the metal layer, the fuse portion is further thinned, and thus the reliability of the fuse operation at the time of dielectric breakdown can be improved.
[0104] For example, in Figure 1 In the thin film capacitor 100 shown, when the fuse part is provided on both the first metal layer 120 and the second metal layer 150, the fuse part provided on both metal layers may overlap with the third recess in the thickness direction, or the fuse part provided on either metal layer may overlap with the third recess in the thickness direction. In addition, the fuse part may be provided on either the first metal layer 120 or the second metal layer 150, and the fuse part may overlap with the third recess in the thickness direction.
[0105] In the film capacitor of the present invention, examples of the metal contained in the metal layer include aluminum and zinc.
[0106] When the material constituting the metal layer is aluminum or zinc, good bonding properties with the external terminal electrodes can be maintained.
[0107] The thickness of the metal layer is not particularly limited, but is preferably 5 nm or more and 50 nm or less.
[0108] The thickness of the metal layer can be determined by observing a cross section of the metallized thin film cut in the thickness direction using an electron microscope such as a field emission scanning electron microscope (FE-SEM).
[0109] [Method for producing film for film capacitor]
[0110] Hereinafter, a method for producing a thin film for a thin film capacitor of the present invention will be described.
[0111] Fig.11A , Fig. 11B , Fig. 11C as well as Fig.11D It is schematically shown Figure 2 FIG. 2 is a process diagram showing an example of a method for producing the film 1 for a film capacitor.
[0112] First, if Fig.11A As shown, the resin solution 15 a is applied to the coating surface of the base film 70 .
[0113] As the base film 70 , for example, a polyethylene terephthalate (PET) film, a polypropylene (PP) film, or the like can be used.
[0114] The resin solution 15a is prepared, for example, by dissolving the first organic material and the second organic material in a solvent and mixing them, and adding additives as needed. In addition, the solvent contained in the resin solution may also exist as a residue in the film after curing. The weight ratio of the first organic material to the second organic material (first organic material / second organic material) is preferably 50 / 50 or more and 75 / 25 or less.
[0115] As the solvent, a mixed solvent containing methyl ethyl ketone (MEK) and tetrahydrofuran (THF) is preferably used. The weight ratio of MEK to THF (MEK / THF) is preferably 15 / 85 or more and 85 / 15 or less.
[0116] After the resin solution 15a is applied to the base film 70, hot air is preferably blown within 10 seconds to dry the solvent. Fig. 11B As shown, the surface of the resin solution 15a is cured, and a coating 15b is formed on the surface of the resin solution 15a.
[0117] If the drying is continued further, since the film 15b is formed on the surface of the resin solution 15a, the solvent in the resin solution 15a is volatilized and discharged from the inside, and the discharge channel of the gas remains as a hole. Fig. 11C As shown, depressions 41 are formed on the surface of the first surface 11, which is the dried surface. After drying, the resin is cured by heat treatment, and the dielectric resin film 10 is formed.
[0118] Then, the dielectric resin film 10 is peeled off from the base film 70. Fig.11D As shown, a film 1 for a film capacitor having depressions 41 on the surface of the first surface 11 of the dielectric resin film 10 is obtained.
[0119] Fig. 12A , Fig. 12B as well as Fig. 12C and Fig.13A , Fig. 13B as well as Fig. 13C It is schematically shown Figure 6 FIG. 2 is a process diagram showing an example of a method for manufacturing the thin film 1A for a thin film capacitor.
[0120] First, if Fig. 12A As shown, the resin solution 15a is applied to the coating surface of the base film 70A.
[0121] The base film 70A has particles 71 such as silica particles inside and on the surface thereof, and the particles 71 are attached to both surfaces thereof. The base film 70A is preferably a film in which the particles 71 are kneaded into a polypropylene film and the particles 71 are attached to both surfaces thereof.
[0122] As the particles 71, inorganic particles are preferably used, and silica particles are more preferably used. The average particle diameter of the particles 71 is preferably 0.1 μm or more and 0.4 μm or less.
[0123] After the resin solution 15a is applied to the base film 70A, hot air is preferably blown within 10 seconds to dry the solvent. Fig. 12B As shown, the surface of the resin solution 15a is cured, and a coating 15b is formed on the surface of the resin solution 15a.
[0124] If the drying is continued further, since the film 15b is formed on the surface of the resin solution 15a, the solvent in the resin solution 15a is volatilized and discharged from the inside, and the discharge channel of the gas remains as a hole. Fig. 12C As shown, depressions 41 are formed on the surface of the first surface 11, which is the dried surface. After drying, the resin is cured by heat treatment to form the dielectric resin film 10A.
[0125] Then, if Fig.13A As shown in FIG. 1 , a step of rolling up the coated film in which the dielectric resin film 10A is formed on the base film 70A is performed. Fig.13A In FIG. , the winding direction is shown by an arrow.
[0126] When the coated film is rolled up, the adjacent base film 70A contacts the first surface 11 of the dielectric resin film 10A. Since the particles 71 are attached to both surfaces of the base film 70A, the particles 71 also contact the first surface 11 of the dielectric resin film 10A.
[0127] Then, the coated film is unwound by rotating it in the opposite direction to the winding direction. Thus, the shape of the particles 71 is transferred to the first surface 11 of the dielectric resin film 10A. As a result, Fig. 13B As shown in FIG. 1 , a depression 41A is formed on the surface of the first surface 11 of the dielectric resin film 10A.
[0128] Then, the dielectric resin film 10A is peeled off from the base film 70A. Thus, the shape of the particles 71 is transferred to the second surface 12 of the dielectric resin film 10A. As a result, Fig. 13C As shown, a film 1A for a thin-film capacitor having depressions 41A on the surface of the first surface 11 of the dielectric resin film 10A and depressions 42 on the surface of the second surface 12 can be obtained.
[0129] In the above example, the step of rolling up the coated film is performed in a state where the resin is cured by heat treatment to form the dielectric resin film 10A, but the step of rolling up the coated film may be performed until the solvent is dried. In this case, after the coated film is unwound by rotating it in the opposite direction to the winding direction, the resin is cured by heat treatment to form the dielectric resin film 10A.
[0130] Alternatively, you may not Fig.13A After the dielectric resin film 10A is formed, the dielectric resin film 10A is peeled off from the base film 70A by the step of rolling up the coated film as shown. In this case, a film for a film capacitor having depressions 41 on the surface of the first surface 11 of the dielectric resin film 10A and depressions 42 on the surface of the second surface 12 can be obtained.
[0131] In addition, even when the base film 70 is used, Fig.13A The process of rolling up the coated film is shown.
[0132] [Manufacturing method of film capacitor]
[0133] Next, a method for manufacturing the film capacitor of the present invention will be described.
[0134] First, a metal layer is formed on the first surface of the dielectric resin film of the film capacitor of the present invention to obtain a metallized film. Examples of methods for forming the metal layer on the first surface of the dielectric resin film include vapor deposition and the like.
[0135] For example, Fig. 11CAs shown in FIG. 1 , in a state where the dielectric resin film 10 is formed on the base film 70, the metal layer 20 can be formed on the surface of the dielectric resin film 10 by performing vapor deposition or the like on the surface of the dielectric resin film 10 on the opposite side to the base film 70. The surface provided with the metal layer 20 thus becomes the first surface 11 of the dielectric resin film 10, and the surface on the base film 70 side becomes the second surface 12 of the dielectric resin film 10. The metallized film obtained by peeling off the base film 70 after the above-mentioned process is Figure 8 The metallized film 30 is shown.
[0136] Or, if Fig. 13B As shown in FIG. 1 , in a state where the dielectric resin film 10A is formed on the base film 70A, the metal layer 20A can be formed on the surface of the dielectric resin film 10A by performing vapor deposition or the like on the surface of the dielectric resin film 10A on the opposite side to the base film 70A. The surface provided with the metal layer 20A thus becomes the first surface 11 of the dielectric resin film 10A, and the surface on the base film 70A side becomes the second surface 12 of the dielectric resin film 10A. The metallized film obtained by peeling off the base film 70A after the above-mentioned process is Fig. 9 The metallized film 30A is shown.
[0137] Alternatively, after the dielectric resin film is peeled off from the base film, the metal layer may be formed on the first surface of the dielectric resin film.
[0138] Two such metallized films are stacked in a state where they are offset by a predetermined distance in the width direction and then rolled up to obtain a laminated body. The laminated body may also be sandwiched in a direction perpendicular to the width direction and pressed into an elliptical cylindrical shape as required.
[0139] Next, external terminal electrodes are formed on the end faces of the laminate to obtain Figure 1 As a method of forming external terminal electrodes on the end faces of the laminate, thermal spraying can be cited.
[0140] Example
[0141] Hereinafter, examples are shown which more specifically disclose the film capacitor and the film for the film capacitor of the present invention. However, the present invention is not limited to these examples.
[0142] (Example 1)
[0143] [Production of film for film capacitors]
[0144] A mixture of a phenoxy resin as a first organic material and 4,4'-diphenylmethane diisocyanate (MDI) and a modified product thereof as a second organic material was dissolved in a mixed solvent of methyl ethyl ketone (MEK) and tetrahydrofuran (THF) (MEK / THF=85 / 15 (weight ratio)) and mixed, and further, a silicone surface conditioner BYK370 (manufactured by BYK Chemical (Japan) Co., Ltd.) was added to prepare a coating composition (resin solution). The weight ratio of the first organic material to the second organic material (first organic material / second organic material) was set to 70 / 30.
[0145] The coating composition was applied to a PET film as a substrate film, and 4.5 seconds after the coating, hot air at 70°C was blown to dry the solvent, forming a film with a thickness of 3 μm. After drying, the coated film was rolled up. Then, the rolled coated film was rotated in the opposite direction to the winding direction and unfolded, and then, the dielectric resin film was cured by heat treatment at 150°C for 4 hours. Furthermore, the dielectric resin film was peeled off from the PET film, thereby preparing a film for a film capacitor of Example 1. The surface opposite to the PET film is the first surface, and the surface on the PET film side is the second surface.
[0146] [Manufacturing of film capacitors]
[0147] A thin film for a thin film capacitor was formed on a PET film by the same method as above. Aluminum was vapor-deposited on the first surface of the thin film capacitor film to a thickness of 20 nm, and then the film was peeled off from the PET film to obtain a metallized film.
[0148] Next, the peeled metallized film was cut into a given width, and then two metallized films were overlapped and wound up by a winder. The obtained cylindrical wound body was pressed into an elliptical shape, and then zinc was metallized on the end surface to form a terminal electrode, and the terminal electrode was connected to the opposite electrode, thereby manufacturing the film capacitor of Example 1.
[0149] [Preparation of samples for self-healing evaluation]
[0150] A terminal conductor was attached to the terminal electrode of the film capacitor of Example 1, and then the wound body was sealed with resin to prepare a sample for evaluating self-healing properties.
[0151] (Example 2)
[0152] A polypropylene film (manufactured by Toray Co., Ltd.: TORAYFAN, 12 μm thick) having silica particles with an average particle size of 0.1 μm (particle size distribution of 0.04 μm to 0.3 μm) and an average particle size of 0.4 μm (particle size distribution of 0.2 μm to 0.6 μm) attached to the surface was used as the substrate film. Except for this, a film for film capacitors, a film capacitor, and a sample for self-healing evaluation were prepared in the same manner as in Example 1.
[0153] (Comparative Example 1)
[0154] A polyvinyl acetoacetal (PVAA) resin as the first organic material and a modified toluene diisocyanate (TDI) as the second organic material were dissolved in MEK and mixed, and a silicone surface conditioner BYK370 was added to prepare a coating composition. In addition, a film for a film capacitor, a film capacitor, and a sample for self-healing evaluation were prepared in the same manner as in Example 1.
[0155] (Comparative Example 2)
[0156] A film for a film capacitor, a film capacitor, and a sample for evaluating self-healing properties were prepared in the same manner as in Example 1 except that polyarylate (UNIFINER, manufactured by Unitika) as a thermoplastic resin was dissolved in THF to prepare a coating composition.
[0157] (Comparative Example 3)
[0158] A phenoxy resin as the first organic material and a mixture of 4,4'-MDI and its modified product as the second organic material were dissolved in MEK and mixed, and a silicone surface conditioning agent BYK370 was further added to prepare a coating composition. The coating composition was applied to a PET film, and a hot air of 70°C was blown 11 seconds after the application to dry the solvent. A film for a film capacitor, a film capacitor, and a sample for evaluating self-healing properties were prepared in the same manner as in Example 1.
[0159] [Glass transition point]
[0160] The glass transition point of the film for the film capacitor of each embodiment and comparative example was measured. The above-mentioned heat-cured film was peeled off from the base film, and the glass transition point was measured using a dynamic viscoelasticity measuring device (RSA-III manufactured by TA Instruments). The measurement conditions were to increase the temperature from room temperature to 250°C at a heating rate of 10°C / min, set the measurement frequency to 10 rad / sec, set the tension (strain) to 0.1%, and calculate it based on the loss tangent (tanδ).
[0161] [Thermal decomposition residue]
[0162] The weight of the thermal decomposition residue of the film for the film capacitor of each embodiment and comparative example was measured. The above-mentioned heat-cured film was peeled off from the base film, and the temperature was raised from room temperature to 600°C at a rate of 5°C / min in a nitrogen atmosphere using a differential thermal gravimetric simultaneous measuring device, and the weight (%) of the residue at 500°C was measured.
[0163] [Number of depressions]
[0164] The number of depressions on the surface of the first and second surfaces of the thin film capacitors of each embodiment and comparative example was measured. The above-mentioned thermally cured film was peeled off from the base film, and the first surface was observed with a SEM at a magnification of 30,000 times, and the number of depressions with a long diameter of more than 30nm and less than 800nm was counted in the observation field of 5μm×5μm (recorded as "5μm□" in Table 1). The second surface was observed with a SEM at a magnification of 10,000 times, and the number of depressions with a long diameter of more than 100nm and less than 800nm was counted in the observation field of 13μm×13μm (recorded as "13μm□" in Table 1).
[0165] In addition, regarding Example 1, the surface of the metallized film peeled off from the base film was also observed by SEM at a magnification of 30,000 times, and the number of depressions with a major diameter of 30 nm or more and 800 nm or less in the observation field of 5 μm×5 μm was counted. As a result, even in the state where the metal layer was vapor-deposited, depressions were confirmed on the surface of the first side of the film, and the number of depressions was the same as that existing on the surface of the first side of the film.
[0166] [Self-repairing]
[0167] For the samples for self-healing evaluation of each embodiment and comparative example, DC1500V was applied at 125°C and the voltage state was observed, and it was evaluated whether the applied voltage would be restored to the original applied voltage even if the applied voltage dropped instantly during insulation breakdown. For each of the five samples, if all samples were restored, the self-healing property was evaluated as 0 (good), if more than one and less than four samples were restored, the self-healing property was evaluated as △ (acceptable), and if all samples were not restored, the self-healing property was evaluated as × (unacceptable).
[0168] [Table 1]
[0169]
[0170] As shown in Table 1, Examples 1 and 2 in which depressions with a major diameter of 30 nm to 800 nm were present on the first surface of the thin film had superior self-healing properties compared to Comparative Examples 1 to 3.
[0171] Although not shown in Table 1, in Example 2 in which depressions with a major diameter of 100 nm to 800 nm were present on the second surface of the film, the slidability when the films were overlapped was improved compared to Example 1.
[0172] In addition, the sliding property when the films were stacked on each other was evaluated by measuring the friction force by the following method.
[0173] Fig.14 This is a schematic diagram for explaining a method of measuring the frictional force when thin films are overlapped.
[0174] The film 211 peeled off from the substrate is placed on the support table 220 so that the first surface is at the top. Next, the film 212 peeled off from the substrate is overlapped so that the second surface is in contact with the first surface of the film 211. Furthermore, a 200g weight 230 is placed on the film 212. The film 212 and the weight 230 are fixed. The weight 230 is pulled horizontally at a speed of 150mm / min, and the force applied at this time is measured using a dynamometer 240 (manufactured by IMADA Co., Ltd., a digital dynamometer).
[0175] Description of Reference Numerals
[0176] 1. 1A: Film for film capacitors;
[0177] 10, 10A, 10B, 10a: dielectric resin film;
[0178] 11: first surface of dielectric resin film;
[0179] 12: The second side of the dielectric resin film;
[0180] 15a: resin solution;
[0181] 15b: coating;
[0182] 20, 20A, 20B: metal layer;
[0183] 21a: Fuse section;
[0184] 21b: insulation slit;
[0185] 21c: split electrode;
[0186] 30, 30A, 30B: metallized film;
[0187] 41, 41A, 42, 43, 43A: concave;
[0188] 70, 70A: substrate film;
[0189] 71: Particles;
[0190] 100: Film capacitor;
[0191] 110: a first dielectric resin film;
[0192] 120: 1st metal layer;
[0193] 130: 1st metallized film;
[0194] 140: a second dielectric resin film;
[0195] 150: 2nd metal layer;
[0196] 160: 2nd metallized film;
[0197] 170: first external terminal electrode;
[0198] 180: second external terminal electrode;
[0199] 211, 212: film;
[0200] 220: support platform;
[0201] 230: weights;
[0202] 240: Dynamometer;
[0203] D: long diameter of the depression.
Claims
1. A film capacitor comprising: a dielectric resin film having a first surface and a second surface facing each other in a thickness direction; and a metal layer disposed on the first surface of the dielectric resin film, in, On the surface of the first surface of the dielectric resin film, there are 25 or more and 125 or less first depressions having a major diameter of 30 nm or more and 800 nm or less per an area of 5 μm×5 μm, On the surface of the metal layer, following the first depression, there are 25 or more and 125 or less third depressions having a major diameter of 30 nm or more and 800 nm or less per an area of 5 μm×5 μm, A fuse portion is provided on the metal layer, The fuse portion overlaps with the third recess in the thickness direction.
2. The film capacitor according to claim 1, wherein: On the surface of the second surface of the dielectric resin film, three or more and 11 or less second depressions having a major diameter of 100 nm to 800 nm exist per an area of 13 μm×13 μm.
3. The film capacitor according to claim 1 or 2, wherein: The glass transition point of the dielectric resin film is 160° C. or higher and 190° C. or lower. The weight of the thermal decomposition residue of the dielectric resin film when heated to 500° C. in a nitrogen atmosphere is less than 20 weight %.
4. The film capacitor according to claim 1 or 2, wherein: The dielectric resin film contains a curable resin as a main component, and the curable resin contains a cured product of a first organic material and a second organic material. The first organic material includes a phenoxy resin, The second organic material includes diphenylmethane diisocyanate, a modified diphenylmethane diisocyanate, or a mixture thereof.
Citation Information
Patent Citations
Film capacitor and metallized film thereof
JP1993251266A
Metalized film capacitor
JP2004363431A
Film capacitor, capacitor module, and power converter
WO2013069485A1
Production of metallized polypropylene film for capacitor
JP1992088160A
Film capacitor, film for film capacitor, method for manufacturing film for film capacitor, and method for manufacturing film capacitor
WO2019069540A1