A method for preparing supercapacitor carbon

By using silicate as an activator, combined with frozen treatment and ball milling technology, the problem of traditional activator etching is solved, and supercapacitor carbon with high specific surface area and rich pore size is formed, which improves the electrochemical performance and energy storage capacity of the supercapacitor.

CN114084887BActive Publication Date: 2024-11-01PU RUIFEN ACTIVATED CARBON PRODUCTION BRANCH OF INNER MONGOLIA SHUANGXIN ENERGY CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111300744.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-04
Publication Date
2024-11-01
Estimated Expiration
2041-11-04

AI Technical Summary

Technical Problem

Traditional activators etch out a large amount of carbon precursors during the activation of biomass carbon, resulting in poor yields. Common KOH activators show narrow microporous properties, limiting the transport of large-sized ions and destroying Electrochemical properties of supercapacitors.

Method used

Silicate is used as the activator, and the carbon precursor is fully mixed with sodium silicate through refrigeration and ball milling, and high-temperature activation carbonization treatment under an inert gas environment to form supercapacitor carbon with rich graded pore size and high specific surface area.

Benefits of technology

Supercapacitor carbon with excellent electrochemical properties was obtained, which improved the specific surface area and pore size distribution, enhanced the energy storage performance of supercapacitors, and was simple in process and low in cost, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114084887B_ABST
    Figure CN114084887B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing supercapacitor carbon, comprising the steps of S1. washing the peel with water, freezing it and then freeze-drying it; S2. crushing and screening it; S3. mixing it with sodium silicate and grinding it; S4. activating carbonization in a reaction furnace and in an inert gas environment and cooling it with the furnace; S5. filtering, washing, drying and cooling it with the furnace. Supercapacitor carbon is obtained. The freeze-drying process preserves the loose pores and pore structure integrity in the peel, and Na2SiO3 is used as an activator to form a porous structure rich in mesopores and macropores and increase its specific surface area. The method of the present invention is simple and convenient, low in cost, and is conducive to large-scale production. The obtained supercapacitor carbon has a porous structure rich in mesopores and macropores and a high surface area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of activated carbon materials, and in particular to a method for preparing supercapacitor carbon. Background Art

[0002] Carbon materials have been widely used in energy storage devices, adsorption or catalysis due to their outstanding features such as diverse morphology, high conductivity, non-toxicity, and large specific surface area. Especially in the energy storage of supercapacitors, carbonaceous materials are the most widely used electrode materials. As supercapacitor electrode materials, carbon materials mainly store charges on the interface double layer through electrochemical double layer capacitors. Carbon materials with rich porous structures with suitable pore sizes, high specific surface areas and rich surface functional groups are urgent requirements for improving the electrochemical performance of supercapacitors.

[0003] Biomass is selected as the carbon source for the preparation of activated carbon because of its extremely abundant source, low cost and renewable nature, thus generating high returns. However, direct pyrolysis of biomass carbon precursors also faces many disadvantages, such as severe shrinkage during pyrolysis, resulting in low specific surface area, surface inertness, lack of active sites, etc. Biomass materials are usually activated to increase specific surface area and rich porous structure. However, traditional activators, such as KOH, NaOH, Na2CO3, K2CO3 or metal chlorides, always etch away a large amount of carbon precursors, resulting in poor yields. In addition, common KOH activators usually show narrow micropore characteristics, which limits the transmission of large-sized ions and destroys its electrochemical performance as a motor material for supercapacitors. Summary of the invention

[0004] In view of the above problems existing in the prior art, the present invention proposes a method for preparing supercapacitor carbon, using silicate as an activator to prepare biomass supercapacitor carbon. The present invention can obtain supercapacitor carbon with rich graded pore size and high specific surface area, excellent electrochemical properties, and can be used as supercapacitor electrode.

[0005] To achieve the above object, the method for preparing supercapacitor carbon according to the present invention comprises the following steps:

[0006] S1. Wash the peel with water, freeze it, and then freeze-dry it to obtain a carbon source;

[0007] S2. crushing and sieving the carbon source to obtain a carbon precursor;

[0008] S3. mixing the carbon precursor with sodium silicate and ball milling;

[0009] S4. The mixture of the carbon precursor and sodium silicate obtained in step S3 is activated and carbonized in an inert gas environment in a reaction furnace and cooled to room temperature with the furnace;

[0010] S5. Filter the mixture of step S4, wash it with water, dry it, and cool it in the furnace.

[0011] According to one aspect of the present invention, in step S1, the freezing treatment is to perform freezing at a temperature of -18°C to -20°C for 12 hours to 24 hours; the freeze drying treatment is to perform freeze drying at a temperature of -20°C to -40°C in a freeze dryer for 8 hours to 12 hours;

[0012] For biomass peels, a large amount of water in the peels is first frozen into a solid state, and then the water is directly sublimated into water vapor and discharged through a freeze dryer, which maximizes the preservation of the integrity of the loose pores and pore structure in the peels, ensuring that the pores and pore structure will not collapse and cause a reduction in the porosity of the carbon raw material, which is crucial for obtaining supercapacitor carbon with a high specific surface area in subsequent steps.

[0013] According to one aspect of the present invention, preferably, in step S1, the freezing treatment is to perform freezing at a temperature of -18°C for 24 hours; the freeze-drying treatment is to perform freeze-drying at a temperature of -20°C in a freeze dryer for 12 hours;

[0014] According to one aspect of the present invention, preferably, in step S1, the freezing treatment is to perform freezing at a temperature of -20°C for 12 hours; the freeze drying treatment is to perform freeze drying at a temperature of -40°C for 8 hours in a freeze dryer;

[0015] According to one aspect of the present invention, preferably, in step S1, the freezing treatment is to perform freezing at a temperature of -19°C for 18 hours; the freeze-drying treatment is to perform freeze-drying at a temperature of -30°C in a freeze dryer for 10 hours;

[0016] According to one aspect of the present invention, in step S2, after being crushed in a crusher for 20-40 minutes, a carbon precursor with a particle diameter of less than or equal to 200 mesh is obtained by sieving. The particle diameter of the carbon precursor is less than or equal to 0.076 mm. The tiny particles are beneficial for sufficient mixing with sodium silicate in the next step.

[0017] According to one aspect of the present invention, in step S3, the carbon precursor and the sodium silicate are mixed at a mass ratio of 1: (1-5), and then ball-milled in a ball mill for 20-60 minutes to obtain a mixture of the carbon precursor and the activated material. The steel balls in the ball mill are in point contact with the material. This grinding method makes the carbon precursor and the sodium silicate finer in particle size, making it easier for the fine sodium silicate particles to enter the pores of the carbon precursor particles. The more sodium silicate particles contained in the carbon precursor particles, the better support can be given to the carbon precursor in the activated carbonization reaction in the next step, forming a large number of mesopores with a pore size of 2nm-50nm and macropores with a pore size of >50nm. Such a graded pore structure can well regulate the distribution of pore size while increasing the specific surface area.

[0018] According to one aspect of the present invention, preferably, in step S3, the carbon precursor and the sodium silicate are mixed at a mass ratio of 1:1, and then ball-milled in a ball mill for 20 minutes to obtain a mixture of the carbon precursor and the activated substance.

[0019] According to one aspect of the present invention, preferably, in step S3, the carbon precursor and the sodium silicate are mixed at a mass ratio of 1:5, and then ball-milled in a ball mill for 60 minutes to obtain a mixture of the carbon precursor and the activated substance.

[0020] According to one aspect of the present invention, preferably, in step S3, the carbon precursor and the sodium silicate are mixed at a mass ratio of 1:3, and then ball-milled in a ball mill for 40 minutes to obtain a mixture of the carbon precursor and the activated substance.

[0021] According to one aspect of the present invention, in step S4, the inert gas is nitrogen or argon; the activated carbonization treatment is to heat up to 700°C-1000°C at a heating rate of 1°C-5°C / min, and keep the temperature constant for 2h-4h. This step is a key step in preparing supercapacitor carbon. Under the protection of the inert gas, a constant heating rate is maintained and the temperature is kept constant for a suitable time. During the heat treatment, the carbon precursor will be converted into carbon, and Na2SiO3 can support the carbon precursor framework to prevent it from shrinking. After Na2SiO3 is washed and etched with water, a carbon material with a rich porous structure and a high specific surface area can be obtained.

[0022] According to one aspect of the present invention, preferably, in step S4, the inert gas is nitrogen or argon; the activated carbonization treatment is to increase the temperature to 700° C. at a heating rate of 1° C. and keep the temperature constant for 2 hours.

[0023] According to one aspect of the present invention, preferably, in step S4, the inert gas is nitrogen or argon; the activated carbonization treatment is to increase the temperature to 1000° C. at a heating rate of 5° C. / min and keep the temperature constant for 4 hours.

[0024] According to one aspect of the present invention, preferably, in step S4, the inert gas is nitrogen or argon; the activated carbonization treatment is to increase the temperature to 850° C. at a heating rate of 3° C. / min and keep the temperature constant for 3 hours.

[0025] According to one aspect of the present invention, in step S5, the mixture is preheated in an oven and then dried in an oven at a temperature of 60°C-80°C for 8h-12h, and then cooled to room temperature in the oven to obtain supercapacitor carbon.

[0026] According to one aspect of the present invention, the peel is one or more of dragon fruit peel and citrus fruit peel. Preferably, the peel is not rotten or air-dried, and its pore structure is in a state of not collapsing or shrinking.

[0027] The peel of pitaya and citrus fruits accounts for 22% to 30% of the weight of fresh fruit. The fresh peel contains 91.19±0.17% water and 4% carbohydrates. After removing the water, the dry matter contains 14.29±0.95% ash, 2.46±0.28% fat, 31.40±0.24% crude fiber, and 6.39±0.13% crude protein. As a biomass raw material, this kind of peel does not contain a lot of ash and volatile matter like coal raw materials, and requires subsequent complex steps to remove it. It has a loose and porous structure and is rich in nitrogen, making it a high-quality source of raw materials for supercapacitor carbon.

[0028] With the widespread application of supercapacitors, people have been looking for more ideal supercapacitor electrode materials through research and development of their energy storage mechanism and preparation methods, in order to create new commercial energy storage devices to improve the power density and energy density of supercapacitors. Moreover, in terms of production cost, biomass carbon materials are undoubtedly the cheapest electrode materials among supercapacitor electrode materials so far. The wide source and low cost of activated carbon are also important reasons why it has always been popular. Supercapacitor carbon obtained by activating and carbonizing biomass carbon materials, as a key material for supercapacitors, directly affects the performance of supercapacitors;

[0029] Activated carbon is a porous material composed of amorphous carbon and graphite microcrystals. Generally, the specific surface area of ​​porous carbon is greater than 500m 2 / g is called activated carbon, and the specific surface area is greater than 1000m 2 / g is called supercapacitor carbon. Due to the large specific surface area of ​​activated carbon due to its micropores, electrode materials containing activated carbon are usually used as electrodes of supercapacitors, so that their surfaces are in contact with electrolytes to form double-layer capacitors. In theory, the larger the specific surface area of ​​an electrode material, the larger its capacity and the more suitable it is as a capacitor electrode material. In fact, studies have found that the actual utilization rate of carbon materials with high specific surface area is not high, because the pore size of carbon materials is divided into micropores, which are pores with a diameter less than 20nm; mesopores are pores with a diameter less than 20nm and greater than 50nm; and macropores are pores with a diameter greater than 50nm. Among them, only materials with a pore size greater than 20nm that are beneficial for forming a double layer can be used as supercapacitor electrodes. Therefore, while increasing the specific surface area, the distribution of pore size must also be regulated.

[0030] The preparation method of supercapacitor carbon to which the present invention relates has the following beneficial effects: first, pitaya and citrus fruits are common fruits, and their peels are rich in vitamins, so they are rich in nitrogen elements and are high-quality carbon and nitrogen precursors. Secondly, for the biomass peel, a large amount of water in the peel is first frozen to freeze into a solid state, and then the water is directly sublimated into water vapor and discharged through a freeze dryer, which maximizes the preservation of the integrity of the loose holes and pore structures in the peel, ensuring that the holes and pore structures will not collapse to cause a reduction in the porosity of the carbon raw material, which is very important for obtaining supercapacitor carbon with a high specific surface area through subsequent steps. In addition, the present invention is used to prepare porous biomass carbon material supercapacitor carbon by using low-cost sodium silicate as an activator. Na2SiO3, as an activator, plays an important role in forming a rich porous structure rich in mesopores and macropores and increasing its specific surface area. Then, in the method involved in the present invention, the mixture of sodium silicate and biomass only needs to be solid ground, followed by activated carbonization and washing to obtain supercapacitor carbon. This solvent-free process is simple and convenient, low-cost, requires simple equipment, and is conducive to large-scale production. The obtained super activated carbon has a hierarchical porous structure rich in mesopores and macropores and a high surface area, which is conducive to improving the electrochemical performance of supercapacitors and obtaining higher specific capacitance.

[0031] In summary, loose and porous peel is used as a carbon source, and it is subjected to freezing and freeze-drying to obtain a carbon precursor. Sodium silicate is used as an activator, and the carbon precursor and the activator are more fully mixed by ball milling. Sodium silicate supports the carbon skeleton to form pores, and prevents it from shrinking and collapsing during the high-temperature activated carbonization process, thereby obtaining a supercapacitor carbon with rich pore structure and high specific surface area, and its specific surface area ranges from 1100g / m 2 -2000g / m 2The specific capacity range at 1A / g is 150F / g-350F / g, the rate range at 10A / g is 65%-80%, and the impedance Rct range is 0.01Ω-0.09Ω. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is a flow chart schematically showing a method for preparing supercapacitor carbon according to the present invention. DETAILED DESCRIPTION

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0034] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The embodiments cannot be described one by one here, but the embodiments of the present invention are not therefore limited to the following embodiments.

[0035] Combination Figure 1 As shown, a method for preparing supercapacitor carbon according to one embodiment of the present invention comprises the following steps:

[0036] S1. Wash the peel with water, freeze it and freeze-dry it to obtain a carbon source; the freezing treatment is freezing at a temperature of -18°C to -20°C for 12h-24h; the freeze-drying treatment is freeze-drying in a freeze dryer at a temperature of -20°C to -40°C for 8h-12h;

[0037] S2. The carbon source is crushed in a pulverizer for 20 min-40 min, and then sieved to obtain a carbon precursor having a particle diameter of less than or equal to 200 mesh;

[0038] S3. After mixing the carbon precursor and sodium silicate at a mass ratio of 1:1-5, the mixture is ball-milled in a ball mill for 20 min-60 min to obtain a mixture of the carbon precursor and the activated product.

[0039] S4. The mixture of the carbon precursor obtained in step S3 and sodium silicate,

[0040] In an inert gas environment, an activated carbonization treatment is carried out in a reaction furnace and cooled to room temperature along with the furnace; the activated carbonization treatment is to increase the temperature to 700°C-1000°C at a heating rate of 1°C-5°C / min and keep the temperature constant for 2h-4h.

[0041] S5. After filtering and washing the mixture in step S4, the mixture is preheated in an oven and then dried at a temperature of 60°C-80°C for 8h-12h and then cooled to room temperature.

[0042] According to an embodiment of the present invention, the peel is one or more of dragon fruit peel and citrus fruit peel. Preferably, the peel is not rotten or air-dried, and its pore structure is in a state of not collapsing or shrinking.

[0043] For biomass peels, a large amount of water in the peels is first frozen into a solid state, and then the water is directly sublimated into water vapor and discharged through a freeze dryer, which maximizes the preservation of the integrity of the loose pores and pore structure in the peels, ensuring that the pores and pore structure will not collapse and cause a reduction in the porosity of the carbon raw material, which is crucial for obtaining supercapacitor carbon with a high specific surface area in subsequent steps.

[0044] A method for preparing supercapacitor carbon according to one embodiment of the present invention comprises the following steps:

[0045] S1. Washing the orange peel whose pore structure is in a state of non-collapse and non-contraction, freezing and freeze-drying the peel to obtain a carbon source; freezing is performed at -18°C for 24 hours; freeze-drying is performed in a freeze dryer at -20°C for 12 hours;

[0046] S2. The carbon source is crushed in a pulverizer for 20 min-40 min, and then sieved to obtain a carbon precursor having a particle diameter of less than or equal to 200 mesh;

[0047] S3. After mixing the carbon precursor and sodium silicate at a mass ratio of 1:1, the mixture is ball-milled in a ball mill for 20 min to 60 min to obtain a mixture of the carbon precursor and the activated substance.

[0048] S4. The mixture of the carbon precursor and sodium silicate obtained in step S3 is subjected to an activated carbonization treatment in a reaction furnace in a nitrogen environment, and then cooled to room temperature along with the furnace; the activated carbonization treatment is performed by heating the temperature to 800°C at a heating rate of 5°C / min and keeping the temperature constant for 2 hours.

[0049] S5. Filter the mixture in step S4, wash it with water, preheat it in an oven, dry it in an oven at 60°C, keep it at a constant temperature for 12 hours, and then cool it to room temperature. The specific surface area of ​​the obtained supercapacitor carbon is 1159g / m 2 The specific capacity at 1A / g is 169F / g, the rate at 10A / g is 69.5%, and the impedance Rct is 0.06Ω.

[0050] A method for preparing supercapacitor carbon according to another embodiment of the present invention comprises the following steps:

[0051] S1. Washing the grapefruit peel whose pore structure is in a state of non-collapse and non-contraction, freezing treatment and freeze-drying treatment to obtain a carbon source; freezing treatment is freezing at -20°C for 12 hours; freeze drying treatment is freeze drying at -40°C in a freeze dryer for 8 hours;

[0052] S2. The carbon source is crushed in a pulverizer for 20 min-40 min, and then sieved to obtain a carbon precursor having a particle diameter of less than or equal to 200 mesh;

[0053] S3. After mixing the carbon precursor and sodium silicate at a mass ratio of 1:4, the mixture is ball-milled in a ball mill for 20 min to 60 min to obtain a mixture of the carbon precursor and the activated substance.

[0054] S4. The mixture of the carbon precursor and sodium silicate obtained in step S3 is subjected to an activated carbonization treatment in a reaction furnace under argon protection, and then cooled to room temperature along with the furnace; the activated carbonization treatment is performed by heating the temperature to 800°C at a heating rate of 5°C / min and keeping the temperature constant for 2 hours.

[0055] S5. Filter the mixture in step S4, wash it with water, preheat it in an oven, dry it in an oven at 80°C, keep it at a constant temperature for 8 hours, and then cool it to room temperature. The specific surface area of ​​the obtained supercapacitor carbon is 1395g / m 2 The specific capacity at 1A / g is 202F / g, the rate at 10A / g is 71.3%, and the impedance Rct is 0.08Ω.

[0056] Preferably, a method for preparing supercapacitor carbon according to another embodiment of the present invention comprises the following steps:

[0057] S1. Wash the pitaya peel whose pore structure is in a state of non-collapse and non-contraction, and then freeze it; then freeze-dry it to obtain a carbon source; the freezing treatment is freezing at -19°C for 18 hours; the freeze-drying treatment is freeze-drying in a freeze dryer at -30°C for 10 hours;

[0058] S2. The carbon source is crushed in a pulverizer for 20 min-40 min, and then sieved to obtain a carbon precursor having a particle diameter of less than or equal to 200 mesh;

[0059] S3. After mixing the carbon precursor and sodium silicate at a mass ratio of 1:3, the mixture is ball-milled in a ball mill for 20 min to 60 min to obtain a mixture of the carbon precursor and the activated product.

[0060] S4. The mixture of the carbon precursor and sodium silicate obtained in step S3 is subjected to an activated carbonization treatment in a reaction furnace under a nitrogen environment, and then cooled to room temperature along with the furnace; the activated carbonization treatment is performed by heating the temperature to 800°C at a heating rate of 5°C / min and keeping the temperature constant for 2 hours.

[0061] S5. Filter the mixture in step S4, wash it with water, preheat it in an oven, dry it in an oven at 70°C, keep it at a constant temperature for 10 hours, and cool it to room temperature. The specific surface area of ​​the obtained supercapacitor carbon is 1573g / m 2 The specific capacity at 1A / g is 256F / g, the rate at 10A / g is 70%, and the impedance Rct is 0.04Ω.

[0062] Preferably, a method for preparing supercapacitor carbon according to another embodiment of the present invention comprises the following steps:

[0063] S1. Wash the pitaya peel whose pore structure is in a state of non-collapse and non-contraction, and then freeze it; then freeze-dry it to obtain a carbon source; the freezing treatment is freezing at -19°C for 18 hours; the freeze-drying treatment is freeze-drying in a freeze dryer at -30°C for 10 hours;

[0064] S2. The carbon source is crushed in a pulverizer for 20 min-40 min, and then sieved to obtain a carbon precursor having a particle diameter of less than or equal to 200 mesh;

[0065] S3. After mixing the carbon precursor and sodium silicate at a mass ratio of 1:2, the mixture is ball-milled in a ball mill for 20 min to 60 min to obtain a mixture of the carbon precursor and the activated substance.

[0066] S4. The mixture of the carbon precursor and sodium silicate obtained in step S3 is subjected to an activated carbonization treatment in a reaction furnace under a nitrogen environment, and then cooled to room temperature along with the furnace; the activated carbonization treatment is performed by heating the temperature to 800°C at a heating rate of 5°C / min and keeping the temperature constant for 2 hours.

[0067] S5. Filter the mixture in step S4, wash it with water, preheat it in an oven, dry it in an oven at 70°C, keep it at a constant temperature for 10 hours, and cool it to room temperature. The specific surface area of ​​the obtained supercapacitor carbon is 1778g / m 2 The specific capacity at 1A / g is 323F / g, the rate at 10A / g is 76.2%, and the impedance Rct is 0.02Ω.

[0068] In the ball mill, the steel balls and materials are in point contact. This grinding method makes the carbon precursor and sodium silicate particles finer, making it easier for the fine sodium silicate particles to enter the pores of the carbon precursor particles. The more sodium silicate particles contained in the carbon precursor particles, the better support the carbon precursor can provide in the next step of the activated carbonization reaction, forming a large number of mesopores, that is, pores with a diameter between 2nm-50nm; and macropores, that is, pores with a diameter greater than 50nm. A pore structure with a large number of mesopores and macropores is formed, which improves the specific surface area while well regulating the distribution of pore size.

[0069] In step S4, this step is a key step in preparing supercapacitor carbon. Under the protection of inert gas, a constant heating rate is maintained and the temperature is kept constant for a suitable time. During the heat treatment process, the carbon precursor is converted into carbon, and Na2SiO3 can support the carbon precursor framework to prevent it from shrinking. After washing and etching Na2SiO3, a carbon material with a rich porous structure and a high specific surface area can be obtained.

[0070] The above contents are merely examples of specific solutions of the present invention. For devices and structures not described in detail therein, it should be understood that they can be implemented by adopting general devices and general methods available in the art.

[0071] The above is only one solution of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing supercapacitor carbon, characterized in that: The following steps are involved: S1. Wash the peel with water, freeze it at -18°C to -20°C for 12h-24h, and then freeze-dry it in a freeze dryer at -20°C to -40°C for 8h-12h; S2. After crushing in a pulverizer for 20min-40min, sieving to obtain a carbon precursor having a particle diameter of less than or equal to 200 mesh; S3. The carbon precursor and sodium silicate are mixed in a mass ratio of 1:1-5, and then ball-milled in a ball mill for 20min-60min to obtain a mixture of a carbon precursor and an activated substance; S4. In a reactor, in an inert gas environment, at a heating rate of 1°C-5°C / min, the temperature is raised to 700°C-1000°C, kept constant for 2h-4h, and cooled with the furnace, the inert gas being nitrogen or argon; S5. Filter and wash. After the mixture is preheated in an oven, it is dried in an oven at a temperature of 60° C. for 12 hours and then cooled in the oven.

2. The method for preparing supercapacitor carbon according to claim 1, characterized in that: In step S1, the freezing treatment is to freeze at -18°C for 24 hours; and the freeze-drying treatment is to freeze-dry in a freeze dryer at -20°C for 12 hours.

3. The method for preparing supercapacitor carbon according to claim 1, characterized in that: In step S1, the freezing treatment is to freeze at -20°C for 12 hours; and the freeze-drying treatment is to freeze-dry in a freeze dryer at -40°C for 8 hours.

4. The method for preparing supercapacitor carbon according to claim 1, characterized in that: In step S1, the freezing treatment is to freeze at a temperature of -19°C for 18 hours; and the freeze-drying treatment is to freeze-dry in a freeze dryer at a temperature of -30°C for 10 hours.

5. The method for preparing supercapacitor carbon according to claim 1, characterized in that: In step S3, the carbon precursor and the sodium silicate are mixed at a mass ratio of 1:1, and then ball-milled in a ball mill for 20 minutes to obtain a mixture of the carbon precursor and the activated substance.

6. The method for preparing supercapacitor carbon according to claim 1, characterized in that: In step S3, the carbon precursor and the sodium silicate are mixed at a mass ratio of 1:4, and then ball-milled in a ball mill for 60 minutes to obtain a mixture of the carbon precursor and the activated product.

7. The method for preparing supercapacitor carbon according to claim 1, characterized in that: In step S3, the carbon precursor and the sodium silicate are mixed at a mass ratio of 1:3, and then ball-milled in a ball mill for 40 minutes to obtain a mixture of the carbon precursor and the activated product.

8. The method for preparing supercapacitor carbon according to claim 1, characterized in that: In step S3, the carbon precursor and the sodium silicate are mixed at a mass ratio of 1:2, and then ball-milled in a ball mill for 40 minutes to obtain a mixture of the carbon precursor and the activated substance.

9. The method for preparing supercapacitor carbon according to claim 1, characterized in that: In step S4, the inert gas is nitrogen or argon; the temperature is increased to 800° C. at a heating rate of 5° C. / min and kept constant at that temperature for 2 hours.

10. The method for preparing supercapacitor carbon according to claim 1, characterized in that: In step S5, the mixture is preheated in an oven and then dried in an oven at a temperature of 80° C. for 8 hours.

11. The method for preparing supercapacitor carbon according to claim 1, characterized in that: In step S5, the mixture is dried in an oven after being preheated, the drying temperature is 70° C., and the drying is carried out at a constant temperature for 10 hours.

12. The method for preparing supercapacitor carbon according to any one of claims 1 to 11, characterized in that: The peel is pitaya peel or citrus fruit peel.

13. A supercapacitor carbon prepared according to the supercapacitor carbon preparation method according to claim 12, characterized in that: The activated carbon for supercapacitor has a specific surface area range of 1100 g / m 2- 2000g / m 2 The specific capacity range at 1A / g is 150F / g-350F / g, the rate range at 10A / g is 65%-80%, and the impedance Rct range is 0.01Ω-0.09Ω.