Based on mixed oxides of cerium and zirconium

By using mixed oxide particles of zirconium, cerium, lanthanum and rare earth elements in gasoline engines, the problem of microparticles, NOx and CO emissions in gasoline engines is solved, and efficient emission reduction and heat resistance are achieved, while meeting the European 6 standards are maintained. Low backpressure.

CN114144380BActive Publication Date: 2024-12-06RHODIA OPERATIONS SAS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080052431.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-19
Filing Date
2020-07-15
Publication Date
2024-12-06
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively reduce particulate, NOx and CO emissions in gasoline engines while maintaining acceptable back pressure, especially when meeting the Euro 6 emission standards.

Method used

Develop a mixed oxide containing zirconium, cerium, lanthanum and optionally rare earth elements to ensure high temperature conditions by providing particles with high specific surface area and high pore volume in the form of an aqueous slurry The heat resistance and low viscosity are suitable for gasoline engine filters.

Benefits of technology

Achieving the high specific surface area and pore volume under high temperature conditions and having low viscosity in water mixed oxide particles can effectively reduce particles, NOx and CO in gasoline engine emissions, meet the requirements of Euro 6 emission standards, and avoid Increased back pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003478334920000151
    Figure BDA0003478334920000151
  • Figure BDA0003478334920000191
    Figure BDA0003478334920000191
  • Figure BDA0003478334920000192
    Figure BDA0003478334920000192
Patent Text Reader

Abstract

Mixed oxide, catalytic composition, catalytic wall-flow monolith, use of the mixed oxide and method for preparing the mixed oxide. The mixed oxide comprises zirconium, cerium, lanthanum and optionally at least one rare earth element other than cerium and lanthanum. The catalytic composition and the wall-flow monolith comprise particles of the mixed oxide. The use of the mixed oxide is in the preparation of a coating on a filter. The method for preparing the mixed oxide comprises jet milling. The mixed oxide is a compromise between calibrated size and low viscosity when in the form of an aqueous slurry while maintaining a high specific surface area and a high pore volume.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims priority to international patent application PCT / CN 2019 / 096864 filed on July 19, 2019, the contents of which are fully incorporated by reference into this application for all purposes. If there are any inconsistencies between this application and the PCT application affecting the clarity of terminology or expression, reference should be made only to this application.

[0002] The present invention relates to mixed oxides based on cerium, zirconium, lanthanum and optionally at least one rare earth element other than cerium and other than lanthanum, which exhibit a compromise between viscosity of the aqueous slurry, porosity and heat resistance at high temperatures. The invention also relates to catalytic compositions comprising particles of said mixed oxides and to the use of said compositions in the preparation of coatings on filters. Background Art

[0003] Gasoline engines produce a combustion exhaust gas stream containing hydrocarbons, carbon monoxide and nitrogen oxides as well as particulates. It is known to treat the gases with three-way catalyst compositions and to recover the particulates in particulate traps such as soot filters.

[0004] Historically, gasoline engines that operate primarily in a stoichiometric manner have been designed to form low levels of particulate matter. However, gasoline direct injection (GDI) engines, which are increasingly being used for their fuel efficiency, can have lean burn conditions and stratified combustion, leading to particulate generation. Particulate emissions from engines fueled by gasoline fuel, such as GDI engines, are regulated, and existing gasoline engine aftertreatment systems are not suitable for achieving proposed particulate matter standards.

[0005] The particulates produced by gasoline engines tend to be finer and at lower levels than those produced by diesel lean-burn engines. This is due to the different combustion conditions of a diesel engine as compared to a gasoline engine. For example, gasoline engines operate at higher temperatures than diesel engines. In addition, the hydrocarbon components produced in the emissions of a gasoline engine as compared to a diesel engine are different.

[0006] Emission standards for unburned hydrocarbons, carbon monoxide, and nitrogen oxide pollutants continue to become more stringent. To meet such standards, catalytic converters containing three-way catalysts (TWCs) are placed in the exhaust line of gasoline-fueled internal combustion engines. Such catalysts promote the oxidation of oxygen and nitrogen oxides in the exhaust stream of unburned hydrocarbons and carbon monoxide, and the accompanying reduction of nitrogen oxides to nitrogen.

[0007] The new Euro 6 (Euro 6 and Euro 6c) emission standards present many challenging design issues for meeting gasoline emission standards. In particular, how to design a filter or exhaust system including a filter to reduce particulate matter (PM) gasoline (forced ignition) emissions while also meeting non-PM pollutants such as nitrogen oxides (NO x ), carbon monoxide (CO) and unburned hydrocarbons (HC)) emissions standards, all at an acceptable backpressure, for example as measured by maximum cycle backpressure on the EU drive cycle.

[0008] It is known to provide a three way catalyst (TWC) in a gasoline system on a substrate support such as a flow-through monolith. It is also known to combine the TWC and particulate removal functions in a single device by coating the TWC onto a wall flow monolith (particulate filter).

[0009] Issues to be resolved

[0010] The mixed oxide is mixed with other inorganic materials in the form of a slurry, and the slurry is coated on a substrate support such as a flow-through monolith or filter. The difficulty is that the slurry maintains a viscosity that is not too high so that it can be easily processed and does not affect the performance of the coating. The object of the present invention is to provide a mixed oxide that can be easily coated on a substrate support, more particularly on a wall-flow monolith or filter, while still exhibiting a high specific surface area and a high pore volume. The mixed oxide of the present invention is a compromise between calibrated size and low viscosity when in the form of an aqueous slurry, while maintaining a high specific surface area S. 1100 ℃ / 4h and high pore volume (TPV and PV 0-300 nm ). Technical Background

[0012] US 8,640,440 discloses a filter having two layers, one of the layers containing an oxygen-storing cerium / zirconium mixed oxide.

[0013] WO 2017 / 060694 discloses a NOx absorber. There is no mention of mixed oxides having d50 or d90 characteristics.

[0014] US 2019 / 168188 discloses mixed oxides of zirconium, cerium, lanthanum and optionally at least one rare earth metal other than cerium and lanthanum, but does not disclose the total pore volume, d50 and d90. Summary of the invention

[0015] The present invention relates to a mixed oxide as disclosed in claims 1 to 32. The mixed oxide comprises zirconium, cerium, lanthanum and optionally at least one rare earth element (RE) other than cerium and lanthanum, and has the following composition:

[0016] ■ between 8.0% and 45.0% by weight of cerium;

[0017] ■ between 1.0% and 15.0% by weight of lanthanum;

[0018] ■ up to 15.0% by weight of the rare earth elements other than cerium and lanthanum;

[0019] ■ the total proportion of lanthanum and the one or more rare earth elements other than cerium and other than lanthanum is lower than or equal to 25.0%, more particularly lower than or equal to 20.0%, even more particularly lower than or equal to 18.0%;

[0020] ■The remainder is zirconium;

[0021] The mixed oxide exhibited the following properties after calcination at 1100°C for 4 hours in air:

[0022] ■Specific surface area (S 1100℃ / 4h ) between 25 and 50m 2 / g, more particularly between 28 and 50 m 2 / g, even more particularly between 30 and 50 m 2 / g between;

[0023] ■ Pore volume (PV) determined by mercury porosimetry for pores with a diameter below 300 nm 0-300nm ) at 0.50cm 3 / g and 0.90cm 3 / g, more particularly between 0.50 cm 3 / g and 0.80cm 3 / g, even more particularly between 0.50 cm 3 / g and 0.70cm 3 / g between;

[0024] The mixed oxide is in the form of particles having the following properties:

[0025] d50 is between 1.0 μm and 2.5 μm, more particularly between 1.0 μm and 2.2 μm, even more particularly between 1.0 μm and 2.0 μm or between 1.5 μm and 2.0 μm;

[0026] • d90 is between 2.0 μm and 9.0 μm, more particularly between 2.0 μm and 8.0 μm, even more particularly between 2.0 μm and 7.0 μm or between 3.0 μm and 8.0 μm or between 3.0 μm and 7.0 μm.

[0027] The invention also relates to a catalytic composition as disclosed in claim 33 and a catalytic wall flow monolith as disclosed in claim 34. The invention also relates to the use of the mixed oxide as disclosed in claim 35 and a method for preparing the mixed oxide as disclosed in claims 36-39.

[0028] More details about these inventions are now given below. DETAILED DESCRIPTION

[0029] Unless otherwise mentioned, the calcinations, more particularly the calcinations for which the values ​​for the specific surface areas are given hereafter, are calcinations in air. For the sake of continuity of the present description, it is also specified that, unless otherwise indicated, the limits are included in the range of all values ​​given. This also applies to expressions including "at least" or "at most" or "up to". Furthermore, rare earth elements other than cerium and other than lanthanum are denoted as RE.

[0030] The above-mentioned elements (Ce, Zr, La, RE) are usually present in the mixed oxide as oxides. However, they may also be present partly in the form of hydroxides or oxyhydroxides.

[0031] In addition to the above-mentioned elements, the mixed oxide of the present invention may also contain the element hafnium. This element is usually present in combination with zirconium in ores present in a natural state. The relative proportion of hafnium relative to zirconium depends on the ore from which the zirconium is extracted. In some ores, the relative proportion of Zr / Hf by weight can be about 50 / 1. Thus, baddeleyite contains approximately 98% ZrO2 and 2% HfO2. Like zirconium, hafnium is usually present as an oxide. However, it is not excluded that hafnium is also partially present in the form of hydroxide or oxyhydroxide. The proportion of hafnium in the mixed oxide is less than or equal to 2.5% (≤2.5%), or even less than or equal to 2.0% (≤2.0%).

[0032] As in the field of mixed oxides, the proportions of the elements are given by weight of the oxide relative to the mixed oxide as a whole. For the calculation of these proportions, the following oxides were considered: CeO2, ZrO2, HfO2, La2O3, RE2O3 (except Pr (for which Pr6O3 was considered) 11 )). As an example, the proportions of the mixed oxide of Example 1 (Zr-Ce-La 60%-35%-5%) correspond to: 60% ZrO2, 35% CeO2 and 5% La2O3. The proportions of the elements are determined by common analytical methods such as X-ray fluorescence or by inductively coupled plasma mass spectrometry.

[0033] The present invention more particularly relates to a mixed oxide consisting of a combination of oxides of: zirconium; cerium; lanthanum; optionally at least one rare earth element (RE) other than cerium and other than lanthanum; and optionally hafnium, the mixed oxide having the following composition:

[0034] ■ between 8.0% and 45.0% by weight of cerium;

[0035] ■ between 1.0% and 15.0% by weight of lanthanum;

[0036] ■ up to 15.0% by weight of the rare earth elements other than cerium and lanthanum;

[0037] ■ the total proportion of lanthanum and the one or more rare earth elements other than cerium and lanthanum is lower than or equal to 25.0%, more particularly lower than or equal to 20.0%, even more particularly lower than or equal to 18.0%;

[0038] ■The proportion of hafnium is less than or equal to 2.5%, or even less than or equal to 2.0%;

[0039] ■The remainder is zirconium;

[0040] The mixed oxide exhibited the following properties after calcination at 1100°C for 4 hours in air:

[0041] ■Specific surface area (S 1100℃ / 4h ) between 25 and 50m 2 / g, more particularly between 28 and 50 m 2 / g, even more particularly between 30 and 50 m 2 / g between;

[0042] ■ The pore volume determined by mercury porosimetry for pores with a diameter below 300 nm is within 0.50 cm 3 / g and 0.90cm 3 / g, more particularly between 0.50 cm 3 / g and 0.80cm 3 / g, even more particularly between 0.50 cm 3 / g and 0.70cm 3 / g between;

[0043] The mixed oxide is in the form of particles having the following properties:

[0044] d50 is between 1.0 μm and 2.5 μm, more particularly between 1.0 μm and 2.2 μm, even more particularly between 1.0 μm and 2.0 μm or between 1.5 μm and 2.0 μm;

[0045] • d90 is between 2.0 μm and 9.0 μm, more particularly between 2.0 μm and 8.0 μm, even more particularly between 2.0 μm and 7.0 μm.

[0046] The mixed oxide of the invention comprises the above-mentioned elements (Ce, Zr, Hf (if any), La, RE (if any)) in the above-mentioned proportions, but the mixed oxide may also contain other elements in addition, like impurities. The impurities may originate from the raw materials or starting materials used in the process for preparing the mixed oxide. The total proportion of these impurities may be generally less than 0.2% by weight relative to the mixed oxide.

[0047] The mixed oxide contains cerium. The proportion of cerium is between 8.0% and 45.0%, more particularly between 18.0% and 44.0%, even more particularly between 18.0% and 42.0%. The proportion may also be between 18.0% and 37.0%, or between 18.0% and 22.0%, or between 20.0% and 35.0%, or between 22.0% and 26.0%, or between 28.0% and 32.0%, or between 33.0% and 37.0%, or between 30% and 45%, or between 38.0% and 42.0%.

[0048] The mixed oxide also contains lanthanum. The proportion of lanthanum is between 1.0% and 15.0%. This proportion may include between 1.0% and 13.0%, more particularly between 1.0% and 8.0%, even more particularly between 2.0% and 8.0% or between 3.0% and 9.0% or between 3.0% and 7.0%.

[0049] The mixed oxide may also contain up to 15.0% by weight of at least one rare earth element (RE) other than cerium and lanthanum. Rare earth metals as defined by IUPAC are one of the set of seventeen chemical elements (specifically fifteen lanthanides and scandium and yttrium) in the periodic table. Rare earth elements are cerium (Ce), dysprosium (Dy), erbium (Er), europium (Eu), gadolinium (Gd), holmium (Ho), lanthanum (La), lutetium (Lu), neodymium (Nd), praseodymium (Pr), promethium (Pm), samarium (Sm), scandium (Sc), terbium (Tb), thulium (Tm), ytterbium (Yb) and yttrium (Y). More particularly, the rare earth elements other than cerium and lanthanum may be Y or Nd or a combination of Y and Nd. The proportion of the one or more rare earth elements other than cerium and lanthanum is therefore between 0% and 15.0%. This proportion may be between 1.0% and 13.0%, more particularly between 1.0% and 8.0%, even more particularly between 2.0% and 8.0% or between 3.0% and 7.0%. The proportion may also be between 10.0% and 13.0%.

[0050] The total proportion of lanthanum and the one or more rare earth elements other than cerium and other than lanthanum is lower than or equal to 25.0%, more particularly lower than or equal to 20.0%, even more particularly lower than or equal to 18.0%.

[0051] As far as the proportion of zirconium is concerned, zirconium is present as the remainder in the mixed oxide. The total amount of all elements is 100%, so the proportion of zirconium corresponds to a 100% supplement to the other elements in the mixed oxide. The proportion of zirconium is higher than 45.0%, more particularly higher than 48.0%, even more particularly higher than or equal to 50.0%. The proportion of zirconium can be between 48.0% and 80.0%. The mixed oxide of the present invention can be described as a Zr-rich mixed oxide, i.e. a mixed oxide with a weight ratio ZrO2 / CeO2>1.0, more particularly a weight ratio ZrO2 / CeO2≥1.25.

[0052] Now a more specific composition according to the invention is given below:

[0053] - Composition C1

[0054] ■ between 18.0% and 37.0% by weight of cerium;

[0055] ■ between 3.0% and 9.0% by weight of lanthanum;

[0056] ■The remainder is zirconium.

[0057] For this composition C1, the proportion of cerium may more particularly be between 18.0% and 22.0% or between 33.0% and 37.0%. The proportion of lanthanum may more particularly be between 3.0% and 7.0%.

[0058] - Composition C2

[0059] ■ between 30.0% and 45.0% by weight of cerium;

[0060] ■ between 3.0% and 9.0% by weight of lanthanum;

[0061] ■ between 3.0% and 9.0% by weight of at least one rare earth element (RE) other than cerium and other than lanthanum;

[0062] ■The remainder is zirconium.

[0063] For this composition C2, the proportion of cerium may more particularly be between 38.0% and 42.0% or between 33.0% and 37.0%. The proportion of lanthanum may more particularly be between 3.0% and 7.0%. The proportion of the one or more rare earth elements other than cerium and lanthanum may more particularly be between 3.0% and 7.0%.

[0064] - Composition C3

[0065] ■ between 20.0% and 35.0% by weight of cerium;

[0066] ■ between 3.0% and 9.0% by weight of lanthanum;

[0067] ■ between 3.0% and 15.0% by weight of at least one rare earth element (RE) other than cerium and other than lanthanum;

[0068] ■The remainder is zirconium.

[0069] For this composition C3, the proportion of cerium may more particularly be between 22.0% and 26.0% or between 28.0% and 32.0%. The proportion of lanthanum may more particularly be between 3.0% and 7.0%. The proportion of the one or more rare earth elements other than cerium and lanthanum may more particularly be between 3.0% and 7.0%.

[0070] The mixed oxide particles of the invention are characterized by the following parameters: The particles exhibit a d50 between 1.0 μm and 2.5 μm, more particularly between 1.0 μm and 2.2 μm, even more particularly between 1.0 μm and 2.0 μm or between 1.5 μm and 2.0 μm. In an embodiment, d50 < 2.5 μm (strictly less than 2.5 μm).

[0071] The particles of the mixed oxide exhibit a d90 of between 2.0 μm and 9.0 μm, more particularly between 2.0 μm and 8.0 μm, even more particularly between 2.0 μm and 7.0 μm or between 3.0 μm and 8.0 μm or between 3.0 μm and 7.0 μm.

[0072] The particles may exhibit a d10 lower than or equal to 1.0 μm (≤1.0 μm), more particularly lower than or equal to 0.8 μm (≤0.8 μm), even more particularly lower than or equal to 0.7 μm (≤0.7 μm). The d10 may be higher than or equal to 0.2 μm (≥0.2 μm), more particularly higher than or equal to 0.3 μm (≥0.3 μm). The d10 may be between 0.2 μm and 1.0 μm, more particularly between 0.2 μm and 0.8 μm, even more particularly between 0.3 μm and 0.8 μm.

[0073] The particles may exhibit a d99 lower than or equal to 20.0 μm, more particularly lower than or equal to 15.0 μm. The d99 may be higher than or equal to 5.0 μm, more particularly higher than or equal to 7.0 μm. The d99 may be between 5.0 μm and 20.0 μm, more particularly between 7.0 μm and 20.0 μm, even more particularly between 7.0 μm and 15.0 μm.

[0074] D10, D50, D90 and D99 (in μm) have the usual meaning used in statistics. Thus, dn (n=10, 50, 90 or 99) represents the following particle size, so that n% of the particles are less than or equal to the particle size. D50 therefore represents the median. These parameters are determined based on the particle size distribution (by volume) obtained with a laser diffraction particle size analyzer. The distribution measurement conditions given in the examples can be applied.

[0075] The mixed oxides are also characterized by a high heat resistance. This resistance is necessary because the coating needs to withstand high temperatures. In this respect, it must be borne in mind that gasoline engines are mainly operated with a stoichiometric air / fuel mixture, so the exhaust gases generally exhibit significantly higher temperatures than lean-burn engines. It is therefore known that gasoline engine filters operate at higher temperatures than more conventional diesel particulate filters. The specific surface area (S) of the mixed oxide after calcination at 1100° C. in air for 4 hours is 2.33 m / s. 1100℃ / 4h )) Between 25 and 50m 2 / g, more particularly between 28 and 50 m 2 / g, even more particularly between 30 and 50 m 2 / g. The specific surface area can be between 25 and 40 m 2 / g or between 25 and 35m 2 / g or between 30 and 35m 2 / g.

[0076] The specific surface area (S) of the mixed oxide after calcination at 1000 °C for 4 hours in air 1000℃ / 4h ) can be between 50 and 70m 2 / g, more particularly between 55 and 70 m 2 / g.

[0077] The term "specific surface area (BET)" is understood to mean the BET specific surface area determined by nitrogen adsorption. The specific surface area is well known to the skilled person and is measured according to the Brunauer-Emmett-Teller method. The theory of this method was originally described in the journal "The Journal of the American Chemical Society, 60, 309 (1938)". More detailed information on this theory can also be found in Chapter 4 of "Powder surface area and porosity", 2nd edition, ISBN 978-94-015-7955-1. The nitrogen adsorption method is disclosed in the standard ASTM D 3663-03 (reapproved in 2008).

[0078] The mixed oxide according to the invention is also characterized in that the pore volume determined by mercury porosimetry for pores with a diameter below 300 nm is between 0.50 cm 3 / g and 0.90cm 3 / g, more particularly between 0.50 cm 3 / g and 0.80cm 3 / g, even more particularly between 0.50 cm 3 / g and 0.70cm 3 This pore volume is determined for the mixed oxide after calcination at 1100° C. for 4 hours in air and is designated as PV in this application. 0-300nm .

[0079] The mixed oxide is also characterized by a total pore volume of 1.40 cm 3 / g and 3.00cm 3 / g, more particularly between 1.50cm 3 / g and 3.00cm 3 / g, even more particularly between 1.50 cm 3 / g and 2.50cm 3 / g or between 1.50cm 3 / g and 2.20cm 3 / g. The total pore volume may be at least 1.60 cm 3 / g. This pore volume is determined after calcination of the oxidic mixture at 1100° C. for 4 hours in air and is designated as TPV in the present application.

[0080] Mercury porosimetry is a standard technique used in the field of porous catalysts and involves gradually forcing mercury into the pores of a porous structure under a controlled pressure. Porosity is measured by mercury intrusion according to well-known techniques in the field. Porosity can be determined using a Micromeritics V 9620 automatic mercury intrusion instrument according to the manufacturer's guidelines. Porosimeters include powder penetrometers. The method is based on the determination of the pore volume as a function of pore size (V = f(d), V represents the pore volume and d represents the pore diameter). From these data, curve (C) can be obtained, resulting in the derivative dV / dlogD. The pore volume PV is determined from curve (C) 0-300nm and total pore volume TPV.

[0081] Preferably the procedure outlined in ASTM International Test Method D 4284-07 is followed. The sample weight is about 0.5 grams, the mercury contact angle is 130°, and the mercury surface tension is 485 dyn / cm under the following conditions.

[0082] It must be noted that when a mixed oxide is milled or ground, its specific surface area and total pore volume generally tend to decrease. The mixed oxide of the present invention is interesting in that, by the process used and despite the reduction in particle size in step (g1), the specific surface area is not reduced too much and the total pore volume remains high.

[0083] The mixed oxide of the present invention is also characterized by a low viscosity of the dispersion of particles in water. In fact, the viscosity of a dispersion containing 43.0 wt % of mixed oxide particles in water and exhibiting a pH of 4.0 ± 0.1 is less than or equal to 20.0 cP (≤ 20.0 cP). The viscosity is measured at 20°C ± 1°C. The viscosity is for a dispersion of 5.0 and 10.0 s -1 The viscosity can be determined by any type of rheometer, more particularly by a rheometer adapted to measure the viscosity of suspensions / dispersions exhibiting low viscosity (<50 cP). The rheometer can be a Brookfield DV2T.

[0084] More specifically, the following method can be applied to measure the viscosity of the dispersion:

[0085] (1) preparing a uniform dispersion of the mixed oxide by mixing particles of the mixed oxide in water;

[0086] (2) Then use a rheometer to record the viscosity over time. When the viscosity stabilizes, measure it.

[0087] In step (1), for example, the powder of the mixed oxide is added to water under stirring in about 15-20min. The pH of the dispersion can be adjusted to the target pH by adding acetic acid. For example, acetic acid can be added with a peristaltic pump to control the pH of the dispersion until the target pH is reached. More specifically, the conditions used in the examples can be applicable.

[0088] Process for preparing the mixed oxide of the invention

[0089] The mixed oxide of the present invention can be prepared by the following method comprising the following steps:

[0090] (a1) contains sulfate anions (SO4 2- ), an aqueous solution of a zirconium chloride salt, a cerium salt and optionally at least one salt of a rare earth element other than cerium and lanthanum (RE salt) reacts with an alkaline aqueous solution to form a precipitate;

[0091] (b1) separating the precipitate obtained at the end of step (a1) from the liquid medium;

[0092] (c1) heating the precipitate obtained at the end of step (b1) in an aqueous medium and optionally in the presence of a lanthanum salt and a basic compound;

[0093] (d1) optionally adding a lanthanum salt, optionally together with a basic compound, to the mixture obtained at the end of step (c1);

[0094] (e1) adding an organic texturizing agent to the mixture obtained at the end of step (d1);

[0095] (f1) separating the solid material obtained at the end of step (e1) from the liquid medium and calcining it in air;

[0096] (g1) Jet milling the solid material obtained at the end of step (f1) to give the mixed oxide according to the invention.

[0097] This method is based on the intimate mixing of the elements of the mixed oxide. This is why the oxides are intimately mixed in the mixed oxide according to the invention. This distinguishes the mixed oxide from a simple mechanical mixture of oxides in solid form.

[0098] In step (a1), the sulfate anion (SO4 2- An aqueous solution (designated CZR solution) of a salt of zirconium chloride, a cerium salt and optionally at least one salt of a rare earth element other than cerium and lanthanum (RE salt) is reacted with an alkaline aqueous solution to form a precipitate. The cerium salt may be cerium nitrate or cerium chloride and also a mixture of these salts. The cerium salt may consist of a cerium (III) salt and optionally a cerium (IV) salt. Cerium salts are ionic compounds generally produced by the neutralization reaction of an acid and a base or by dissolving a cerium compound (such as cerium hydroxide) with an acid. They consist of a cerium cation and an anion, so that the product is electrically neutral.

[0099] The salt of RE may be, for example, a nitrate or a chloride, such as praseodymium nitrate, and neodymium nitrate, yttrium(III) chloride (YCl3) or yttrium nitrate (Y(NO3)3). The aqueous solution may contain one or more rare earth salts.

[0100] The zirconium chloride salt is preferably ZrOCl2.

[0101] The CZR solution contains between 0.5 and 2.0 moles of sulfate anions (SO4) per mole of zirconium and cerium. 2- ). Molar ratio SO4 2- / (Zr+Ce) is preferably in the range of 0.5-1.0, more particularly in the range of 0.5-0.8. The sulfate anion is conveniently provided by adding sulfuric acid.

[0102] The alkaline aqueous solution used may contain an alkaline compound, such as an alkali hydroxide or ammonia. The alkaline compound may be, for example, sodium hydroxide, potassium hydroxide, or ammonia, or a mixture thereof. The alkaline compound may be NaOH. The amount of the alkaline compound may be easily determined by measuring the pH change of the solution. Typically, a sufficient amount is such that the pH of the solution is not less than 7, and a preferred amount is such that the pH is between 7.0 and 11.0. The amount of the alkaline compound is generally such that the alkaline compound is in molar excess relative to Zr, Ce, and RE.

[0103] In order to carry out the reaction in step (a1), contacting can be carried out in any order of introducing the reactants. However, it is preferred that the CZR solution is introduced into a tank containing an alkaline aqueous solution. This reaction can be carried out under an inert atmosphere, notably in a closed reactor or in a semi-closed reactor. Contacting is usually carried out in a stirred tank reactor.

[0104] Step (a1 ) may be carried out at a temperature comprised between 5°C and 50°C.

[0105] In step (b1), the precipitate obtained at the end of step (a1) is separated from the liquid medium. The separation can be carried out, for example, by centrifugation using a Nutsche filter or by decantation. The precipitate can optionally be washed with water. Washing can notably allow reducing the amount of free ions, notably to an amount less than or equal to 500 ppm, preferably less than or equal to 300 ppm for each of these ions, ppm being expressed as the amount by weight of each ion / weight of the solid precipitate expressed as oxide x 100. For example, when the starting materials for the preparation of the mixed oxide are: ZrOCl2, H2SO4, CeCl3 and optionally at least one chloride or nitrate of RE, washing is used to reduce the amount of SO4 remaining in the precipitate. 2- 、Na + and Cl - The amount of NO3 is preferably reduced to an amount lower than or equal to 500 ppm, preferably lower than or equal to 300 ppm for each of these ions. - The amount should also be below these values.

[0106] Furthermore, the precipitate may optionally be dried, notably at a temperature comprised between 40 and 80°C.

[0107] In step (c1), the precipitate obtained at the end of step (b1) is heated in an aqueous medium and optionally in the presence of a lanthanum salt and an alkaline compound. The lanthanum salt is preferably selected from the group consisting of nitrates, chlorides, sulfates, phosphates or carbonates. La(NO3)3 is a convenient La source that can be used. This heat treatment comprises heating the medium and maintaining it at a temperature generally included between 60°C and 200°C, and more particularly between 95°C and 150°C. The duration of this treatment can be between 1 hour and 4 hours. This treatment can also be carried out under an inert atmosphere, and the description of this atmosphere for step (a) is also applicable here. Similarly, the treatment can be carried out in a stirred reactor. After the heat treatment, the solid material can be washed with water. The washing can be carried out in various ways with or without solid / liquid separation. It can thus be carried out by separating solid particles from the liquid phase, for example by frontal filtration, sedimentation or centrifugation. The resulting solid is then resuspended in the aqueous phase. The method can also be carried out by tangential filtration. This washing can optionally be repeated if necessary, for example until a given conductivity of the suspension is obtained, whereby this conductivity is a measure for the amount of impurities present in this suspension.

[0108] In an optional step (d1), a lanthanum salt (notably in liquid or solid form) may be added to the mixture obtained at the end of step (c1). It must be noted that the lanthanum salt is added (i) in step (c1) and / or (ii) in step (d1). When the lanthanum salt is added in step (c1) and step (d1), a portion of the lanthanum salt is added in step (c1) and another portion thereof is added in step (d1).

[0109] In step (e1), an organic texturizing agent (also generally designated by the term "templating agent") is added to the mixture obtained at the end of step (d1). An organic texturizing agent refers to an organic compound capable of controlling the porous structure, notably the mesoporous structure, of the mixed oxide, such as a surfactant. The term "mesoporous structure" refers to an inorganic structure comprising pores with a diameter comprised between 2 and 50 nm, described by the term "mesopores". The organic texturizing agent may be added in the form of a solution or a suspension. The amount of organic texturizing agent, expressed as a percentage by weight of the additive relative to the weight of the mixed oxide obtained after the calcination step (g1), is generally between 5% and 100% and more particularly between 15% and 60%.

[0110] Organic texturizing agent is preferably selected from the group consisting of anionic surfactants, nonionic surfactants, polyethylene glycol, carboxylic acid and its salt and carboxymethylated fatty alcohol ethoxylate type surfactants. About this additive, reference can be made to the teaching of application WO-98 / 45212, and the surfactant described in this document can be used. As anionic surfactants, ethoxy carboxylates, ethoxylated fatty acids, sarcosinates, phosphates, sulfates such as alcohol sulfates, alcohol ether sulfates and sulfated alkanolamide ethoxylates, and sulfonates such as sulfosuccinates and alkylbenzene or alkylnaphthalene sulfonates can be mentioned. As nonionic surfactants, acetylenic surfactants, alcohol ethoxylates, alkanolamides, amine oxides, ethoxylated alkanolamides, long-chain ethoxylated amines, copolymers of ethylene oxide / propylene oxide, sorbitan derivatives, ethylene glycol, propylene glycol, glycerine, polyglycerol esters and their ethoxylated derivatives, alkylamines, alkyl imidazolines, ethoxylated oils and alkylphenol ethoxylates can be mentioned. In particular, mention may be made of trademarks and Products sold. As for carboxylic acids, in particular aliphatic monocarboxylic acids or dicarboxylic acids can be used, and among these, more particularly saturated acids. Fatty acids and more particularly saturated fatty acids can also be used. Thus, formic acid, acetic acid, propionic acid, butyric acid, isobutyric acid, valeric acid, caproic acid, caprylic acid, capric acid, lauric acid, myristic acid and palmitic acid can be mentioned in particular. As dicarboxylic acids, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid and sebacic acid can be mentioned.

[0111] It is also possible to use the salts of carboxylic acids, in particular ammonium. By way of example, mention may more particularly be made of lauric acid and ammonium laurate.

[0112] Finally, it is also possible to use surfactants chosen from those of the carboxymethylated alcohol ethoxylate type.The expression "carboxymethylated alcohol ethoxylate type product" is intended to mean a product consisting of ethoxylated or propoxylated fatty alcohols comprising a -CH2-COOH group at the end of the chain.

[0113] These products can be represented by the following formula:

[0114] R1-O-(CR2R3-CR4R5-O) n -CH2-COOH

[0115] wherein R1 represents a saturated or unsaturated carbon-based chain, the length of which is generally up to 22 carbon atoms, preferably at least 12 carbon atoms; R2, R3, R4 and R5 may be identical and may represent hydrogen, or R2 may represent an alkyl group such as a CH3 group and R3, R4 and R5 represent hydrogen; n is a non-zero integer which may be up to 50 and more particularly between 5 and 15 (these values ​​are included). It should be noted that the surfactant may consist of a mixture of products having the above formula (wherein R1 may be saturated or unsaturated, respectively) or alternatively a mixture of products containing both -CH2-CH2-O- and -C(CH3)=CH2-O- groups.

[0116] In step (f1), the solid material obtained at the end of step (e1) is separated from the liquid medium and calcined in air. The separation can be carried out as in step (b1). The solid material can optionally be washed with an aqueous solution, preferably with water at an alkaline pH (e.g., an aqueous solution of ammonia). In addition, the precipitate can be optionally dried to a suitable degree. The calcination temperature can include between 500°C and 1200°C, more particularly between 800°C and 900°C. The choice of temperature can be carried out as desired, depending on the required values ​​of specific surface area and porosity. The duration of calcination can be appropriately determined according to the temperature, and preferably can be between 1 hour and 20 hours. For example, calcination in air can be carried out at 850°C for 4 hours.

[0117] In step (g1 ), the solid material obtained at the end of step (f1 ) is jet milled to produce the mixed oxide of the invention. More details on jet milling are provided below.

[0118] The invention also relates to a method for preparing a mixed oxide as disclosed herein, which method comprises jet milling a mixed oxide having the same composition as said mixed oxide.

[0119] In the context of the present invention, the term "jet milling" refers to an operation in which particles of a solid material are drawn into an accelerating gas stream and milled by interparticle collisions in the jet stream. The comminution is essentially the result of interparticle collisions in the jet stream. Conveniently, the gas used is air. The forces obtained in jet milling change the particle size and alter the particle size distribution of the particles. The gas is usually accelerated at very high speeds through a series of one or more nozzles.

[0120] A particularly convenient type of jet mill that can be used is a fluidized bed jet mill because it is energy efficient. Comminution occurs within a fluidized bed of material. An example of a fluidized bed jet mill that can be used is disclosed in US 5,992,773.

[0121] An example of a jet mill that can be conveniently used and effectively used is the fluidized bed air jet mill 100AFG commercialized by Hosokawa (see https: / / www.hosokawa-alpine.com / powder- particle-processing / machines / jet-mills / afg-fluidised-bed-opposed-jet-mill / or https: / / www.hosokawa-alpine.com / fileadmin / user_upload / content / Mechanische_ Verfahrenstechnik / Applikationen / P / API-Inhaler / 0007-EN-2013-04_-_ Pharmaceutical_Technology_-_GMP.pdf Get more details: In the latter document, which is available online, the following is disclosed: "Operating principle - The AFG consists of two components: a classifier head and a grinding chamber with integrated nozzles, the number of which depends on the grinder size. The material particles entering the jet are accelerated and collide with each other at the focal point where the air jets intersect. Due to inter-particle collisions at the focal point and shear flows at the edges of the air jets, comminution occurs. The risk of contamination due to abrasion is therefore almost non-existent. The high-performance Turboplex classifier discharges the end product from the internal grinding process to the separator system. The fineness can be set by adjusting the air flow rate, the grinding air pressure and the classifying wheel speed").

[0122] The equipment is usually equipped with a dynamic inducer air classifier, which can be operated at different speeds to change the fineness of the product. The parameters of this equipment that can be varied are the following: the pressure in the mill, the number and configuration of fluid nozzles on the mill and the presence of a classifier, which removes particles with the desired particle size while leaving other particles in the mill for additional grinding. The conditions of use of this equipment selected for the preparation of the mixed oxides of the present invention can be found in the examples and in the following table:

[0123]

[0124] The increase of classifier frequency, feed pressure and milling pressure and the reduction of feed frequency make it possible to obtain the target particle size distribution of mixed oxide of the present invention together with the use of nozzle.Therefore, improve the frequency of classifier to select fine particles.In addition, nozzle is installed to improve the speed of compressed air entering the milling chamber, thereby material is milled more.Feed frequency and feed pressure have an impact on the particle quantity in the grinding chamber.Therefore, the reduction of feed frequency and the increase of feed pressure affect the number of collisions in this chamber.

[0125] The invention also relates to a mixed oxide obtainable by the process disclosed above.

[0126] Use of the mixed oxides of the invention

[0127] The mixed oxides of the invention can be used in the field of exhaust gas treatment.The mixed oxides of the invention can be used to reduce the amount of pollutants present in exhaust gases released by vehicle internal combustion engines.

[0128] The mixed oxide can be used to prepare a catalytic converter, which is used to treat the exhaust gas released by the internal combustion engine of a vehicle. The catalytic converter includes at least one catalytically active layer prepared by depositing a catalytic composition on a solid support. The function of this layer is to chemically convert some pollutants in the exhaust gas into products that are less harmful to the environment. The solid support can be a monolith made of ceramic (such as cordierite), silicon carbide, aluminum titanate or mullite or metal (such as Fecralloy). The support is usually made of cordierite, showing a large specific surface area and a low pressure drop. The monolith is usually honeycomb-type.

[0129] The catalytic composition comprises:

[0130] (i) Aluminium oxide;

[0131] (ii) one or more platinum group metals; and

[0132] (iii) at least one mixed oxide according to the invention.

[0133] Mixed oxides can be used to prepare catalytic wall-flow monoliths. The catalytic wall-flow monoliths include a porous support and a catalytic composition on the surface of the support. Wall-flow monoliths are well known in the art for use as particulate filters. These particulate filters work by passing an exhaust gas stream (including particulate matter) through a wall formed by a porous support. Porosity helps retain particulate matter. The monolith preferably has a first face and a second face defining a longitudinal direction therebetween. In use, one of the first face and the second face will be the inlet face of the exhaust gas, and the other face will be the outlet face of the treated exhaust gas. As is conventional for wall-flow monoliths, it has a first and a second plurality of channels extending in a longitudinal direction. The first plurality of channels opens at the first face and closes at the second face. The second plurality of channels opens at the second face and closes at the first face. The channels are preferably parallel to each other to provide a constant wall thickness between the channels. Therefore, a gas entering one of the plurality of channels cannot leave the monolith without diffusing through the channel wall into the other plurality of channels. The channel is closed by introducing a sealant material into the open end of the channel.

[0134] Preferably, the number of channels in the first plurality of channels is equal to the number of channels in the second plurality of channels, and each plurality of channels is evenly distributed throughout the monolith. Preferably, the wall flow monolith has from 100 to 500 channels per square inch (cpsi), preferably from 200 to 400 cpsi, in a plane perpendicular to the longitudinal direction. For example, on the first face, the density of the open first channels and the closed second channels is from 200 to 400 channels per square inch. The channels may have a cross-section of a rectangular, square, circular, elliptical, triangular, hexagonal or other polygonal shape.

[0135] In order to facilitate the passage of the exhaust gas to be treated through the channel wall, the monolith is formed by a porous substrate. The substrate also serves as a support for the catalytic composition. Suitable materials for forming the porous substrate include ceramic-like materials (such as cordierite), silicon carbide, silicon nitride, zirconium oxide, mullite, spodumene, alumina-silicon dioxide-magnesium oxide or zirconium silicate, or porous refractory metals. The wall-flow substrate can also be formed by a ceramic fiber composite material. The preferred wall-flow substrate is formed by cordierite and silicon carbide. Such materials can withstand the environment encountered in the treatment of exhaust gas flow, especially high temperatures, and can be made sufficiently porous. Such materials and their use in the manufacture of porous monolithic substrates are well known in the art.

[0136] The catalytic composition is applied in the form of a layer on a porous substrate. Traditionally, the loading of the layer should not be too high to avoid back pressure. The loading can be between 1.0 g / in 3 Up to 0.1g / in 3 Between, preferably from 0.7g / in 3 Up to 0.25g / in 3 , and most preferably from 0.6 g / in 3 Up to 0.5g / in 3 .

[0137] The catalytic composition comprises alumina, preferably γ-alumina. The alumina may also contain lanthanum, praseodymium or a combination of the two. The alumina is preferably lanthanum-stabilized alumina. Alumina is an advantageous support material because it exhibits a high surface area and is a refractory metal oxide. This results in a good heat capacity required for the high temperature conditions encountered. The catalytic composition also comprises one or more platinum group metals (PGM). The PGM is selected from the group consisting of Pt, Pd, Rh, Re, Ir. The PGM is used to catalyze the reactions required for the treatment of exhaust gases and the combustion of soot particles. Preferably, the PGM is Pt, Pd and Rh; Pd and Rh; or only Pd; or only Rh.

[0138] A method for preparing a catalytic wall flow monolith is disclosed in WO 2017 / 109514, the contents of which are fully incorporated by reference. More particularly, the method disclosed in Example 3 of WO 2017 / 109514 can be used.

[0139] The mixed oxides of the present invention can also be used to prepare catalytic monoliths for exhaust gas treatment systems. The monoliths are usually in the form of honeycomb monoliths.

[0140] Examples

[0141] The following examples are given to illustrate the invention. The elemental proportions of the mixed oxides are given by weight of the oxides.

[0142] Particle size distribution

[0143] The particle size distribution was determined using a laser particle size analyzer (model LS13320 from Beckman-Coulter). The Fraunhofer mode was used following the manufacturer's guidelines. The particle size distribution (by volume) was obtained from a dispersion of particles in water in the presence of a dispersant (sodium hexametaphosphate). A relative refractive index of 1.6 was used. From the distribution by volume, the values ​​of d10, d50, d90 and d99 were obtained. In the table below, they are given in μm.

[0144] Specific surface area (BET)

[0145] The specific surface area was determined automatically by N2 adsorption on a Quantachrome NOVA 4000e. Prior to any measurement, the samples were degassed to desorb volatile substances and clean the surface.

[0146] Porosity

[0147] The porosity was obtained using an autopore V 9620 automated mercury intrusion porosimeter following the manufacturer's instructions. Calcination of the mixed oxides at 1100 °C for 4 h in air gave TPV and PV 0-300 nm The procedure outlined in ASTM International Test Method D 4284-07 was followed; the sample weight was approximately 0.5 grams, the mercury contact angle was 130°, and the mercury surface tension was 485 dyn / cm.

[0148] Viscosity: Measurement of the viscosity V of the dispersion of the mixed oxide according to the invention in water

[0149] (1) A homogeneous dispersion of the mixed oxide according to the invention was prepared by mixing the particles of the mixed oxide in water in a 1 L beaker with the aid of a rotor (diameter 8.7 cm) rotating at 360 rpm and positioned 2 cm above the bottom of the beaker:

[0150] (1a) Add 500 mL of water to a beaker;

[0151] (1b) then adding the mixed oxide (377.2 g) in powder form over about 15 min;

[0152] (1c) adjusting the pH to 4.0±0.1 with acetic acid;

[0153] (2) Then use a rheometer to record the viscosity over time. When the viscosity is constant, measure it.

[0154] Step (1b) can be performed by adding the mixed oxide by a vibrating feeder.Step (1c) can be performed by adding acetic acid with a peristaltic pump and by controlling the pH of the dispersion until the target pH is reached.

[0155] The rheometer used was a Brookfield DV2T.

[0156] Example 1: Preparation of mixed oxide Zr-Ce-La 60%-35%-5%

[0157] First, a co-chloride solution (CZR solution) was prepared with 47 L of H2O and 16 L of CeCl3 aqueous solution (1.53 mol / L and density 1.33), to which 20.2 kg of ZrOCl2 aqueous solution (36.2 wt% ZrO2; LOI 63.6%) was added. Then, H2SO4 aqueous solution (8.77 wt% and density 1.05) was added.

[0158] The CZR solution was transferred to a precipitation tank pre-filled with 110 L of NaOH aqueous solution (10.8% wt and density 1.099) within 50 min. During precipitation, the stirring speed was fixed at 220 rpm. The slurry was washed by filtration / re-slurrying to remove all SO4 2- 、Na + and Cl - ions (less than 200 ppm each). After reslurrying in water at 80 g / L, the slurry was aged at 125° C. for 1 hour. After aging, La(NO3)3 was introduced in order to obtain the desired amount of lanthanum oxide (5%wt of La2O3). 4 kg of lauric acid were then added to the dispersion under stirring over 1 hour. The suspension was then filtered and the solid was calcined at 850° C. for 3 hours. The resulting oxide material was jet milled under the following conditions.

[0159] The characteristics of the ground mixed oxide are: d50 is 1.9 μm, and d90 is 6.0 μm. The specific surface area of ​​the product after calcination at 1100°C for 4 hours in air is: S 1100 ℃ / 4h =28m 2 / g. Viscosity is measured at 20.0 cP.

[0160]

[0161] Examples 2 to 6: Preparation of mixed oxides with other compositions

[0162] The same method as described for Example 1 was used to prepare mixed oxides with various other compositions:

[0163] ● Example 2: Zr-Ce-La-Y 50%-40%-5%-5%

[0164] ● Example 3: Zr-Ce-La-Y 55%-35%-7.5%-2.5%

[0165] ● Example 4: Zr-Ce-La-Y 60%-24%-3.5%-12.5%

[0166] ● Example 5: Zr-Ce-La-Y 60%-30%-5%-5%

[0167] ●Example 6: Zr-Ce-La 75%-20%-5%

[0168] For mixed oxides containing Y, the CZR solution contains the required amounts of CeCl3, ZrOCl2 and Y(NO3)3. H2SO4 is also added to make SO4 2- / (Zr+Ce) molar ratio is between 0.5 and 0.8.

[0169] The mixed oxide obtained after calcination at 850° C. was jet milled under the same conditions as in Example 1. The particle size characteristics obtained were: d50 between 1.0 μm and 2.5 μm, and d90 between 2.0 μm and 9.0 μm (see Table I).

[0170] Table I: Examples 1-6

[0171]

[0172]

[0173] Comparative Example 1: Preparation of mixed oxide Zr-Ce-La 60%-35%-5% by "soft" jet milling

[0174] This comparative example relates to the preparation of a mixed oxide having the same composition as the mixed oxide of Example 1. The preparation conditions of the mixed oxide are the same as those of Example 1, except for the grinding conditions. The grinding is carried out by a jet milling process under softer and more conventional conditions as described in the table below:

[0175]

[0176] After grinding, the mixed oxide exhibits a d50 between 3.5 μm and 4.5 μm and a d90 below 15 μm. The specific surface area of ​​the product after calcination at 1100° C. for 4 hours in air is: S 1100 ℃ / 4h =29m 2 The measured viscosity is over 1000 cP, which is much higher than the viscosity of the product in Example 1.

[0177] Comparative Example 2: Mixed oxide Zr-Ce-La 60%-35%-5%, which is prepared by WO 2012 / 072439 and ground with a hammer mill

[0178] This comparative example relates to the preparation of a mixed oxide having the same composition as the mixed oxide of Example 1. The mixed oxide is prepared according to the method involving nitrates disclosed in WO 2012 / 072439. Two nitrate solutions are prepared in advance, one consisting of cerium nitrate and zirconium nitrate, and the other consisting of lanthanum nitrate. 324 mL of water are introduced into a first beaker, which has 102 mL of an aqueous zirconium nitrate ZrO(NO3)2 solution ([ZrO2] = 265 g / L, and d = 1.408) and 68 mL of cerium nitrate Ce. IV Aqueous solution ([CeO2] = 270 g / L, and d = 1.43). 5.5 mL of an aqueous lanthanum nitrate solution ([La2O3] = 454 g / L, and d = 1.687) were introduced into a second beaker.

[0179] In a reactor equipped with a pitched-blade stirring rotor, aqueous ammonia solution (12 mol / L) and then distilled water were introduced under stirring to obtain a total volume of 0.5 liters and a 40% stoichiometric excess of aqueous ammonia relative to the cation to be precipitated.

[0180] The first nitrate solution is introduced into the reactor stirred at 500 rpm over the course of 45 minutes, the second nitrate solution is introduced over the course of 15 minutes and stirring is fixed at 250 rpm. The resulting precipitate suspension is placed in a stainless steel autoclave equipped with a stirring rotor. The temperature of the medium is brought to 150° C. for 2 hours under stirring. 33 g of lauric acid are added to the resulting suspension. The suspension is kept stirred for 1 hour.

[0181] The suspension was filtered through a Buchner funnel and then washed with an aqueous ammonia solution. The resulting product was then calcined in air at 850° C. for 4 hours. The resulting product was ground with a hammer mill. The characteristics of the ground mixed oxide were: d50=2.0 μm, and d90=6.0 μm. The specific surface area of ​​the ground product was: S 1100℃ / 4h =22m 2 / g, lower than the product of Example 1 (28m 2 / g).

[0182] Comparative Example 3: Grinding with "soft" jet + Preparation of mixed oxide Zr-Ce-La60%-35%-5% by wet grinding

[0183] This example relates to the preparation of a mixed oxide having the same composition as in Example 1, i.e., the composition is based on cerium, zirconium, and lanthanum in corresponding proportions of 35%, 60%, and 5% by weight of the oxides. First, a co-chloride solution is prepared with deionized water (47 L), an aqueous solution of cerium chloride CeCl3 (16 L, [C]=1.53 mol / l, and density 1.33), and an aqueous solution of lanthanum chloride LaCl3 to obtain an aqueous solution of 5%wt La2O3 and ZrOCl2 (20.2 kg, 36.2 wt% ZrO2, LOI 63.6%). Then an aqueous solution of H2SO4 (65 L, 8.77 wt% and density 1.05) is introduced. Within 50 min, the solution is transferred to a precipitation tank previously filled with 110 L of an aqueous solution of NaOH (10.8%wt and density 1.099). During precipitation, the stirring speed is fixed at 220 rpm. The slurry is washed by filtration / re-slurrying to remove all SO4 2- 、Na + and Cl - ions (less than 200 ppm for each ion). After reslurrying in water at 80 g / L, the slurry was aged at 97°C for 1 hour.

[0184] 4 kg of lauric acid were then added to the dispersion under stirring over 1 hour. The suspension was then filtered and the solid was calcined at 850°C for 3 hours. The material was jet milled under soft conventional conditions as in Comparative Example 1. 400 g of the resulting powder was then dispersed in 1 L of distilled water and the pH was adjusted to 4 by acetic acid. The obtained suspension was further milled by a wet milling apparatus to obtain a d50 between 0.8 μm and 1.0 μm and a d90 below 5 μm. The solid was further separated and calcined for characterization. The specific surface area of ​​the resulting material after calcination at 1100°C for 4 hours was very low: S 1100℃ / 4h =18m 2 / g.

[0185] Table II: Comparative Examples 1-3

[0186]

[0187]

[0188] These comparative examples show that the mixed oxides of the present invention exhibit 1100℃ / 4h ,TPV,PV 0-300nm A compromise between V and low viscosity.

[0189] Comparative Example 4: Preparation of mixed oxide Zr-Ce-La-Y 55%-35%-7.5%-2.5% by soft grinding

[0190] A mixed oxide having the same composition as in Example 3 (Zr-Ce-La-Y 55%-35%-7.5%-2.5%) was prepared under the same conditions except for the grinding conditions. As in Comparative Example 1, the grinding was carried out by a jet milling process under softer and more conventional conditions.

[0191] As can be observed, on the one hand, the particle size is lower in Example 3 than in Comparative Example 4 due to grinding under more severe conditions; on the other hand, the TPV is larger. The pore volume (PV) for pores below 300 nm is 0-300nm ), the same trend was observed.

[0192] Comparative Examples 5 and 6: Mixed oxide Zr-Ce- Preparation of La-Y 55%-35%-7.5%-2.5% - Effect of Grinding Conditions

[0193] As described in Comparative Example 2 (except for the grinding conditions), two mixed oxides with the same composition as in Example 3 (Zr-Ce-La-Y 55%-35%-7.5%-2.5%) were prepared by the method of WO 2012 / 072439 involving nitrates. The grinding was carried out by a jet milling process:

[0194] - Comparative Example 5: Stronger conditions as in Example 1;

[0195] - Comparative Example 6: Soft and usual conditions as in Comparative Example 1.

[0196] As can be observed, in the case of mixed oxides based on the process of WO 2012 / 072439, when the particle size is lower due to grinding under more intensive conditions, the TPV is also lower. For pores below 300 nm, the pore volume (PV 0-300nm ), the same trend was observed.

[0197] Table III: Comparative Examples 4-5

[0198]

[0199] The preparation method of the mixed oxide also has an impact. The mixed oxide of Example 3 was prepared with a co-chloride solution, while the mixed oxide of Comparative Example 5 was prepared with a nitrate solution. Although the grinding was the same, the specific surface area, TPV and PV of Comparative Example 5 were 0-300nm Lower.

Claims

1. A mixed oxide comprising zirconium, cerium, lanthanum and optionally at least one rare earth element RE other than cerium and lanthanum, the mixed oxide having the following composition: ▪ Between 8.0% and 45.0% by weight of cerium; ▪ Between 1.0% and 15.0% by weight of lanthanum; ▪ Up to 15.0% by weight of such rare earth elements other than cerium and other than lanthanum; ▪ the total proportion of lanthanum and the one or more rare earth elements other than cerium and lanthanum is less than or equal to 25.0%; ▪The remainder is zirconium; The proportions of these elements Ce, Zr, La, RE are given by weight of the oxide relative to the total mixed oxide. The mixed oxide exhibits the following properties after calcination at 1100°C for 4 hours in air: ▪Specific surface area S 1100°C / 4 h Between 25 and 50 m 2 / g between; ▪Pore volume PV determined by mercury porosimetry for pores with a diameter below 300 nm 0-300 nm At 0.50 cm 3 / g and 0.90 cm 3 / g between; The mixed oxide is in the form of particles having the following properties: d50 between 1.5 µm and 2.5 µm; d90 between 2.0 µm and 9.0 µm; The abovementioned elements are usually present in the mixed oxide as oxides.

2. A mixed oxide consisting of a combination of oxides of: zirconium; cerium; lanthanum; optionally at least one rare earth element RE other than cerium and lanthanum; and optionally hafnium, the mixed oxide having the following composition: ▪ Between 8.0% and 45.0% by weight of cerium; ▪ Between 1.0% and 15.0% by weight of lanthanum; ▪ Up to 15.0% by weight of such rare earth elements other than cerium and other than lanthanum; ▪ the total proportion of lanthanum and the one or more rare earth elements other than cerium and lanthanum is less than or equal to 25.0%; ▪The proportion of hafnium is less than or equal to 2.5%; ▪The remainder is zirconium; The proportions of these elements Ce, Zr, Hf, La, RE are given by weight of the oxide relative to the total mixed oxide. The mixed oxide exhibits the following properties after calcination at 1100°C for 4 hours in air: ▪Specific surface area S 1100°C / 4 h Between 25 and 50 m 2 / g between; ▪Pore volume determined by mercury porosimetry for pores with diameters below 300 nm at 0.50 cm 3 / g and 0.90 cm 3 / g between; The mixed oxide is in the form of particles having the following properties: d50 between 1.5 µm and 2.5 µm; ●d90 is between 2.0 µm and 9.0 µm.

3. The mixed oxide according to claim 1 or 2, characterized in that the following ratios: ▪ Between 18.0% and 37.0% by weight of cerium; ▪Between 3.0% and 9.0% by weight of lanthanum; ▪The remainder is zirconium; or ▪ Between 30.0% and 45.0% by weight of cerium; ▪Between 3.0% and 9.0% by weight of lanthanum; ▪ between 3.0% and 9.0% by weight of at least one rare earth element RE other than cerium and other than lanthanum; ▪The remainder is zirconium; or ▪ Between 20.0% and 35.0% by weight of cerium; ▪Between 3.0% and 9.0% by weight of lanthanum; ▪ between 3.0% and 15.0% by weight of at least one rare earth element RE other than cerium and other than lanthanum; ▪The remainder is zirconium.

4. The mixed oxide according to claim 1 or 2, wherein: The total proportion of lanthanum and the one or more rare earth elements other than cerium and lanthanum is lower than or equal to 20.0%.

5. The mixed oxide according to claim 1 or 2, wherein: The total proportion of lanthanum and the one or more rare earth elements other than cerium and lanthanum is lower than or equal to 18.0%.

6. The mixed oxide according to claim 1 or 2, further comprising hafnium, the proportion of hafnium in the mixed oxide being lower than or equal to 2.0%, this proportion being given by weight of the oxide relative to the mixed oxide as a whole.

7. The mixed oxide according to claim 1 or 2, wherein: The proportion of cerium is between 18.0% and 44.0%.

8. The mixed oxide according to claim 1 or 2, wherein The proportion of cerium is between 18.0% and 42.0%.

9. The mixed oxide according to claim 1 or 2, wherein: The proportion of cerium is between 18.0% and 22.0%.

10. The mixed oxide according to claim 1 or 2, wherein: The proportion of cerium is between 22.0% and 26.0%.

11. The mixed oxide according to claim 1 or 2, wherein: The proportion of cerium is between 28.0% and 32.0%.

12. The mixed oxide according to claim 1 or 2, wherein: The proportion of cerium is between 33.0% and 37.0%.

13. The mixed oxide according to claim 1 or 2, wherein: The proportion of cerium is between 38.0% and 42.0%.

14. The mixed oxide according to claim 1 or 2, wherein: The proportion of lanthanum is between 1.0% and 13.0%.

15. The mixed oxide according to claim 1 or 2, wherein: The proportion of lanthanum is between 1.0% and 8.0%.

16. The mixed oxide according to claim 1 or 2, wherein: The proportion of lanthanum is between 2.0% and 8.0%.

17. The mixed oxide according to claim 1 or 2, wherein: The proportion of lanthanum is between 3.0% and 7.0%.

18. The mixed oxide according to claim 1 or 2, wherein: The proportion of the rare earth element(s) is comprised between 1.0% and 13.0%.

19. The mixed oxide according to claim 1 or 2, wherein: The proportion of the rare earth element(s) is comprised between 1.0% and 8.0%.

20. The mixed oxide according to claim 1 or 2, wherein: The proportion of the rare earth element(s) is comprised between 2.0% and 8.0%.

21. The mixed oxide according to claim 1 or 2, wherein: The proportion of the rare earth element(s) is comprised between 3.0% and 7.0%.

22. The mixed oxide according to claim 1 or 2, wherein: The proportion of the rare earth element(s) is comprised between 10.0% and 13.0%.

23. The mixed oxide according to claim 1 or 2, wherein: The proportion of zirconium is higher than 45%.

24. The mixed oxide according to claim 1 or 2, wherein: The proportion of zirconium is higher than 48%.

25. The mixed oxide according to claim 1 or 2, wherein: The proportion of zirconium is greater than or equal to 50%.

26. The mixed oxide according to claim 1 or 2, characterized in that Weight ratio ZrO2 / CeO2 > 1.

0.

27. The mixed oxide according to claim 1 or 2, characterized in that Weight ratio ZrO2 / CeO2 ≥ 1.

25.

28. The mixed oxide according to claim 1 or 2, wherein: d50 is strictly less than 2.5 µm.

29. The mixed oxide according to claim 1 or 2, wherein: These particles exhibit a d10 lower than or equal to 1.0 μm.

30. The mixed oxide according to claim 1 or 2, wherein: These particles exhibit a d10 lower than or equal to 0.8 μm.

31. The mixed oxide according to claim 1 or 2, wherein: These particles exhibit a d10 lower than or equal to 0.7 μm.

32. The mixed oxide according to claim 1 or 2, wherein: These particles exhibit a d10 greater than or equal to 0.2 μm.

33. The mixed oxide according to claim 1 or 2, wherein: These particles exhibit a d10 greater than or equal to 0.3 μm.

34. The mixed oxide according to claim 1 or 2, wherein: These particles exhibit a d99 less than or equal to 20.0 μm.

35. The mixed oxide according to claim 1 or 2, wherein: These particles exhibit a d99 less than or equal to 15.0 μm.

36. The mixed oxide according to claim 1 or 2, wherein: These particles exhibit a d99 greater than or equal to 5.0 μm.

37. The mixed oxide according to claim 1 or 2, wherein: These particles exhibit a d99 greater than or equal to 7.0 μm.

38. The mixed oxide according to claim 1 or 2, which exhibits a temperature between 50 and 70 m / s after calcination at 1000 ° C for 4 hours in air. 2 / g specific surface area.

39. The mixed oxide according to claim 1 or 2, which exhibits a temperature between 55 and 70 m / s after calcination at 1000 ° C for 4 hours in air. 2 / g specific surface area.

40. The mixed oxide according to claim 1 or 2, which exhibits a peak at 1.40 cm after calcination at 1100° C. for 4 hours in air. 3 / g and 3.00 cm 3 The total pore volume determined by mercury porosimetry is between 1.17 and 1.13 Å / g.

41. The mixed oxide according to claim 1 or 2, which exhibits a peak at 1.50 cm after calcination at 1100° C. for 4 hours in air. 3 / g and 3.00 cm 3 The total pore volume determined by mercury porosimetry is between 1.17 and 1.13 Å / g.

42. The mixed oxide according to claim 1 or 2, which exhibits a peak at 1.50 cm after calcination at 1100° C. for 4 hours in air. 3 / g and 2.50 cm 3 The total pore volume determined by mercury porosimetry is between 1.17 and 1.13 Å / g.

43. The mixed oxide according to claim 1 or 2, which exhibits a peak at 1.50 cm after calcination at 1100° C. for 4 hours in air. 3 / g and 2.20 cm 3 The total pore volume determined by mercury porosimetry is between 1.17 and 1.13 Å / g.

44. The mixed oxide according to claim 1 or 2, wherein: The viscosity of a dispersion containing 43.0 wt% of the particles of the mixed oxide in water and exhibiting a pH of 4.0 ± 0.1 is lower than or equal to 20.0 cP, the viscosity being 20°C ± 1°C and for the conditions between 5.0 and 10.0 s -1 The shear rate applied is measured between 45. The mixed oxide according to claim 1 or 2, wherein: After calcination at 1100 °C for 4 h in air, the mixed oxide exhibits 2 The specific surface area S 1100°C / 4 h .

46. ​​The mixed oxide according to claim 1 or 2, wherein: After calcination at 1100 °C for 4 h in air, the mixed oxide exhibits 2 The specific surface area S 1100°C / 4 h .

47. The mixed oxide according to claim 1 or 2, wherein: After calcination at 1100 °C for 4 h in air, the mixed oxide exhibits 3 / g and 0.80 cm 3 The pore volume PV determined by mercury porosimetry for pores with a diameter below 300 nm is between 1.5 and 2.5 μm. 0-300 nm .

48. The mixed oxide according to claim 1 or 2, wherein: After calcination at 1100 °C for 4 h in air, the mixed oxide exhibits 3 / g and 0.70 cm 3 The pore volume PV determined by mercury porosimetry for pores with a diameter below 300 nm is between 1.5 and 2.5 μm. 0-300 nm .

49. The mixed oxide according to claim 40, wherein After calcination at 1100 °C for 4 h in air, the mixed oxide exhibits a 3 / g of total pore volume determined by mercury porosimetry.

50. The mixed oxide according to claim 1 or 2, wherein: RE is Y or Nd or a combination of Y and Nd.

51. The mixed oxide according to claim 1 or 2, wherein: d50 is between 1.5 µm and 2.2 µm.

52. The mixed oxide according to claim 1 or 2, wherein: d50 is between 1.5 µm and 2.0 µm.

53. The mixed oxide according to claim 1 or 2, wherein: d90 is between 2.0 µm and 8.0 µm.

54. The mixed oxide according to claim 1 or 2, wherein: d90 is between 2.0 µm and 7.0 µm.

55. The mixed oxide according to claim 1 or 2, wherein: d90 is between 3.0 µm and 8.0 µm.

56. The mixed oxide according to claim 1 or 2, wherein: d90 is between 3.0 µm and 7.0 µm.

57. The mixed oxide according to claim 1 or 2, wherein: The mixed oxide contains impurities and the total proportion of these impurities is generally below 0.2% by weight, relative to the mixed oxide.

58. A catalytic composition comprising: Alumina, especially lanthanum-stabilized alumina; one or more platinum group metals; and A mixed oxide according to any one of claims 1 to 57.

59. A catalytic wall flow monolith comprising a porous support and the catalytic composition according to claim 58 on the surface of the support.

60. Use of the mixed oxide according to any one of claims 1 to 57 for the preparation of a catalytic converter or a catalytic wall-flow monolith.

61. A method for preparing a mixed oxide according to any one of claims 1 to 57, comprising the following steps: (a1) Contains sulfate anion SO4 2- , a zirconium chloride salt, a cerium salt, and optionally an aqueous solution of a salt of at least one rare earth element other than cerium and lanthanum, reacting with an alkaline aqueous solution to form a precipitate; (b1) separating the precipitate obtained at the end of step (a1) from the liquid medium; (c1) heating the precipitate obtained at the end of step (b1) in an aqueous medium and optionally in the presence of a lanthanum salt and a basic compound; (d1) a lanthanum salt may optionally be added, optionally together with a basic compound, to the mixture obtained at the end of step (c1); (e1) adding an organic texturizing agent to the mixture obtained at the end of step (d1); (f1) separating the solid material obtained at the end of step (e1) from the liquid medium and calcining it in air; (g1) Jet milling the solid material obtained at the end of step (f1).

62. The method of claim 61, wherein: The zirconium chloride salt is ZrOCl2.

63. The method of claim 61 or 62, wherein: The molar ratio of the aqueous solution in step (a1) is SO4 2- / (Zr+ Ce) is in the range of 0.5-1.

0.