Rubber composition for tire and tire
By using styrene-butadiene rubber and polybutadiene compositions with high vinyl and trans content in tire rubber compositions, combined with appropriate fillers and vulcanizing agents, the problem of tire wet grip performance and wear resistance deteriorating over time has been solved, achieving long-term performance stability and excellent performance.
Patent Information
- Application Number
- CN202080051695.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-05
- Filing Date
- 2020-07-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-07-06
AI Technical Summary
Existing tire rubber compositions deteriorate rapidly over time in terms of wet grip and abrasion resistance, making it difficult to maintain good performance over a long period.
A styrene-butadiene rubber and polybutadiene composition with a specific ratio, a vinyl content of more than 20 mol%, and a trans content of more than 50 mol%, combined with highly polar functional groups exposed on the tire surface, improves the tire's hydrophilicity, enhances wet grip performance, and reduces performance degradation over time through appropriate combinations of fillers and vulcanizing agents.
This technology enables tire rubber compositions to maintain good wet grip performance while significantly reducing the degradation of wet grip and wear resistance over time, thus improving the long-term performance of the tire.
Smart Images

Figure GDA0003473636940000181
Abstract
Description
Technical Field
[0001] The present invention relates to a tire rubber composition and a tire. Background Art
[0002] For safety reasons, it is desirable for tires to have improved wet grip performance (braking performance on wet roads).
[0003] For example, Patent Document 1 discloses a rubber composition containing predetermined amounts of two specific types of silica to improve wet grip performance.
[0004] Reference List
[0005] Patent Literature
[0006] Patent Document 1: JP 2008-50570 A Summary of the invention
[0007] Technical issues
[0008] Through extensive research and experiments, the present inventors have discovered that conventional technologies have room for improvement in reducing the degradation of wet grip performance and wear resistance over time.
[0009] The present invention aims to solve the new problems found by the inventors and to provide a tire rubber composition and a tire having good wet grip performance and excellent ability to reduce the deterioration of wet grip performance and wear resistance over time.
[0010] Solution to the problem
[0011] The present invention relates to a tire rubber composition, comprising: one or more rubber components, wherein the total content of styrene-butadiene rubber and polybutadiene in the rubber components is 90% by mass or more; one or more fillers; and one or more vulcanizing agents; each of which has a vinyl content of 20 mol% or more and a trans content of 50 mol% or more, based on the total amount of butadiene structural units in the butadiene part of the styrene-butadiene rubber and the polybutadiene being 100 mol%.
[0012] Preferably, the vinyl content is 30 mol% or more, more preferably 35 mol% or more, and further preferably 36 mol% or more.
[0013] Preferably, the rubber composition contains 80 parts by mass or more of silica relative to 100 parts by mass of the rubber component.
[0014] Preferably, the rubber composition comprises styrene-butadiene rubber and polybutadiene.
[0015] Preferably, the rubber composition comprises syndiotactic 1,2-polybutadiene.
[0016] The invention also relates to a tire having a tread, the tread comprising the rubber composition.
[0017] Beneficial effects of the present invention
[0018] The present invention provides a tire rubber composition, which comprises: one or more rubber components, wherein the total content of styrene-butadiene rubber and polybutadiene in the rubber components is 90% by mass or more; one or more fillers; and one or more vulcanizing agents; each of which has a vinyl content of 20 mol% or more and a trans content of 50 mol% or more, based on the total amount of butadiene structural units in the butadiene part of the styrene-butadiene rubber and polybutadiene as 100 mol%. Such a tire rubber composition has good wet grip performance and excellent ability to reduce the deterioration of wet grip performance and wear resistance over time. DETAILED DESCRIPTION
[0019] The tire rubber composition of the present invention comprises: one or more rubber components, the total content of styrene-butadiene rubber and polybutadiene of the rubber components is 90% by mass or more; one or more fillers; and one or more vulcanizing agents; each of which has a vinyl content of 20 mol% or more and a trans content of 50 mol% or more, based on the total amount of butadiene structural units in the butadiene part of the styrene-butadiene rubber and polybutadiene as 100 mol%. Therefore, the wet grip performance is good, and the ability to reduce the deterioration of wet grip performance over time and the ability to reduce the deterioration of wear resistance over time are improved.
[0020] The tire rubber composition provides the above-mentioned effects. The reason for such beneficial effects is not entirely clear, but can be explained as follows.
[0021] The tire rubber composition comprises one or more rubber components based on styrene-butadiene rubber (SBR) and / or polybutadiene (BR). The vinyl content of the entire rubber composition (hereinafter also referred to as the vinyl content of the rubber composition) is 20 mol% or more and the trans content (hereinafter also referred to as the trans content of the rubber composition) is 50 mol% or more, respectively, based on the total amount of butadiene structural units in the butadiene part of the styrene-butadiene rubber and the polybutadiene being 100 mol%.
[0022] Herein, such butadiene-based structural units include cis-1,4-units, trans-1,4-units and vinyl-1,2-units. The cis-1,4-units and trans-1,4-units have one double bond in the main chain, while the vinyl-1,2-units do not have a double bond in the main chain.
[0023] In addition, the vinyl content of the rubber composition refers to the amount of vinyl-1,2-units based on 100 mol% of the total amount of butadiene-based structural units derived from styrene-butadiene rubber and polybutadiene. The trans content of the rubber composition refers to the amount of trans-1,4-units based on 100 mol% of the total amount of butadiene-based structural units derived from styrene-butadiene rubber and polybutadiene. The following cis content of the rubber composition refers to the amount of cis-1,4-units based on 100 mol% of the total amount of butadiene-based structural units derived from styrene-butadiene rubber and polybutadiene.
[0024] When the vinyl content of the rubber composition is 20 mol% or more, the amount of double bonds in the polymer main chain is reduced, making the molecular chain of the polymer less likely to be damaged by ozone erosion, thereby reducing the deterioration of wet grip performance and wear resistance over time. Therefore, good wet grip performance can also be obtained.
[0025] When the trans content of the rubber composition is 50 mol% or more, the high polarity functional groups can be more exposed to the tire surface, thereby improving the hydrophilicity of the entire tire. Therefore, better wet grip performance can be obtained.
[0026] Furthermore, when the vinyl content of the rubber composition is 20 mol% or more and the trans content of the rubber composition is 50 mol% or more, the wet grip performance is synergistically improved and good wet grip performance can be maintained for a long time.
[0027] As described above, the tire rubber composition contains one or more rubber components based on styrene-butadiene rubber and polybutadiene, and has a vinyl content of 20 mol% or more and a trans content of 50 mol% or more, so that the wet grip performance is good and the ability to reduce the deterioration of the wet grip performance over time and the ability to reduce the deterioration of the wear resistance over time are improved.
[0028] The vinyl content of the entire tire rubber composition (vinyl content of the rubber composition) is 20 mol% or more, preferably 20.1 mol% or more, more preferably 20.2 mol% or more, further preferably 20.9 mol% or more, particularly preferably 22.9 mol% or more, most preferably 23 mol% or more, further preferably 26.8 mol% or more, further preferably 28.1 mol% or more, further preferably 29.4 mol% or more, further preferably 30 mol% or more, based on the total amount of butadiene structural units in the butadiene portion of the styrene-butadiene rubber and the polybutadiene as 100 mol%. % or more, more preferably 30.4 mol% or more, more preferably 30.7 mol% or more, more preferably 31.3 mol% or more, more preferably 31.4 mol% or more, more preferably 35 mol% or more, more preferably 36 mol% or more, more preferably 36.3 mol% or more, but preferably 85 mol% or less, more preferably 80 mol% or less, more preferably 60 mol% or less, particularly preferably 55 mol% or less, most preferably 50 mol% or less, more preferably 45 mol% or less, more preferably 40.1 mol% or less. When the vinyl content is within the above range, the beneficial effects can be more suitably achieved.
[0029] The total amount of butadiene structural units in the butadiene part of the styrene-butadiene rubber and the polybutadiene is 100 mol%, and the trans content of the entire tire rubber composition (trans content of the rubber composition) is 50 mol% or more, preferably 50.1 mol% or more, more preferably 50.2 mol% or more, further preferably 50.6 mol% or more, particularly preferably 51 mol% or more, most preferably 51.1 mol% or more, further preferably 51.3 mol% or more, but preferably 80 mol% or less, more preferably 75 mol% or less, further preferably 70 mol% or less, particularly preferably 68.3 mol% or less, most preferably 65 mol% or less, further preferably 61.1 mol% or less, further preferably 60 mol% or less, further preferably 58.1 mol% or less, further preferably 57.9 mol% or less, further preferably 55.7 mol% or less, further preferably 54.6 mol% or less, further preferably 53.5 mol% or less. When the trans content is within the above range, the beneficial effect can be more suitably achieved.
[0030] Based on the total amount of butadiene structural units in the butadiene portion of the styrene-butadiene rubber and the polybutadiene as 100 mol%, the cis content of the entire tire rubber composition (cis content of the rubber composition) is preferably 5 mol% or more, more preferably 9.3 mol% or more, further preferably 10 mol% or more, particularly preferably 11.6 mol% or more, most preferably 13 mol% or more, further preferably 13.5 mol% or more, further preferably 13.9 mol% or more, further preferably 14.1 mol% or more, further preferably 15.3 mol% or more The cis content is preferably 16.2 mol% or more, but preferably 60 mol% or less, more preferably 50 mol% or less, more preferably 40 mol% or less, particularly preferably 30 mol% or less, most preferably 25.2 mol% or less, more preferably 20 mol% or less, more preferably 19.6 mol% or less, more preferably 18.9 mol% or less, more preferably 18.7 mol% or less, more preferably 18.5 mol% or less, more preferably 18 mol% or less, and more preferably 17.1 mol% or less. When the cis content is within the above range, the beneficial effects can be more suitably achieved.
[0031] The above-mentioned vinyl content of the rubber composition, trans content of the rubber composition and cis content of the rubber composition can be achieved by using a suitable combination of SBR and / or BR.
[0032] For example, rubber components such as SBR having a high trans content, BR having a high trans content, and BR having a high vinyl content may be combined.
[0033] Chemicals that can be used in the rubber composition are described below.
[0034] The tire rubber composition comprises styrene-butadiene rubber (SBR) and / or polybutadiene (BR). In order to more suitably achieve the beneficial effects, the tire rubber composition preferably comprises SBR and BR.
[0035] Any SBR can be used. Examples include those commonly used in the tire industry, such as emulsion polymerization SBR (E-SBR) and solution polymerization SBR (S-SBR). These can be used alone or in combination of two or more. Among these, the combination of two or more types of SBR having different vinyl content and / or different trans content is preferred.
[0036] The styrene content of SBR is preferably 10% by mass or more, more preferably 15% by mass or more, further preferably 20% by mass or more, but preferably 50% by mass or less, more preferably 40% by mass or less, more preferably 30% by mass or less, and particularly preferably 25% by mass or less. When the styrene content is within the above range, the beneficial effects tend to be more appropriately achieved.
[0037] The vinyl content of SBR is preferably 10 mol% or more, more preferably 15 mol% or more, further preferably 20 mol% or more, but is preferably 80 mol% or less, more preferably 70 mol% or less, even more preferably 50 mol% or less, particularly preferably 40 mol% or less. When the vinyl content is within the above range, the beneficial effects tend to be more appropriately achieved.
[0038] The trans content of SBR is preferably 10 mol% or more, more preferably 15 mol% or more, further preferably 20 mol% or more, particularly preferably 40 mol% or more, and most preferably 60 mol% or more, but is preferably 90 mol% or less, more preferably 85 mol% or less, and further preferably 80 mol% or less. When the trans content is within the above range, the beneficial effects tend to be more appropriately achieved.
[0039] By using SBR having a trans content within the above range (high trans content), the high polarity functional groups can be more exposed to the tire surface, thereby improving the hydrophilicity of the entire tire. Therefore, better wet grip performance can be obtained.
[0040] The cis content of SBR is preferably 3 mol% or more, more preferably 5 mol% or more, and further preferably 10 mol% or more, but is preferably 40 mol% or less, and more preferably 30 mol% or less. When the cis content is within the above range, beneficial effects tend to be more appropriately achieved.
[0041] Herein, the vinyl content, trans content and cis content of SBR all refer to the content based on 100 mol % of the butadiene-based structural units in SBR.
[0042] The SBR may be unmodified SBR or modified SBR.
[0043] Modified SBR can be any SBR with functional groups that interact with fillers (such as silica). Examples include: chain end modified SBR (i.e., chain end modified SBR terminated with functional groups) obtained by modifying at least one chain end of SBR with a compound (modifier) having a functional group; main chain modified SBR with functional groups in the main chain; main chain and chain end modified SBR (for example, the main chain has functional groups and at least one chain end is modified by a modifier) having functional groups in the main chain and chain end; and chain end modified SBR introducing hydroxyl or epoxy groups by modification (coupling) with a polyfunctional compound having two or more epoxy groups in the molecule. These can be used alone or in combination of two or more.
[0044] The example of functional group comprises: amino, amide group, silyl, alkoxysilyl, isocyanate group, imino group, imidazolyl, urea group, ether group, carbonyl group, oxycarbonyl group, sulfhydryl group, thioether group, disulfide group, sulfonyl group, sulfinyl group, thiocarbonyl group, ammonium group, imido group, hydrazine group, azo group, diazo group, carboxyl group, nitrile group, pyridyl group, alkoxy group, hydroxyl group, oxy group and epoxy group.These functional groups can be substituted.Among these, preferably amino (preferably the amino that hydrogen atom is replaced by C1-C6 alkyl), alkoxy group (preferably C1-C6 alkoxy), alkoxysilyl group (preferably C1-C6 alkoxysilyl) and amide group.
[0045] SBR products manufactured or sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc. can be used as SBR.
[0046] The SBR is preferably SBR 1 having a styrene content of 30 mass % or more and a trans content of 55 mol % or less, or SBR 2 having a styrene content of 25 mass % or less and a trans content of 60 mol % or more, and a combination of SBR 1 and SBR 2 is more preferred.
[0047] The styrene content of SBR 1 is preferably 35% by mass or more, but is preferably 50% by mass or less, and more preferably 45% by mass or less. In addition, the trans content of SBR 1 is preferably 10 mol% or more, more preferably 15 mol% or more, further preferably 20 mol% or more, and particularly preferably 40 mol% or more.
[0048] The styrene content of SBR 2 is preferably 10% by mass or more, more preferably 15% by mass or more, and further preferably 20% by mass or more. The trans content of SBR 2 is preferably 90 mol% or less, more preferably 85 mol% or less, and further preferably 80 mol% or less.
[0049] The vinyl content and cis content of SBR 1 and SBR 2 are as described above for the vinyl content and cis content of SBR.
[0050] The amount of SBR is preferably 10% by mass or more, preferably 20% by mass or more, more preferably 40% by mass or more, further preferably 60% by mass or more, particularly preferably 70% by mass or more, based on 100% by mass of the rubber component, and may be 100% by mass, but is preferably 90% by mass or less, more preferably 85% by mass or less. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0051] The amount of SBR 1 is preferably 10% by mass or more, more preferably 25% by mass or more, but is preferably 60% by mass or less, more preferably 50% by mass or less, based on 100% by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0052] The amount of SBR 2 is preferably 10% by mass or more, more preferably 35% by mass or more, but is preferably 70% by mass or less, more preferably 55% by mass or less, based on 100% by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0053] Any polybutadiene (BR) can be used, examples include those commonly used in the tire industry, such as high cis BR with a high cis content, low cis BR with a low cis content, BR containing syndiotactic polybutadiene crystals, and BR synthesized using a rare earth catalyst (rare earth catalyzed BR). Crystalline BR, such as syndiotactic 1,2-polybutadiene, can also be used. These can be used alone or in combination of two or more.
[0054] In addition, BR may be unmodified BR or modified BR. Examples of modified BR include those into which the above-mentioned functional groups are introduced. Examples of modified BR are as described above for modified SBR.
[0055] BR can be purchased from Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, and the like.
[0056] In particular, BR is preferably BR 1 or syndiotactic 1,2-polybutadiene (BR2) having a trans content of 45 mol% or more, more preferably syndiotactic 1,2-polybutadiene (BR 2). BR is also preferably a combination of BR 1 having a trans content of 45 mol% or more and syndiotactic 1,2-polybutadiene (BR 2).
[0057] In particular, by adding syndiotactic 1,2-polybutadiene, the number of double bonds in the polymer main chain is reduced, making the molecular chain of the polymer less likely to be damaged by ozone attack, thereby more appropriately reducing the deterioration of wet grip performance and wear resistance over time. BR containing syndiotactic polybutadiene crystals (such as VCR available from Ube Industries, Ltd.) is also generally used and has a cis-1,4-linked main chain, while syndiotactic 1,2-polybutadiene (BR 2) has a vinyl-1,2-linked main chain, thereby more appropriately reducing the deterioration of wet grip performance and wear resistance over time.
[0058] The trans content of BR 1 is preferably 45 mol% or more, more preferably 50 mol% or more. The trans content is also preferably 70 mol% or less, more preferably 60 mol% or less, and further preferably 55 mol% or less. When the trans content is within the above range, the beneficial effects tend to be better achieved.
[0059] The vinyl content of BR 1 is preferably 20 mol% or less, more preferably 15 mol% or less. The vinyl content is also preferably 5 mol% or more, more preferably 10 mol% or more. When the vinyl content is within the above range, the beneficial effects tend to be better achieved.
[0060] The cis content of BR 1 is preferably 20 mol% or more, more preferably 30 mol% or more. The cis content is also preferably 50 mol% or less, more preferably 40 mol% or less. When the cis content is within the above range, the beneficial effects tend to be better achieved.
[0061] The vinyl content of syndiotactic 1,2-polybutadiene (SPB, BR 2) is preferably 80 mol% or more, more preferably 85 mol% or more, further preferably 90 mol% or more, particularly preferably 93 mol% or more, and may be 100 mol%. When the vinyl content is within the above range, the beneficial effects tend to be better achieved.
[0062] The trans content and cis content of BR 2 are each preferably 6 mol% or less, more preferably 3 mol% or less, and may be 0 mol%. When the trans and cis contents are each within the above range, the beneficial effects tend to be better achieved.
[0063] The melting point of BR 2 is not limited, but is preferably 80° C. or higher, more preferably 100° C. or higher, and further preferably 105° C. or higher, but is preferably 180° C. or lower, more preferably 150° C. or lower, and further preferably 130° C. or lower. When the melting point is within the above range, the beneficial effects tend to be better achieved.
[0064] Herein, the melting point of BR refers to the melting peak temperature in a DSC curve measured according to JIS K7121.
[0065] The crystallinity of BR 2 is not limited, but is preferably 15% or more, more preferably 25% or more, but is preferably 50% or less, more preferably 40% or less. When the crystallinity is within the above range, the advantageous effects tend to be better achieved.
[0066] In this paper, the crystallinity is calculated from the density measured by the water displacement method, where the density of 1,2-polybutadiene with a crystallinity of 0% is 0.889 g / cm 3 , while the density of 1,2-polybutadiene with 100% crystallinity is 0.963 g / cm 3 .
[0067] The amount of BR is preferably 5% by mass or more, more preferably 10% by mass or more, and further preferably 15% by mass or more, but is preferably 40% by mass or less, and more preferably 30% by mass or less, based on 100% by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0068] The amount of BR 1 is preferably 5% by mass or more, more preferably 8% by mass or more, but is preferably 20% by mass or less, more preferably 15% by mass or less, based on 100% by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0069] The amount of BR 2 (SPB) is preferably 5% by mass or more, more preferably 8% by mass or more, but is preferably 20% by mass or less, more preferably 15% by mass or less, based on 100% by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0070] The total amount of SBR and BR is 90% by mass or more, preferably 95% by mass or more, more preferably 98% by mass or more, and may be 100% by mass, based on 100% by mass of the rubber component. When the total amount of SBR and BR is within the above range, the beneficial effects tend to be better achieved.
[0071] Examples of available rubber components other than SBR and BR include diene rubbers, such as isoprene-based rubbers, styrene-isoprene-butadiene rubber (SIBR), acrylonitrile-butadiene rubber (NBR), chloroprene rubber (CR) and butyl rubber (IIR). The rubber component can be used alone or in combination of two or more. Among these, diene rubbers are preferred, and isoprene-based rubbers are more preferred.
[0072] Preferably, the term "rubber component" refers to a rubber having a weight average molecular weight (Mw) of 150,000 or more, more preferably 350,000 or more. The upper limit of Mw is not limited, but is preferably 4,000,000 or less, more preferably 3,000,000 or less.
[0073] Examples of isoprene-based rubbers include natural rubber (NR), polyisoprene rubber (IR), refined NR, modified NR, and modified IR. NR can be NR commonly used in the tire industry, such as SIR20, RSS#3, or TSR20. Any IR can be used, and examples include those commonly used in the tire industry, such as IR2200. Examples of refined NR include deproteinized natural rubber (DPNR) and highly purified natural rubber (UPNR). Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized polyisoprene rubber, hydrogenated polyisoprene rubber, and grafted polyisoprene rubber. These can be used alone or in combination of two or more. Among these, NR is preferred.
[0074] Herein, the weight average molecular weight (Mw) and the number average molecular weight (Mn) can be measured by a gel permeation chromatograph (GPC) calibrated with a polystyrene standard (GPC-8000 series purchased from Tosoh Tosoh Corporation, detector: differential refractometer, chromatographic column: TSKGEL SUPERMULTIPORE HZ-M purchased from Tosoh Tosoh Corporation).
[0075] The cis content, vinyl content and trans content can be 13 C-NMR analysis. In addition, the styrene content can be measured by 1 Measured by H-NMR analysis.
[0076] The vinyl content of the rubber composition, the trans content of the rubber composition, and the cis content of the rubber composition can be determined by 13 The C-NMR analysis can be measured directly on the rubber composition or can be calculated from the vinyl content, trans content and cis content measured separately on the raw rubber (in proportion to the amount of raw rubber).
[0077] The rubber composition contains one or more fillers (reinforcing fillers).
[0078] Any filler can be used, examples include: silica, carbon black, calcium carbonate, talc, alumina, clay, aluminum hydroxide and mica. These can be used alone or in combination of two or more. Among these, silica and carbon black are preferred, and silica is more preferred. A combination of silica and carbon black is also preferred.
[0079] The amount of the filler is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, and further preferably 60 parts by mass or more, but is preferably 200 parts by mass or less, more preferably 180 parts by mass or less, further preferably 160 parts by mass or less, particularly preferably 130 parts by mass or less, and most preferably 110 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0080] Any carbon black may be used, and examples include: N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. These may be used alone or in combination of two or more.
[0081] The nitrogen adsorption specific surface area (N2SA) of carbon black is preferably 80 m 2 / g or more, more preferably 100m 2 / g or more, but preferably 200m 2 / g or less, more preferably 150m 2 / g or less, more preferably 125m 2 When N2SA is within the above range, the beneficial effects tend to be better achieved.
[0082] Herein, N2SA of carbon black is measured in accordance with JIS K6217-2:2001.
[0083] Carbon black can be purchased from Asahi Carbon Co., Ltd., Cabot (Japan) Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Shin Nichika Carbon Co., Ltd., Columbia Carbon, and the like.
[0084] The amount of carbon black is preferably 3 parts by mass or more, but is preferably 80 parts by mass or less, more preferably 50 parts by mass or less, further preferably 30 parts by mass or less, particularly preferably 20 parts by mass or less, and most preferably 10 parts by mass or less relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0085] Examples of silica include dry-process silica (anhydrous silicic acid) and wet-process silica (hydrated silicic acid). Wet-process silica is preferred because it has a large number of silanol groups. These may be used alone or in combination of two or more.
[0086] The nitrogen adsorption specific surface area (N2SA) of silicon dioxide is 40 m 2 / g or more, preferably 70m 2 / g or more, more preferably 80m 2 / g or more, more preferably 140m 2 / g or more, particularly preferably 160m 2 / g or more. N2SA is also preferably 600m 2 / g or less, more preferably 300m 2 / g or less, more preferably 250m 2 / g or less, particularly preferably 200m 2 When N2SA is within the above range, beneficial effects tend to be more suitably achieved.
[0087] The N2SA of silica is measured by the BET method according to ASTM D3037-81.
[0088] Silica can be purchased from Degussa, Rhodia, Tosoh Silicon Corporation, Solvay (Japan), Tokuyama Corporation, and the like.
[0089] The amount of silica is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, further preferably 20 parts by mass or more, particularly preferably 40 parts by mass or more, most preferably 60 parts by mass or more, further preferably 80 parts by mass or more, further preferably 100 parts by mass or more, but is preferably 200 parts by mass or less, more preferably 180 parts by mass or less, further preferably 160 parts by mass or less, and particularly preferably 140 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0090] The amount of silica is preferably 30% by mass or more, more preferably 50% by mass or more, further preferably 70% by mass or more, particularly preferably 85% by mass or more, most preferably 90% by mass or more, based on 100% by mass of the filler (reinforcing filler) in the rubber composition, and may be 100% by mass. When the amount is within the above range, the beneficial effects tend to be more suitably achieved.
[0091] The rubber composition containing silica preferably further contains one or more silane coupling agents.
[0092] Any silane coupling agent may be used. Examples include sulfide-based silane coupling agents such as bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)tetrasulfide, bis(3-triethoxysilylpropyl) disulfide, bis(2-triethoxysilylethyl) disulfide, bis(4-triethoxysilylbutyl) disulfide, bis(3-trimethoxysilylpropyl) disulfide, bis(2-trimethoxysilylethyl) disulfide, bis(4-trimethoxysilylbutyl) disulfide, 3-trimethoxysilylpropyl-N,N- dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silane coupling agents, such as 3-mercaptopropyltrimethoxysilane and 2-mercaptoethyltriethoxysilane; vinyl-based silane coupling agents, such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silane coupling agents, For example, 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silane coupling agents, such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silane coupling agents, such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chlorine-based silane coupling agents, such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Commercial products purchased from Degussa, Momentive, Shin-Etsu Silicone, Tokyo Chemical Industry Co., Ltd., AZmax Company, DuPont Toray Specialty Materials Co., Ltd., etc. can be used. These can be used alone or in combination of two or more. Among these, sulfide-based silane coupling agents are preferred, and disulfide silane coupling agents having a disulfide bond, such as bis(3-triethoxysilylpropyl) disulfide, are more preferred, because they tend to achieve better beneficial effects.
[0093] The amount of the silane coupling agent is preferably 3 parts by mass or more, more preferably 6 parts by mass or more, but is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and more preferably 10 parts by mass or less relative to 100 parts by mass of silica. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0094] The rubber composition preferably contains sulfur as a cross-linking agent (vulcanizing agent).
[0095] Examples of sulfur include those commonly used in the rubber industry, such as powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, and soluble sulfur. These may be used alone or in combination of two or more.
[0096] Examples of the vulcanizing agent other than sulfur include organic peroxides.
[0097] Sulfur can be purchased from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flextronics, Nippon Senryu Industry Co., Ltd., Hosoi Chemical Industry Co., Ltd., and the like.
[0098] The amount of the vulcanizing agent (preferably sulfur) is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, further preferably 0.3 parts by mass or more, particularly preferably 0.5 parts by mass or more, but is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, further preferably 2 parts by mass or less, particularly preferably 1.5 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0099] The rubber composition preferably contains one or more vulcanization accelerators.
[0100] Examples of the vulcanization accelerator include: thiazole vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazole disulfide, and N-cyclohexyl-2-benzothiazole sulfenamide; thiuram vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, N-tert-butyl-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine vulcanization accelerators such as diphenylguanidine, di-o-tolylguanidine, and o-tolylbiguanide. These may be used alone or in combination of two or more. Among these, a sulfenamide vulcanization accelerator and / or a guanidine vulcanization accelerator are preferred, and a combination of a sulfenamide vulcanization accelerator and a guanidine vulcanization accelerator is more preferred.
[0101] The vulcanization accelerator can be purchased from Kawaguchi Chemical Industry Co., Ltd., Ouchi Shinko Chemical Industry Co., Ltd., Rhein Chemie, and the like.
[0102] The amount of the vulcanization accelerator is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and further preferably 2 parts by mass or more, but is preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0103] The rubber composition may contain more than one resin.
[0104] Any resin may be used, and examples include solid alkylphenol resins, styrene resins, coumarone-indene resins, terpene resins, rosin resins, acrylic resins, and dicyclopentadiene resins (DCPD resins). These may be used alone or in combination of two or more.
[0105] The resin can be purchased from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemical, BASF, Arizona Chemical, Nitto Chemical Co., Ltd., Nippon Shokubai Co., Ltd., JXTG Nippon Oil & Energy Co., Ltd., Arakawa Chemical Industries, Ltd., Taoka Chemical Co., Ltd., and the like.
[0106] The amount of the resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and further preferably 5 parts by mass or more relative to 100 parts by mass of the rubber component. The amount of the resin is also preferably 80 parts by mass or less, more preferably 50 parts by mass or less, and further preferably 20 parts by mass or less.
[0107] The rubber composition may contain more than one softener.
[0108] Any softener may be used, and examples include oils and liquid diene polymers. These may be used alone or in combination of two or more.
[0109] Examples of oils include process oils, vegetable oils and mixtures thereof. Examples of process oils include paraffin process oils, aromatic process oils and naphthenic process oils. Examples of vegetable oils include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice bran oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia oil and tung oil. These can be used alone or in combination of two or more. In order to achieve the beneficial effect well, among these, process oils are preferred, and aromatic process oils are more preferred.
[0110] The oil can be purchased from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Nippon Energy Co., Ltd., Orison, H&R, Toyokuni Oil Manufacturing Co., Ltd., Showa Shell Sekiyu Co., Ltd., Fuji Chemical Industry Co., Ltd., and the like.
[0111] The liquid diene polymer refers to a diene polymer that is liquid at room temperature (25° C.).
[0112] The weight average molecular weight (Mw) of the liquid diene polymer is preferably 3.0×10 3 More preferably, 4.0×10 3 Above, but preferably 1.0×10 5Less than, more preferably 1.5×10 4 When the Mw is within the above range, advantageous effects can be more suitably achieved.
[0113] Examples of liquid diene polymers include liquid styrene-butadiene copolymers (liquid SBR), liquid polybutadiene polymers (liquid BR), liquid polyisoprene polymers (liquid IR) and liquid styrene-isoprene copolymers (liquid SIR). These can be used alone or in combination of two or more. Among them, liquid SBR is preferred in order to more appropriately achieve beneficial effects.
[0114] The liquid diene polymer can be purchased from Sartomer, Kuraray Co., Ltd., and the like.
[0115] The amount of the softener (preferably oil) is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, but is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, more preferably 20 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved. Herein, the amount of the softener (if used) includes the amount of oil contained in the rubber (oil-extended rubber).
[0116] The rubber composition may contain more than one wax.
[0117] Any wax can be used, examples include: petroleum waxes such as paraffin wax and microcrystalline wax; naturally occurring waxes such as vegetable wax and animal wax; and synthetic waxes such as polymers of ethylene, propylene or other similar monomers. These can be used alone or in combination of two or more. Among these, petroleum wax is preferred, and paraffin wax is more preferred.
[0118] Wax can be purchased from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., and the like.
[0119] The amount of the wax is preferably 0.3 parts by mass or more, more preferably 0.5 parts by mass or more, but is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0120] The rubber composition may include more than one antioxidant.
[0121] Examples of antioxidants include naphthylamine antioxidants such as phenyl-α-naphthylamine; diphenylamine antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; p-phenylenediamine antioxidants such as N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and N,N'-di-2-naphthyl-p-phenylenediamine; quinoline antioxidants such as 2,2,4-trimethyl-1,2-dihydroquinoline polymers; monophenol antioxidants such as 2,6-di-tert-butyl-4-methylphenol and styrenated phenol; and bisphenol antioxidants, triphenol antioxidants or polyphenol antioxidants such as tetrakis[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane. These may be used alone or in combination of two or more. Among these, a p-phenylenediamine antioxidant and / or a quinoline antioxidant is preferred, and a combination of a p-phenylenediamine antioxidant and a quinoline antioxidant is more preferred.
[0122] Antioxidants can be purchased from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., Flextronics, and the like.
[0123] The amount of the antioxidant is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, but is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0124] The rubber composition may include stearic acid.
[0125] Conventional stearic acid can be used, for example, stearic acid available from NOF Corporation, Kao Corporation, Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., and the like.
[0126] The amount of stearic acid is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, but is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0127] The rubber composition may include zinc oxide.
[0128] Conventional zinc oxide, for example, zinc oxide available from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Industry Co., Ltd., Shiramizu Techno Co., Ltd., Shodo Chemical Industry Co., Ltd., Sakai Chemical Co., Ltd., and the like can be used.
[0129] The amount of zinc oxide is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, but is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0130] In addition to the above components, the rubber composition may contain additives commonly used in the tire industry. The amount of these additives is preferably 0.1 to 200 parts by mass relative to 100 parts by mass of the rubber component.
[0131] For example, the rubber composition can be prepared by kneading the components in a rubber kneading machine such as an open roll mill or a Banbury mixer, and then vulcanizing the kneaded mixture.
[0132] The kneading conditions are as follows. In the basic kneading step of kneading additives other than the vulcanizing agent and the vulcanization accelerator, the kneading temperature is usually 100 to 180°C, preferably 120 to 170°C. In the final kneading step of kneading the vulcanizing agent and the vulcanization accelerator, the kneading temperature is usually 120°C or less, preferably 80 to 110°C. In addition, the composition obtained after kneading the vulcanizing agent and the vulcanization accelerator is usually vulcanized by, for example, press vulcanization. The vulcanization temperature is usually 140 to 190°C, preferably 150 to 185°C. The vulcanization time is usually 5 to 15 minutes.
[0133] The rubber composition can be used for tire components (i.e., as a tire rubber composition), including, for example, tread (coasting surface), sidewall, base tread, undertread, clinch, bead apex, breaker cushion rubber, carcass cord topping rubber, insulation layer, bead chafer and inner liner, and side reinforcement layer of run-flat tire. The rubber composition is particularly suitable for tread.
[0134] The tire (e.g., pneumatic tire) of the present invention can be produced from a rubber composition by conventional methods. Specifically, an unvulcanized rubber composition containing additives can be extruded into the shape of a tire component (particularly a tread surface) as required, and then molded in a tire molding machine in a usual manner and assembled with other tire components to produce an unvulcanized tire, which can then be heated and pressurized in a vulcanizer to produce a tire.
[0135] The non-limiting example of tire comprises pneumatic tire, solid tire and airless tire.Among these, pneumatic tire is preferred.
[0136] The tire is suitable for use as any of the following tires: passenger car tires, large passenger car tires, large SUV tires, truck and bus tires, two-wheeler tires, racing tires, winter tires (studless winter tires, snow tires, studded tires), all-season tires, run-flat tires, aircraft tires, mining tires, etc.
[0137] Example
[0138] The present invention is specifically described with reference to the embodiments, but the present invention is not limited to the embodiments.
[0139] The chemicals used in Examples and Comparative Examples are listed below.
[0140] SBR 1: modified SBR produced in the following Production Example 1 (styrene content: 40 mass %, cis content: 21 mol %, trans content: 49 mol %, vinyl content: 30 mol %, Mw: 950,000);
[0141] SBR 2: a two-terminally modified E-SBR polymerized according to the production method of polymer 7 described in JP 2018-76432A (styrene content: 23.5 mass %, cis content: 12 mol %, trans content: 71 mol %, vinyl content: 17 mol %);
[0142] BR 1: modified BR produced in the following Production Example 2 (cis content: 36 mol%, trans content: 52 mol%, vinyl content: 12 mol%, Mw: 550,000);
[0143] BR 2: RB840 (syndiotactic 1,2-polybutadiene, melting point: 126°C, cis content: 3 mol%, trans content: 3 mol%, vinyl content: 94 mol%, crystallinity: 36%), purchased from JSR Corporation;
[0144] Carbon black: Seast I (N220, N2SA: 114m 2 / g), purchased from Mitsubishi Chemical Corporation;
[0145] Silica: Ultrasil VN3(N2SA:175m 2 / g), purchased from Evonik Degussa;
[0146] Stearic acid: stearic acid "TSUBAKI", purchased from NOF Corporation;
[0147] Wax: Ozoace 0355, purchased from Nippon Seira Co., Ltd.;
[0148] Oil: Diana Process NH-70S (aromatic process oil), purchased from Idemitsu Kosan Co., Ltd.;
[0149] Silane coupling agent: Si266 (bis(3-triethoxysilylpropyl) disulfide), purchased from Evonik Degussa;
[0150] Zinc oxide: Zinc oxide #2, purchased from Mitsui Mining & Smelting Co., Ltd.;
[0151] Antioxidant 1: NOCRAC 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine), purchased from Ouchi Shinko Chemical Industry Co., Ltd.;
[0152] Antioxidant 2: NOCRAC RD (poly(2,2,4-trimethyl-1,2-dihydroquinoline)), purchased from Ouchi Shinko Chemical Industry Co., Ltd.;
[0153] Sulfur containing 5% oil: powdered sulfur (sulfur containing 5% oil), purchased from Tsurumi Chemical Industry Co., Ltd.;
[0154] Vulcanization accelerator CZ: Soxinol CZ (N-cyclohexyl-2-benzothiazole sulfenamide), purchased from Sumitomo Chemical Co., Ltd.;
[0155] Vulcanization accelerator DPG: Soxinol D (N,N'-diphenylguanidine), purchased from Sumitomo Chemical Co., Ltd.
[0156] (Production Example 1)
[0157] Cyclohexane, tetrahydrofuran, styrene and 1,3-butadiene were charged into a nitrogen-purged autoclave reactor. The temperature of the reactor contents was adjusted to 20°C, and then n-butyl lithium was added to initiate polymerization. The polymerization was carried out under adiabatic conditions, with the maximum temperature reaching 85°C. Once the polymerization conversion reached 99%, 1,3-butadiene was further added, followed by polymerization for 5 minutes. Subsequently, N,N-bis(trimethylsilyl)-3-aminopropyltriethoxysilane was added as a modifier and the reaction was carried out. After the polymerization reaction was completed, 2,6-di-tert-butyl-p-cresol was added. Thereafter, the solvent was removed by stripping. The product was dried on a hot roller adjusted to 110°C to obtain SBR 1.
[0158] (Production Example 2)
[0159] Under a nitrogen atmosphere, 3-dimethylaminopropyltrimethoxysilane was added to a measuring bottle, and then anhydrous hexane was added to prepare a terminal modifier.
[0160] n-Hexane, butadiene and TMEDA were placed in a pressure-resistant container purged with sufficient nitrogen and then heated to 60°C. Next, butyl lithium was added, and the mixture was heated to 50°C and stirred for 3 hours. Subsequently, a terminal modifier was added and the mixture was stirred for 30 minutes. Methanol and 2,6-tert-butyl-p-cresol were added to the reaction solution, and the resulting reaction solution was placed in a stainless steel container containing methanol. Aggregates were then collected. The aggregates were dried under reduced pressure for 24 hours to obtain modified polybutadiene rubber (BR 1).
[0161] (Examples and Comparative Examples)
[0162] In a 1.7L Banbury mixer (Kobe Steel), the chemicals except sulfur and vulcanization accelerator of the formulation shown in Table 1 were kneaded at 150°C for 4 minutes to obtain a kneaded mixture. Then, sulfur and vulcanization accelerator were added to the kneaded mixture, and they were kneaded at 80°C for 4 minutes in an open roll mill to prepare an unvulcanized rubber composition. Then, the unvulcanized rubber composition was press-vulcanized at 170°C for 12 minutes in a 0.5mm thick mold to obtain a vulcanized rubber composition.
[0163] Furthermore, the unvulcanized rubber composition prepared as above was formed into a tread shape and assembled with other tire components to produce an unvulcanized tire. The unvulcanized tire was press-vulcanized at 170° C. for 10 minutes to prepare a test tire (size: 195 / 65R15).
[0164] The vulcanized rubber composition and the test tire prepared as above were placed in an oven at 40° C. for 60 days to prepare aged vulcanized rubber compositions and test tires.
[0165] The following evaluations were performed on the vulcanized rubber composition (new), the vulcanized rubber composition (after aging), the test tire (new), and the test tire (after aging). The results are shown in Table 1.
[0166] <Wet Grip Performance>
[0167] According to ASTM E303-83, a portable side skid test bench (Stanley) was used to analyze the vulcanized rubber composition. The results are expressed as an index (wet grip performance index) relative to the vulcanized rubber composition (new product) of Example 1, wherein Example 1 is 105. The higher the index, the shorter the braking distance, and therefore the wet anti-skid performance (wet grip performance) is better. In this article, it is believed that the wet grip performance (before aging) index is 80 or more, indicating that the wet grip performance is good.
[0168] In addition, the wet grip performance maintenance rate is calculated from the evaluation results of the vulcanized rubber composition (new product) and the vulcanized rubber composition (after aging). The higher the wet grip performance maintenance rate, the better the ability to reduce the deterioration of wet grip performance over time. In this article, it is considered that a wet grip performance maintenance rate of 80 or more indicates a good ability to reduce the deterioration of wet grip performance over time.
[0169] <Abrasion resistance>
[0170] A set of test tires (new) or test tires (after aging) were mounted on a front-engine front-wheel drive car manufactured in Japan. After driving 8,000 kilometers, the groove depth of the tread portion of the tire was measured. The distance that caused the tire groove depth to decrease by 1 mm was calculated and expressed as an index (wear resistance index) relative to Example 6, where Example 6 was 100. The higher the index, the longer the distance that caused the tire groove depth to decrease by 1 mm, and therefore the better the wear resistance.
[0171] In addition, the wear resistance maintenance rate is calculated from the evaluation results of the test tire (new product) and the test tire (after aging). The higher the wear resistance maintenance rate, the better the ability to reduce the deterioration of wear resistance over time. In this article, it is considered that a wear resistance maintenance rate of 80 or more indicates a good ability to reduce the deterioration of wear resistance over time.
[0172]
[0173] As shown in Table 1, the examples using the following rubber compositions show good wet grip performance and excellent ability to reduce the deterioration of wet grip performance and wear resistance over time: the rubber composition comprises one or more rubber components (the total content of styrene-butadiene rubber and polybutadiene of the rubber components is 90% by mass or more), one or more fillers and one or more vulcanizing agents; each based on 100 mol% of the total amount of butadiene structural units in the butadiene part of the styrene-butadiene rubber and polybutadiene, the vinyl content of the entire rubber composition is 20 mol% or more, and the trans content is 50 mol% or more.
Claims
1. A tire rubber composition comprising: One or more rubber components, wherein the total content of styrene-butadiene rubber and polybutadiene in the rubber component is 90% by mass or more; One or more fillers, the fillers comprising carbon black and silica; and More than one vulcanizing agent; The total amount of butadiene structural units in the butadiene part of the styrene-butadiene rubber and the polybutadiene is 100 mol %, the vinyl content of the entire rubber composition is 20 mol % or more, and the trans content is 50 mol % or more, in, The tire rubber composition comprises styrene-butadiene rubber and polybutadiene; The amount of the carbon black is 3 to 80 parts by mass, and the amount of the silica is 5 to 200 parts by mass, relative to 100 parts by mass of the rubber component.
2. The tire rubber composition according to claim 1, in, The vinyl content is 30 mol% or more.
3. The tire rubber composition according to claim 1, in, The vinyl content is 35 mol% or more.
4. The tire rubber composition according to claim 1, in, The vinyl content is 36 mol% or more.
5. The tire rubber composition according to any one of claims 1 to 4, in, The tire rubber composition includes 80 parts by mass or more of silica relative to 100 parts by mass of the rubber component.
6. The tire rubber composition according to any one of claims 1 to 4, in, The tire rubber composition includes syndiotactic 1,2-polybutadiene.
7. A tire having a tread, the tread comprising the tire rubber composition according to any one of claims 1 to 6.