By increasing the bonding force between the dielectric layer and the cathode layer, the cathode layer and the graphite silver paste layer in the conductive polymer tantalum capacitor, using three stages to form the conductive polymer cathode layer, and setting up a moisture-proof barrier layer, the problem of conductive polymer tantalum capacitors is solved. Stability issues under high thermoelectric stress improve the stability and reliability of capacitors.

CN114156089BActive Publication Date: 2024-10-01BEIJING 718 YOUYI ELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111403929.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-24
Publication Date
2024-10-01
Estimated Expiration
2041-11-24

AI Technical Summary

Technical Problem

Existing conductive polymer tantalum capacitors have problems with low stability under high thermoelectric stress. This is mainly due to the mismatch in thermal expansion coefficients between the dielectric layer and the cathode layer, and the interface thermal expansion coefficient between the cathode layer. This causes stress, which in turn leads to cracking of the cathode layer and interlayer The contact resistance increases, increasing the equivalent series resistance (ESR) of the capacitor.

Method used

By increasing the bonding force and mechanical strength between the dielectric layer and the conductive polymer cathode layer, and between the conductive polymer cathode layer and the graphite silver paste layer, the conductive polymer cathode layer is formed in three stages: inner layer, transition layer, and outer layer. A moisture-proof barrier layer is set on the tantalum core group to enhance interface stability and mechanical strength.

Benefits of technology

It improves the interface bonding strength between the dielectric layer and the cathode layer, and between the cathode layer and the graphite silver paste layer, enhances the stability and reliability of the capacitor, and can maintain the ESR stability of the capacitor under high temperature and load baking conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114156089B_ABST
    Figure CN114156089B_ABST
Patent Text Reader

Abstract

The invention discloses a chip-type conductive polymer tantalum capacitor and a preparation method thereof, the method comprising: coating a treatment liquid on the surface of a dielectric layer to enhance the adhesion between the dielectric layer and the conductive polymer layer; coating a conductive polymer inner layer, a transition layer, and an outer layer outside the treatment layer in sequence, and improving the adhesion between the sublayers of the conductive polymer outer layer by a crosslinking agent; coating a graphene composite material layer on the polymer outer layer; coating graphite and silver paste to form a graphite silver paste layer, and leading out the positive and negative electrodes through a lead frame to obtain a tantalum core group, performing moisture-proof treatment on the tantalum core group and molding and packaging, that is, preparing a chip-type conductive polymer tantalum capacitor. The tantalum capacitor prepared by the invention has strong interface adhesion and high mechanical strength of the cathode layer, and the cathode film layer is continuous and dense, and the capacitor has higher performance stability under long-term thermal and electrical stress.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solid tantalum capacitors, and in particular to a chip-type conductive polymer tantalum capacitor with good stability and a preparation method thereof. Background Art

[0002] Solid electrolytic capacitors, especially tantalum solid electrolytic capacitors, have made important contributions to the miniaturization of electronic circuits.

[0003] In recent years, conductive polymers have been used as cathode materials for solid tantalum capacitors due to their high conductivity and good stability. Compared with traditional manganese dioxide cathodes, conductive polymers can effectively reduce the equivalent series resistance (ESR) of tantalum capacitors and have better high-frequency performance.

[0004] However, the stability of the ESR of tantalum capacitors requires that the interfaces between the dielectric layer and the cathode layer, between the cathode layers, between the cathode conductive layer, the conductive adhesive and the lead frame have good and stable mechanical integrity under thermoelectric stress. However, the current tantalum capacitors with conductive polymers as cathode materials are subjected to high thermoelectric stress during installation and use. The mismatch of the coefficient of thermal expansion (CTE) between the interfaces will cause stress between the interfaces, resulting in cracking or delamination of the cathode layer. Any material separation between the interfaces will increase the interlayer contact resistance, which in turn leads to an increase in the ESR of the tantalum capacitor under high thermoelectric stress, making the existing conductive polymer tantalum capacitors have the problem of low stability under long-term thermal and electrical stress. Summary of the invention

[0005] The purpose of the present invention is to provide a chip-type conductive polymer tantalum capacitor, which can improve the interface bonding strength between the capacitor dielectric layer and the cathode layer, between the cathode layers, and between the cathode layer and the graphite silver paste layer, thereby enhancing the stability and reliability of the capacitor, and further solving the above-mentioned technical problems existing in the prior art.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] The embodiment of the present invention provides a chip-type conductive polymer tantalum capacitor, comprising:

[0008] Anode tantalum block, dielectric layer, adhesive guide layer, conductive polymer cathode layer, graphene composite material layer, graphite silver paste layer, moisture barrier layer, packaging shell, positive lead and negative lead; wherein,

[0009] The outer surface of the anode tantalum block is coated with the dielectric layer, the adhesive guide layer, the conductive polymer cathode layer, the graphene composite material layer and the graphite silver paste layer in sequence from the inside to the outside;

[0010] The positive electrode lead is electrically connected to the anode tantalum block, and the negative electrode lead is electrically connected to the graphite silver paste layer to form a tantalum core group;

[0011] The moisture-proof barrier layer is coated outside the tantalum core group;

[0012] The tantalum core group package covering the moisture-proof barrier layer is arranged in the package shell;

[0013] The positive electrode lead is led out from one side of the packaging shell to the outside of the epoxy resin shell;

[0014] The negative electrode lead is led out from the other side of the package case to the outside of the package case.

[0015] The embodiment of the present invention further provides a method for preparing a chip-type conductive polymer tantalum capacitor, which is used to prepare the chip-type conductive polymer tantalum capacitor of the present invention, comprising:

[0016] Step 1, immersing the anode tantalum block with a Ta2O5 film formed on the surface after energization into the guide layer treatment solution A for 1 to 15 minutes, and drying and forming at 50 to 150° C.;

[0017] Step 2, immersing the anode tantalum block obtained in step 1 in a dispersion of poly (3,4-ethylenedioxythiophene) particles having a solid content of 0.5% to 2.5% and a particle size of 20 to 30 nm under vacuum for 1 to 10 minutes, and drying the dispersion under a vacuum environment of 80° C. to 150° C., and repeating this step 5 to 15 times;

[0018] Step 3, immersing the anode tantalum block obtained in step 2 in a dispersion of poly (3,4-ethylenedioxythiophene) particles having a solid content of 1% to 5% and a particle size of 30 to 50 nm under vacuum for 1 to 10 minutes, and drying the dispersion under a vacuum environment of 80 to 150° C., and repeating this step 2 to 8 times;

[0019] Step 4, immersing the anode tantalum block obtained in step 3 in a dispersion of poly 3,4-ethylenedioxythiophene particles with a solid content of 2% to 10% and a particle size of 50 to 100 nm under vacuum for 1 to 10 minutes, and drying it under a vacuum environment of 80° C. to 150° C., then immersing the dried anode tantalum block in a crosslinking agent B for 1 to 5 minutes, and drying it at 80° C. to 150° C., and repeating this step 2 to 6 times;

[0020] Step 5, immersing the anode tantalum block obtained in step 4 in a graphene composite material system C having a solid content of 0.05% to 5% and a particle size of 50 to 500 nm, and drying it at 120° C. to 150° C., repeating this step 1 to 2 times to obtain an anode tantalum block having an outer layer of a conductive polymer containing a graphene structure;

[0021] Step 6, impregnating the conductive polymer outer layer of the anode tantalum block obtained in step 5 with graphite and silver paste to form a graphite silver paste layer, and then using a lead frame to lead out the positive and negative electrodes to obtain a tantalum core group;

[0022] Step 7, coating a moisture-proof barrier layer D on the tantalum core group obtained in step 6, and performing mold packaging to obtain a chip-type conductive polymer tantalum capacitor.

[0023] Compared with the prior art, the chip-type conductive polymer tantalum capacitor and the preparation method thereof provided by the present invention have the following beneficial effects:

[0024] By treating the dielectric layer and the conductive polymer cathode layer, between the conductive polymer cathode layers, and between the outer layer of the conductive polymer cathode layer and the graphite and silver paste layers, the bonding force and mechanical strength between the interfaces are increased, and the interface stability is improved. When forming the conductive polymer cathode layer, a three-stage formation process of an inner layer, a transition layer, and an outer layer is adopted, which is more conducive to forming a continuous and dense conductive polymer cathode layer. A moisture-proof barrier layer is set on the tantalum core group after the film is coated for moisture-proof treatment, so that the tantalum capacitor formed by the preparation method has an enhanced ability to withstand high-temperature load baking and can maintain the stability of the capacitor ESR. The tantalum capacitor and its preparation method enhance the stability and reliability of the tantalum capacitor by improving the interface bonding strength between the dielectric layer and the cathode layer, between the cathode layers, and between the cathode layer and the graphite silver paste layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0026] Figure 1 A schematic cross-sectional structure diagram of a chip-type conductive polymer tantalum capacitor is provided for an embodiment of the present invention;

[0027] Figure 2 A schematic flow chart of a method for preparing a chip-type conductive polymer tantalum capacitor is provided for an embodiment of the present invention;

[0028] Figure 1 Middle: 1-anode tantalum block; 2-dielectric layer; 3-adhesive guide layer; 4-conductive polymer cathode layer; 5-graphene composite material layer; 6-graphite silver paste layer; 7-moisture-proof barrier layer; 8-packaging shell; 9-positive electrode lead; 10-negative electrode lead. DETAILED DESCRIPTION

[0029] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the specific content of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, which does not constitute a limitation of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0030] First, the terms that may be used in this article are explained as follows:

[0031] The term “and / or” means that either or both of them can be realized at the same time. For example, X and / or Y means both “X” or “Y” and “X and Y”.

[0032] The terms "include", "comprises", "contains", "has" or other descriptions with similar semantics should be interpreted as non-exclusive inclusion. For example, including certain technical feature elements (such as raw materials, components, ingredients, carriers, dosage forms, materials, dimensions, parts, components, mechanisms, devices, steps, procedures, methods, reaction conditions, processing conditions, parameters, algorithms, signals, data, products or products, etc.) should be interpreted as including not only certain technical feature elements explicitly listed, but also other technical feature elements known in the art that are not explicitly listed.

[0033] The term "consisting of..." means excluding any technical feature elements not explicitly listed. If this term is used in a claim, it will make the claim closed, so that it does not contain technical feature elements other than the technical feature elements explicitly listed, except for the conventional impurities related to them. If this term only appears in a clause of a claim, it only limits the elements explicitly listed in the clause, and the elements recorded in other clauses are not excluded from the overall claim.

[0034] The term "parts by mass" refers to the mass ratio relationship between multiple components. For example, if it is described that component X is x parts by mass and component Y is y parts by mass, then the mass ratio of component X to component Y is x:y. 1 part by mass can represent any mass, for example, 1 part by mass can be represented as 1 kg or 3.1415926 kg. The sum of the parts by mass of all components is not necessarily 100 parts, but can be greater than 100 parts, less than 100 parts or equal to 100 parts. Unless otherwise specified, the parts, proportions and percentages described herein are all measured by mass.

[0035] Unless otherwise specified or limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example: it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this article can be understood according to specific circumstances.

[0036] When concentration, temperature, pressure, size or other parameters are expressed in the form of a numerical range, the numerical range should be understood to specifically disclose all ranges formed by the pairing of any upper limit, lower limit, and preferred value in the numerical range, regardless of whether the range is explicitly stated; for example, if a numerical range of "2 to 8" is stated, the numerical range should be interpreted as including ranges such as "2 to 7", "2 to 6", "5 to 7", "3 to 4 and 6 to 7", "3 to 5 and 7", "2 and 5 to 7", etc. Unless otherwise specified, the numerical ranges stated herein include both their end values ​​and all integers and fractions within the numerical range.

[0037] The orientation or position relationship indicated by terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc. are based on the orientation or position relationship shown in the drawings and are only for the convenience and simplification of description, and do not explicitly or implicitly indicate that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation of this document.

[0038] The following is a detailed description of the chip-type conductive polymer tantalum capacitor and its preparation method provided by the present invention. The contents not described in detail in the embodiments of the present invention belong to the prior art known to professional and technical personnel in the field. If no specific conditions are specified in the embodiments of the present invention, the conventional conditions in the field or the conditions recommended by the manufacturer are followed. The reagents or instruments used in the embodiments of the present invention without indicating the manufacturer are all conventional products that can be purchased commercially.

[0039] like Figure 1 As shown, an embodiment of the present invention provides a chip-type conductive polymer tantalum capacitor, comprising:

[0040] Anode tantalum block, dielectric layer, adhesive guide layer, conductive polymer cathode layer, graphene composite material layer, graphite silver paste layer, moisture barrier layer, packaging shell, positive lead and negative lead; wherein,

[0041] The outer surface of the anode tantalum block is coated with the dielectric layer, the adhesive guide layer, the conductive polymer cathode layer, the graphene composite material layer and the graphite silver paste layer in sequence from the inside to the outside;

[0042] The positive electrode lead is electrically connected to the anode tantalum block, and the negative electrode lead is electrically connected to the graphite silver paste layer to form a tantalum core group;

[0043] The moisture-proof barrier layer is coated outside the tantalum core group;

[0044] The tantalum core group package covering the moisture-proof barrier layer is arranged in the package shell;

[0045] The positive electrode lead is led out from one side of the packaging shell to the outside of the epoxy resin shell;

[0046] The negative electrode lead is led out from the other side of the package case to the outside of the package case.

[0047] In the above tantalum capacitor, the adhesion guide layer may be a thin film layer formed of one or more of a polyhydroxyl functional monomer, a polyhydroxyl functional polymer, an organic functional silane or a hydrolyzate thereof.

[0048] In the above tantalum capacitor, the polyhydroxy functional group polymer adopts a polymer containing at least two hydroxyl repeating units and a copolymer thereof;

[0049] The organofunctional silane is one or more of aminosilane, vinylsilane, epoxysilane and the like.

[0050] In the above-mentioned tantalum capacitor, the graphene contained in the graphene composite material layer may be reduced graphene oxide, and the average cross-sectional size of the graphene is not greater than 500nm;

[0051] The conductive polymer cathode layer comprises: an inner layer, a transition layer and an outer layer;

[0052] The moisture-proof barrier layer is a moisture-proof layer formed by curing a hydrophobic material and an auxiliary agent.

[0053] In the above-mentioned tantalum capacitor, the inner layer of the conductive polymer cathode layer is a capacity extraction layer formed by depositing a dispersion of poly 3,4-ethylenedioxythiophene particles having an average particle size of 20 to 30 nm;

[0054] The transition layer of the conductive polymer cathode layer is an intermediate transition layer formed by depositing a dispersion of poly 3,4-ethylenedioxythiophene particles with an average particle size of 30 to 50 nm;

[0055] The outer layer of the conductive polymer cathode layer is a thickness-increasing layer formed by depositing a dispersion of poly 3,4-ethylenedioxythiophene particles having an average particle size of 50 to 100 nm;

[0056] The hydrophobic material used in the moisture-proof barrier layer is any one of silane material, acrylic material, polyurethane material and epoxy resin material.

[0057] The inner layer, transition layer and outer layer of the conductive polymer cathode layer are formed by using dispersions with different and continuously distributed particle sizes, and in combination with a staged formation method, a continuous and dense cathode layer can be obtained.

[0058] In the above tantalum capacitor, a cross-linking layer is provided between the outer layer of the conductive polymer cathode layer and the transition layer of the conductive polymer cathode layer.

[0059] In the above tantalum capacitor, the cross-linked layer is made of polycationic salts, amino compounds or their derivatives.

[0060] The embodiment of the present invention further provides a method for preparing a chip-type conductive polymer tantalum capacitor, which is used for the above-mentioned chip-type conductive polymer tantalum capacitor, comprising:

[0061] Step 1, immersing the tantalum anode block with a Ta2O5 film formed on the surface after energization into the treatment solution A for 1 to 15 minutes, and drying and forming at 50 to 150° C.;

[0062] Step 2, immersing the anode tantalum block obtained in step 1 in a dispersion of poly (3,4-ethylenedioxythiophene) particles having a solid content of 0.5% to 2.5% and a particle size of 20 to 30 nm under vacuum for 1 to 10 minutes, and drying the dispersion under a vacuum environment of 80° C. to 150° C., and repeating this step 5 to 15 times; this step forms an inner layer of the conductive polymer cathode layer, which is composed of multiple sublayers and has higher bonding force and mechanical strength;

[0063] Step 3, immersing the anode tantalum block obtained in step 2 in a dispersion of poly(3,4-ethylenedioxythiophene) particles having a solid content of 1% to 5% and a particle size of 30 to 50 nm under vacuum for 1 to 10 minutes, and drying the dispersion under a vacuum environment of 80 to 150° C., and repeating this step 2 to 8 times; this step forms a transition layer of the conductive polymer cathode layer, which is composed of multiple sublayers and has higher bonding force and mechanical strength;

[0064] Step 4, immersing the anode tantalum block obtained in step 3 in a dispersion of poly 3,4-ethylenedioxythiophene particles with a solid content of 2% to 10% and a particle size of 50 to 100 nm under vacuum for 1 to 10 minutes, and drying it under a vacuum environment of 80°C to 150°C, then immersing the dried anode tantalum block in a crosslinking agent B under normal pressure for 1 to 5 minutes, and drying it at 80°C to 150°C, and repeating this step 2 to 6 times; this step will form an outer layer of the conductive polymer cathode layer, which is composed of multiple sublayers, and each sublayer has a crosslinking layer, thereby improving its bonding force and mechanical strength;

[0065] Step 5, immersing the anode tantalum block obtained in step 4 in a graphene composite material system C having a solid content of 0.05% to 5% and a particle size of 50 to 500 nm, and drying it at 120° C. to 150° C., repeating this step 1 to 2 times to obtain an anode tantalum block having an outer layer of a conductive polymer containing a graphene structure;

[0066] Step 6, impregnating the conductive polymer outer layer of the anode tantalum block obtained in step 5 with graphite and silver paste to form a graphite silver paste layer, and then using a lead frame to lead out the positive and negative electrodes to obtain a tantalum core group;

[0067] Step 7, coating a moisture-proof barrier layer D on the tantalum core group obtained in step 6, and performing mold packaging to obtain a chip-type conductive polymer tantalum capacitor.

[0068] In the above preparation method, the guide layer treatment liquid A in step 1 is a treatment liquid formed by mixing any one or more of a polyhydroxyl functional monomer, a polyhydroxyl functional polymer, an organic functional silane or a hydrolyzate thereof with a solvent A;

[0069] The crosslinking agent B in step 4 is a mixed solution formed by mixing any one of a polycationic salt, a compound, and an amine compound with a solvent B;

[0070] The graphene composite material system C in step 5 is composed of graphene, an additive and a solvent C, wherein the graphene content is 0.01wt.% to 10wt.%, the solvent C content is 75wt.% to 99wt.%, and the rest is an additive, wherein the additive is preferably a crosslinking agent and a dispersant, and other additives may also be used as needed. Preferably, the graphene is reduced graphene oxide.

[0071] In the above preparation method, the solvent A in the guide layer treatment liquid A adopts any one or more of water, alcohol solvents, ether solvents, and ketone solvents, such as methanol, ethanol, propanol, isopropanol, methyl ether, ethyl ether, methyl tert-butyl ether, anisole, acetone, butanone, etc.; preferably, the polyhydroxy functional polymer in the guide layer treatment liquid A includes: polyethylene glycol, polyvinyl alcohol and other polymers containing at least two hydroxyl repeating units and their copolymers; the organic functional silane includes: one or more of aminosilane, vinyl silane, epoxy silane, etc.

[0072] The solvent B in the crosslinking agent B is any one or more of water, aliphatic alcohol solvents, and ketone solvents; the crosslinking agent in the crosslinking agent B can be a polycationic salt, compound or amine compound;

[0073] The crosslinking agent in the graphene composite material system C is a polycationic salt, compound or amine compound; the solvent C in the graphene composite material system C is any one or more of water, aliphatic alcohol solvents and ketone solvents.

[0074] In summary, the chip-type conductive polymer tantalum capacitor and its preparation method of the embodiment of the present invention increase the bonding force and mechanical strength between the interfaces and improve the interface stability by processing between the dielectric layer and the inner layer of the conductive polymer cathode, between the sublayers of the conductive polymer outer layer, and between the outer layer of the conductive polymer cathode and the graphene composite material layer. The inner layer, transition layer, and outer layer three-stage formation process is adopted when forming the conductive polymer cathode layer, which is more conducive to forming a continuous and dense conductive polymer cathode layer, and a moisture-proof barrier layer is set for the anode tantalum block after the film is coated for moisture-proof treatment, so that the tantalum capacitor formed by the preparation method has an enhanced ability to withstand high-temperature load baking and can maintain the stability of the capacitor ESR. The tantalum capacitor and its preparation method enhance the stability and reliability of the tantalum capacitor by improving the interface bonding strength between the dielectric layer and the cathode layer, between the cathode layers, and between the cathode layer and the graphite silver paste layer.

[0075] In order to more clearly demonstrate the technical solution and technical effects provided by the present invention, the chip-type conductive polymer tantalum capacitor and the preparation method thereof provided by the embodiment of the present invention are described in detail with reference to specific embodiments below.

[0076] Example 1

[0077] like Figure 1 As shown, this embodiment provides a chip-type conductive polymer tantalum capacitor, which can improve the bonding strength between the dielectric layer and the conductive polymer cathode layer, between the conductive polymer cathode layers, and between the conductive polymer cathode layer and the graphite silver paste layer. The preparation method of the tantalum capacitor includes (see Figure 2 ):

[0078] Step 1, immersing the anode tantalum block with Ta2O5 formed on the surface after energization into the guide layer treatment solution A;

[0079] Step 2, coating the anode tantalum block processed in step 1 with an inner layer, a transition layer, and an outer layer of a conductive polymer as a whole conductive polymer cathode layer;

[0080] Step 3, coating the outer layer of the conductive polymer cathode layer of the anode tantalum block treated in step 2 with a graphene composite material to form a graphene composite material layer;

[0081] Step 4, coating the outer surface of the graphene composite material layer of the anode tantalum block treated in step 3 with graphite and silver paste to form a graphite silver paste layer, and leading out the positive and negative electrodes through a lead frame to form a tantalum core group;

[0082] Step 5, coating the surface of the tantalum core group formed after the treatment in step 4 with a moisture barrier layer and molding to form a chip-type conductive polymer tantalum capacitor.

[0083] In step 1 of the above method, the guide layer treatment liquid A can be a mixture of a polyhydroxyl functional polymer and a solvent, wherein the polyhydroxyl functional polymer adopts a polymer containing repeating units of at least two hydroxyl groups and its copolymer, such as polyethylene glycol, polyvinyl alcohol, polyvinyl alcohol copolymer, polysaccharide, etc.; or a mixture of an organic functional silane and a solvent, wherein the organic functional silane adopts one or more of aminosilane, vinyl silane, epoxy silane, mercaptosilane, acryloxypropyl silane, etc.; the solvent used is one or more of water, alcohols, ethers, and ketones, such as methanol, ethanol, propanol, isopropanol, methyl ether, ethyl ether, methyl tert-butyl ether, anisole, acetone, butanone, etc.

[0084] The specific treatment of the above step 1 is: immerse the anode tantalum block with a Ta2O5 dielectric layer formed on the surface into the treatment solution A at a speed of 0.03mm-0.5mm / s for 1-15min, place it at 20℃-30℃ for 5-15min, and dry it at 50℃-150℃ for 30min; in one embodiment, the content of polyvinyl alcohol or polyethylene glycol and its copolymer is 0.01wt.%-1wt.%, and in some other embodiments, the content of polyvinyl alcohol or polyethylene glycol and its copolymer is 0.05wt.%-5wt.%; in one embodiment, the content of organic functional silane is 0.005wt.%-2wt.%, and in some embodiments, the content of organic functional silane is about 0.1wt.%-1.5wt.%. This method can obtain a uniform thickness of the adhesive guide layer to ensure its mechanical strength.

[0085] In step 2 of the above method, the conductive polymer dispersion used for coating the conductive polymer consists of polyanion composite particles, wherein the polyanion is a PSS copolymer.

[0086] The conductive polymer layer is divided into a polymer inner layer, a transition layer, and an outer layer, each layer including several polymer sublayers, which are formed by impregnating dispersions of different particle sizes and drying. In the conductive polymer outer layer, there is a crosslinking layer between each adjacent conductive polymer sublayer to improve the interlayer adhesion and the edge and corner adhesion rate; the crosslinking layer includes: polycation salts, compounds or amine compounds; more preferably, the crosslinking layer uses an amino compound containing at least two amine groups and its derivatives; the crosslinking layer can also contain a strong acid or a weak acid as a counter ion, such as monohydrated toluenesulfonic acid, acetic acid, phosphoric acid, etc.

[0087] In the above step 2, the specific preparation method of the conductive polymer cathode layer includes:

[0088] Step 21, immersing the anode tantalum block with a dielectric layer coating formed on the surface in a dispersion of poly (3,4-ethylenedioxythiophene) particles with a solid content of about 0.5% to 2.5% and a particle size of 20 to 30 nm at a speed of 0.05 to 0.5 mm / s under vacuum for 1 to 10 minutes, and drying it under a vacuum environment of 120° C. to 150° C. for 20 minutes, and repeating this step 5 to 15 times to perform capacity extraction;

[0089] Step 22, immersing the above-mentioned anode tantalum block in a dispersion of poly (3,4-ethylenedioxythiophene) particles with a solid content of about 1% to 5% and a particle size of 30 to 50 nm at a speed of 0.05 to 0.5 mm / s under vacuum for 1 to 10 minutes, and drying it under a vacuum environment of 120° C. to 150° C. for 20 minutes. This step is repeated 2 to 8 times to enhance the stability of the cathode layer;

[0090] Step 23, immerse the above-mentioned anode tantalum block in a dispersion of poly (3,4-ethylenedioxythiophene) particles with a solid content of about 2% to 10% and a particle size of 50 to 100 nm at a speed of 0.05 to 0.5 mm / s under vacuum for 1 to 10 minutes, and dry it in a vacuum environment at 120°C to 150°C for 30 minutes, then immerse the dried core in a cross-linking agent for 1 to 5 minutes, and dry it at 120°C to 150°C for 20 minutes, and repeat this step alternately 2 to 6 times to form a continuous and dense polymer film layer of suitable thickness.

[0091] In the above step 3, the added graphene composite material layer has excellent electrical conductivity, thermal conductivity and good toughness, and can transfer the heat generated inside the tantalum capacitor to the outside in time, thereby improving the thermomechanical stability and strength of the tantalum capacitor. Specifically, the graphene composite material is composed of: graphene and its derivatives, a cross-linking agent, a dispersant and a solvent. The graphene can be reduced graphene oxide, and its functional groups can be selectively chemically modified to improve its hydrophilicity, suitable functional groups, such as: carboxyl, amine, hydroxyl, thiol, etc. The cross-linking agent can improve the adhesion of graphene, which can be a polycationic salt, compound or amine compound. The solvent can be one or more of water, aliphatic alcohols, and ketones. The dispersant adopts a surfactant having two opposite properties, hydrophilicity and lipophilicity, including: inorganic dispersants and organic dispersants; among them, the inorganic dispersants include silicates (such as water glass) and alkali metal phosphates (such as sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate, etc.); the organic dispersants include triethylhexyl phosphate, sodium dodecyl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum, fatty acid polyethylene glycol esters, etc.

[0092] The anode tantalum block is immersed in a graphene composite material system C with a solid content of 0.1% to 3% and a particle size of 50 to 500 nm, and dried at 120° C. to 150° C. for 20 minutes, and this step is repeated 1 to 2 times.

[0093] In the above step 5, the moisture-proof barrier layer is a protective film formed by treating a moisture-proof treatment liquid composed of a hydrophobic material and an auxiliary agent, and the moisture-proof treatment liquid is usually a silane, acrylic, polyurethane, epoxy resin, etc. Among them, the hydrophobic resin content of the hydrophobic material is 10% to 60%, and the hydrophobic resin content of the hydrophobic material in some embodiments is 20% to 80%. The treatment for forming the moisture-proof barrier layer is: immersing the tantalum core group in a moisture-proof treatment liquid to treat the surface of the tantalum core group, and using a solvent to clean the excess part, and then placing the tantalum core group at 120°C to 150°C for curing for 1 hour.

[0094] The beneficial effects of this embodiment are as follows: the tantalum capacitor performs interface treatment between the dielectric layer and the conductive polymer cathode layer, between the outer layers of the conductive polymer cathode layer, and between the outer layer of the conductive polymer cathode layer and the graphite silver paste layer, thereby increasing the bonding force and mechanical strength between the interfaces and improving the interface stability. The conductive polymer cathode layer is formed by adopting a three-stage formation process of inner layer, transition layer, and outer layer, which is more conducive to forming a continuous and dense conductive polymer layer. The core group after coating is subjected to moisture-proof treatment, so that the capacitor formed by this process has enhanced heat and electricity resistance and can maintain the stability of the capacitor ESR.

[0095] Example 2

[0096] like Figure 1As shown, in this embodiment, a 16V 220μF E-shell tantalum electrolytic capacitor product is taken as an example to illustrate the preparation method of the present invention, comprising:

[0097] First, tantalum powder with a specific capacity of 35000 μF·V / g was uniformly mixed with a 3wt.% binder, and after the powder was dried, it was pressed into an anode sample with a sample size of 4.8×3.3×3.3 and a weight of 314 mg, and sintered at 1450°C to obtain a tantalum block, and then the obtained tantalum block was immersed in a phosphoric acid solution with a conductivity of 8.4 mS / cm and oxidized to 48V for anodization treatment;

[0098] The tantalum anode block obtained by the above anodization treatment is immersed in a polyethylene glycol guide layer treatment solution A with a content of 0.1wt.% at a speed of 0.3mm / s for 5min, placed at 20℃~30℃ for 5min, and dried at 150℃ for 30min;

[0099] The anode tantalum block coated with the dielectric layer is immersed in a dispersion of poly (3,4-ethylenedioxythiophene) particles with a solid content of 1.5% and a particle size of 20 to 30 nm at a speed of 0.3 mm / s under vacuum for 5 minutes, and dried under a vacuum environment of 120° C. for 20 minutes. This step is repeated 10 times;

[0100] The treated anode tantalum block is immersed in a dispersion of poly(3,4-ethylenedioxythiophene) particles having a solid content of 2% and a particle size of 30-50 nm at a speed of 0.3 mm / s under vacuum for 5 minutes, and dried under a vacuum environment of 120° C. for 20 minutes. This step is repeated 5 times;

[0101] The treated tantalum anode block is immersed in a dispersion of poly(3,4-ethylenedioxythiophene) particles having a solid content of 3% and a particle size of 50 to 100 nm at a speed of 0.15 mm / s under vacuum for 5 minutes, and dried at 50 to 150° C. in a vacuum environment for 30 minutes. The dried tantalum anode block is then immersed in a cross-linking agent for 5 minutes, and dried at 120° C. for 20 minutes. This step is repeated alternately 4 times.

[0102] The anode tantalum block is immersed in a water mixture (i.e., a graphene composite material system) in which graphene oxide is dispersed and has a solid content of 2% and a viscosity of 1200 mPa·s. After coating, the anode tantalum block is dried at 125° C. for 20 min, and this process is repeated twice;

[0103] The treated tantalum anode block is impregnated with graphite and silver paste and solidified to form a graphite silver paste layer;

[0104] The graphite silver paste layer is installed on a lead frame to lead out positive and negative electrodes to obtain a tantalum core group of a tantalum capacitor;

[0105] The tantalum core group is immersed in a 45wt.% methyl silicone oil moisture-proof treatment liquid to treat the surface of the tantalum core group, and the excess part is cleaned with a solvent, and then the tantalum core group is placed at 150° C. for curing for 1 hour. After curing, it is naturally cooled at room temperature to form a protective film on the surface of the tantalum core group as a moisture-proof barrier layer;

[0106] The core group is molded and packaged to form a capacitor.

[0107] In the coating process, 16V 220E conductive polymer tantalum capacitors were selected, and 500 were randomly selected for processing comparison according to the method of this embodiment 2 and the process of the prior art, and the qualified rates of the two were compared. At the same time, 100 were randomly selected for accelerated life test (125°C, 1.2 times the rated voltage for 2000h continuous life test), and the comparative structural results are shown in Table 1.

[0108] Table 1

[0109]

[0110] It can be seen from the above comparison that the tantalum capacitors prepared by the present invention have a higher product qualification rate than the tantalum capacitors prepared by the prior art, and have more stable performance, longer life and higher reliability.

[0111] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims. The information disclosed in the background technology section of this article is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or in any form that the information constitutes prior art known to those skilled in the art.

Claims

1. A chip-type conductive polymer tantalum capacitor, characterized in that: include: Anode tantalum block, dielectric layer, adhesive guide layer, conductive polymer cathode layer, graphene composite material layer, graphite silver paste layer, moisture barrier layer, packaging shell, positive lead and negative lead; wherein, The outer surface of the anode tantalum block is coated with the dielectric layer, the adhesive guide layer, the conductive polymer cathode layer, the graphene composite material layer and the graphite silver paste layer in sequence from the inside to the outside; The positive electrode lead is electrically connected to the anode tantalum block, and the negative electrode lead is electrically connected to the graphite silver paste layer to form a tantalum core group; The moisture-proof barrier layer is coated outside the tantalum core group; The tantalum core group package covering the moisture-proof barrier layer is arranged in the package shell; The positive electrode lead is led out from one side of the packaging shell to the outside of the packaging shell; The negative electrode lead is led out from the other side of the packaging shell to the outside of the packaging shell; The conductive polymer cathode layer comprises: an inner layer, a transition layer and an outer layer; The inner layer of the conductive polymer cathode layer is a capacity extraction layer formed by depositing a dispersion of poly 3,4-ethylenedioxythiophene particles with an average particle size of 20 to 30 nm; The transition layer of the conductive polymer cathode layer is an intermediate transition layer formed by depositing a dispersion of poly 3,4-ethylenedioxythiophene particles with an average particle size of 30 to 50 nm; The outer layer of the conductive polymer cathode layer is a thickness-increasing layer formed by depositing a dispersion of poly 3,4-ethylenedioxythiophene particles having an average particle size of 50 to 100 nm; The hydrophobic material used in the moisture-proof barrier layer is any one of silane material, acrylic material, polyurethane material and epoxy resin material.

2. The chip-type conductive polymer tantalum capacitor according to claim 1, characterized in that: The adhesive guide layer is a thin film layer formed of one or more of a polyhydroxyl functional monomer, a polyhydroxyl functional polymer, an organic functional silane or a hydrolyzate thereof.

3. The chip-type conductive polymer tantalum capacitor according to claim 2, characterized in that: The polyhydroxyl functional polymer is a polymer containing at least two hydroxyl repeating units and a copolymer thereof; The organofunctional silane is one or more of aminosilane, vinylsilane, epoxysilane and the like.

4. The chip-type conductive polymer tantalum capacitor according to any one of claims 1 to 3, characterized in that: The graphene contained in the graphene composite material layer is reduced graphene oxide, and the average cross-sectional size of the graphene is not greater than 500nm; The moisture-proof barrier layer is a moisture-proof layer formed by curing a hydrophobic material and an auxiliary agent.

5. The chip-type conductive polymer tantalum capacitor according to claim 1, characterized in that: The outer layer of the conductive polymer cathode layer is composed of multiple sublayers, and a cross-linking layer is provided between each sublayer; A cross-linking layer is provided between the outer layer and the transition layer.

6. The chip-type conductive polymer tantalum capacitor according to claim 5, characterized in that: The cross-linked layer is made of polycationic salts, amine compounds or derivatives thereof.

7. A method for preparing a chip-type conductive polymer tantalum capacitor, characterized in that: The method for preparing the chip-type conductive polymer tantalum capacitor according to any one of claims 1 to 6 comprises: Step 1, immersing the anode tantalum block with a Ta2O5 film formed on the surface after energization into the guide layer treatment solution A for 1 to 15 minutes, and drying and forming at 50 to 150° C.; Step 2, immersing the anode tantalum block obtained in step 1 in a dispersion of poly (3,4-ethylenedioxythiophene) particles having a solid content of 0.5% to 2.5% and an average particle size of 20 to 30 nm under vacuum for 1 to 10 minutes, and drying the dispersion under a vacuum environment of 80° C. to 150° C., and repeating this step 5 to 15 times; Step 3, immersing the anode tantalum block obtained in step 2 in a dispersion of poly (3,4-ethylenedioxythiophene) particles having a solid content of 1% to 5% and an average particle size of 30 to 50 nm under vacuum for 1 to 10 minutes, and drying the dispersion under vacuum at 80 to 150° C., and repeating this step 2 to 8 times; Step 4, immersing the anode tantalum block obtained in step 3 in a dispersion of poly 3,4-ethylenedioxythiophene particles having a solid content of 2% to 10% and an average particle size of 50 to 100 nm under vacuum for 1 to 10 minutes, and drying it under a vacuum environment of 80° C. to 150° C., then immersing the dried anode tantalum block in a crosslinking agent B at normal pressure for 1 to 5 minutes, and drying it at 80° C. to 150° C., and repeating this step 2 to 6 times; Step 5, immersing the anode tantalum block obtained in step 4 in a graphene composite material system C having a solid content of 0.05% to 5% and a particle size of 50 to 500 nm, and drying the anode tantalum block at 120° C. to 150° C., and repeating this step 1 to 2 times to obtain an anode tantalum block having an outer layer of a conductive polymer containing a graphene structure; Step 6, impregnating the conductive polymer outer layer of the anode tantalum block obtained in step 5 with graphite and silver paste to form a graphite silver paste layer, and then using a lead frame to lead out the positive and negative electrodes to obtain a tantalum core group; Step 7, coating a moisture-proof barrier layer D on the tantalum core group obtained in step 6, and performing mold packaging to obtain a chip-type conductive polymer tantalum capacitor.

8. The method for preparing a chip-type conductive polymer tantalum capacitor according to claim 7, characterized in that: The guide layer treatment liquid A in step 1 is a treatment liquid formed by mixing any one or more of a polyhydroxyl functional monomer, a polyhydroxyl functional polymer, an organic functional silane or a hydrolyzate thereof with a solvent A; The crosslinking agent B in step 4 is a mixed solution formed by mixing any one of a polycationic salt, a compound, and an amine compound with a solvent B; The graphene composite material system C in step 5 is composed of graphene, an additive and a solvent C, wherein the content of graphene is 0.01wt.% to 10wt.%, the content of solvent C is 75wt.% to 99wt.%, and the rest is the additive.

9. The method for preparing a chip-type conductive polymer tantalum capacitor according to claim 8, characterized in that: The solvent A in the guide layer treatment liquid A is any one or more of water, alcohol solvent, ether solvent and ketone solvent; The solvent B in the cross-linking agent B is any one or more of water, aliphatic alcohol solvents, and ketone solvents; The crosslinking agent in the graphene composite material system C is a polycationic salt, compound or amine compound; the solvent C in the graphene composite material system C is any one or more of water, aliphatic alcohol solvents and ketone solvents.