Composite film for direct-type backlight module without diffusion plate and manufacturing method thereof
By adopting a composite film structure without diffusion plate in the direct backlight module, the arrangement of the microprism layer, honeycomb hemispherical lens and cylindrical prism is solved, and the problem of light loss and complex structure is achieved, and higher light concentration is achieved and brightness while improving stability and visual effects.
Patent Information
- Application Number
- CN202111505288.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-12-10
AI Technical Summary
The existing direct-down luminous backlight modules have severe light loss and complex structure due to the use of diffusion plates, which affects stability.
A composite film structure with no diffusion plate is adopted, including the upper layer, the intermediate layer and the bottom layer. Each layer is connected by an adhesive, and a microprism layer is provided to achieve light concentration and brightness improvement, and the periodic arrangement between the honeycomb hemispherical lens and the cylindrical prism is reduced. Interference phenomenon, simplify structure.
It achieves higher light concentration effect and brightness improvement, while improving the scratch resistance and peeling force of the product, simplifying the structure, reducing the influence of molar patterns, and improving the visual effect.
Smart Images

Figure CN114153094B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical films, and in particular to a composite film for a direct-type backlight module without a diffusion plate and a manufacturing method thereof. Background Art
[0002] The backlight module is a widely used technology in liquid crystal display technology. The backlight module can be classified into two types according to the light-emitting mode: side-light-emitting architecture and direct-light-emitting architecture. Among them, the existing direct-light-emitting architecture needs to use a diffusion plate to shield and diffuse the point light source to achieve the conversion from the point light source to the surface light source. Since the diffusion plate has its own shielding effect, the existing direct-light-emitting architecture has serious light loss. At the same time, the use of a diffusion plate will also make the structure of the backlight module using the direct-light-emitting architecture complicated, making its thermal stability poor. Therefore, the existing direct-light-emitting architecture urgently needs to be improved. Summary of the invention
[0003] The present invention aims at the defects of the prior art such as serious light loss in the composite film with a diffusion plate, and the composite film structure becoming complicated due to the diffusion plate, which affects the stability, and provides a new composite film for a direct-type backlight module without a diffusion plate and a manufacturing method thereof.
[0004] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:
[0005] A composite film for a direct-down backlight module without a diffusion plate comprises an upper layer, an intermediate layer, a bottom layer, a first adhesive layer, a second adhesive layer, and a back coating layer, wherein the upper layer is connected to the intermediate layer via the first adhesive layer, the intermediate layer is connected to the bottom layer via the second adhesive layer, the back coating layer is arranged on the lower surface of the bottom layer, the upper layer, the intermediate layer and the bottom layer are all independent film structures, a third microprism layer is arranged on the upper layer, a first microprism layer is arranged on the intermediate layer, and a second microprism layer is arranged on the bottom layer, the first microprism layer is composed of triangular microprisms arranged in a high-low interval, the second microprism layer is composed of a first honeycomb hemispherical lens and a columnar prism arranged in a periodic arrangement of one high and N low, wherein the columnar prism is greater than the first honeycomb hemispherical lens in height, and N is greater than or equal to 1, and the third microprism layer is composed of a second honeycomb hemispherical lens.
[0006] The upper layer, the middle layer and the bottom layer of the present invention all adopt independent film structures, and respectively play a supporting role for the microprism layer on each film layer; wherein the third microprism layer in the upper layer plays a role of focusing light and can improve its own brightness. The third microprism layer adopts the second honeycomb hemispherical lens to replace the conventional diffusion particles to achieve the effect of focusing light and improving brightness, and also improves the hardness of the upper layer surface, so that the scratch resistance of the present invention is significantly improved; the first microprism layer in the middle layer reflects the light that passes through the bottom layer and irradiates the middle layer, thereby playing a role of changing the direction of the light, focusing light and improving brightness, and at the same time, the spike ends of the more prominent triangular microprisms arranged in a high-low interval manner can penetrate into the adhesive arranged between the upper layer and the middle layer, so as to have a higher peeling force and ensure the stable connection between the upper layer and the middle layer; the second microprism layer in the bottom layer adopts a structure of a first honeycomb hemispherical lens and a cylindrical prism arranged in a circular manner, which can reduce the interference and moiré phenomenon generated by the prism while focusing light to increase brightness, thereby optimizing the visual effect of the reflected light generated by the reflection of the present invention.
[0007] Therefore, the present invention can better replace the function of the diffusion plate in the traditional backlight module, and has a better light focusing effect while increasing the brightness, and simplifies the structure.
[0008] Preferably, in the composite film for a direct-type backlight module without a diffusion plate described above, the height of the triangular microprisms in the first microprism layer ranges from 26μm to 40μm, and the spacing between adjacent triangular microprisms is 50μm to 75μm, and the refractive index of the first microprism layer ranges from 1.53 to 1.56.
[0009] The first microprism layer adopts a triangular microprism arrangement structure with high and low intervals, which increases the number of connections between the triangular microprisms with larger height values and the adhesives set between the upper and middle layers to a greater extent, enhances the peeling force and improves the connection stability. At the same time, the triangular microprisms with smaller height values are arranged at intervals, ensuring that the efficiency of focusing and emission per unit area is not affected, thereby improving the brightness of the product.
[0010] Preferably, in the composite film for a direct-type backlight module without a diffusion plate described above, the second microprism layer is composed of a first honeycomb hemispherical lens and a cylindrical prism arranged in a cycle of 1 high and 4 low, the diameter of the first honeycomb hemispherical lens ranges from 45μm to 55μm, the height of the first honeycomb hemispherical lens ranges from 25μm to 30μm, the height of the cylindrical prism ranges from 60μm to 80μm, and the spacing between adjacent cylindrical prisms ranges from 180μm to 200μm.
[0011] The first micro-prism layer is provided with a first honeycomb hemispherical lens and a cylindrical prism, and the heights of the two are different, so that light interference can be reduced, the influence of moiré is eliminated, and the bad appearance defect caused by moiré is overcome.
[0012] Preferably, in the above-mentioned composite film for a direct-type backlight module without a diffusion plate, the diameter of the second honeycomb hemispherical lens in the third microprism layer ranges from 26μm to 50μm, the height of the second honeycomb hemispherical lens ranges from 11μm to 23μm, and the refractive index of the third microprism layer ranges from 1.45 to 1.50.
[0013] The second honeycomb hemispherical lens can not only focus light, but also improve the anti-scratch performance of the upper surface.
[0014] Preferably, the above-mentioned method for manufacturing a composite film for a direct-lit backlight module without a diffusion plate comprises the following steps:
[0015] S1. Take a roll of PET film as an intermediate base film, apply a layer of polyurethane acrylic resin on the upper surface of the intermediate base film, and complete the initial curing process by UV lamp irradiation to form a first polyurethane acrylic resin layer on the upper surface of the intermediate base film, and use a first prism roller mold to transfer the first polyurethane acrylic resin layer to form a first micro-prism layer, the first micro-prism layer and the intermediate base film together constitute an intermediate layer;
[0016] S2. Take a roll of PET film as the upper base film, apply adhesive A to one side of the upper base film to form a first adhesive layer, laminate the upper base film with the first adhesive layer and the intermediate layer, and bond the first adhesive layer to the first microprism layer to form a first semi-finished product, and irradiate the first semi-finished product with a UV lamp to complete the full curing process;
[0017] S3. Take a roll of PET film as the bottom base film, apply a layer of polyurethane acrylic resin on the upper surface of the bottom base film, and complete the initial curing process by UV light irradiation to form a second polyurethane acrylic resin layer on the upper surface of the bottom base film, and use a second prism roller mold to transfer the second polyurethane acrylic resin layer to form a second microprism layer, and the second microprism layer and the bottom base film together constitute the bottom layer;
[0018] S4. Adhesive B is applied to the lower surface of the intermediate base film in the first semi-finished product to form a second adhesive layer, the intermediate base film with the second adhesive layer is laminated with the second micro-prism layer of the bottom layer, the first semi-finished product is bonded to the bottom layer to form a second semi-finished product, and a UV lamp is used to irradiate the second semi-finished product to complete the full curing process;
[0019] S5. Take the second semi-finished product, apply a layer of polyurethane acrylic resin on the upper surface of the upper base film, and perform a primary curing process by UV lamp irradiation to form a third polyurethane acrylic resin layer on the upper surface of the upper base film, use a third prism roller mold to transfer the third polyurethane acrylic resin layer to form a third micro-prism layer, and use a UV lamp again to perform a full curing process on the third micro-prism layer after the transfer. The product obtained through the above steps is the third semi-finished product;
[0020] S6. Take the third semi-finished product, and coat the lower surface of the bottom base film in the third semi-finished product with a mixture of TiO 2 The coating liquid of the particles and PMMA diffusion particles is dried in an oven and / or UV-cured to form a back coating layer with a thickness ranging from 10 μm to 20 μm on the lower surface of the bottom base film, completing the entire preparation process.
[0021] The initial curing process in the above steps S1, S3, and S5 is beneficial to weakening the fluidity of the surface of the polyurethane acrylic resin layer coated in each step, and is beneficial to reducing the adhesion of the surface of the polyurethane acrylic resin layer to the first prism roller mold, making it easier to demold. The polyurethane acrylic resin layer has stronger plasticity after initial curing and can more perfectly transfer the texture on the prism roller mold in each step.
[0022] After the adhesive layers in the respective steps are bonded to the corresponding microprism layers in the above steps S2 and S4, a full curing process is performed. On the one hand, the corresponding microprism layer can be completely cured and the corresponding adhesive layer can be cured at the same time, so that the obtained product structure is more stable; on the other hand, it is beneficial to release the stress between the upper and lower layers during bonding, play an anti-warping role, and greatly reduce the defective rate of the product.
[0023] Preferably, in the above-mentioned method for manufacturing a composite film for a direct-type backlight module without a diffusion plate, the viscosity of the first polyurethane acrylic resin layer in step S1 is between 50cps and 800cps, and the thickness is greater than or equal to 31μm, and the UV lamp irradiation energy range in the initial curing process is controlled within 50MJ / cm 2 ~80MJ / cm 2 The UV lamp irradiation energy range in the full curing process in step S2 is controlled within 300MJ / cm 2 ~450MJ / cm 2 between.
[0024] The viscosity range and thickness range of the first polyurethane acrylic resin layer in step S1 are affected by the height of the first prism layer after final curing. The energy range of the UV lamp for initial curing of the first polyurethane acrylic resin layer is controlled within 50 MJ / cm 2 ~80MJ / cm2 The above-mentioned viscosity range and thickness range of the first polyurethane acrylic resin layer can be well applied, so that the surface of the first polyurethane acrylic resin layer after the initial curing process can achieve a more suitable transfer effect. The UV lamp irradiation energy range in the full curing process in step S2 is controlled at 300MJ / cm 2 ~450MJ / cm 2 The first semi-finished product can be cured faster.
[0025] Preferably, in the above-mentioned method for manufacturing a composite film for a direct-type backlight module without a diffusion plate, the thickness of the second polyurethane acrylic resin layer in step S3 is greater than or equal to 65 μm, and the UV lamp irradiation energy range in the initial curing process is controlled within 20 MJ / cm 2 ~50MJ / cm 2 The UV lamp irradiation energy range in the full curing process in step S4 is controlled within 200MJ / cm 2 ~1000MJ / cm 2 between.
[0026] The thickness range of the second polyurethane acrylic resin layer in step S3 is affected by the height of the second prism layer after final curing. The energy range of the UV lamp for initial curing of the second polyurethane acrylic resin layer is controlled within 20 MJ / cm 2 ~50MJ / cm 2 The thickness range of the second polyurethane acrylic resin layer can be well applied to the above-mentioned second polyurethane acrylic resin layer, so that the surface of the second polyurethane acrylic resin layer after the initial curing process can achieve a more suitable transfer effect. The UV lamp irradiation energy range in the full curing process in step S4 is controlled to be 200MJ / cm 2 ~1000MJ / cm 2 The first semi-finished product can be cured faster.
[0027] Preferably, in the above-mentioned method for manufacturing a composite film for a direct-type backlight module without a diffusion plate, the viscosity of the third polyurethane acrylic resin layer in step S5 is between 20cps and 150cps, and the thickness is greater than or equal to 15μm, and the UV lamp irradiation energy range in the initial curing process is controlled within 10MJ / cm 2 ~30MJ / cm 2 The UV lamp irradiation energy range in the full curing process is controlled within 100MJ / cm 2 ~300MJ / cm 2 between.
[0028] Preferably, in the above-mentioned method for manufacturing a composite film for a direct-type backlight module without a diffusion plate, the linear speed of the first prism roller mold in the transfer process of step S1 is controlled between 3m / min and 30m / min, the linear speed of the third prism roller mold in the transfer process of step S5 is controlled between 7m / min and 35m / min, and the thickness of the first adhesive layer and the second adhesive layer in step S2 and step S4 is between 1μm and 5μm.
[0029] The linear speed of the first prism roller mold is related to the thickness of the first polyurethane acrylic resin layer and the height of the first microprism finally formed. The linear speed of the third prism roller mold is related to the thickness of the third polyurethane acrylic resin layer and the height of the third microprism finally formed. Controlling the linear speeds of the first prism roller mold and the third prism roller mold within the above-mentioned ranges is beneficial to improving the product integrity of the prism structure finally formed after transfer and reducing the defective rate.
[0030] Preferably, in the above-mentioned method for manufacturing a composite film for a direct-lit backlight module without a diffusion plate, the coating liquid in step S6 comprises the following components in weight ratio:
[0031]
[0032] The TiO in the coating solution 2 The particle size of the particles is between 1 μm and 3 μm, the particle size of the PMMA diffusion particles is between 5 μm and 10 μm, the solvent is prepared by mixing a benzene solution with butanone or isopropanol in a ratio of 1:1, and the benzene solution is toluene or xylene. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of the structure of the present invention. DETAILED DESCRIPTION
[0034] The following is combined with Figure 1 The present invention is further described in detail with specific embodiments, but they are not intended to limit the present invention:
[0035] Example 1
[0036] A composite film for a direct-type backlight module without a diffusion plate, comprising an upper layer 1, an intermediate layer 2, a bottom layer 3, a first adhesive layer, a second adhesive layer, and a back coating layer, wherein the upper layer 1 is connected to the intermediate layer 2 through the first adhesive layer, the intermediate layer 2 is connected to the bottom layer 3 through the second adhesive layer, the back coating layer is arranged on the lower surface of the bottom layer 3, the upper layer 1, the intermediate layer 2 and the bottom layer 3 are all independent film structures, the upper layer 1 is provided with a third microprism layer 11, the intermediate layer 2 is provided with a third microprism layer 12, and the A microprism layer 21, a second microprism layer 31 is provided on the bottom layer 3, the first microprism layer 21 is composed of triangular microprisms arranged in a high and low interval, the second microprism layer 31 is composed of a first honeycomb hemispherical lens 311 and a cylindrical prism 312 arranged in a periodic cycle of high N low, wherein the height of the cylindrical prism 312 is greater than that of the first honeycomb hemispherical lens 311, and N is greater than or equal to 1, and the third microprism layer 11 is composed of a second honeycomb hemispherical lens.
[0037] Preferably, the height of the triangular microprisms in the first microprism layer 21 is 26 μm, and the interval between adjacent triangular microprisms is 50 μm. The refractive index of the first microprism layer 21 is 1.53.
[0038] Preferably, the second microprism layer 31 is composed of a first honeycomb hemispherical lens 311 and a cylindrical prism 312 arranged in a cycle of 1 high and 4 low, the diameter of the first honeycomb hemispherical lens 311 is 45 μm, the height of the first honeycomb hemispherical lens 311 is 25 μm, the height of the cylindrical prism 312 is 60 μm, and the spacing between adjacent cylindrical prisms 312 is 180 μm.
[0039] Preferably, the diameter of the second honeycomb hemispherical lens in the third microprism layer 11 is 26 μm, the height of the second honeycomb hemispherical lens is 11 μm, and the refractive index of the third microprism layer 11 is 1.45.
[0040] As a preference, the method comprises the following steps:
[0041] S1. Take a roll of PET film as an intermediate base film, apply a layer of polyurethane acrylic resin on the upper surface of the intermediate base film, and complete the initial curing process by UV lamp irradiation to form a first polyurethane acrylic resin layer on the upper surface of the intermediate base film, and use a first prism roller mold to transfer the first polyurethane acrylic resin layer to form a first micro-prism layer 21, and the first micro-prism layer 21 and the intermediate base film together constitute an intermediate layer 2;
[0042] S2. Take a roll of PET film as the upper base film, apply adhesive A to one side of the upper base film to form a first adhesive layer, laminate the upper base film with the first adhesive layer and the intermediate layer, and bond the first adhesive layer to the first microprism layer 21 to form a first semi-finished product, and irradiate the first semi-finished product with a UV lamp to complete the full curing process;
[0043] S3. Take a roll of PET film as the bottom base film, apply a layer of polyurethane acrylic resin on the upper surface of the bottom base film, and complete the initial curing process by UV lamp irradiation to form a second polyurethane acrylic resin layer on the upper surface of the bottom base film, and use a second prism roller mold to transfer the second polyurethane acrylic resin layer to form a second microprism layer 31, and the second microprism layer 31 and the bottom base film together constitute the bottom layer 3;
[0044] S4. Adhesive B is applied to the lower surface of the intermediate base film in the first semi-finished product to form a second adhesive layer, the intermediate base film with the second adhesive layer is laminated with the second micro-prism layer 31 of the bottom layer 3, the first semi-finished product is bonded to the bottom layer to form a second semi-finished product, and a UV lamp is used to irradiate the second semi-finished product to complete the full curing process;
[0045] S5. Take the second semi-finished product, apply a layer of polyurethane acrylic resin on the upper surface of the upper base film, and perform a primary curing process by UV lamp irradiation to form a third polyurethane acrylic resin layer on the upper surface of the upper base film, use a third prism roller mold to transfer the third polyurethane acrylic resin layer to form a third micro-prism layer 11, and use a UV lamp again to perform a full curing process on the third micro-prism layer 11 after the transfer. The product obtained through the above steps is the third semi-finished product;
[0046] S6. Take the third semi-finished product, and coat the lower surface of the bottom base film in the third semi-finished product with a mixture of TiO 2 The coating liquid of the particles and PMMA diffusion particles is dried in an oven and / or UV-cured to form a back coating layer with a thickness of 10 μm on the lower surface of the bottom base film, completing the entire preparation process.
[0047] Preferably, the viscosity of the first polyurethane acrylic resin layer in step S1 is 50 cps, the thickness is greater than or equal to 31 μm, and the UV lamp irradiation energy in the initial curing process is controlled at 50 MJ / cm 2 The UV lamp irradiation energy in the full curing process in step S2 is controlled at 300MJ / cm 2 .
[0048] Preferably, the thickness of the second polyurethane acrylic resin layer in step S3 is greater than or equal to 65 μm, and the UV lamp irradiation energy in the initial curing process is controlled at 20 MJ / cm 2 The UV lamp irradiation energy in the full curing process in step S4 is controlled at 200MJ / cm 2 .
[0049] Preferably, the viscosity of the third polyurethane acrylic resin layer in step S5 is 20 cps, the thickness is greater than or equal to 15 μm, and the UV lamp irradiation energy in the initial curing process is controlled at 10 MJ / cm 2 The UV lamp irradiation energy in the full curing process is controlled at 100MJ / cm 2 .
[0050] Preferably, the linear speed of the first prism roller mold in the transfer process of step S1 is controlled at 3m / min, the linear speed of the third prism roller mold in the transfer process of step S5 is controlled at 7m / min, and the thickness of the first adhesive layer and the second adhesive layer in step S2 and step S4 is 1μm.
[0051] Preferably, the coating solution in step S6 comprises the following components in weight ratio:
[0052]
[0053] The TiO in the coating solution 2 The particle size of the particles is 1 μm, the particle size of the PMMA diffusion particles is 5 μm, the solvent is prepared by mixing a benzene solution with butanone or isopropanol in a ratio of 1:1, and the benzene solution is toluene or xylene.
[0054] Example 2
[0055] A composite film for a direct-type backlight module without a diffusion plate, comprising an upper layer 1, an intermediate layer 2, a bottom layer 3, a first adhesive layer, a second adhesive layer, and a back coating layer, wherein the upper layer 1 is connected to the intermediate layer 2 through the first adhesive layer, the intermediate layer 2 is connected to the bottom layer 3 through the second adhesive layer, the back coating layer is arranged on the lower surface of the bottom layer 3, the upper layer 1, the intermediate layer 2 and the bottom layer 3 are all independent film structures, the upper layer 1 is provided with a third microprism layer 11, the intermediate layer 2 is provided with a third microprism layer 12, and the A microprism layer 21, a second microprism layer 31 is provided on the bottom layer 3, the first microprism layer 21 is composed of triangular microprisms arranged in a high and low interval, the second microprism layer 31 is composed of a first honeycomb hemispherical lens 311 and a cylindrical prism 312 arranged in a periodic cycle of high N low, wherein the height of the cylindrical prism 312 is greater than that of the first honeycomb hemispherical lens 311, and N is greater than or equal to 1, and the third microprism layer 11 is composed of a second honeycomb hemispherical lens.
[0056] Preferably, the height of the triangular microprisms in the first microprism layer 21 is 40 μm, and the interval between adjacent triangular microprisms is 75 μm. The refractive index of the first microprism layer 21 is 1.56.
[0057] Preferably, the second microprism layer 31 is composed of a first honeycomb hemispherical lens 311 and a cylindrical prism 312 arranged in a cycle of 1 high and 4 low, the diameter of the first honeycomb hemispherical lens 311 is 55 μm, the height of the first honeycomb hemispherical lens 311 is 30 μm, the height of the cylindrical prism 312 is 80 μm, and the spacing between adjacent cylindrical prisms 312 is 200 μm.
[0058] Preferably, the diameter of the second honeycomb hemispherical lens in the third microprism layer 11 is 50 μm, the height of the second honeycomb hemispherical lens is 23 μm, and the refractive index of the third microprism layer 11 is 1.50.
[0059] As a preference, the method comprises the following steps:
[0060] S1. Take a roll of PET film as an intermediate base film, apply a layer of polyurethane acrylic resin on the upper surface of the intermediate base film, and complete the initial curing process by UV lamp irradiation to form a first polyurethane acrylic resin layer on the upper surface of the intermediate base film, and use a first prism roller mold to transfer the first polyurethane acrylic resin layer to form a first micro-prism layer 21, and the first micro-prism layer 21 and the intermediate base film together constitute an intermediate layer 2;
[0061] S2. Take a roll of PET film as the upper base film, apply adhesive A to one side of the upper base film to form a first adhesive layer, laminate the upper base film with the first adhesive layer and the intermediate layer, and bond the first adhesive layer to the first microprism layer 21 to form a first semi-finished product, and irradiate the first semi-finished product with a UV lamp to complete the full curing process;
[0062] S3. Take a roll of PET film as the bottom base film, apply a layer of polyurethane acrylic resin on the upper surface of the bottom base film, and complete the initial curing process by UV lamp irradiation to form a second polyurethane acrylic resin layer on the upper surface of the bottom base film, and use a second prism roller mold to transfer the second polyurethane acrylic resin layer to form a second microprism layer 31, and the second microprism layer 31 and the bottom base film together constitute the bottom layer 3;
[0063] S4. Adhesive B is applied to the lower surface of the intermediate base film in the first semi-finished product to form a second adhesive layer, the intermediate base film with the second adhesive layer is laminated with the second micro-prism layer 31 of the bottom layer 3, the first semi-finished product is bonded to the bottom layer to form a second semi-finished product, and a UV lamp is used to irradiate the second semi-finished product to complete the full curing process;
[0064] S5. Take the second semi-finished product, apply a layer of polyurethane acrylic resin on the upper surface of the upper base film, and perform a primary curing process by UV lamp irradiation to form a third polyurethane acrylic resin layer on the upper surface of the upper base film, use a third prism roller mold to transfer the third polyurethane acrylic resin layer to form a third micro-prism layer 11, and use a UV lamp again to perform a full curing process on the third micro-prism layer 11 after the transfer. The product obtained through the above steps is the third semi-finished product;
[0065] S6. Take the third semi-finished product, and coat the lower surface of the bottom base film in the third semi-finished product with a mixture of TiO 2 The coating liquid of the particles and PMMA diffusion particles is dried in an oven and / or UV-cured to form a back coating layer with a thickness of 20 μm on the lower surface of the bottom base film, completing the entire preparation process.
[0066] Preferably, the viscosity of the first polyurethane acrylic resin layer in step S1 is 800 cps, the thickness is greater than or equal to 31 μm, and the UV lamp irradiation energy in the initial curing process is controlled at 80 MJ / cm 2 The UV lamp irradiation energy in the full curing process in step S2 is controlled at 450MJ / cm 2 .
[0067] Preferably, the thickness of the second polyurethane acrylic resin layer in step S3 is greater than or equal to 65 μm, and the UV lamp irradiation energy in the initial curing process is controlled at 50 MJ / cm 2 The UV lamp irradiation energy in the full curing process in step S4 is controlled at 1000MJ / cm 2 .
[0068] Preferably, the viscosity of the third polyurethane acrylic resin layer in step S5 is 150 cps, the thickness is greater than or equal to 15 μm, and the UV lamp irradiation energy in the initial curing process is controlled at 30 MJ / cm 2 The UV lamp irradiation energy in the full curing process is controlled at 300MJ / cm 2 .
[0069] Preferably, the linear speed of the first prism roller mold in the transfer process of step S1 is controlled at 30m / min, the linear speed of the third prism roller mold in the transfer process of step S5 is controlled at 35m / min, and the thickness of the first adhesive layer and the second adhesive layer in step S2 and step S4 is 5μm.
[0070] Preferably, the coating solution in step S6 comprises the following components in weight ratio:
[0071]
[0072] The TiO in the coating solution 2 The particle size of the particles is 3 μm, the particle size of the PMMA diffusion particles is 10 μm, the solvent is prepared by mixing a benzene solution with butanone or isopropanol in a ratio of 1:1, and the benzene solution is toluene or xylene.
[0073] Example 3
[0074] A composite film for a direct-type backlight module without a diffusion plate, comprising an upper layer 1, an intermediate layer 2, a bottom layer 3, a first adhesive layer, a second adhesive layer, and a back coating layer, wherein the upper layer 1 is connected to the intermediate layer 2 through the first adhesive layer, the intermediate layer 2 is connected to the bottom layer 3 through the second adhesive layer, the back coating layer is arranged on the lower surface of the bottom layer 3, the upper layer 1, the intermediate layer 2 and the bottom layer 3 are all independent film structures, the upper layer 1 is provided with a third microprism layer 11, the intermediate layer 2 is provided with a third microprism layer 12, and the A microprism layer 21, a second microprism layer 31 is provided on the bottom layer 3, the first microprism layer 21 is composed of triangular microprisms arranged in a high and low interval, the second microprism layer 31 is composed of a first honeycomb hemispherical lens 311 and a cylindrical prism 312 arranged in a periodic cycle of high N low, wherein the height of the cylindrical prism 312 is greater than that of the first honeycomb hemispherical lens 311, and N is greater than or equal to 1, and the third microprism layer 11 is composed of a second honeycomb hemispherical lens.
[0075] Preferably, the height of the triangular microprisms in the first microprism layer 21 is 32 μm, and the distance between adjacent triangular microprisms is 63 μm. The refractive index of the first microprism layer 21 is 1.54.
[0076] Preferably, the second microprism layer 31 is composed of a first honeycomb hemispherical lens 311 and a cylindrical prism 312 arranged in a cycle of 1 high and 4 low, the diameter of the first honeycomb hemispherical lens 311 is 50 μm, the height of the first honeycomb hemispherical lens 311 is 27 μm, the height of the cylindrical prism 312 is 70 μm, and the spacing between adjacent cylindrical prisms 312 is 190 μm.
[0077] Preferably, the diameter of the second honeycomb hemispherical lens in the third microprism layer 11 is 40 μm, the height of the second honeycomb hemispherical lens is 17 μm, and the refractive index of the third microprism layer 11 is 1.48.
[0078] As a preference, the method comprises the following steps:
[0079] S1. Take a roll of PET film as an intermediate base film, apply a layer of polyurethane acrylic resin on the upper surface of the intermediate base film, and complete the initial curing process by UV lamp irradiation to form a first polyurethane acrylic resin layer on the upper surface of the intermediate base film, and use a first prism roller mold to transfer the first polyurethane acrylic resin layer to form a first micro-prism layer 21, and the first micro-prism layer 21 and the intermediate base film together constitute an intermediate layer 2;
[0080] S2. Take a roll of PET film as the upper base film, apply adhesive A to one side of the upper base film to form a first adhesive layer, laminate the upper base film with the first adhesive layer and the intermediate layer, and bond the first adhesive layer to the first microprism layer 21 to form a first semi-finished product, and irradiate the first semi-finished product with a UV lamp to complete the full curing process;
[0081] S3. Take a roll of PET film as the bottom base film, apply a layer of polyurethane acrylic resin on the upper surface of the bottom base film, and complete the initial curing process by UV lamp irradiation to form a second polyurethane acrylic resin layer on the upper surface of the bottom base film, and use a second prism roller mold to transfer the second polyurethane acrylic resin layer to form a second microprism layer 31, and the second microprism layer 31 and the bottom base film together constitute the bottom layer 3;
[0082] S4. Adhesive B is applied to the lower surface of the intermediate base film in the first semi-finished product to form a second adhesive layer, the intermediate base film with the second adhesive layer is laminated with the second micro-prism layer 31 of the bottom layer 3, the first semi-finished product is bonded to the bottom layer to form a second semi-finished product, and a UV lamp is used to irradiate the second semi-finished product to complete the full curing process;
[0083] S5. Take the second semi-finished product, apply a layer of polyurethane acrylic resin on the upper surface of the upper base film, and perform a primary curing process by UV lamp irradiation to form a third polyurethane acrylic resin layer on the upper surface of the upper base film, use a third prism roller mold to transfer the third polyurethane acrylic resin layer to form a third micro-prism layer 11, and use a UV lamp again to perform a full curing process on the third micro-prism layer 11 after the transfer. The product obtained through the above steps is the third semi-finished product;
[0084] S6. Take the third semi-finished product, and coat the lower surface of the bottom base film in the third semi-finished product with a mixture of TiO 2 The coating liquid of the particles and PMMA diffusion particles is dried in an oven and / or UV-cured to form a back coating layer with a thickness of 15 μm on the lower surface of the bottom base film, completing the entire preparation process.
[0085] Preferably, the viscosity of the first polyurethane acrylic resin layer in step S1 is 400 cps, the thickness is greater than or equal to 31 μm, and the UV lamp irradiation energy in the initial curing process is controlled at 65 MJ / cm 2 The UV lamp irradiation energy in the full curing process in step S2 is controlled at 375 J / cm 2 .
[0086] Preferably, the thickness of the second polyurethane acrylic resin layer in step S3 is greater than or equal to 65 μm, and the UV lamp irradiation energy in the initial curing process is controlled at 35 MJ / cm 2 The UV lamp irradiation energy in the full curing process in step S4 is controlled at 600MJ / cm 2 .
[0087] Preferably, the viscosity of the third polyurethane acrylic resin layer in step S5 is 90 cps, and the thickness is greater than or equal to 15 μm, and the UV lamp irradiation energy in the initial curing process is controlled at 20 MJ / cm 2 The UV lamp irradiation energy in the full curing process is controlled at 200MJ / cm 2 .
[0088] Preferably, the linear speed of the first prism roller mold in the transfer process of step S1 is controlled at 20m / min, the linear speed of the third prism roller mold in the transfer process of step S5 is controlled at 20m / min, and the thickness of the first adhesive layer and the second adhesive layer in step S2 and step S4 is 3μm.
[0089] Preferably, the coating solution in step S6 comprises the following components in weight ratio:
[0090]
[0091] The TiO in the coating solution 2 The particle size of the particles is 2 μm, the particle size of the PMMA diffusion particles is 7 μm, the solvent is prepared by mixing a benzene solution with butanone or isopropanol in a ratio of 1:1, and the benzene solution is toluene or xylene.
[0092] In conclusion, the above is only a preferred embodiment of the present invention, and all equivalent changes and modifications made within the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A composite film for a direct-type backlight module without a diffusion plate, characterized in that: The invention comprises an upper layer (1), an intermediate layer (2), a bottom layer (3), a first adhesive layer, a second adhesive layer, and a back coating layer, wherein the upper layer (1) and the intermediate layer (2) are connected via the first adhesive layer, the intermediate layer (2) and the bottom layer (3) are connected via the second adhesive layer, the back coating layer is arranged on the lower surface of the bottom layer (3), the upper layer (1), the intermediate layer (2) and the bottom layer (3) are all independent film structures, the upper layer (1) is provided with a third micro-prism layer (11), the intermediate layer (2) is provided with a first micro-prism layer (21), a second microprism layer (31) is provided on the bottom layer (3), the first microprism layer (21) is composed of triangular microprisms arranged in a high and low pattern, the second microprism layer (31) is composed of first honeycomb hemispherical lenses (311) and columnar prisms (312) arranged in a cycle of one high and N low, wherein the columnar prism (312) is greater than the first honeycomb hemispherical lens (311) in height, and N is greater than or equal to 1, and the third microprism layer (11) is composed of second honeycomb hemispherical lenses; The height of the triangular microprisms in the first microprism layer (21) ranges from 26 μm to 40 μm, and the spacing between adjacent triangular microprisms ranges from 50 μm to 75 μm. The refractive index of the first microprism layer (21) ranges from 1.53 to 1.
56. The second microprism layer (31) is composed of a first honeycomb hemispherical lens (311) and a cylindrical prism (312) arranged in a cycle of 1 high and 4 low, the diameter of the first honeycomb hemispherical lens (311) is in the range of 45 μm to 55 μm, the height of the first honeycomb hemispherical lens (311) is in the range of 25 μm to 30 μm, the height of the cylindrical prism (312) is in the range of 60 μm to 80 μm, and the spacing between adjacent cylindrical prisms (312) is in the range of 180 μm to 200 μm.
2. The composite film for a direct-lit backlight module without a diffusion plate according to claim 1, characterized in that: The diameter of the second honeycomb hemispherical lenses in the third microprism layer (11) is in the range of 26 μm to 50 μm, the height of the second honeycomb hemispherical lenses is in the range of 11 μm to 23 μm, and the refractive index of the third microprism layer (11) is in the range of 1.45 to 1.
50.
3. The method for manufacturing a composite film for a direct-lit backlight module without a diffusion plate according to claim 1, characterized in that: The following steps are involved: S1. Take a roll of PET film as the middle layer base film, apply a layer of polyurethane acrylic resin on the upper surface of the middle layer base film, and complete the initial curing process by UV lamp irradiation to form a first polyurethane acrylic resin layer on the upper surface of the middle layer base film, and use a first prism roller mold to transfer the first polyurethane acrylic resin layer to form a first microprism layer (21), and the first microprism layer (21) and the middle layer base film together constitute the middle layer (2); S2. Take a roll of PET film as the upper layer base film, use adhesive A to apply a first adhesive layer on one side of the upper layer base film, and place the upper layer base film with the first adhesive layer on the upper layer base film. The film is laminated with the intermediate layer, so that the first adhesive layer and the first micro-prism layer (21) are bonded to form a first semi-finished product, and the first semi-finished product is irradiated with a UV lamp to complete the full curing process; S3. A roll of PET film is taken as a bottom base film, a layer of polyurethane acrylic resin is coated on the upper surface of the bottom base film, and a UV lamp is irradiated to complete the initial curing process to form a second polyurethane acrylic resin layer on the upper surface of the bottom base film, and a second prism roller mold is used to transfer the second polyurethane acrylic resin layer to form a second micro-prism layer (31), and the second micro-prism layer (31) and the bottom base film together constitute the bottom layer (3); S4. Adhesive B is used to coat the lower surface of the intermediate base film in the first semi-finished product to form a second adhesive layer, and the intermediate base film with the second adhesive layer is overlapped with the second micro-prism layer (31) of the bottom layer (3), so that the first semi-finished product and the bottom layer are bonded to form a second semi-finished product, and a UV lamp is used to irradiate the second semi-finished product to complete the full curing process; S5. Take the second semi-finished product, coat a layer of polyurethane acrylic resin on the upper surface of the upper base film, and irradiate the upper surface of the upper base film with a UV lamp to complete the initial curing process to form a third polyurethane acrylic resin layer on the upper surface of the upper base film, and use a third prism roller mold The third polyurethane acrylic resin layer is transferred to form a third microprism layer (11), and the third microprism layer (11) after the transfer is fully cured by a UV lamp again. The product obtained through the above steps is a third semi-finished product; S6. The third semi-finished product is taken, and a coating liquid mixed with TiO2 particles and PMMA diffusion particles is coated on the lower surface of the bottom base film in the third semi-finished product by an anilox roller or a slit coating method, and a back coating layer with a thickness ranging from 10μm to 20μm is formed on the lower surface of the bottom base film after drying in an oven and / or UV curing the coating liquid, thereby completing the entire preparation process.
4. The method for manufacturing a composite film for a direct-lit backlight module without a diffusion plate according to claim 3, characterized in that: The viscosity of the first polyurethane acrylic resin layer in step S1 is between 50cps and 800cps, and the thickness is greater than or equal to 31μm. The UV lamp irradiation energy range in the initial curing process is controlled within 50MJ / cm 2 ~80MJ / cm 2 The UV lamp irradiation energy range in the full curing process in step S2 is controlled within 300MJ / cm 2 ~450MJ / cm 2 between.
5. The method for manufacturing a composite film for a direct-lit backlight module without a diffusion plate according to claim 3, characterized in that: The thickness of the second polyurethane acrylic resin layer in step S3 is greater than or equal to 65 μm, and the UV lamp irradiation energy range in the initial curing process is controlled within 20 MJ / cm 2 ~50MJ / cm 2 The UV lamp irradiation energy range in the full curing process in step S4 is controlled within 200MJ / cm 2 ~1000MJ / cm 2 between.
6. The method for manufacturing a composite film for a direct-lit backlight module without a diffusion plate according to claim 3, characterized in that: The viscosity of the third polyurethane acrylic resin layer in step S5 is between 20cps and 150cps, and the thickness is greater than or equal to 15μm. The UV lamp irradiation energy range in the initial curing process is controlled within 10MJ / cm 2 ~30MJ / cm 2 The UV lamp irradiation energy range in the full curing process is controlled within 100MJ / cm 2 ~300MJ / cm 2 between.
7. The method for manufacturing a composite film for a direct-lit backlight module without a diffusion plate according to claim 3, characterized in that: The linear speed of the first prism roller mold in the transfer process of step S1 is controlled between 3m / min and 30m / min, the linear speed of the third prism roller mold in the transfer process of step S5 is controlled between 7m / min and 35m / min, and the thickness of the first adhesive layer and the second adhesive layer in step S2 and step S4 is between 1μm and 5μm.
8. The method for manufacturing a composite film for a direct-lit backlight module without a diffusion plate according to claim 3, characterized in that: The coating solution in step S6 includes the following components in weight ratio: TiO2 particles 0.1 parts, 1~2 parts of PMMA diffusion particles, 1~2 parts of polyurethane acrylate, 1~2 parts of acrylic acid, 2~3 parts of solvent, The particle size of the TiO2 particles in the coating liquid is between 1 μm and 3 μm, the particle size of the PMMA diffusion particles is between 5 μm and 10 μm, and the solvent is prepared by mixing a benzene solution with butanone or isopropanol in a ratio of 1:1, and the benzene solution is toluene or xylene.