Process for preparing a catalyst for ammonia synthesis by reducing iron oxides
The water concentration during iron oxide reduction process was measured by an NDIR detector and the gas flow rate and heating rate were adjusted, which solved the problem of water toxicity in ammonia synthesis, improved the activation efficiency and speed of the catalyst, and simplified the measurement process.
Patent Information
- Application Number
- CN202080047795.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-24
- Filing Date
- 2020-07-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-07-08
AI Technical Summary
During the ammonia synthesis process, the water formed during the reduction of iron oxides is used as a catalyst poison, resulting in a slow and time-consuming reduction process. The existing methods determine the water content cumbersome and delayed.
The water concentration in the gas phase was measured by non-dispersive infrared spectroscopy (NDIR) and the flow rate and heating rate of the reducing gas were adjusted according to the measurement results to control the water concentration within a specific range and simplify the reduction process.
Directly measuring the water concentration through the NDIR detector simplifies the reduction process, significantly reduces the harmful concentration of the catalyst to water, improves the activation efficiency and activation speed of the catalyst, and reduces time overhead.
Smart Images

Figure CN114096348B_ABST
Abstract
Description
Background Art
[0001] In the preparation of catalysts and / or catalyst precursors based on iron oxides for ammonia synthesis, the iron oxides are usually reduced in a reactor using a reducing gas. In this case, highly catalytically active forms of elemental iron are formed, in particular the alpha iron form in the cubic space center. Reduced iron catalysts of this type can be used particularly well as catalysts for ammonia synthesis, in particular the Haber-Bosch synthesis.
[0002] During the reduction of the iron oxides, water is formed, which can act as a catalyst poison. In order to limit the amount of water formed during the reduction, the reduction process is therefore often carried out very slowly and carefully. In addition, the concentration of the water formed is determined at regular intervals by the asbestos method. In this analysis, the water content is determined by passing a defined amount of sample gas through an adsorbent, which adsorbs only the water in the sample gas. The weight difference of the adsorbent is then determined and the amount of water is calculated using the measured volume flow. This type of method is very time-consuming and only provides information about the water content of the sample with a certain delay. Summary of the invention
[0003] The object of the present invention is to provide a method for activating catalysts and catalyst precursors for ammonia synthesis which improves on the above-mentioned disadvantages. Furthermore, the use of an NDIR detector for determining the water concentration during the reduction of iron oxides is described.
[0004] The subject of the present invention is a method for activating catalysts and catalyst precursors for ammonia synthesis, comprising the following method steps:
[0005] (A) reducing the iron oxides using at least one reducing gas and by heating in order to activate the catalyst,
[0006] (B) measuring the concentration of water formed in the gas phase during the reduction by means of non-dispersive infrared spectroscopy (NDIR), and
[0007] (C) The flow rate of the reducing gas and / or the heating rate are set according to the concentration of water formed.
[0008] Non-dispersive infrared spectroscopy (NDIR) involves emitting infrared radiation of a defined wavelength into a sample to measure the spectroscopic analysis of the gas. As a function of the gas concentration in the beam path, the infrared beam is attenuated due to absorption. Pressure differences are thus generated inside the photopneumatic receiver, i.e. inside the NDIR sensor, which pressure differences can be converted into voltages, for example, by a micro flow sensor, and give information about the number of absorbing gas molecules in the sample. For the construction of NDIR sensors known to those skilled in the art, reference is made to the manual "XStream Gas Analyzers, XStream X2 Series" by Emerson Process Management GmbH & Co. OHG, May 2017 edition, sections 3.1.2 and 3.1.3.
[0009] In this case, the water concentration can be determined directly with the aid of NDIR and, in contrast to conventional methods, does not require tedious analysis, so that the flow rate of the reducing gas and / or the heating rate can be set particularly simply as a function of the water concentration in the reactor outlet gas and, thus, the occurrence of water concentrations that are harmful to the catalyst can be reduced during the reduction.
[0010] With the method according to the invention, it is possible to prepare finished catalysts from iron oxides or to activate them and to use them directly after activation for the synthesis of ammonia from synthesis gas, for example, which contains a mixture of nitrogen and hydrogen. It is also possible with the method according to the invention to prepare prereduced catalyst precursors, which are first reduced under controlled conditions and subsequently passivated in an oxidizing atmosphere and then used as catalysts in the synthesis of ammonia. These prereduced catalysts can be activated significantly faster and under milder conditions than iron oxides.
[0011] In addition, the concentration of water determined in method step (B) can be compared with a predetermined limit value of water in method step (C). This can be done, for example, by defining a range around the limit value and setting the flow rate and / or heating rate of the reducing gas as a function of the measured water concentration so that the concentration of water fluctuates within a predetermined range near the limit value. In particular, at the beginning of the method, the water concentration may fluctuate within this range near the limit value and may therefore also be located outside this range. In particular, if the method has not yet been stably operated, the water concentration may exceed 200 ppmv (parts per million by volume) near the limit value for up to 1 h or 400 ppmv for up to 20 min. Once the method is stably operated, the water concentration fluctuates mainly within a range near the limit value.
[0012] In a further embodiment of the process according to the invention, at least one of the following sub-steps is carried out in process step (C):
[0013] (C1) if the water concentration determined in method step (B) is below a range around a predetermined limit value, increasing the heating rate, or
[0014] (C2) if the water concentration determined in method step (B) is above a range around a predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or
[0015] (C3) If the water concentration determined in method step (B) is within a range around a predetermined limit value, maintaining the flow rate and / or the heating rate.
[0016] The inventors of the present invention have recognized that the concentration of water formed in the gas phase during the reduction of the iron oxides should advantageously not exceed a limit value of 4000 ppmv, preferably 3400 ppmv, more preferably 3200 ppmv, and even more preferably 3000 ppmv. Reduced iron catalysts activated at higher water concentrations in the gas phase generally show lower activity in the subsequent ammonia synthesis. Activating the iron oxides with a higher proportion of water in the gas phase thus leads to a catalyst with lower activity in the subsequent ammonia synthesis, but at the same time a higher proportion of water can also activate the catalyst faster and therefore more economically. In particular, the range around the limit value is selected from the following ranges: ±1000 ppmv, ±800 ppmv, ±600 ppmv, ±400 ppmv, ±300 ppmv and ±200 ppmv. The range is preferably ±300 ppmv, more preferably ±200 ppmv. Possible is a limit value of 3000 ppmv and a range of ±600 ppmv. Particularly preferred is a limit value of 3000 ppmv and a range of ±200 ppmv.
[0017] In the case of low temperatures in the reactor apparatus, the heating rate can be very large and can be up to 40 K / h, especially at the beginning of the reduction. Conversely, during the reduction of the iron oxides, the heating rate can be in the range of 0 K / h to 2 K / h, as long as the water concentration is within the desired range. The time period for which these small heating rates are employed can be up to 48 h, depending on the flow rate and the catalyst volume.
[0018] According to an advantageous embodiment of the method according to the invention, it can be carried out in a continuous process, wherein method steps (A), (B) and (C) are carried out continuously. Thus, in particular during the reduction of the iron oxides in method step (A), the concentration of water formed during the reduction can be determined by means of NDIR in method step (B) at the same time, and in method step (C) the flow rate of the reducing gas and / or the heating rate can be adjusted accordingly within a short period of time. Thus, all method steps (A) to (C) can advantageously be carried out in parallel or simultaneously with one another, which means a significant time advantage compared to conventional methods in which the result of the caustic soda asbestos method must first be awaited. Thus, the concentration of water can be measured continuously in method step (B) by means of NDIR (two measured values per second), whereas with the caustic soda asbestos method only one measured value is usually obtained every 1 to 2 hours. Furthermore, depending on the water concentration determined in method step (B), substeps (C1), (C2) or (C3) can be carried out successively as many times as desired.
[0019] In another variant of the method according to the invention, the measurement of the water formed during the reduction is carried out in real time in method step (B). This allows to react immediately to changes in the concentration of the formed water and adjust the flow rate and / or heating rate accordingly. In the case of this variant of the method according to the invention, it is especially possible to react to changes in the amount of the formed water within a time period of 1 to 10 min. Depending on the heating rate, the water concentration can be increased from 0 ppmv to a value of up to 3000 ppmv within a time period of 0.5 h to 2 h. Typically, the water concentration in method step (B) is continuously carried out by means of NDIR and controlled every 15 min, and the flow rate and / or heating rate of the reducing gas in method step (C) are adjusted accordingly according to the measured water concentration.
[0020] Advantageously, in the case of the method according to the invention, in method step (A), a mixture containing hydrogen and nitrogen is used as reducing gas, wherein ammonia may have been formed during the reduction of the catalyst due to partial activation of the catalyst. In the case of this type of variant of the method according to the invention, the activation of the catalyst during the method can also be determined by the increased content of ammonia formed in the gas phase. If the method according to the invention is carried out in a reactor that is also used for ammonia synthesis, ammonia synthesis can be started immediately after the activation of the catalyst has been completed, which is particularly simple. The reducing gas can also contain noble gases, such as argon. In particular, all noble gases present in the air can be present in the reducing gas. In addition, methane can also be present in the reducing gas, which has not yet been converted during the reforming of methane to form hydrogen.
[0021] In the case of another advantageous variant of the method according to the invention, in method step (B), the concentration of water formed during the reduction is measured in the wavelength range of 2.6 μm to 3 μm, preferably in the range of 2.7 to 2.8 μm, more preferably in the range of 2.75 μm to 2.79 μm. Usually, the concentration of water is measured at a wavelength of about 6 μm, but here the interference of the absorption band of ammonia is particularly large in this wavelength range. Therefore, in order to reduce this overlap, it is preferred to measure in the wavelength range of 2.6 μm to 3 μm given above.
[0022] Particularly advantageously, in method step (B), an NDIR instrument is used for measuring the water formed, wherein the absorption band of ammonia is calculated by calibration in the wavelength range of 2.6 μm to 3 μm, more preferably in the range of 2.75 μm to 2.79 μm. For example, a calibration curve for calibration can be established by means of experimental data, wherein gas samples with about 0% by volume to 20% by volume are measured by means of NDIR. These calibration curves make it possible to determine the background signal of ammonia in the wavelength range given above as a function of the ammonia concentration and to take it into account in this wavelength range when analyzing water accordingly. The inventors of the method have found that during the reduction of iron oxides with a mixture of hydrogen and nitrogen, ammonia can be formed in an amount of 0% by volume to 20% by volume, wherein the proportion of ammonia in the gas phase increases as the reduction progresses.
[0023] Particularly advantageously, in method step (B), the concentration of ammonia formed during the reduction process can also be determined by means of NDIR. The determination of ammonia, which can also be formed during the reduction process in the presence of nitrogen in the gas phase, can particularly advantageously provide information about the activation process of the catalyst or catalyst precursor. The determination of the concentration of ammonia formed in the gas phase can in this case be carried out particularly simply by means of NDIR in a similar manner to the determination of water in the gas phase, which allows particularly rapid determination of the values. In particular, it is possible to determine ammonia in the sample simultaneously with water by means of NDIR, wherein the concentration of ammonia is advantageously determined in the wavelength range of 10.8 μm to 11.2 μm, preferably at 11 μm. In this range, water does not absorb infrared radiation, so that the concentration of ammonia can be determined particularly simply without correction of the values.
[0024] In the case of another advantageous variant of the method according to the invention, the reduction in method step (A) is carried out in a reactor equipped with a feed line for feeding a reducing gas and a discharge line for discharging a gaseous reaction mixture from the reduction, the reaction mixture containing in particular water formed in the reduction and ammonia that may be formed. The discharge line has a sample line at the reactor outlet for extracting a sample for NDIR measurement. The sample line is advantageously thermally insulated and may also have an additional heating device that ensures that the temperature in the sample line does not drop too much. A drop in temperature leads to condensation of water, which can distort the measurement results obtained by NDIR. If the sample to be measured is obtained directly at the reactor outlet, the heat loss in the reactor outlet line no longer plays such a large role. In the case of this type of variant of the method according to the invention, in method step (B), the sample to be analyzed in the gas phase can be extracted particularly simply through the sample line and the concentration of water and / or the concentration of ammonia can be determined particularly reliably by means of NDIR.
[0025] In particular, the sample to be analyzed can be depressurized to a pressure of about 0.01 to 2 bar gauge (0.0.1 to 2 bar above atmospheric pressure) and then the water content and / or ammonia content can be determined by means of NDIR. The dew point of the sample gas is reduced from about 70° C. to 80° C. before expansion to 0° C. to 10° C. after expansion, preferably to about 10° C., wherein the temperature in the NDIR instrument is usually 40° C. to 50° C. The gas mixture to be measured is allowed to have a temperature of up to 60° C., wherein the lowest temperature can be barely above the dew point. In addition, the sample gas flow to be analyzed can also be filtered to avoid contamination of the NDIR detector. Advantageously, the same flow rate is always set in the measuring device to better obtain reproducible measurement results. The flow rate during the NDIR measurement can be in particular in the range of 0.2 l / min to 1.5 l / min, preferably at 1.5 l / min.
[0026] In another variant of the process according to the invention, the ammonia and / or water formed during the reduction are discharged from the reactor in process step (C) and condensed by means of a cooler. This allows particularly simple extraction of water and any ammonia formed during the reduction process and thus prevents the accumulation of water during the reduction process.
[0027] In method step (C), the temperature of the cooler can also be set so that it is at least 10 K, preferably at least 5 K, above the freezing point of the aqueous ammonia solution. In the case of a method of this type, on the one hand, the temperature of the cooler can be set so that disadvantageous freezing of the cooler is avoided, but on the other hand, the temperature of the cooler can also be reduced to such an extent that a reliable condensation of water and / or ammonia or an aqueous ammonia solution is very likely. Due to the particularly simple and fast NDIR measurement of water and / or ammonia, the reduced method parameters, such as pressure, temperature and flow rate, can be adapted to the respectively measured concentration of water and / or ammonia in the gas phase in order to enable reliable condensation.
[0028] It is particularly easy to feed at least one reducing gas, for example a mixture containing nitrogen and hydrogen, back into the reduction process after separation of water and / or ammonia. Since not all of the reducing gas is consumed during the reduction process, this type of variant of the method according to the invention is particularly economical.
[0029] For the process according to the invention, a reactor device can be used in process step (A) which comprises a reactor for reducing iron oxides, the reactor having a feed line for feeding a reducing gas and a discharge line for discharging a gaseous reaction mixture from the reduction. The reactor device can in particular have a gas circuit, in which the gaseous reaction mixture discharged from the reactor is fed back into the reaction process via a feed line after separation of water and / or ammonia. This type of reactor system can in particular include a reactor for ammonia synthesis, in which a catalyst is obtained from a catalyst precursor by activation by reduction before starting operation. Alternatively, the reactor device can also be a reactor designed to reduce the catalyst, and after the catalyst precursor has been reduced and possibly passivated, they can be removed and discharged therefrom.
[0030] In the case of another embodiment of the method according to the invention, in method step (A), in particular magnetite or pyrite or a combination thereof, preferably pyrite, is used as the iron oxide. Magnetite is a mixed iron oxide having the general chemical formula Fe3O4 and containing divalent and trivalent iron. In contrast, pyrite is iron (II) oxide FeO, which can also have a non-stoichiometric composition Fe 1-x O.
[0031] In process step (A), during the reduction, the temperature can be set in the range from 360° C. to 450° C., preferably in the range from 370° C. to 400° C. (for wüstite). At these temperatures, the reduction of iron oxides, such as wüstite or magnetite, can be carried out particularly reliably.
[0032] The inventors have established that the reduction of wüstite proceeds already at relatively low temperatures of about 370° C. to 400° C. Water is released during the reduction. In contrast, for the reduction of magnetite with release of water, temperatures of more than 400° C., in particular in the range of 420° C. to 460° C., are required. Therefore, in particular in the case of the reduction of wüstite, it is advantageous to effectively control the process by means of the heating rate and / or the flow rate in order to avoid an excessive increase in the concentration of water in the gas phase already at relatively low temperatures.
[0033] In method step (C), the flow rate (gas hourly space velocity, GHSV) can be set in particular at 1000 h -1 Up to 70000h -1 , preferably 3000h -1 Up to 60000h -1 In process step (A), the pressure can be set at a value of 60 bar to 600 bar, preferably 60 bar to 300 bar, more preferably 60 bar to 180 bar, and more preferably 80 bar to 150 bar. At the beginning, the pressure is about 80 bar, and as the reduction progresses, the pressure can be up to 600 bar, preferably up to 300 bar.
[0034] In process step (A), the reduction can be carried out in particular in a system which has a heating device for heating the at least one reducing gas. The heating device can be present both in the reactor and outside the reactor, such as Figure 1 . The heating device can also be, for example, a heat exchanger in which the heat from the reactor space is transferred to the newly introduced reducing gas. The heating device is necessary in particular at the beginning of the method according to the invention in order to reach the temperature required for the reduction. As the method according to the invention progresses, the proportion of the heating device in the overall heat balance in method step (A) can decrease and the share of the heat of reaction from the formation of ammonia can increase, so that the flow rate can therefore be increased.
[0035] In the case of a further embodiment of the process according to the invention, in process step (D), the catalyst and / or catalyst precursor from process step (C) is exposed to an oxidizing gas in order to form a protective layer on the catalyst and / or catalyst precursor. As oxidizing gas, in particular a gas mixture comprising oxygen or air can be used. In this case, it is particularly advantageous to change the composition of the gas after the reduction has ended and to feed, for example, an oxidizing gas comprising nitrogen and air, so that a passivation layer is formed on the reduced catalyst by oxidation. Before the start-up of the reactor for ammonia synthesis, these catalyst precursors can be subjected to a short reduction step particularly simply and subsequently used as catalyst for ammonia synthesis.
[0036] A subject of the invention is also the use of an NDIR detector for determining the concentration of water formed during the reduction of iron oxides when activating catalysts and catalyst precursors for ammonia synthesis.
[0037] In this type of use, the water concentration can in particular be determined in real time. The reduction can be carried out with the aid of a reducing gas, and the flow rate of the reducing gas and / or the heating rate can be set as a function of the water concentration formed.
[0038] Furthermore, all embodiments which have been mentioned above with regard to the method for activating a catalyst can also be implemented within the scope of use of an NDIR detector.
[0039] The present invention will be described in more detail below with the help of specific embodiments and drawings.
[0040] - Figure 1 A reactor system for carrying out the process according to the invention is shown,
[0041] - Figure 2 and 3 Flow chart showing the method steps for determining water and ammonia by means of NDIR and the subsequent control method,
[0042] - Figure 4 and 5 shows the effect of water content on catalytic activity when reducing iron oxides, and
[0043] - Figure 6 A diagram is shown for the measurement of the water content by means of NDIR during the reduction of iron oxides.
[0044] Figure 1The reactor device for carrying out the method according to the present invention is schematically shown. There is a reactor 10, which has different catalyst beds 10A. The iron oxide to be reduced is located in the catalyst bed 10A. The reactor 10 is equipped with a pipe system 60 with a feed line 60A, through which at least one reducing gas is introduced into the reactor, and equipped with a discharge line 60B, through which the reduced gaseous reaction mixture is discharged from the reactor, so that the gas can be circulated in the reactor device. The direction of the arrow here represents the circulation direction of the gas in the reactor device. During the reduction of the iron oxide, at least one reducing gas can be heated by means of a heating device 50. In addition, there is an NDIR sensor 5, which can measure the water content and / or ammonia content of the reaction gas of the reduction process at the discharge line 60B. For this reason, there is an insulated and heatable pipeline 6 at the discharge line 60B. The pipeline 6 can have a thermal insulation material or a heating device here, which can be used to keep the temperature of the gas mixture to be analyzed high enough to avoid the condensation of water and the distortion of the NDIR measurement results. The pressure in the discharge line 6 was reduced in steps of 1 to 2 barg and then to 0.01 to 0.5 barg for NDIR measurement.
[0045] The operation of an embodiment of the method according to the invention in this reactor arrangement is explained in more detail below.
[0046] At least one reducing gas, which preferably contains hydrogen and nitrogen, can be compressed by means of a compressor 25 via a gas feed line 60C and then supplied to the interior of the reactor 10 via a feed line 60A. At the start of the process, the gas mixture can be brought to the required temperature, for example to a maximum of 450° C., preferably to 370° C. to 390° C., by means of a heating device 50 and then guided through the catalyst bed 10A. In order to adjust the gas flow rate, a control accessory 15 is present in the entire system. The further the catalyst bed 10A is arranged downstream in the reactor 10, the larger the size of the catalyst bed 10A. During the reduction, the gas mixture produced by the reduction, which contains water and / or ammonia as well as unreacted hydrogen and nitrogen, is discharged from the reactor via a discharge line 60B. The water content and / or ammonia content of the gas mixture is then determined by means of an NDIR sensor 5, which is connected to the discharge line 60B at the reactor outlet via a line 6. The gas mixture produced by the reduction can then at least partially give off the heat still present via a heat exchanger 40. The gas mixture is then introduced into the waste heat boiler 20, where it gives additional heat to the water guided through the waste heat boiler. The water is fed into the waste heat boiler 20 by means of a connector 21 and discharged from the waste heat boiler through a connector 22 as water vapor. The water vapor can be used, for example, to improve the energy efficiency and thermal efficiency of the entire device to operate the compressor by means of a steam turbine. The gas mixture can then be passed through another heat exchanger 40 or through an ammonia cooler 40A to give additional heat, so that the separation of a mixture of ammonia and / or water can then occur in the separator 30. The separated water / ammonia mixture can then be removed from the system through a discharge line 30A. The reducing gas mixture containing hydrogen and nitrogen can then be reintroduced into the compressor 25 to be used for the reduction of iron oxides in another cycle.
[0047] Depending on the concentration of water and / or ammonia in the system determined by the NDIR sensor 5, the flow rate of the reducing gas and / or the heating rate can be set accordingly so that during the reduction, the concentration of water formed fluctuates within a range around certain limit values. In addition, the temperature in the separator 30 can also be set by means of the NDIR sensor 5 so that freezing of ammonia does not occur, which would impair the operation of the separator.
[0048] Figure 2The flow chart of the subsequent process and sub-steps after the water determination by means of the NDIR sensor is shown. In this embodiment, the limit value of the concentration of water in the gas phase can be, for example, 3000ppmv and the range near the limit value is ±200ppmv. Starting from the elements with reference numerals 80 and 81, the water content determined by means of NDIR is first read out on the analyzer of the reactor device, and the value is compared with the limit value. According to the result of the comparison, there are then three different sub-steps (C1), (C2) or (C3). If it is found that the measured value is greater than 200ppmv above the limit value, the flow rate is increased or the heating rate (82A) is reduced in the method step (C2). Therefore, the concentration of the water formed in the gas phase can be reduced by either setting a higher flow rate (which causes the water concentration in the gas phase to be diluted faster) or reducing the reduction by reducing the heating rate. If it is found that the measured value is greater than 200ppmv below the limit value, the reduction state (82B) in the catalyst bed of the reactor is checked, which can be carried out, for example, by measuring the temperature of the catalyst bed, or if the reducing gas contains nitrogen and hydrogen, it can be carried out by the ammonia concentration in the gas phase. For temperature measurement, temperature sensors can be present at the inlet and outlet of the catalyst bed. When the ammonia concentration no longer increases under constant pressure and temperature, the reduction of the catalyst bed can be considered complete. If it is found that the reduction in the catalyst bed has not yet ended, the heating rate (83B) can be increased in method step (C1). If it is found that the concentration of water in the gas phase is within the range of ± 200ppmv near the limit value, the flow rate and / or heating rate (82C) can be maintained in substep (C3).
[0049] If the reduction of the iron oxides in one catalyst bed is found to be complete, it can be verified whether there are further catalyst beds with iron oxides to be reduced in the reactor (83A). If this is not the case, the reduction is ended (84) or, if there are further catalyst beds, the inlet temperature of the subsequent bed can be increased by closing the valve to start the reduction of the next catalyst bed (85). The heating rate can be set by adjusting the control valve.
[0050] Figure 3The process steps and sub-steps that occur after the determination of ammonia are shown in a flow chart. For this purpose, in a first step (90), the concentration of ammonia in the gas phase is determined, and then the temperature (91) of the respective current freezing point of the ammonia solution is calculated based on method parameters such as pressure, water content in the gas phase and the calculation. The temperature of the cooling device is then compared with the calculated freezing point of the ammonia solution (92), and different sub-steps are performed depending on the result. The method sub-steps can be, in particular, method steps (C4), wherein if the temperature of the cooling device is less than 5K above the calculated freezing point of the ammonia solution, the temperature of the cooling device is increased (92B). In addition, there is the possibility that, if the temperature of the cooling device is greater than 10K above the calculated freezing point of the ammonia solution, the temperature of the cooling device is further reduced in method step (C5). Here, it is first determined whether the device allows the temperature of the cooler to be further reduced (92C). Many devices do not allow the cooler temperature to be further reduced, especially when the cooler temperature is already at -20°C. Depending on whether it is possible to further reduce it, either the cooler temperature is further reduced (92D) or the operating parameters are maintained (92E). This type of in Figure 3 The method illustrated in the figure with corresponding sub-steps can particularly reliably condense water and / or ammonia from the gas phase and at the same time prevent freezing of the cooling device. If the temperature of the cooler is in the range of 5 to 10° C. above the freezing point of the aqueous ammonia solution, the temperature of the cooler can be maintained (92A).
[0051] Figure 4 The temperature curve experimentally determined during the reduction of iron oxides with a synthesis gas containing 76.5% hydrogen, 22.5% nitrogen and 10% argon (in each case in % by volume) and the water content experimentally determined in the gas phase in % by volume are shown in a diagram. At different synthesis gas flow rates, the iron oxides are reduced for different periods of time, wherein the water content in the gas phase can be reduced by increasing the flow rate. The curve marked with 100 here shows the relationship between the water content and the temperature in the case of a reduction at a flow rate of 250 l / h over 25 hours. The curve marked with 101 shows the course of the water concentration in the gas phase in the case of a reduction at a flow rate of 400 l / h over 30 hours. The course of the water concentration in the 30-hour reduction at a flow rate of 400 l / h is indicated by the curve marked with 102. Another reduction (curve marked with 103) is also carried out at a flow rate of 1200 l / h over a period of 40 hours. It can be clearly seen that the water concentration decreases with increasing flow rate due to the dilution effect of the newly arriving gas, but on the other hand the time required for reduction increases. Figure 4It is also shown that, due to the increase in flow rate, the maximum concentration of water formed can be continuously reduced from a very high value of about 12000 ppmv at a flow rate of 250 l / h, so that at a flow rate of 1200 l / h, a concentration of water formed of below 1500 ppmv is finally reached, which no longer impairs the catalytic activity of the catalyst or catalyst precursor formed.
[0052] Figure 5 The experimentally determined catalytic activities of six different catalysts based on wüstite, which were exposed to different water contents from below 2000 ppmv to 8000 ppmv during reduction, are shown. It can be clearly seen that the catalytic activity decreases by about 5% to 10% with increasing water content, especially starting from a limit of about 4000 ppmv.
[0053] Figure 6 The course of the water concentration in the gas phase at the reactor outlet in ppmv (curve marked with 110) and the temperature course (curve marked with 120) are shown over a specific time period t. The water concentration was measured by means of an NDIR sensor. Iron oxides based on wüstite were reduced at a pressure of 90 bar in a hydrogen-containing atmosphere at a flow rate of 1200 NL / h (NL=normal pressure liters (volume at 1013.25 mbar and 0° C.)). It can be clearly seen that at the beginning of the reduction, the temperature and the water content in the gas phase are still relatively low, and over time, due to the increase in temperature, the reduction rate increases, which leads to a higher water content at the reactor outlet. Finally, a maximum value of the water content is reached, in which case the water content at the reactor outlet decreases again due to the reduced reduction rate. It can be clearly seen that water contents in the gas phase of more than 3000 ppmv or more than 3500 ppmv can be measured when reducing wüstite. This type of high water content can be effectively prevented by the method according to the invention for activating iron oxides.
[0054] The present invention is not limited by the description with the aid of specific embodiments. Rather, the present invention includes every new feature and every combination of features, which in particular includes every combination of features in the claims, even if the feature or the combination itself is not explicitly given in the claims or specific embodiments.
Claims
1. A method for activating catalysts and catalyst precursors for ammonia synthesis, comprising the following method steps: (A) reducing wüstite using at least one reducing gas and by heating in order to activate the catalyst, (B) measuring the concentration of water formed in the gas phase during the reduction by means of non-dispersive infrared spectroscopy NDIR, and (C) adjusting the flow rate of the reducing gas and / or the heating rate according to the concentration of water formed, wherein in method step (C), the water concentration determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±1000 ppmv.
2. A method for activating catalysts and catalyst precursors for ammonia synthesis, comprising the following method steps: (A) reducing wüstite using at least one reducing gas and by heating in order to activate the catalyst, (B) measuring the concentration of water formed in the gas phase during the reduction by means of non-dispersive infrared spectroscopy NDIR, and (C) adjusting the flow rate of the reducing gas and / or the heating rate according to the concentration of water formed, wherein in method step (C), the water concentration determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±800 ppmv.
3. A method for activating catalysts and catalyst precursors for ammonia synthesis, comprising the following method steps: (A) reducing wüstite using at least one reducing gas and by heating in order to activate the catalyst, (B) measuring the concentration of water formed in the gas phase during the reduction by means of non-dispersive infrared spectroscopy NDIR, and (C) adjusting the flow rate of the reducing gas and / or the heating rate according to the concentration of water formed, wherein in method step (C), the water concentration determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±600 ppmv.
4. A method for activating catalysts and catalyst precursors for ammonia synthesis, comprising the following method steps: (A) reducing wüstite using at least one reducing gas and by heating in order to activate the catalyst, (B) measuring the concentration of water formed in the gas phase during the reduction by means of non-dispersive infrared spectroscopy NDIR, and (C) adjusting the flow rate of the reducing gas and / or the heating rate according to the concentration of water formed, wherein in method step (C), the water concentration determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±400 ppmv.
5. A method for activating catalysts and catalyst precursors for ammonia synthesis, comprising the following method steps: (A) reducing wüstite using at least one reducing gas and by heating in order to activate the catalyst, (B) measuring the concentration of water formed in the gas phase during the reduction by means of non-dispersive infrared spectroscopy NDIR, and (C) adjusting the flow rate of the reducing gas and / or the heating rate according to the concentration of water formed, wherein in method step (C), the water concentration determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±300 ppmv.
6. A method for activating catalysts and catalyst precursors for ammonia synthesis, comprising the following method steps: (A) reducing wüstite using at least one reducing gas and by heating in order to activate the catalyst, (B) measuring the concentration of water formed in the gas phase during the reduction by means of non-dispersive infrared spectroscopy NDIR, and (C) adjusting the flow rate of the reducing gas and / or the heating rate according to the concentration of water formed, wherein in method step (C), the water concentration determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±200 ppmv.
7. The method according to any one of claims 1 to 6, wherein the limit value is 3400 ppmv.
8. The method according to any one of claims 1 to 6, wherein the limit value is 3200 ppmv.
9. The method according to any one of claims 1 to 6, wherein the limit value is 3000 ppmv.
10. The process according to any one of claims 1 to 6, wherein process steps (A), (B) and (C) are carried out continuously.
11. The method according to any one of claims 1 to 6, wherein the measurement of the water formed during the reduction is carried out in real time in method step (B). 12 . The method according to claim 1 , wherein in method step (B) the concentration of water formed during the reduction is measured in the wavelength range from 2.6 μm to 3 μm. 13 . The method according to claim 1 , wherein in method step (B) the concentration of water formed during the reduction is measured in the wavelength range from 2.7 μm to 2.8 μm. 14 . The method according to claim 1 , wherein in method step (B) the concentration of water formed during the reduction is measured at a wavelength of 2.7 μm. 15 . The process according to claim 1 , wherein in process step (A) a mixture comprising hydrogen and nitrogen is used as reducing gas and ammonia is formed during the reduction of the catalyst.
16. The method according to claim 1, wherein in method step (B), an NDIR instrument is used to measure the water formed, wherein the absorption band of ammonia is calculated in the wavelength range from 2.6 μm to 3 μm by means of calibration.
17. The process according to claim 1, wherein in process step (B), the concentration of ammonia formed during the reduction is determined by means of NDIR.
18. The process according to claim 1, wherein the ammonia and / or water formed during the reduction is condensed by means of a cooler.
19. The method according to claim 18, wherein the temperature of the cooler is adjusted in method step (C) such that it is at least 10 K above the freezing point of the aqueous ammonia solution.
20. The method according to claim 18, wherein the temperature of the cooler is adjusted in method step (C) such that it is at least 5 K above the freezing point of the aqueous ammonia solution.
21. The process according to any one of claims 1 to 6, wherein the temperature in process step (A) is adjusted to a temperature in the range of 360°C to 450°C.
22. The process according to any one of claims 1 to 6, wherein the temperature in process step (A) is adjusted to a temperature in the range of 370°C to 400°C.
23. The process according to any one of claims 1 to 6, wherein the heating in process step (A) is to a temperature in the range of 370°C to 400°C.
24. The process according to any one of claims 1 to 6, wherein in process step (B) a mixture comprising hydrogen and nitrogen is used as reducing gas, and aqueous ammonia solution is condensed off during the reduction.
25. The method according to any one of claims 1 to 6, wherein the method further comprises a method step (D) in which the catalyst and / or catalyst precursor from method step (C) is exposed to an oxidizing gas to form a protective layer on the catalyst and / or catalyst precursor.
26. Use of an NDIR detector for determining the concentration of water which is formed during the reduction of wüstite when activating catalysts and catalyst precursors for ammonia synthesis, wherein the reduction is carried out by means of at least one reducing gas, and (B) the concentration of water formed in the gas phase during the reduction is measured by means of NDIR, and (C) the flow rate of the reducing gas and / or the heating rate is adjusted as a function of the concentration of water formed, wherein in method step (C) the concentration of water determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±1000 ppmv.
27. Use of an NDIR detector for determining the concentration of water which is formed during the reduction of wüstite when activating catalysts and catalyst precursors for ammonia synthesis, wherein the reduction is carried out by means of at least one reducing gas, and (B) the concentration of water formed in the gas phase during the reduction is measured by means of NDIR, and (C) the flow rate and / or the heating rate of the reducing gas is adjusted as a function of the concentration of water formed, wherein in method step (C) the concentration of water determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±800 ppmv.
28. Use of an NDIR detector for determining the concentration of water which is formed during the reduction of wüstite when activating catalysts and catalyst precursors for ammonia synthesis, wherein the reduction is carried out by means of at least one reducing gas, and (B) the concentration of water formed in the gas phase during the reduction is measured by means of NDIR, and (C) the flow rate and / or the heating rate of the reducing gas is adjusted as a function of the concentration of water formed, wherein in method step (C) the concentration of water determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) Maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±600 ppmv.
29. Use of an NDIR detector for determining the concentration of water which is formed during the reduction of wüstite when activating catalysts and catalyst precursors for ammonia synthesis, wherein the reduction is carried out by means of at least one reducing gas, and (B) the concentration of water formed in the gas phase during the reduction is measured by means of NDIR, and (C) the flow rate and / or the heating rate of the reducing gas is adjusted as a function of the concentration of water formed, wherein in method step (C) the concentration of water determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±400 ppmv.
30. Use of an NDIR detector for determining the concentration of water which is formed during the reduction of wüstite when activating catalysts and catalyst precursors for ammonia synthesis, wherein the reduction is carried out by means of at least one reducing gas, and (B) the concentration of water formed in the gas phase during the reduction is measured by means of NDIR, and (C) the flow rate of the reducing gas and / or the heating rate is adjusted as a function of the concentration of water formed, wherein in method step (C) the concentration of water determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±300 ppmv.
31. Use of an NDIR detector for determining the concentration of water which is formed during the reduction of wüstite when activating catalysts and catalyst precursors for ammonia synthesis, wherein the reduction is carried out by means of at least one reducing gas, and (B) the concentration of water formed in the gas phase during the reduction is measured by means of NDIR, and (C) the flow rate and / or the heating rate of the reducing gas is adjusted as a function of the concentration of water formed, wherein in method step (C) the concentration of water determined in method step (B) is compared with a predetermined limit value for water, and Wherein in method step (C), at least one of the following sub-steps is performed: (C1) if the water concentration determined in method step (B) is below the lower limit of the range around the predetermined limit value, increasing the heating rate, or (C2) if the water concentration determined in method step (B) is above the upper limit of the range around the predetermined limit value, increasing the flow rate and / or decreasing the heating rate, or (C3) maintaining the flow rate and / or heating rate if the water concentration determined in method step (B) is within a range around a predetermined limit value, wherein the limit value is in the range between 3000 ppmv and 4000 ppmv and wherein the range around the limit value is ±200 ppmv.
Citation Information
Patent Citations
Analyzing fault gas concentration in liquid
CA3005371A1
Moisture content measuring method for plastics mass - heating test flask and measuring absorption of IR radiation using vapour products in carrier gas in measuring cell
CH681392A5
Preparation method and preparation device for synthesis ammonia prereduction catalyst
CN105435861A
Pre-reduction type ammonia synthesis catalyst and preparing process
CN1114239A