Flashing carbon coating on active surface, method of making the same and articles containing the same

By applying a pulse voltage on the electroactive particles, the carbon-adhesive particles are converted into graphite-adhesive particles, and the problem of time and high temperature in the prior art is solved, and a safer and more efficient graphite coating manufacturing is achieved.

CN114068928BActive Publication Date: 2024-11-01GM GLOBAL TECHNOLOGY OPERATIONS LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110494201.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-07
Filing Date
2021-05-07
Publication Date
2024-11-01
Estimated Expiration
2041-05-07

AI Technical Summary

Technical Problem

The existing graphite carbon conformal coating manufacturing method takes a long time, uses high temperature and flammable precursors, and is not friendly to electroactive particles, and has scalability problems.

Method used

By mixing electroactive particles with carbonaceous materials, applying pulse voltage to convert carbon-adhesive particles into graphite-adhesive particles, local Joule heating method is used to avoid high temperatures and long-term cycles, use multiple carbon sources and form graphite on electroactive substrates layer.

Benefits of technology

A shorter time and safer processing process is achieved, the processing volume and scalability are improved, the damage to the electroactive particles by high temperature is avoided, and an efficient graphite coating can be formed on the electroactive substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114068928B_ABST
    Figure CN114068928B_ABST
Patent Text Reader

Abstract

Disclosed herein is a method comprising mixing electroactive particles with a carbonaceous material to form a particle mixture including carbon-attached particles; applying a pulse voltage to the carbon-attached particles between parallel plate electrodes or between rollers of a rolling mill; and converting the carbon-attached particles into graphite-attached particles by localized Joule heating. Also disclosed herein is an apparatus comprising a mixing device operable to mix the electroactive particles with the carbonaceous material to form a particle mixture including carbon-attached particles; and a device for applying a pulse voltage to the particle mixture; applying the pulse voltage when the particle mixture is located between opposing plate electrodes or between opposing rollers of a rolling mill; and the device for applying the pulse voltage converts the carbon-attached particles into graphite-attached particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a flash carbon coating for an active surface, a method for making the same, and an article containing the same. In particular, the present disclosure relates to a graphite coating for an active surface, a method for making the same, and an article containing the same. Background Art

[0002] Graphitic carbon conformal coatings of electroactive particles in certain types of anodes have been shown to increase the durability and capacity retention of cells (e.g., batteries and capacitors). Carbon coatings (in graphitic form) are currently produced by chemical vapor deposition, in which organic precursors react at high temperatures and are deposited on the surface of the electroactive particles.

[0003] However, these currently used methods are time-consuming, use high temperatures (above 1500°C), use flammable precursors (which are not always environmentally friendly), and have scalability issues. The high temperatures used in the chemical vapor deposition process can sometimes damage the electroactive particles.

[0004] Therefore, it is desirable to develop a new technology that achieves higher throughput using shorter durations, safer precursors, and greater scalability potential. Summary of the invention

[0005] In one exemplary embodiment, a method includes mixing electroactive particles with a carbonaceous material to form a particle mixture including carbon-coated particles. The carbon-coated particles are subjected to a pulse voltage between parallel plate electrodes or between rollers of a rolling mill. The carbon-coated particles are converted to graphite-coated particles by local Joule heating.

[0006] In another exemplary embodiment, the pulse voltage is 10 to 200 volts.

[0007] In yet another exemplary embodiment, the pulse voltage has a pulse duration of 5 to 50 milliseconds.

[0008] In yet another exemplary embodiment, the particle mixture further includes a solvent.

[0009] In yet another exemplary embodiment, the parallel plate electrodes include a high temperature resistant material.

[0010] In yet another exemplary embodiment, the high temperature resistant material is copper, graphite, or tungsten.

[0011] In yet another exemplary embodiment, the graphite-adhered particle includes an amorphous layer and a graphite layer.

[0012] In yet another exemplary embodiment, the graphite-coated particles include only a graphite layer disposed on an electro-active substrate.

[0013] In yet another exemplary embodiment, the particle mixture is conveyed while a pulse voltage is applied to the particle mixture.

[0014] In yet another exemplary embodiment, the particle mixture is discharged from the mixing device to parallel plate electrodes.

[0015] In yet another exemplary embodiment, the particulate mixture is discharged from the mixing device onto a moving sheet.

[0016] In yet another exemplary embodiment, the moving sheet is a current collector.

[0017] In one embodiment, an apparatus includes a mixing device operable to mix electroactive particles with a carbonaceous material to form a particle mixture including carbon-coated particles. A device for applying a pulse voltage to the particle mixture is located downstream of the mixing device. The pulse voltage is applied when the particle mixture is located between opposing plate electrodes or between opposing rollers of a rolling mill. The device for applying the pulse voltage converts the carbon-coated particles into graphite-coated particles.

[0018] In another embodiment, parallel plate electrodes are disposed on opposite sides of a conduit conveying the particle mixture.

[0019] In another exemplary embodiment, the particle mixture is in motion when the carbon-attached particles are converted to graphite-attached particles.

[0020] In another exemplary embodiment, the pulse voltage is applied through opposing rollers of a rolling mill.

[0021] In another exemplary embodiment, the apparatus includes a pair of reels on which the current collector sheet is unwound and wound, and the particle mixture is disposed on the current collector.

[0022] In another exemplary embodiment, the pulse voltage is between 10 and 200 volts and the pulse duration applied is between 5 and 50 milliseconds. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Other features, advantages and details appear by way of example only in the following detailed description, which refers to the accompanying drawings, in which:

[0024] Figure 1 is an exemplary schematic diagram of a method for producing graphite-attached particles;

[0025] Figure 2 is an exemplary schematic diagram of a method for producing an electrode comprising graphite-attached particles;

[0026] Figure 3 is an exemplary description of graphite attached particles;

[0027] Figure 4is an exemplary schematic diagram of a continuous process for producing graphite-attached particles;

[0028] Figure 5 is an exemplary schematic diagram of a continuous process for producing an electrode comprising graphite-attached particles. DETAILED DESCRIPTION

[0029] The following description is merely exemplary in nature and is not intended to limit the present disclosure, its application, or uses. It should be understood that throughout the drawings, corresponding reference numerals indicate like or corresponding parts and features.

[0030] Disclosed herein is a method for preparing a coating comprising graphite on an electroactive surface. The electroactive surface may include the surface of an electroactive particle (also referred to herein as an electroactive substrate). The terms electroactive particle and electroactive substrate are used interchangeably.

[0031] The method includes applying a carbonaceous material to the surface of an electroactive substrate to form carbon-attached particles, and then converting the particles into graphite-attached particles. For simplicity, the carbon-attached particles or surfaces will be referred to as "carbon-attached particles" hereinafter. The carbon-attached particles are then placed between parallel plate electrodes and a pulse voltage is applied. The carbon-attached particles are placed between the parallel plate electrodes and in contact with the electrodes. The carbon-attached particles are also in contact with each other when placed between the electrodes. In short, the pulse voltage induces an electric current, which passes from one electrode through the carbon-attached particles to the opposite electrode through conductivity. The current causes a temperature increase through Joule heating. The method of instantaneously converting a carbonaceous coating into graphite (thereby producing a graphite layer on an electroactive substrate) is sometimes referred to as "flash graphene synthesis", which is based on local Joule heating on a very short time scale (milliseconds). After conversion, the carbon-attached particles are referred to as "graphite-attached particles". This method is advantageous because it does not use a heating furnace and does not use extremely high temperatures for a long period of time used in other conventional methods. On the other hand, it can use a variety of carbon sources and can be a high-throughput source for making electroactive substrates having graphite layers disposed thereon.

[0032] The coating (on the electroactive substrate) after conversion to graphite may contain some amorphous carbon in addition to graphitic carbon. The ratio of amorphous carbon to graphitic carbon can be adjusted by adjusting the voltage, the time period during which the carbon-attached particles are subjected to the pulse voltage, or both. This will be discussed in detail later.

[0033] Figure 1 and Figure 2 is an exemplary schematic diagram of an apparatus 100 showing a method for synthesizing flash graphene, which is used to produce a graphene layer on an electroactive substrate. Figure 1 In FIG. 1 , the electroactive substrate is depicted as electroactive particles 104, while in FIG. Figure 2 In the embodiment, a particle mixture comprising electroactive particles with attached carbonaceous material (carbon-attached particles) has been arranged on a current collector 304 (which can subsequently be used as an electrode). The carbon-attached particles (from the particle mixture) are converted into graphite-attached particles. It should be noted that in Figure 1 and Figure 2 In the process, other carbonaceous materials used in the particle mixture, such as solvents, binders, etc., can also be converted into graphite when subjected to the pulse voltage.

[0034] refer to Figure 1 , the device 100 includes a voltage source 202 in contact with parallel plate electrodes 204. Electroactive particles 104 (carbon-coated particles) provided with a carbonaceous coating 106 are disposed between the parallel plate electrodes 204. The carbon-attached particles may be in the form of dry particles or a mixture of wet particles (this will be described in detail later). When the carbon-attached particles are subjected to a pulse voltage (as indicated by the arrows), a portion of the carbonaceous coating 106 is converted into a graphite conformal graphite coating 110 (hereinafter referred to as the graphite coating 110) to form graphite-attached particles. The pulse voltage causes local Joule heating on an extremely short time scale to convert the carbonaceous coating 106 into the graphite coating 110. A conformal coating (or compliant coating) is a coating that retains the shape of a substrate contour or conforms to the shape of a substrate contour. In this particular case, the graphite coating 110 conforms to the contour of the electroactive particle 104 (see Figure 1 and 3 ). Thus, the electroactive particles 104 serve as a substrate on which the graphite coating 110 is disposed.

[0035] refer to Figure 2 , the device 100 includes a voltage source 202 in contact with parallel plate electrodes 204. A current collector 304 having a carbonaceous coating 306 (including carbon-attached particles) is placed between the parallel plate electrodes 204. The carbonaceous coating 306 is bonded to the current collector 304 before graphitization. When the current collector 304 having the carbonaceous coating 306 disposed thereon is subjected to a pulse voltage between the parallel plate electrodes 204, the carbonaceous material in the carbon-attached particles is converted into graphite. As described above, any other carbonaceous material (e.g., solvent, binder, catalyst, initiator, etc.) used in the particle mixture may also be converted into graphite. The current collector 304 having a graphite network layer 310 (having graphite-attached particles) may be used as an electrode (e.g., an anode) in another device, such as a battery, a capacitor, etc. The graphite network layer 310 (after graphitization) is not in the form of a powder or particle mixture, but is a solid graphite composite layer (in which an electroactive substrate is dispersed) firmly bonded to the current collector 304.

[0036] In one embodiment (ref. Figure 1), the entire carbonaceous coating 106 may be converted into the graphite coating 110. In another embodiment, only a portion of the carbonaceous coating 106 may be converted into the graphite coating, while the remaining portion is in the form of amorphous carbon.

[0037] In order to produce graphite-attached particles, the electroactive substrate must first have a carbonaceous coating attached to it (i.e., carbon-attached particles are first produced). This can be accomplished in a mixing device, such as a ball mill, a Waring mixer, a Henschel mixer, an extruder (e.g., a single screw or twin screw extruder), a roller mill, etc. The mixing device applies the carbonaceous coating to the electroactive substrate through tensile forces and shear forces to produce carbon-attached particles. If desired, mixing can be carried out at high temperatures and pressures, but ambient temperature and pressure are generally suitable. The carbonaceous material and the electroactive substrate, as well as optional solvents and binders, are first mixed in a mixing device to form a particle mixture containing carbon-attached particles. The term "particle mixture" includes dry particle mixtures (particle mixtures in the absence of liquid) and wet particle mixtures (particle mixtures in the presence of liquid). As Figure 1 and 2 As shown, the particle mixture is then placed between electrodes and a pulsed voltage is applied, resulting in a graphite coating on the electroactive substrate.

[0038] The electroactive substrate may be conductive or semiconductive. In one embodiment, the electroactive substrate may include a metal having a metal oxide layer disposed thereon (e.g., silicon disposed with silicon oxide, aluminum disposed with aluminum oxide, etc.). Suitable electroactive substrates include silicon, silicon-containing materials and alloys, such as silicon carbide, silicon oxide, silicon nitride, silicon boride, lithium silicide, etc., or combinations thereof. Prior to being subjected to the pulse voltage, the silicon may be amorphous, crystalline, or polycrystalline.

[0039] Other electroactive materials may include metals or semi-metals including tin, germanium, aluminum, boron, etc., or combinations thereof.

[0040] The electroactive substrate can have a variety of geometric shapes and can be in the form of spherical particles, fibers, rods, whiskers, fibrils (linear or bifurcated), flakes, ellipsoids, cuboids, etc., or combinations thereof. A preferred geometric form is spherical particles. The average particle size of the electroactive particles is 5 nanometers to 100 microns, preferably 30 nanometers to 50 microns, and more preferably 50 nanometers to 10 microns. The average particle size is determined by the radius of gyration of the substrate. The electroactive substrate can have a unimodal or multimodal size distribution. Bimodal size distributions (or more, such as trimodal size distributions) are preferred because they have excellent penetration effects. In one embodiment, the average particle size can be determined by x-rays or light scattering. For fibrous electroactive particles, the average aspect ratio is greater than 5, preferably greater than 10, and more preferably greater than 50.

[0041] As described above, the particle mixture comprises an electroactive substrate, a carbonaceous material, and an optional solvent or binder. A particle mixture without a solvent is a dry particle mixture, while a particle mixture containing a solvent is a wet particle mixture. When the particle mixture is a wet particle mixture (i.e., comprising a liquid such as a solvent), the content of the electroactive substrate in the particle mixture can be 30 to 70 weight percent (wt%), preferably 35 to 50 wt%, preferably 40 to 48 wt%, based on the total weight of the particle mixture.

[0042] When the particle mixture is a dry particle mixture (ie, free of liquid), the electroactive substrate may be present in the particle mixture in an amount of 75-97 weight percent (wt%), preferably 80-93 wt%, based on the total weight of the particle mixture.

[0043] Carbonaceous materials that can be used to make graphite coatings include carbon-containing solids, such as carbon black, graphite flakes, coke, soot, polymers, etc., or combinations thereof; carbon-containing fluids (liquids and gases at room temperature), such as carbon monoxide, carbon dioxide; aliphatic hydrocarbons, such as alkanes (e.g., methane, ethane, pentane, hexane, decane, dodecane, etc., or combinations thereof); alkynes (e.g., ethylene, propylene, acetylene, etc., or combinations thereof); alcohols (e.g., methanol, ethanol, butanol, propanol, ethylene glycol, etc., or combinations thereof); aromatic hydrocarbons (e.g., benzene, toluene, xylene, cumene, ethylbenzene, naphthalene, phenanthrene, anthracene, etc., or combinations thereof); or combinations thereof. Oxygenated hydrocarbons can also be used to generate graphite layers. Suitable examples of oxygenated hydrocarbons include formaldehyde, acetaldehyde, acetone, methanol or ethanol or mixtures thereof; including carbon monoxide and carbon dioxide. It can be noted from the list of carbonaceous materials above that the conversion from carbonaceous materials to graphite layers using pulse voltages can be carried out in the gas phase or the liquid phase.

[0044] Polymers can be used as carbonaceous solids to attach electroactive substrates. When other carbonaceous materials (e.g., carbon black, coke, etc.) are used to form carbonaceous coatings, polymers can be used as adhesives. When subjected to pulse voltages, the adhesive will decompose to form a part of the graphite coating, and the remainder of the graphite coating is formed by other carbonaceous materials encapsulated by the adhesive. Polymers with lower degradation temperatures are preferably used as adhesives. Catalysts and initiators that promote degradation and decomposition can also be used in particle mixtures.

[0045] Examples of polymers that can be used as carbonaceous solids include various thermoplastic polymers, mixtures of thermoplastic polymers, thermosetting polymers, or mixtures of thermoplastic polymers and thermosetting polymers. The organic polymer can also be a blend of a polymer, copolymer, terpolymer, or combination comprising at least one of the aforementioned organic polymers. The organic polymer can also be an oligomer, a homopolymer, a copolymer, a block copolymer, an alternating block copolymer, a random polymer, a random copolymer, a random block copolymer, a graft copolymer, a star block copolymer, a dendritic polymer, a polyelectrolyte (a polymer having some repeating groups containing electrolytes), a polyampholyte (a polyelectrolyte having a repeating group of cations and anions), an ionomer, etc., or a combination comprising at least one of the aforementioned organic polymers. The number average molecular weight of the organic polymer is greater than 10000 g / mol, preferably greater than 20000 g / mol, and more preferably greater than 50000 g / mol.

[0046] Examples of thermoplastic polymers include polyacetals, polyacrylic acids, polycarbonates, polyolefins, polystyrenes, polyolefins, polyesters, polyamides, polyaramids, polyamideimides, polyarylates, polyurethanes, epoxy resins, phenolic resins, silicones, polyarylsulfones, polyethersulfones, polyphenylene sulfide, polysulfones, polyimides, polyetherimides, polytetrafluoroethylene, polyetherketones, polyetheretherketones, polyetherketoneketones, polybenzoxazoles, polyoxadiazoles, polybenzothiazines, polybenzothiazines, polybenzothiazoles, polypyrazinoquinoxalines, polypyrrolamides, polypyrrolooxalines, polybenzimidazoles, polyindoles, Polyoxyisoindolines, polydioxyisoindolines, polytriazines, polypyridazine, polypiperazines, polypyrido, polytriazoles, polypyrazoles, polycarbonates, polydibenzofurans, polyphthalides, polyacetals, polyanhydrides, polyvinyl ethers, polyvinyl sulfides, polyvinyl alcohols, polyvinyl ketones, polyvinyl halides, polyvinyl nitrile, polyvinyl esters, polysulfones, polysulfides, polythioesters, polysulfones, polysulfones, polysulfoneamides, polyureas, polyphosphazenes, polysilazanes, polypropylene, polyethylene, polyethylene terephthalate, polyvinylidene fluoride, polysiloxanes, etc., or combinations thereof.

[0047] Examples of polyelectrolytes are polystyrene sulfonic acid, polyacrylic acid, pectin, carrageenan, alginate, carboxymethyl cellulose, polyvinyl pyrrolidone, and the like, or combinations thereof.

[0048] Examples of thermosetting polymers include epoxy polymers, unsaturated polyester polymers, polyimide polymers, bismaleimide polymers, bismaleimide triazine polymers, cyanate polymers, vinyl polymers, benzoxazine polymers, benzocyclobutene polymers, acrylic resins, alkyd resins, novolacs, resols, melamine-formaldehyde polymers, urea-formaldehyde polymers, hydroxymethyl furan, isocyanates, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, unsaturated polyester imides, and the like, or combinations thereof.

[0049] Other naturally occurring carbonaceous materials can also be used to produce the graphite layers. Examples of naturally occurring materials are cellulose, e.g., methylcellulose, ethylcellulose, hydroxymethylcellulose, hydroxyethylcellulose, coffee grounds, rice husks, crushed walnut shells, fruit shells, etc., or combinations thereof. Naturally occurring materials should be pulverized prior to being dispersed into the particle mixture. The use of natural materials makes the materials and methods used (to make the graphite-coated particles) environmentally sustainable.

[0050] For dry particulate mixtures, it is desirable that the carbonaceous particles be as small as possible so that they can electrostatically bond to the electroactive particles.

[0051] When the particle mixture is a wet particle mixture (i.e., containing a solvent), the content of the carbonaceous material in the particle mixture can be 1 to 10 weight percent (wt%), preferably 2 to 5 wt%, based on the total weight of the particle mixture. When the particle mixture is a dry particle mixture (i.e., without a solvent), the content of the carbonaceous material in the particle mixture can be 3 to 25 weight percent (wt%), preferably 7 to 20 wt%, based on the total weight of the particle mixture.

[0052] Solvents can be optionally used to achieve deposition of carbonaceous materials on electroactive substrates. In one embodiment, solvents and cosolvents (which can dissolve polymers at high temperatures) can be used. After the carbonaceous material is attached to the electroactive substrate, the solvent can be removed (e.g., by vacuum means) (i.e., the particle mixture can be a dry particle mixture). Alternatively, the solvent can be left in the particle mixture (i.e., the particle mixture can be a wet particle mixture) and undergo graphitization during the application of the pulse voltage.

[0053] The solvent can be a liquid aprotic polar solvent, a polar protic solvent, a nonpolar solvent or a combination thereof. The solvent can be selected according to the type of the electroactive substrate used, the type of the carbonaceous material used or both. It is desirable that the solvent dissolves a portion of any polymeric carbonaceous material that can be used to attach the electroactive substrate. Liquid aprotic polar solvents such as propylene carbonate, ethylene carbonate, butyrolactone, acetonitrile, benzonitrile, nitromethane, nitrobenzene, cyclopentane, dimethylformamide, N-methylpyrrolidone, etc., or a combination thereof can be used. Polar protic solvents such as water, methanol, acetonitrile, nitromethane, ethanol, propanol, isopropanol, butanol, etc., or a combination thereof can be used. Other nonpolar solvents such as benzene, toluene, methylene chloride, carbon tetrachloride, hexane, ether, tetrahydrofuran, etc., or a combination thereof can also be used. Examples of preferred solvents are water, ethanol, tetrahydrofuran, acetone, or a combination thereof.

[0054] If a solvent is used, the solvent content may be 25 to 69 wt%, 40 to 65 wt%, preferably 50 to 60 wt%, based on the total weight of the particle mixture.

[0055] After the particle mixture is prepared, it is placed between two electrodes and graphitized by applying a pulse voltage. The preparation of the particle mixture and the subsequent graphitization step can be carried out in a batch process or a continuous process. Examples of batch processes and continuous processes are described in detail below. First, a general graphitization process (using a pulse voltage) for producing a graphite-attached electroactive substrate will be described in detail.

[0056] like Figure 1 and 2 As shown, a particle mixture comprising an electroactive substrate having a carbonaceous layer disposed thereon can be disposed between a pair of electrodes (parallel plate electrodes). The parallel plate electrodes include high temperature resistant materials such as copper, graphite or tungsten. The particle mixture is subjected to a pulse voltage of 10 to 200 volts or more, preferably 30 to 75 volts, more preferably 60 to 150 volts, for a period of 0.5 milliseconds to 10 minutes. Multiple pulse voltages of multiple pulse durations applied in multiple time periods can be used for pulses. For example, a first pulse voltage of 140 volts with a first pulse duration of 5 milliseconds can be applied in a first time period of 1 minute, and then a second pulse voltage of 130 volts with a second pulse duration of 5 milliseconds can be applied in a second time period of 5 minutes.

[0057] The application of pulsed voltage results in rapid graphitization of carbonaceous materials due to local temperature spikes between parallel plate electrodes. The high voltage produces local heating on a very short time scale (e.g., less than 10 milliseconds). Upon cooling, the carbon transforms into the lowest energy structure, graphite. Graphite includes multiple graphene sheets.

[0058] The pulse intensity (voltage) and pulse duration determine the degree of heating, which can be controlled to optimize the degree of graphitization in the carbon coating and to prevent the electroactive substrate (e.g., silicon particles) (see Figure 1 ) or current collector (see Figure 2 ) damage. Carbon generally undergoes graphitization at temperatures of about 1000°C or higher.

[0059] Each voltage pulse is millisecond-level. The preferred time interval of each pulse is 5 to 50 milliseconds, preferably 7 to 30 milliseconds, and more preferably 10 to 20 milliseconds. It should be noted that voltage and time period (the total time that the particle mixture is between the electrodes, which should not be confused with the pulse duration) are inversely related to each other. In other words, graphitization can be achieved by using a higher voltage in a shorter time, or, it can be achieved by using a lower voltage in a longer time. Longer times at a given voltage generally result in greater conversion of carbonaceous materials to graphite. By retaining the particle mixture between the electrodes for a longer time, all carbonaceous materials can be converted into graphite. When all carbonaceous materials are converted into graphite, there is substantially no amorphous carbon between the electroactive substrate and the graphite layer.

[0060] The resulting graphite-attached particles preferably contain at least one layer of graphene on an electrically active substrate. Graphene refers to a single-layer planar structure of carbon atoms arranged in a repeating hexagonal lattice. Graphite includes multiple graphene sheets stacked on top of each other. Figure 3 is a schematic, exemplary depiction of a graphite-attached particle 103 including an electroactive particle 104 on which an optional amorphous carbon layer 108 and a graphite coating 110 are disposed. The graphite layer preferably includes at least one layer of graphene that partially or completely encapsulates the electroactive substrate. Figure 3 In the graphite particles, there are shown three graphene layers 1 10A, 110B and 110C, which are parallel to each other. The d spacing between the graphene layers can be 0.34 nanometers or greater. The graphite layers generally have a thickness of 0.34 nanometers to 100 nanometers, preferably 1 nanometer to 15 nanometers, and more preferably 3 nanometers to 10 nanometers.

[0061] In one embodiment, the graphite coating 110 preferably includes at least 3 or more layers of graphene, preferably 10 or more layers of graphene, more preferably 15 or more layers of graphene, which partially or completely encapsulate the electroactive substrate. In a preferred embodiment, the graphite layer preferably completely encapsulates the electroactive substrate.

[0062] In one embodiment, the graphite layer preferably completely encapsulates the amorphous layer, which in turn encapsulates the electrically active substrate. In another embodiment, the amorphous layer encapsulates the graphite layer, which in turn encapsulates the electrically active substrate.

[0063] The graphite layer may be provided directly on the surface of the electrically active substrate. The amorphous layer is an optional layer, the thickness of which may be varied by subjecting it to a prolonged pulse voltage or some other form of thermal treatment.

[0064] In one embodiment, the graphene layer is disposed on the outer surface of the amorphous layer and has a larger average radius than the amorphous layer. In one embodiment, the amorphous layer contacts the electroactive substrate and the graphene layer contacts the amorphous layer. The graphene layers are conformal layers and generally have a shape similar to the shape of the surface they contact. The graphene layer is substantially parallel to the outer surface of the amorphous layer or the outer surface of the electroactive substrate.

[0065] The thickness of the amorphous layer varies in the range of 0% to more than 200%, preferably 2% to more than 100%, and more preferably 5% to more than 50% of the thickness of the graphite layer. The graphite layer is generally more conductive than the amorphous layer and more conductive than the electrically active substrate. In one embodiment, the graphite layer is more conductive than the amorphous layer, which in turn is more conductive than the electrically active substrate. In another embodiment, the graphite layer is more conductive than the electrically active substrate, which in turn is more conductive than the amorphous layer.

[0066] The preparation of graphite-coated particles from carbon-coated particles can be carried out as a batch process or a continuous process.

[0067] In a batch process, a particle mixture is first produced in a mixing device. The electroactive particles, carbonaceous material, optional solvent, and binder are added to the mixing device and stirred to produce a particle mixture that includes a coating of carbonaceous material disposed on an electroactive substrate (i.e., to produce carbon-coated particles). The particle mixture can then be stored on a shelf for future use or transferred to a Figure 1 or 2 to be subjected to a pulse voltage, thereby producing a graphite coating on the electroactive substrate (ie, producing attached graphite particles). The device for applying the pulse voltage is located downstream of the mixing device.

[0068] In a continuous process, the particle mixture is set in motion during the application of the pulsed voltage. During the application of the pulsed voltage, the particle mixture is transported through a parallel plate arrangement (which is located on opposite sides of the conduit) (see Figure 4 The particle mixture can be transported by a moving current collector (see Figure 5 ).exist Figure 4 and Figure 5 In the case of graphite, the conversion to graphite occurs during the movement of the carbonaceous material (i.e., accompanied by transport). Therefore, these processes can be referred to as dynamic graphitization processes.

[0069] In a continuous process, a particle mixture is produced in a mixing device and transferred directly to an apparatus which continuously subjects the particle mixture stream to a pulsed voltage for graphitizing the carbonaceous coating. Figure 4An exemplary embodiment of such a continuous manufacturing process is shown. Apparatus two 400 includes a mixing device 402 that produces carbon-attached particles in the form of a particle mixture 502. The mixing device can be selected from the list detailed above. A ball mill is preferred for mixing. The particle mixture 502 is then discharged into a conduit 405 (located downstream of the mixing device 402) containing parallel electrodes 404.

[0070] In one embodiment, the particle mixture 502 can be pumped into the conduit 405 from the mixing device 402 by a pump (not shown). In another embodiment, the particle mixture 502 can be transported by gravity (with the help of a static pressure head). The combination of a static pressure head and a pump can be used to transport the particle mixture through an electric field, in which the particle mixture is subjected to a pulse voltage. Parallel electrodes 404 are arranged on the opposite side of the conduit 405 and are connected to the voltage source two 403. When the particle mixture passes through the conduit, a pulse voltage is applied to it by parallel electrodes 404, causing the carbonaceous material to be converted into graphite. The conduit can have a cross section such as a square, a rectangle or a circle. When the cross section of the conduit is circular, the relative electrodes can be arranged to cross each other in the conduit, and can have a curved surface. Then, the electroactive substrate with a graphite layer 504 thereon is discharged into the current collector sheet 506 for further downstream use.

[0071] Figure 5 shows the use of the previously Figure 2 A continuous method for producing an electrode as shown in FIG. In this method, a current collector is transported through an electric field and a particle mixture (including carbon-attached particles) is disposed on the current collector. The current collector can be unrolled from a reel and, after being subjected to a pulse voltage while provided with carbon-attached particles (converted to graphite-attached particles when subjected to the pulse voltage), wound onto another reel. The pulse voltage is applied by rollers of a rolling mill.

[0072] Reference Figure 5, the apparatus 2 400 includes a mixing device 402, which mixes the electroactive substrate and the carbonaceous material and the optional solvent and binder to form a particle mixture 502. The mixing device can be selected from the list detailed above. A ball mill is the first choice for mixing. The particle mixture 502 is then discharged onto the current collector sheet 506. The current collector sheet is located downstream of the mixing device. The current collector sheet is unrolled from a reel 1 602. During its journey to the next reel 2 604 (on which it is rewound), the particle mixture is placed on it. The particle mixture 502, together with the current collector sheet 506, is subjected to a pulse voltage before contacting the reel 2 604. In one embodiment, the particle mixture 502 can be pumped from the mixing device 402 to the current collector sheet 506 by a pump (not shown). Parallel electrodes 404 (in the form of a roller mill located downstream of the mixing device) are arranged on opposite sides of the current collector sheet 506, and each roller is connected to a voltage source 2 403. When the particle mixture (arranged on the current collector sheet 506) passes through the roller (of the rolling mill), a pulse voltage is applied thereto, causing the carbonaceous material to be converted into graphite. The relative rollers of the rolling mill are used to apply the pulse voltage. Therefore, when the carbonaceous material moves, conversion to graphite occurs. The tensile and shear forces applied to the particle mixture by the rollers also promote adhesion between the graphitized material and the current collector to form an electrode. The rolling mill can also be used to calender the electrode during the anode formation process. The electrode can be cut into smaller parts (not shown) for further downstream use.

[0073] The methods disclosed above for graphitizing carbonaceous materials are superior to currently used methods because they operate at high temperatures for shorter periods of time, thereby preventing damage to the electroactive substrate. The methods also do not use expensive graphene additives during the mixing process. Compared to existing processes, the methods are environmentally friendly and cost-effective.

[0074] Although the above disclosure has been described with reference to exemplary embodiments, it will be appreciated by those skilled in the art that various changes may be made and equivalents may be substituted for its elements without departing from the scope of the present invention. In addition, many modifications may be made to adapt specific circumstances or materials to the teachings of the present disclosure without departing from the basic scope of the present disclosure. Therefore, the present disclosure is not limited to the specific embodiments disclosed, but will include all embodiments falling within its scope.

Claims

1. A method for preparing graphite-attached particles, comprising: mixing the electroactive particles with a carbonaceous material to form a particle mixture comprising carbon-attached particles; applying a pulse voltage to the carbon-attached particles between parallel plate electrodes or between the rollers of a rolling mill; as well as The carbon-attached particles are converted into graphite-attached particles by localized Joule heating, and the graphite-attached particles include an amorphous carbon layer and a graphite layer on an electrically active substrate, the graphite layer including at least one layer of graphene.

2. The method according to claim 1, wherein: The pulse voltage is 10 to 200 volts, and the pulse voltage has a pulse duration of 5 to 50 milliseconds.

3. The method according to claim 1, wherein: The particle mixture also includes a solvent.

4. The method according to claim 1, wherein: The parallel plate electrodes include a high temperature resistant material, which is copper, graphite or tungsten.

5. The method according to claim 1, wherein: The graphite-adhered particles include an amorphous layer and a graphite layer, and the amorphous layer is disposed between the electroactive particles and the graphite layer. 6 . The method of claim 1 , further comprising conveying the particle mixture while applying a pulse voltage to the particle mixture.

7. The method of claim 1 further comprising discharging the particle mixture from the mixing device to parallel plate electrodes.

8. The method of claim 1 further comprising discharging the particle mixture from the mixing device onto a moving sheet.

9. The method according to claim 8, wherein: The moving sheet is the current collector.