Catalysts for oxygen evolution reaction in water electrolysis

By depositing iridium compounds under alkaline conditions and avoiding high-temperature heat treatment, a highly electrochemically active catalyst composition is prepared, which solves the problems of low activity of existing catalysts under acidic conditions and corrosion of carbon carriers, and is suitable for PEM water electrolysis and fuel cells. the anode side.

CN114072939BActive Publication Date: 2024-10-18HERAEUS DEUTSCHLAND GMBH & CO KG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202080048658.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-08
Publication Date
2024-10-18
Estimated Expiration
2040-06-08

AI Technical Summary

Technical Problem

Existing catalysts exhibit low catalytic activity in the oxygen evolution reaction under acidic conditions, and the carbon support material is easily corroded when the battery polarity is reversed, resulting in reduced performance.

Method used

The iridium compound is deposited on the carrier material under alkaline conditions, and the catalyst composition is prepared by a wet chemical method to avoid high-temperature heat treatment and ensure that the carrier material is dried at moderate temperatures to maintain high electrochemical activity.

Benefits of technology

It achieves high catalytic activity and corrosion resistance under acidic conditions, and is suitable as a catalyst on the anode side of PEM water electrolyzers or fuel cells, improving battery performance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004841158500000091
    Figure GDA0004841158500000091
  • Figure GDA0004841158500000101
    Figure GDA0004841158500000101
Patent Text Reader

Abstract

The present invention relates to a method for preparing a catalyst composition, wherein, in an aqueous medium containing an iridium compound, at a pH value ≥ 9, an iridium-containing solid is deposited on a carrier material, and the carrier material loaded with the iridium-containing solid is separated from the aqueous medium and dried, wherein in the method, the carrier material loaded with the iridium-containing solid is not subjected to a heat treatment at a temperature exceeding 250° C. for a duration exceeding 1 hour.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to the preparation of catalyst compositions which can be used as catalysts in water electrolysis, in particular for the oxygen evolution reaction at the anode, or as catalysts for fuel cells, for example in combination with Pt- or Pd-containing catalysts supported on carbon.

[0002] Hydrogen is considered to be the energy carrier of the future because it enables sustainable energy storage, is available over long periods of time, and can also be produced using renewable energy technologies.

[0003] The most commonly used method for producing hydrogen is steam reforming, in which methane and water vapor react to form hydrogen and CO.

[0004] Water electrolysis is another alternative to produce hydrogen. High-purity hydrogen can be obtained through water electrolysis.

[0005] There are various methods for water electrolysis, in particular alkaline water electrolysis, acidic water electrolysis using polymer electrolyte membranes ("PEM"; PEM water electrolysis), and high temperature solid oxide electrolysis.

[0006] A water electrolyzer comprises a half-cell with an electrode at which an oxygen evolution reaction (OER) occurs, and another half-cell with an electrode at which a hydrogen evolution reaction (HER) occurs. The electrode at which the oxygen evolution reaction occurs is called the anode.

[0007] For a technical review of water electrolysis, especially PEM water electrolysis, see, for example, International Journal of Hydrogen Energy, 38, 2013, by M. Carmo et al., pp. 4901-4934; and Materials Science for Energy Technologies, 2, 2019, by V. Himabindu et al., pp. 442-454.

[0008] In a polymer electrolyte membrane water electrolyzer (hereinafter also referred to as a PEM water electrolyzer), the polymer membrane serves as a proton transport medium and electrically insulates electrodes from each other.

[0009] The oxygen evolution reaction occurring at the anode of a PEM water electrolyzer can be represented by the following reaction equation:

[0010] 2H2O→4H + +O2+4e -

[0011] Due to its complex reaction mechanism, the oxygen evolution reaction has slow reaction kinetics, so a significant overpotential at the anode is required to obtain a sufficiently high conversion rate.

[0012] The efficient operation of a water electrolyzer requires the presence of a catalyst. In order to catalyze the oxygen evolution reaction at the anode of a PEM water electrolyzer, in particular iridium, iridium oxide, ruthenium oxide or an Ir-Ru mixed oxide are used. The catalytically active material may optionally be present on a support material (for example in the form of nanoparticles or a film) in order to thereby increase the specific surface area of ​​the catalyst material.

[0013] For a review of catalysts for the oxygen evolution reaction under acidic conditions (that is, at the anode of a PEM water electrolyzer), see, for example, Adv. Energy Mater., 7, 2017, 1601275 by P. Strasser et al. and Progress in Energy and Combustion Science, 58, 2017, pp. 1 to 35 by FM Sapountzi et al. As a requirement for the electrocatalyst, the publication by FM Sapountzi et al. mentions a conductivity as high as possible so that efficient electron transfer can occur.

[0014] There are a number of different processes by which iridium oxide and / or ruthenium oxide can be prepared in supported form, optionally on a support material.

[0015] A possible variant is wet chemical precipitation from an alkaline aqueous medium containing an iridium-containing precursor compound. The precipitated iridium-containing solid is generally amorphous and has a relatively low electrical conductivity. By calcining the precipitated material at high temperature, crystalline IrO2 is obtained, the electrical conductivity of which is significantly higher than that of amorphous iridium oxide hydroxide.

[0016] WO 2005 / 049199 A1 describes a method for preparing a catalyst composition for water electrolysis. In this method, iridium oxide is deposited on an oxide support material in an aqueous medium containing an iridium precursor compound (e.g. an Ir(III) or Ir(IV) compound). The method includes a thermal treatment at 300° C. to 800° C. A high iridium content in the catalyst composition is disadvantageous from an economic point of view.

[0017] EP 2 608 297 A1 likewise describes a process for preparing a supported iridium-containing catalyst composition for water electrolysis, wherein iridium oxide is wet-chemically deposited on an oxide support material under alkaline conditions. Likewise, the support material loaded with iridium oxide is subjected to a heat treatment at 300° C. to 800° C.

[0018] EP 2 608 298 A1 describes an electrocatalyst for a fuel cell having the following components: (i) an oxide support material as a core, (ii) an iridium oxide coating applied to the core, and (iii) a catalytically active noble metal, such as platinum, which is present in the form of nanoparticles on the iridium oxide coating. As can be seen from the examples, the iridium oxide coating is subjected to a heat treatment at 400° C.

[0019] For polyelectrolyte membrane fuel cells ("PEM" fuel cells), carbon materials loaded with noble metals (e.g., metallic platinum or platinum alloys supported on carbon materials) are usually used as catalyst compositions. Under certain conditions, in the case of so-called fuel starvation, cell polarity reversal can occur during the operation of PEM fuel cells. In normal operation, the hydrogen oxidation reaction (HOR) occurs on the anode side of the fuel cell:

[0020] 2H2→4H + +4e -

[0021] After the cell polarity is reversed, the cell operates in electrolysis mode, where the oxygen evolution reaction occurs at the anode:

[0022] 2H2O→4H + +O2+4e -

[0023] Further, carbon corrosion may occur according to the following equation:

[0024] C + 2H2O → CO2 + 4H + +4e -

[0025] Due to the oxidation of the carbon, the support material can be significantly and irreversibly damaged. However, if, in addition to the conventional fuel cell catalysts which catalyze the hydrogen oxidation reaction, an additional catalyst is present which catalyzes the oxygen evolution reaction in the event of a reversal of the cell polarity, water electrolysis is preferred over carbon corrosion and damage to the carbon-based support material is reduced.

[0026] It is an object of the present invention to provide a composition which has a high catalytic activity with respect to the oxygen evolution reaction and is therefore suitable as a catalyst on the anode side of a water electrolysis cell or a fuel cell after a reversal of the cell polarity.

[0027] This object is achieved by a process for preparing a catalyst composition, wherein

[0028] - depositing the iridium-containing solid on a support material in an aqueous medium comprising an iridium compound at a pH value ≥ 9,

[0029] - separating the support material carrying the iridium-containing solid from the aqueous medium and drying it,

[0030] Wherein in the method, the support material carrying the iridium-containing solid is not subjected to a heat treatment at a temperature exceeding 250° C. for a duration exceeding 1 hour.

[0031] The method of the present invention is a wet chemical method that is easy to implement. In an aqueous medium in which an iridium compound is dissolved, an iridium-containing solid is precipitated under alkaline conditions. In the presence of a carrier material, the iridium-containing solid is deposited on the carrier. In the context of the present invention, it has been found that if long-term heat treatment at high temperatures is avoided, the carrier material loaded with the iridium-containing solid has a very high electrochemical activity. Therefore, if the loaded carrier material is dried at a moderate temperature, and there is no need to subsequently calcine the material at a high temperature, or at least the duration of the heat treatment at a higher temperature remains relatively short, the material shows high catalytic activity in the oxygen evolution reaction under acidic conditions, and is therefore excellently suitable as a catalyst in the anode side of a PEM water electrolyzer or a PEM fuel cell.

[0032] Suitable support materials on which the iridium-containing solid can be wet-chemically deposited are known to the person skilled in the art. For example, the support material is an oxide of a transition metal, such as titanium oxide (e.g. TiO2), zirconium oxide (e.g. ZrO2), niobium oxide (e.g. Nb2O5), tantalum oxide (e.g. Ta2O5) or cerium oxide, an oxide of a main group metal (e.g. tin oxide such as SnO2 or aluminum oxide such as Al2O3), SiO2 or a carbon material or a mixture of two or more of the above support materials.

[0033] The carrier material is usually a powdered or granular carrier material.

[0034] The carrier material has a diameter of, for example, less than 100 m 2 / g, preferably less than 60m 2 / g, and more preferably less than 40m 2 / g BET specific surface area. For example, the BET specific surface area of ​​the carrier material is 5m 2 / g to 100m 2 / g, more preferably 10m 2 / g to 60m 2 / g or 10m 2 / g to 40m 2 / g.

[0035] Suitable support materials are commercially available or can be prepared via conventional methods known to those skilled in the art.

[0036] In the case of oxide supports, the oxide may be doped with suitable elements in order to improve the electrical conductivity. For example, tin oxide may contain antimony ("ATO", English: "antimony-doped tin oxide").

[0037] If the support material is a carbon material, it is preferred that the carbon material has a relatively high degree of graphitization. This increases the electrical conductivity and improves the corrosion resistance of the carbon material. The increase in the degree of graphitization of the carbon material can be achieved, for example, by a suitable heat treatment. This is known to those skilled in the art.

[0038] For example, the carbon material serving as the support material has a degree of graphitization of at least 60%, more preferably at least 63% (eg, 60% to 90% or 63% to 80%).

[0039] As described in EP 2 954 951 A1, the degree of graphitization g is determined with the aid of the following formula (1):

[0040] g = (344pm-d002) / (344pm-335.4pm) (1)

[0041] Here, d002 is the graphite basal plane distance, which is determined by X-ray imaging using the (002) plane diffraction line of the graphitized carbon material.

[0042] The preparation of carbon-based support materials having a high degree of graphitization is described, for example, in EP 2 954 951 A1.

[0043] Suitable carbon-based support materials with a high degree of graphitization are also commercially available, for example from Heraeus as The name is obtained.

[0044] The support material is present dispersedly in the aqueous medium.

[0045] The aqueous medium comprises an iridium compound which can be precipitated as an iridium-containing solid under alkaline conditions. Such iridium compounds are known to those skilled in the art. The iridium compound is preferably an iridium (IV) or iridium (III) compound.

[0046] Suitable iridium (III) or iridium (IV) compounds which precipitate as solids in aqueous solution under alkaline conditions are known to those skilled in the art. For example, the iridium (III) or iridium (IV) compound is a salt (e.g. an iridium halide such as IrCl3 or IrCl4; its anion is a chloro complex IrCl6 2- iridium nitrate or iridium acetate) or an iridium-containing acid such as, for example, H2IrCl6. In a preferred embodiment, the aqueous medium comprises an iridium (IV) halide, in particular iridium (IV) chloride.

[0047] Optionally, ruthenium (III) and / or ruthenium (IV) compounds may also be present in an aqueous medium. This makes it possible for the iridium ruthenium oxide to oxidize ruthenium hydroxide to be deposited on a support material. If a ruthenium precursor compound is present in an aqueous medium, the ruthenium precursor compound may be, for example, a Ru (III) salt or a Ru (IV) salt, such as a halide salt, a nitrate or an acetate.

[0048] Preferably, the pH of the aqueous medium used to deposit the iridium-containing solid on the support material is ≥ 10, more preferably ≥ 11. For example, the pH of the aqueous medium is 9 to 14, more preferably 10 to 14 or 11 to 14.

[0049] The aqueous medium generally comprises water in a proportion of at least 50% by volume, more preferably at least 70% by volume or even at least 90% by volume.

[0050] For depositing the iridium-containing solid on the support material, the temperature of the aqueous medium is, for example, from 40°C to 100°C, more preferably from 60°C to 80°C.

[0051] In the context of the process of the invention, the support material can, for example, be dispersed in an aqueous medium which already contains one or more iridium (III) and / or iridium (IV) compounds but has a pH value <9 (for example at room temperature). Subsequently, the pH value of the aqueous medium is raised to ≥9 by adding a base, and optionally the temperature of the aqueous medium is also raised, until the iridium-containing solid is deposited on the support material via a precipitation reaction. Alternatively, for example, it is also possible to disperse the support material in an aqueous medium which does not yet contain an iridium compound, and to add the iridium (III) and / or iridium (IV) compound to the aqueous medium only after adjusting a suitable pH value and optionally a specific precipitation temperature.

[0052] For example, the weight ratio of the support material to the total amount of iridium (III) and / or iridium (IV) compounds in the aqueous medium is selected such that the support material loaded with the iridium-containing solid contains iridium in a content of at most 50% by weight, more preferably at most 45% by weight. For example, the loaded support material has an iridium content in the range of 10% to 50% by weight, more preferably 15% to 45% by weight.

[0053] If ruthenium (III) and / or ruthenium (IV) compounds are also present in the aqueous medium, the solid applied to the support material by precipitation contains ruthenium in addition to iridium. The atomic ratio of iridium to ruthenium can be, for example, in the range of 90 / 10 to 10 / 90.

[0054] The support material loaded with the iridium-containing solid is removed from the aqueous medium by methods known to those skilled in the art, for example by filtration.

[0055] The support material carrying the iridium-containing solid is dried. The dried iridium-containing solid present on the support material is iridium oxide hydroxide. Iridium oxide hydroxide contains hydroxide anions in addition to oxide anions and can be represented, for example, by the following formula: IrO(OH)x; 1≤x<2.

[0056] As mentioned above, in the process of the present invention, the support material carrying the iridium-containing solid is not subjected to a heat treatment at a temperature exceeding 250° C. for a duration exceeding 1 hour.

[0057] Preferably, in the process, the support material loaded with the iridium-containing solid is not subjected to a heat treatment at a temperature exceeding 200° C. for a duration exceeding 30 minutes.

[0058] For example, the support material loaded with the iridium-containing solid is dried at a temperature of up to 200° C. and is not subjected to further heat treatment after drying.

[0059] For example, the drying of the support material loaded with the iridium-containing solid is carried out at a temperature and for a period of time such that the iridium oxide oxidized iridium (IV) to iridium (III) present on the support material after drying has an atomic ratio of iridium (IV) to iridium (III) of at most 1.7 / 1.0, more preferably at most 1.5 / 1.0, as determined via X-ray photoelectron spectroscopy (XPS). The drying of the loaded support material is carried out, for example, at a temperature of ≤250° C., more preferably ≤200° C., and even more preferably ≤150° C.

[0060] The term "iridium (IV)" refers to an iridium atom in the oxidation state +4, while the term "iridium (III)" refers to an iridium atom in the oxidation state +3.

[0061] The iridium oxyhydroxide obtained after drying has, for example, an atomic iridium(IV) / iridium(III) ratio in the range of 1.0 / 1.0 to 1.7 / 1.0, more preferably 1.2 / 1.0 to 1.5 / 1.0.

[0062] Preferably, the iridium oxide hydroxide does not contain iridium (0). Iridium (0) refers to iridium in oxidation state 0. That is, preferably no metallic iridium is present on the support material. The presence or absence of iridium (0) can be verified by XPS.

[0063] Optionally, the dried iridium hydroxide loaded support material may be dispersed in a liquid medium to provide a catalyst-containing ink.

[0064] Suitable liquid media are known to those skilled in the art, which serve as inks for supporting catalysts and can be used to prepare catalyst-coated electrodes in electrolyzers (e.g., PEM electrolyzers for water electrolysis) or PEM fuel cells. For example, the ink comprises an ionomer (e.g., a polymer comprising a sulfonic acid group-containing monomer) and one or more short-chain alcohols (e.g., methanol, ethanol or n-propanol or a mixture of at least two of these alcohols).

[0065] Furthermore, the present invention relates to a catalyst composition obtainable by the above process.

[0066] That is, the catalyst composition comprises a support material and iridium hydroxide oxidizes on the support material. With regard to the preferred characteristics of suitable support materials and iridium hydroxide oxidizes on the support material, reference may be made to the above embodiments.

[0067] As mentioned above, it is preferred that the iridium oxide hydroxide oxidizes the iridium hydroxide present on the support material has an atomic ratio of iridium (IV) to iridium (III) of at most 1.7 / 1.0, more preferably at most 1.5 / 1.0, as determined via X-ray photoelectron spectroscopy (XPS). For example, the iridium oxide hydroxide has an atomic iridium (IV) / iridium (III) ratio in the range of 1.0 / 1.0 to 1.7 / 1.0, more preferably 1.2 / 1.0 to 1.5 / 1.0. Preferably, the iridium oxide hydroxide oxidizes does not contain iridium (0). Iridium (0) means iridium in oxidation state 0. That is, metallic iridium is preferably not present on the support material. The presence or absence of iridium (0) can be verified by XPS.

[0068] The iridium oxyhydroxide present on the support material is preferably amorphous, ie it exhibits no diffraction reflections in the X-ray diffraction pattern.

[0069] The catalyst composition has, for example, less than 100 m 2 / g, preferably less than 60m 2 / g, and more preferably less than 40m 2 For example, the BET specific surface area of ​​the catalyst composition is 5 m 2 / g to 100m 2 / g, more preferably 10m 2 / g to 60m 2 / g or 10m 2 / g to 40m 2 / g.

[0070] Preferably, the catalyst composition comprises no further noble metals besides iridium and optionally ruthenium.

[0071] Furthermore, the present invention relates to an electrolyzer, in particular a PEM electrolyzer for water electrolysis, comprising the above-mentioned catalyst composition of the present invention.

[0072] The components required for constructing a PEM electrolyzer are known to those skilled in the art.Polymer electrolyte membranes ("PEMs"), for example, comprise polymers having monomers containing sulfonic acid groups.

[0073] Preferably, the catalyst composition is present in the half-cell where oxygen evolution occurs (ie, on the anode side of the electrolyser).

[0074] Furthermore, the present invention relates to a fuel cell, in particular a PEM fuel cell, comprising the catalyst composition of the present invention.

[0075] The components required for constructing a PEM fuel cell are known to those skilled in the art.Polymer electrolyte membranes ("PEMs"), for example, comprise polymers having monomers containing sulfonic acid groups.

[0076] Preferably, the catalyst composition is present on the anode side of the fuel cell, for example together with a conventional catalyst composition comprising a carbon material as a support material and a noble metal, in particular platinum or palladium, applied to the support material in the form of a simple metal or a metal alloy.

[0077] Furthermore, the present invention relates to use of the catalyst composition of the present invention as a catalyst for oxygen evolution reaction in water electrolysis.

[0078] Measurement method

[0079] The following measurement methods are used in the context of the present invention:

[0080] BET surface area

[0081] The BET surface area was determined according to the BET theory (multipoint method, ISO 9277:2010) at 77 K using nitrogen as adsorbate.

[0082] Atomic ratio of Ir(IV) to Ir(III)

[0083] The relative proportion of Ir atoms in the oxidation state +4 and oxidation state +3 in the supported iridium hydroxide oxidase and the atomic Ir(IV) / Ir(III) ratio are determined by X-ray photoelectron spectroscopy (XPS). In the detailed spectrum of the Ir(4f) doublet (BE of 75 to 55 eV, Al-kα source), the ratio is determined by asymmetric peak fitting (Shirley Background, Gaus-Lorentz mixture, Gaus content of 30%, clipping factor of 0.7). In addition, the presence of IrOH species is also detected in the O(1s) detail spectrum (BE of about 531 eV, Al-kα source) with the aid of asymmetric peak fitting (Shirley Background, Gaus-Lorentz mixture, Gaus content of 30%). The corresponding procedure is described, for example, in Abbott et al., Chem. Mater, 2016, 6591-6604.

[0084] Through XPS analysis, the presence of iridium (0) in the composition can also be checked.

[0085] Iridium content of support material loaded with iridium hydroxide

[0086] The iridium content and, if present, the ruthenium content were determined via inductively coupled plasma optical emission spectroscopy (ICP-OES).

[0087] The invention is explained in more detail with the aid of the examples described below. Example

[0088] Example 1 (EB1) of the present invention and comparative examples 1 to 3 (VB1-VB3)

[0089] The same carrier material is used in EB1 and VB1-VB3, i.e., a 60m 2 / g of BET specific surface area of ​​TiO2.

[0090] Further, in EB1 and VB1-VB3, the iridium-containing solid precipitated at alkaline pH was wet-chemically deposited on the TiO2 support material in the same manner. The wet-chemical deposition was performed as follows:

[0091] 124.56 g of iridium (IV) chloride (IrCl4 hydrate, Heraeus Deutschland GmbH & Co. KG) was dissolved in 4000 ml of water at room temperature. Subsequently, 60.17 g of TiO2 (P25, Evonik, BET surface area: 60 m2 / g) was added. The pH value was adjusted to 9.7 by adding NaOH. The aqueous medium was heated to 70°C and the pH value was adjusted to 11. The mixture was stirred at 70°C overnight. The pH value was maintained at 11. The TiO2 carrier material loaded with iridium-containing solids was filtered and washed.

[0092] After separation of the support material loaded with the iridium-containing solid from the aqueous deposition medium, different thermal treatments were carried out in EB1 and VB1-VB3:

[0093] The loaded support materials of Examples EB1 and VB1-VB3 each had an iridium content of about 45% by weight.

[0094] EB1: The loaded support material was dried overnight at 120° C. XPS analysis showed that the dried iridium-containing solid present on the support was iridium hydroxide oxidizing iridium.

[0095] VB1: The loaded support material was heated at 300°C for 4 hours.

[0096] VB2: The loaded support material was heated at 360°C for 4 hours.

[0097] VB3: The loaded support material was heated at 400°C for 4 hours.

[0098] For the catalyst compositions obtained in EB1 and VB1 to VB3, the electrochemical activity (in mA per mg of iridium) with respect to the oxygen evolution reaction in water electrolysis was determined in each case. The activity was determined in electrochemical measurements at a rotating disk electrode.

[0099] The electrochemical characterization was performed in a three-electrode configuration with a graphite rod as counter electrode, a saturated calomel electrode as reference electrode (all potentials converted to RHE) and the catalyst materials of Examples EB1 and VB1-VB3, each of which was present as a thin film on a glassy carbon substrate as working electrode (loading: 100 μg / cm 2 ). The measurements were carried out at 60° in air in 0.5MH2SO4 at a rotation speed of 1600 U / m. Considering that the anode and cathode potentials are 1.5 V RHE Under hysteresis, determine the activity value.

[0100] Table 1 shows the results of these measurements.

[0101] Table 1: Electrochemical activity

[0102]

[0103]

[0104] The results show that the support material loaded with iridium-containing solids has a very high electrochemical activity if heat treatment at high temperatures is avoided. Thus, if the loaded support material is dried at moderate temperatures and there is no need to subsequently calcine the material at high temperatures, the material exhibits high catalytic activity in the oxygen evolution reaction under acidic conditions and is therefore excellently suitable as a catalyst in the anode side of a PEM water electrolyzer or a PEM fuel cell.

[0105] Embodiment 2 of the present invention (EB2)

[0106] In EB2, porous carbon materials ( Heraeus) instead of TiO2 as carrier material. The amount ratio between the iridium starting compound and the carrier material is selected so that a loaded carrier material with an iridium content of about 30% by weight is obtained. In addition, the deposition of the iridium-containing solid on the carrier material is carried out under the same conditions as in EB1.

[0107] After separation from the aqueous deposition medium, the loaded support material was dried at 120° C. No downstream thermal treatment at higher temperatures was performed. XPS analysis showed that the dry iridium-containing solid present on the support was iridium oxyhydroxide oxidized.

[0108] The carbon material loaded with iridium oxide oxidized by hydrazine dried at 120° C. was subjected to the above-mentioned electrochemical activity measurement. The activity of iridium was measured to be 625 mA / g. Therefore, even in the case where a carbon-based support material is used instead of an oxide support material, if no thermal post-treatment at high temperature is required, a very high electrochemical activity is exhibited in terms of oxygen evolution reaction.

Claims

1. A method for preparing a catalyst composition, wherein: - depositing the iridium-containing solid on the support material in an aqueous medium comprising an iridium compound at a temperature of 40° C. to 100° C. and at a pH value of ≥ 9, - separating the support material carrying the iridium-containing solid from the aqueous medium and drying it, wherein in the method, the support material carrying the iridium-containing solid is not subjected to a heat treatment at a temperature exceeding 250° C. for a duration exceeding 1 hour, and The iridium-containing solid obtained after drying is iridium oxyhydroxide.

2. The method according to claim 1, wherein the support material is an oxide of a transition metal, an oxide of a main group metal, SiO2 or a carbon material; and / or the BET specific surface area of ​​the support material is less than 100 m 2 / g.

3. The method according to claim 2, wherein the transition metal oxide is titanium oxide, zirconium oxide, niobium oxide, tantalum oxide or cerium oxide.

4. The method of claim 3, wherein the transition metal oxide is TiO2.

5. The method according to claim 2, wherein the carbon material serving as a support material has a degree of graphitization of at least 60%.

6. The process according to one of the preceding claims, wherein the iridium compound present in the aqueous medium is an iridium(IV) compound or an iridium(III) compound.

7. The method of claim 6, wherein the iridium (IV) or iridium (III) compound is a salt or an iridium-containing acid.

8. The method according to claim 7, wherein the salt is an iridium halide, the anion is a chloride complex IrCl6 2- salt, iridium nitrate or iridium acetate.

9. The process according to claim 1, wherein the pH of the aqueous medium used to deposit the iridium-containing solid on the support material is ≥ 10.

10. The method according to claim 9, wherein the pH value of the aqueous medium is ≥ 11.

11. The process of claim 1, wherein the support material carrying the iridium-containing solid is not subjected to a heat treatment at a temperature exceeding 200°C for a duration exceeding 30 minutes during the process.

12. The process of claim 1, wherein the support material carrying the iridium-containing solid is dried at a temperature not exceeding 200°C and is not subjected to further heat treatment after drying.

13. The process according to claim 1, wherein the support material on which the iridium hydroxide oxidizes contains a maximum proportion of 50% by weight of iridium; and / or the iridium hydroxide oxidized on the support material has an atomic ratio of iridium (IV) to iridium (III) of 1.0 / 1.0 to 1.7 / 1.0 as determined by X-ray photoelectron spectroscopy (XPS).

14. The process according to claim 1, wherein the support material on which the iridium hydroxide oxidizes contains a maximum proportion of 50% by weight of iridium; and / or the iridium hydroxide oxidizes present on the support material has an atomic ratio of iridium (IV) to iridium (III) of 1.2 / 1.0 to 1.5 / 1.0 as determined by X-ray photoelectron spectroscopy (XPS).

15. The method of claim 1, wherein the support material carrying the iridium-containing solid is dispersed in a liquid medium after drying to obtain a catalyst-containing ink.

16. A catalyst composition obtainable by the process according to one of claims 1 to 15, comprising a support material and iridium hydroxide oxidized on the support material.

17. The catalyst composition of claim 16, wherein the iridium hydroxide oxidized on the support material has an atomic ratio of iridium (IV) to iridium (III) of 1.0 / 1.0 to 1.7 / 1.0 as determined via X-ray photoelectron spectroscopy (XPS).

18. The catalyst composition of claim 16, wherein the iridium hydroxide oxidized on the support material has an atomic ratio of iridium (IV) to iridium (III) of 1.2 / 1.0 to 1.5 / 1.0 as determined via X-ray photoelectron spectroscopy (XPS).

19. An electrolysis cell comprising the catalyst composition according to any one of claims 16 to 18.

20. The electrolyser of claim 19, which is a PEM electrolyser.

21. A fuel cell comprising the catalyst composition according to any one of claims 16 to 18.

22. The fuel cell according to claim 21, which is a PEM fuel cell.

23. Use of the catalyst composition according to any one of claims 16 to 18 as a catalyst for oxygen evolution reaction in water electrolysis.

Citation Information

Patent Citations

  • Precious metal oxide catalyst for water electrolysis

    EP2608297A1

  • Electro-catalyst for fuel cells and method for its production

    EP2608298A1

  • Carrier catalyst and method for producing a porous graphitised carbon material coated with metal nanoparticles

    EP2954951A1

  • Precious metal oxide catalyst for water electrolysis

    WO2005049199A1

  • Electrode catalyst for fuel cell and method of preparation, membrane electrode assembly (mea) including the catalyst, and fuel cell including the mea

    EP2575202A2