A ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters and its preparation method and application
Through the synergistic action of Pd, Cu, Zn ternary metal catalysts and the optimization of modified metal elements, the problem of insufficient activity and selectivity of existing catalysts in the synthesis of alkenyl carboxylic acids is solved, and efficient catalytic effect is achieved , activity and selectivity are significantly improved.
Patent Information
- Application Number
- CN202111554509.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-12-17
AI Technical Summary
The existing catalysts have low yield and selectivity in the synthesis of low-carbon alkenyl carboxylic acid esters, making it difficult to meet industrial needs.
Using Pd, Cu, Zn ternary metal catalysts, a highly active and selective catalyst was prepared through the synergistic action of impregnation, precipitation, reduction and co-active components, and the reaction conditions were optimized in the micro reactor to improve the catalytic effect.
The activity and selectivity of the catalyst were significantly improved, with the activity reaching 377.17g/L·h, the selectivity reaching 97.67%, and further increased to 98.23% by adding modified metal elements, which significantly improved the synthesis of low-carbon carboxylic acid alkenyl ester. efficiency.
Smart Images

Figure BDA0003418242350000151 
Figure BDA0003418242350000152 
Figure BDA0003418242350000161
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and relates to a ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters, and a preparation method and application thereof. Background Art
[0002] In the synthesis method of low-carbon carboxylic acid alkenyl ester, low-carbon carboxylic acid alkenyl ester is mainly obtained by gas phase reaction of low-carbon olefins, low-carbon chain carboxylic acids and oxygen, among which supported precious metal catalysts are widely used, and the active component Pd and the alkali metal / alkaline earth metal of the auxiliary active component are loaded on the carrier.
[0003] Invention patent EP0361484A2 discloses a method for preparing a catalyst loaded with a main active component and an auxiliary active component. The specific manufacturing process is as follows: adding a mixed solution of a prepared precious metal and an auxiliary active component, drying, then treating with an alkaline precipitant such as sodium silicate to precipitate the originally water-soluble metal salt into hydroxylated palladium and copper, then reducing it to metallic palladium and copper in a reducing atmosphere to obtain a palladium and copper catalyst, washing, drying, soaking in potassium acetate, and drying to obtain the catalyst. The space-time yield and selectivity of the catalyst obtained by this method are both low.
[0004] Invention patent CN101657259 discloses a method for preparing a catalyst loaded with a main active component noble metal and an auxiliary active component metal. The specific process of manufacturing the auxiliary active component is as follows: (1) Add the prepared noble metal and auxiliary active component mixed solution into a rotating impregnation tank and dry it with hot air; (2) Take a certain amount of alkaline solution such as sodium silicate and add it to the dried catalyst to convert the original water-soluble palladium and gold salts into water-insoluble hydroxylated palladium and gold; (3) Reduce the hydroxylated palladium and gold catalysts in reducing gas, that is, reduce them to metallic palladium and gold catalysts; (4) Wash until there is no chloride ion and dry; (5) Soak in potassium acetate and dry to obtain the catalyst. The space-time yield and selectivity of the catalyst obtained by this method are both low. Summary of the invention
[0005] In order to improve the activity and selectivity of the catalyst, the present invention provides a ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters, and a preparation method and application thereof.
[0006] After a large number of experiments, it was found that the three metals Pd, Cu and Zn can play a good synergistic role in the preparation of catalysts for synthesizing low-carbon carboxylic acid alkenyl esters. Therefore, the present invention firstly develops a ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters, and its components include an active component, a carrier, an auxiliary active component and a modifying component, and the active component is a ternary metal of Pd, Cu and Zn.
[0007] Furthermore, the content of Pd in the catalyst is preferably 1.0 to 10 g / L; the content of Cu is preferably 0.1 to 5.0 g / L; and the content of Zn is preferably 0.1 to 5.0 g / L.
[0008] Optionally, the modified metal element is at least one of IIIA elements and VIII elements, the IIIA element is preferably at least one of B, Ga and In, the VIII element is preferably at least one of Fe, Co, Ni, Ru and Pt, and most preferably at least one of Ga, Fe and Co; the content of the modified component is 0.1 to 1.00 g / L.
[0009] The modified metal element has a good synergistic effect in terms of catalyst activity and selectivity. When the catalyst carrier uses at least one modified metal element of the IIIA element and the VIII element at the same time, a more outstanding technical effect is achieved (see Examples 5-8 for details).
[0010] Optionally, the carrier is a porous material, and the porous material is preferably one of silica, alumina, and silica-alumina; the porous material is in the shape of powder, sphere or particle, preferably sphere.
[0011] The silicon dioxide is not limited to SiO 2 , including silicon dioxide containing impurities.
[0012] Optionally, the auxiliary active component is an alkali metal acetate, and the alkali metal acetate is preferably potassium acetate; the content is preferably 10 to 120 g / L.
[0013] The specific surface area of the carrier substrate is 100 to 500 m 2 / g, and the pore volume is 0.85~1.40ml / g.
[0014] Secondly, the preparation method of the ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters comprises the following specific steps:
[0015] (a) impregnating the support with a mixed impregnation solution containing salts of Pd, Cu, Zn and a modified metal compound to obtain a catalyst precursor I;
[0016] (b) using an alkaline solution to convert the salt containing Pd, Cu, and Zn from a solution into a precipitate to obtain a catalyst precursor II;
[0017] (c) washing the catalyst precursor II in step (b) with water until it becomes neutral;
[0018] (d) reducing the combined Pd, Cu, Zn and modified metal in the precipitate to a metallic state to obtain a catalyst precursor III;
[0019] (e) impregnating the active ingredient solution;
[0020] (f) drying to obtain the catalyst.
[0021] The alkaline solution in step (b) is Na 2 SiO 3 9H 2 O, NaOH, KOH, Na 2 CO 3 One of the following, preferably Na 2 SiO 3 9H 2 O.
[0022] Optionally, in step (d), the reduction method is one of hydrazine hydrate reduction, propylene gas phase reduction, and hydrogen gas phase reduction, preferably hydrazine hydrate reduction.
[0023] Finally, the preparation method of a low-carbon carboxylic acid alkenyl ester described in the present invention is: a catalyst is loaded into a microreactor, a nitrogen leak test is performed, olefins and nitrogen are introduced after no leaks are found, the temperature is raised to a catalyst bed temperature of 120°C, an organic acid and water are introduced, oxygen is added after 20 minutes, and oxygen is introduced after 30 minutes to prepare a low-carbon carboxylic acid alkenyl ester.
[0024] The oxygen injection refers to the stage before the reaction, in which the oxygen flow rate is slowly increased to the flow rate required for the reaction to prevent a large amount of oxygen from being introduced instantly to react with olefins and cause the reactor to overheat.
[0025] The amount of catalyst loaded into the microreactor is 10 ml, the flow rate of olefin is 0.5-1.0 mol / h, the flow rate of nitrogen is 0.5-1.0 mol / h, the amount of organic acid introduced is 0.05-0.5 mol / h, the amount of water is 0.1-0.5 mol / h, and the amount of oxygen introduced is 0.05-0.3 mol / h.
[0026] During the reaction, the reaction temperature is 120-180°C, preferably 150-180°C; the reaction pressure is 0.1-1.0 MPa, preferably 0.5-0.9 MPa; the molar ratio is preferably olefin: organic acid: oxygen: water = 1: (0.1-0.3): (0.1-0.2): (0.2-0.4).
[0027] Optionally, the olefin is an olefin having a carbon number less than 6, preferably an unsaturated hydrocarbon having 2 to 4 carbon atoms, more preferably ethylene or propylene.
[0028] Optionally, the organic acid is one of aliphatic organic acids having a carbon number <4, preferably a straight-chain organic acid having 1 to 4 carbon atoms, more preferably acetic acid or propionic acid.
[0029] The content of each component in the reaction product was analyzed by gas chromatography, and the activity and selectivity of the catalyst were calculated according to the following formula:
[0030] Activity = amount of low-carbon carboxylic acid alkenyl ester produced by reaction / catalyst volume * reaction time (g / L*h);
[0031] Selectivity = (the number of moles of acetic acid produced by the reaction to form low-carbon carboxylic acid alkenyl esters / the number of moles of acetic acid consumed by the reaction)*100%.
[0032] Beneficial Effects
[0033] The catalyst prepared by the present invention using three metals, Pd, Cu and Zn, has an activity of 377.17 g / L·h and a selectivity of 97.67%. When the ternary metal catalyst uses at least one modified metal element of the IIIA element and the VIII element at the same time, a more outstanding technical effect is achieved, and the activity can reach 377.77 g / L·h and the selectivity can reach 98.23%, achieving a more outstanding technical effect. DETAILED DESCRIPTION
[0034] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] (1) Spherical SiO 2 The BET specific surface area is 210m 2 / g, and the pore volume is 1.10ml / g.
[0037] (2) The preparation contained 1.0 g Pd(NO 3 ) 2 、0.20g Cu(NO 3 ) 2 and 0.25 g Zn(NO 3 ) 2 The aqueous solution was used to obtain 90 ml of impregnation solution. The solution was impregnated on the support in a rotary single-mouth bottle, and then dried at 40°C by rotary evaporation to obtain catalyst precursor I;
[0038] (3) 150 ml contains 13.6 g Na 2 SiO 3 9H 2The solution of O was added to a rotary single-mouth bottle and fully mixed with the catalyst precursor I, aged for 4 hours, washed with water until neutral, and dried at 40°C using a rotary evaporator to obtain a catalyst precursor II;
[0039] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) is reduced with 90 ml of hydrazine hydrate, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor III;
[0040] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III and dried at 40° C. using a rotary evaporator to obtain the catalyst.
[0041] ICP determination showed that the Pd content of the catalyst was 4.36 g / L, the Cu content was 0.39 g / L, the Zn content was 0.87 g / L, and the potassium acetate content was 23.5 g / L.
[0042] Synthesis of Allyl Acetate:
[0043] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2 The system was fully purged and after the system was heated up, a certain amount of propylene and N 2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.68MPa; the raw material volume space velocity: 2000h -1 ; Raw material composition: propylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0044] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0045] The activity of the catalyst was calculated to be 377.17 g / L·h, and the selectivity to allyl acetate was 97.67%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0046] Example 2
[0047] (1) Spherical SiO 2 The BET specific surface area is 210m 2 / g, and the pore volume is 1.10ml / g.
[0048] (2) The preparation contained 1.0 g Pd(NO3 ) 2 、0.40g Cu(NO 3 ) 2 and 0.25 g Zn(NO 3 ) 2 The aqueous solution was used to obtain 90 ml of impregnation solution. The solution was impregnated on the support in a rotary single-mouth bottle, and then dried at 40°C by rotary evaporation to obtain catalyst precursor I;
[0049] (3) 150 ml contains 13.6 g Na 2 SiO 3 9H 2 The solution of O was added into a rotary single-mouth bottle and fully mixed with the catalyst precursor I, aged for 4 hours, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor II;
[0050] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) is reduced with 90 ml of hydrazine hydrate, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor III;
[0051] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III and dried at 40° C. using a rotary evaporator to obtain the catalyst.
[0052] ICP determination showed that the Pd content of the catalyst was 4.38 g / L, the Cu content was 0.81 g / L, the Zn content was 0.83 g / L, and the potassium acetate content was 23.7 g / L.
[0053] Synthesis of Allyl Acetate:
[0054] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2 After the system is fully purged and heated up, a certain amount of propylene and N 2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.70MPa; the raw material volume space velocity: 2000h -1 ; Raw material composition: propylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0055] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0056] The activity of the catalyst was calculated to be 376.75 g / L·h, and the selectivity to allyl acetate was 97.65%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0057] Example 3
[0058] (1) Spherical SiO 2 The BET specific surface area is 210m 2 / g, and the pore volume is 1.10ml / g.
[0059] (2) The preparation contained 1.0 g Pd(NO 3 ) 2 、0.20g Cu(NO 3 ) 2 and 0.50 g Zn(NO 3 ) 2 The aqueous solution was used to obtain 90 ml of impregnation solution. The solution was impregnated on the support in a rotary single-mouth bottle, and then dried at 40°C by rotary evaporation to obtain catalyst precursor I;
[0060] (3) 150 ml contains 13.6 g Na 2 SiO 3 9H 2 The solution of O was added into a rotary single-mouth bottle and fully mixed with the catalyst precursor I, aged for 4 hours, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor II;
[0061] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) is reduced with 90 ml of hydrazine hydrate, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor III;
[0062] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III and dried at 40° C. using a rotary evaporator to obtain the catalyst.
[0063] ICP determination showed that the Pd content of the catalyst was 4.41 g / L, the Cu content was 0.40 g / L, the Zn content was 1.59 g / L, and the potassium acetate content was 23.7 g / L.
[0064] Synthesis of Allyl Acetate:
[0065] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2 The system was fully purged and after the system was heated up, a certain amount of propylene and N2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.69MPa; the raw material volume space velocity: 2000h -1 ; Raw material composition: propylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0066] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0067] The activity of the catalyst was calculated to be 376.28 g / L·h, and the selectivity to allyl acetate was 97.12%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0068] Example 4
[0069] (1) Spherical SiO 2 The BET specific surface area is 210m 2 / g, and the pore volume is 1.10ml / g.
[0070] (2) The preparation contained 1.0 g Pd(NO 3 ) 2 、0.40g Cu(NO 3 ) 2 and 0.50 g Zn(NO 3 ) 2 The aqueous solution was used to obtain 90 ml of impregnation solution. The solution was impregnated on the support in a rotary single-mouth bottle, and then dried at 40°C by rotary evaporation to obtain catalyst precursor I;
[0071] (3) 150 ml contains 13.6 g Na 2 SiO 3 9H 2 The solution of O was added into a rotary single-mouth bottle and fully mixed with the catalyst precursor I, aged for 4 hours, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor II;
[0072] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) is reduced with 90 ml of hydrazine hydrate, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor III;
[0073] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III and dried at 40° C. using a rotary evaporator to obtain the catalyst.
[0074] ICP determination showed that the Pd content of the catalyst was 4.37 g / L, the Cu content was 0.78 g / L, the Zn content was 1.62 g / L, and the potassium acetate content was 23.9 g / L.
[0075] Synthesis of Vinyl Acetate:
[0076] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2 The system is fully purged and after the system is heated up, a certain amount of ethylene and N 2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.69MPa; the raw material volume space velocity: 2000h -1 ; Raw material composition: ethylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0077] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0078] The activity of the catalyst was calculated to be 375.91 g / L·h, and the selectivity to vinyl acetate was 97.36%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0079] Example 5
[0080] (1) Spherical SiO 2 The BET specific surface area is 210m 2 / g, and the pore volume is 1.10ml / g.
[0081] (2) The preparation contained 1.0 g Pd(NO 3 ) 2 、0.20g Cu(NO 3 ) 2 , 0.25g Zn(NO 3 ) 2 and 0.12gGa(NO 3 ) 3 The aqueous solution was used to obtain 90 ml of impregnation solution. The solution was impregnated on the support in a rotary single-mouth bottle, and then dried at 40°C by rotary evaporation to obtain catalyst precursor I;
[0082] (3) 150 ml contains 13.6 g Na 2 SiO 3 9H 2 The solution of O was added into a rotary single-mouth bottle and fully mixed with the catalyst precursor I, aged for 4 hours, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor II;
[0083] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) is reduced with 90 ml of hydrazine hydrate, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor III;
[0084] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III and dried at 40° C. using a rotary evaporator to obtain the catalyst.
[0085] ICP determination showed that the Pd content of the catalyst was 4.40 g / L, the Cu content was 0.39 g / L, the Zn content was 0.84 g / L, the Ga content was 0.35 g / L, and the potassium acetate content was 23.8 g / L.
[0086] Synthesis of Allyl Acetate:
[0087] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2 After the system is fully purged and heated up, a certain amount of propylene and N 2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.68MPa; the raw material volume space velocity: 2000h -1 ; Raw material composition: propylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0088] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0089] The activity of the catalyst was calculated to be 377.65 g / L·h, and the selectivity to allyl acetate was 97.98%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0090] Example 6
[0091] (1) Spherical SiO 2The BET specific surface area is 210m 2 / g, and the pore volume is 1.10ml / g.
[0092] (2) The preparation contained 1.0 g Pd(NO 3 ) 2 、0.20g Cu(NO 3 ) 2 , 0.25g Zn(NO 3 ) 2 and 0.15 gFe(NO 3 ) 3 The aqueous solution was used to obtain 90 ml of impregnation solution. The solution was impregnated on the support in a rotary single-mouth bottle, and then dried at 40°C by rotary evaporation to obtain catalyst precursor I;
[0093] (3) 150 ml contains 13.6 g Na 2 SiO 3 9H 2 The solution of O was added into a rotary single-mouth bottle and fully mixed with the catalyst precursor I, aged for 4 hours, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor II;
[0094] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) is reduced with 90 ml of hydrazine hydrate, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor III;
[0095] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III and dried at 40° C. using a rotary evaporator to obtain the catalyst.
[0096] ICP determination showed that the Pd content of the catalyst was 4.39 g / L, the Cu content was 0.41 g / L, the Zn content was 0.86 g / L, the Fe content was 0.41 g / L, and the potassium acetate content was 24.0 g / L.
[0097] Synthesis of Allyl Acetate:
[0098] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2 After the system is fully purged and heated up, a certain amount of propylene and N 2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.68MPa; the raw material volume space velocity: 2000h -1; Raw material composition: propylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0099] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0100] The activity of the catalyst was calculated to be 377.77 g / L·h, and the selectivity to allyl acetate was 98.23%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0101] Example 7
[0102] (1) Spherical SiO 2 The BET specific surface area is 210m 2 / g, and the pore volume is 1.10ml / g.
[0103] (2) The preparation contained 1.0 g Pd(NO 3 ) 2 、0.20g Cu(NO 3 ) 2 , 0.25g Zn(NO 3 ) 2 and 0.10gIn(NO 3 ) 3 , 0.15 g Fe(NO 3 ) 2 The aqueous solution was used to obtain 90 ml of impregnation solution. The solution was impregnated on the support in a rotary single-mouth bottle, and then dried at 40°C by rotary evaporation to obtain catalyst precursor I;
[0104] (3) 150 ml contains 13.6 g Na 2 SiO 3 9H 2 The solution of O was added into a rotary single-mouth bottle and fully mixed with the catalyst precursor I, aged for 4 hours, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor II;
[0105] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) is reduced with 90 ml of hydrazine hydrate, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor III;
[0106] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III and dried at 40° C. using a rotary evaporator to obtain the catalyst.
[0107] ICP determination showed that the Pd content of the catalyst was 4.43 g / L, the Cu content was 0.42 g / L, the Zn content was 0.85 g / L, the In content was 0.29 g / L, the Fe content was 0.39 g / L, and the potassium acetate content was 24.1 g / L.
[0108] Synthesis of Allyl Acetate:
[0109] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2 After the system is fully purged and heated up, a certain amount of propylene and N 2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.68MPa; the raw material volume space velocity: 2000h -1 ; Raw material composition: propylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0110] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0111] The activity of the catalyst was calculated to be 377.21 g / L·h, and the selectivity to allyl acetate was 98.14%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0112] Example 8
[0113] (1) Spherical SiO 2 The BET specific surface area is 210m 2 / g, and the pore volume is 1.10ml / g.
[0114] (2) The preparation contained 1.0 g Pd(NO 3 ) 2 、0.20g Cu(NO 3 ) 2 , 0.25g Zn(NO 3 ) 2 and 0.12gGa(NO 3 ) 3 , 0.20g Co(NO 3 ) 2 The aqueous solution was used to obtain 90 ml of impregnation solution. The solution was impregnated on the support in a rotary single-mouth bottle, and then dried at 40°C by rotary evaporation to obtain catalyst precursor I;
[0115] (3) 150 ml contains 13.6 g Na 2 SiO 3 9H 2 The solution of O was added into a rotary single-mouth bottle and fully mixed with the catalyst precursor I, aged for 4 hours, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor II;
[0116] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) is reduced with 90 ml of hydrazine hydrate, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor III;
[0117] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III and dried at 40° C. using a rotary evaporator to obtain the catalyst.
[0118] ICP determination showed that the Pd content of the catalyst was 4.41 g / L, the Cu content was 0.39 g / L, the Zn content was 0.86 g / L, the Ga content was 0.33 g / L, the Co content was 0.57 g / L, and the potassium acetate content was 24.2 g / L.
[0119] Synthesis of Vinyl Acetate:
[0120] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2 The system is fully purged and after the system is heated up, a certain amount of ethylene and N 2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.68MPa; the raw material volume space velocity: 2000h -1 ; Raw material composition: ethylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0121] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0122] The activity of the catalyst was calculated to be 377.53 g / L·h, and the selectivity to vinyl acetate was 97.97%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0123] Example 9
[0124] (1) The particles SiO2 The BET specific surface area is 356m 2 / g, and the pore volume is 1.87ml / g.
[0125] (2) The preparation contained 1.0 g Pd(NO 3 ) 2 、0.20g Cu(NO 3 ) 2 and 0.25 g Zn(NO 3 ) 2 The aqueous solution was prepared to obtain 90 ml of impregnation solution. The impregnation solution was impregnated on the support in a beaker and dried in an oven at 100°C for 12 hours to obtain catalyst precursor I;
[0126] (3) 150 ml contains 13.6 g Na 2 SiO 3 9H 2 The solution of O was added into a rotating single-mouth bottle and fully mixed with the catalyst precursor I, aged for 4 hours, washed with water, and dried in an oven at 100°C for 12 hours to obtain the catalyst precursor II;
[0127] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) was reduced with 90 ml of hydrazine hydrate, washed with water, and dried in an oven at 100° C. for 12 h to obtain a catalyst precursor III;
[0128] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III. After drying in an oven at 100° C. for 12 h, the catalyst was obtained.
[0129] ICP determination showed that the Pd content of the catalyst was 4.38 g / L, the Cu content was 0.41 g / L, the Zn content was 0.82 g / L, and the potassium acetate content was 24.0 g / L.
[0130] Synthesis of Allyl Acetate:
[0131] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2 The system was fully purged and after the system was heated up, a certain amount of propylene and N 2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.68MPa; the raw material volume space velocity: 2000h -1 ; Raw material composition: propylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0132] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0133] The activity of the catalyst was calculated to be 376.78 g / L·h, and the selectivity to allyl acetate was 97.69%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0134] Comparative Example 1
[0135] (1) Spherical SiO 2 The BET specific surface area is 210m 2 / g, and the pore volume is 1.10ml / g.
[0136] (2) The preparation contained 1.0 g Pd(NO 3 ) 2 and 0.20 g Cu(NO 3 ) 2 The aqueous solution was used to obtain 90 ml of impregnation solution. The solution was impregnated on the support in a rotary single-mouth bottle, and then dried at 40°C by rotary evaporation to obtain catalyst precursor I;
[0137] (3) 150 ml contains 13.6 g Na 2 SiO 3 9H 2 The solution of O was added into a rotary single-mouth bottle and fully mixed with the catalyst precursor I, aged for 4 hours, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor II;
[0138] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) is reduced with 90 ml of hydrazine hydrate, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor III;
[0139] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III and dried at 40° C. using a rotary evaporator to obtain the catalyst.
[0140] ICP analysis showed that the Pd content of the catalyst was 4.33 g / L, the Cu content was 0.40 g / L, and the potassium acetate content was 23.9 g / L.
[0141] Synthesis of Allyl Acetate:
[0142] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2After the system is fully purged and heated up, a certain amount of propylene and N 2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.68MPa; the raw material volume space velocity: 2000h -1 ; Raw material composition: propylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0143] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0144] The activity of the catalyst was calculated to be 362.28 g / L·h, and the selectivity to allyl acetate was 94.58%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0145] Comparative Example 2
[0146] (1) Spherical SiO 2 The BET specific surface area is 210m 2 / g, and the pore volume is 1.10ml / g.
[0147] (2) The preparation contained 1.0 g Pd(NO 3 ) 2 and 0.25 g Zn(NO 3 ) 2 The aqueous solution was used to obtain 90 ml of impregnation solution. The solution was impregnated on the support in a rotary single-mouth bottle, and then dried at 40°C by rotary evaporation to obtain catalyst precursor I;
[0148] (3) 150 ml contains 13.6 g Na 2 SiO 3 ·9H2O solution was added to a rotary single-mouth bottle and fully mixed with catalyst precursor I, aged for 4 hours, washed with water, and dried at 40°C by rotary evaporation to obtain catalyst precursor II;
[0149] (4) Use a solution of 5% (in N 2 H 4 ·H 2 O weight ratio) is reduced with 90 ml of hydrazine hydrate, washed with water, and dried at 40° C. using a rotary evaporator to obtain a catalyst precursor III;
[0150] (5) 2.5 g of potassium acetate was dissolved in pure water to obtain 90 ml of the impregnation solution, which was impregnated on the precursor III and dried at 40° C. using a rotary evaporator to obtain the catalyst.
[0151] ICP analysis showed that the Pd content of the catalyst was 4.42 g / L, the Zn content was 0.82 g / L, and the potassium acetate content was 24 g / L.
[0152] Synthesis of Vinyl Acetate:
[0153] 10 ml of catalyst was loaded into a fixed bed reactor and heated with N 2 After leak testing, use N 2 The system is fully purged and after the system is heated up, a certain amount of ethylene and N 2 The mixture is heated to a catalyst bed temperature of 120°C, acetic acid and water are added, the temperature is continued to rise, oxygen is added, the reaction temperature is controlled at 172°C, the reaction pressure is 0.68MPa; the raw material volume space velocity: 2000h -1 ; Raw material composition: ethylene / acetic acid / oxygen / water (molar ratio) = 1 / 0.18 / 0.2 / 0.3. After the reaction was continued for 100 hours, the reaction was stopped.
[0154] Product analysis: The reaction mixture obtained from the above reaction was cooled, decompressed, separated, and the liquid phase was analyzed by gas chromatography-mass spectrometry.
[0155] The activity of the catalyst was calculated to be 358.07 g / L·h, and the selectivity to vinyl acetate was 95.19%. For comparison purposes, the carrier modification conditions and the main preparation conditions of the catalyst are listed in Table 1, and the physical properties and catalytic performance of the catalyst are listed in Table 2.
[0156] Table 1 Catalyst preparation and modification data
[0157]
[0158] Table 2 Catalyst properties and evaluation data
[0159]
[0160]
[0161] By comparing the examples, it can be found that the activity and selectivity of the Pd, Zn and Pd, Cu binary metal catalysts impregnated separately are quite different from those of the Pd, Cu, Zn ternary metal catalyst of the present invention, and after adding the modified metal to the Pd, Cu, Zn ternary metal catalyst, its activity and selectivity are further improved. This shows that there is a good synergistic effect between Pd, Cu, and Zn, which can act as a synergistic active component to catalyze, and the modified metal element also has a promoting effect on the catalyst activity and selectivity.
[0162] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters, comprising an active component, a carrier, a co-active component and a modifying component, characterized in that: The active components include metals Pd, Cu, and Zn; the modified metal element is at least one of IIIA elements and VIII elements; wherein the IIIA element is at least one of B, Ga, and In; the VIII element is at least one of Fe, Co, Ni, Ru, and Pt; the auxiliary active component is an alkali metal acetate; The ternary metal catalyst is prepared by the following method: (a) impregnating the support with a mixed impregnation solution containing salts of Pd, Cu, Zn and a modified metal compound to obtain a catalyst precursor I; (b) using an alkaline solution to convert the salt containing Pd, Cu, and Zn from a solution into a precipitate to obtain a catalyst precursor II; (c) washing the catalyst precursor II in step (b) with water until it becomes neutral; (d) reducing the combined Pd, Cu, Zn and modified metal in the precipitate to a metallic state to obtain a catalyst precursor III; (e) impregnating the active ingredient solution; (f) drying to obtain the catalyst.
2. A ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters according to claim 1, characterized in that: The content of Pd in the catalyst is 1.0-10 g / L; the content of Cu is 0.1-5.0 g / L; and the content of Zn is 0.1-5.0 g / L.
3. A ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters according to claim 1, characterized in that: The IIIA element is selected from Ga, and the VIII element is selected from Fe or Co; the content of the modified component is 0.1-1.00 g / L.
4. A ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters according to claim 1, characterized in that: The carrier is a porous material, and the porous material is selected from one of silica, alumina, and silica-alumina; the porous material is in the shape of powder, sphere, and particle.
5. A ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters according to claim 4, characterized in that: The porous material is spherical in shape.
6. A ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters according to claim 1, characterized in that: The alkali metal acetate is potassium acetate.
7. A ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters according to claim 6, characterized in that: The content of the auxiliary active component is 10-120 g / L.
8. A method for preparing a ternary metal catalyst for synthesizing low-carbon carboxylic acid alkenyl esters, characterized in that: The specific steps are: (a) impregnating the support with a mixed impregnation solution containing salts of Pd, Cu, Zn and a modified metal compound to obtain a catalyst precursor I; (b) using an alkaline solution to convert the salt containing Pd, Cu, and Zn from a solution into a precipitate to obtain a catalyst precursor II; (c) washing the catalyst precursor II in step (b) with water until it becomes neutral; (d) reducing the combined Pd, Cu, Zn and modified metal in the precipitate to a metallic state to obtain a catalyst precursor III; (e) impregnating the active ingredient solution; (f) drying to obtain the catalyst; Wherein, the modified metal element is at least one of IIIA element and VIII element; wherein, the IIIA element is selected from at least one of B, Ga and In; the VIII element is selected from at least one of Fe, Co, Ni, Ru and Pt; and the auxiliary active component is alkali metal acetate.
9. The method for preparing a ternary metal catalyst according to claim 8, characterized in that: The solute of the alkaline solution in step (b) is one of Na2SiO3·9H2O, NaOH, KOH, and Na2CO3; in step (d), the reduction method is one of hydrazine hydrate reduction, propylene gas phase reduction, and hydrogen gas phase reduction.
10. The method for preparing a ternary metal catalyst according to claim 9, characterized in that: The solute of the alkaline solution in step (b) is Na2SiO3·9H2O.
11. The method for preparing a ternary metal catalyst according to claim 9, characterized in that: In the step (d), the reduction method is hydrazine hydrate reduction.
12. A method for preparing low-carbon carboxylic acid alkenyl esters, characterized in that: A ternary metal catalyst according to any one of claims 1 to 7 or a catalyst prepared by the preparation method according to any one of claims 8 to 11 is loaded into a microreactor, and a nitrogen test is performed. After no leak is found, olefins and nitrogen are introduced, and the temperature is raised at the same time, and organic acids and water are introduced. Oxygen is first added and then oxygen is introduced to prepare low-carbon carboxylic acid alkenyl esters.
13. The method for preparing a low-carbon carboxylic acid alkenyl ester according to claim 12, characterized in that: The amount of catalyst loaded into the microreactor is 10 ml, the flow rate of olefin is 0.5-1.0 mol / h, the flow rate of nitrogen is 0.5-1.0 mol / h, the temperature is raised to the catalyst bed temperature reaching 120° C., the amount of organic acid introduced is 0.05-0.5 mol / h, the amount of water is 0.1-0.5 mol / h, and the amount of oxygen introduced is 0.05-0.3 mol / h; during the reaction process, the reaction temperature is controlled at 120-180° C.; the reaction pressure is 0.1-1.0 MPa.
14. The method for preparing a low-carbon carboxylic acid alkenyl ester according to claim 13, characterized in that: The reaction temperature is controlled at 150-180°C during the reaction.
15. The method for preparing a low-carbon carboxylic acid alkenyl ester according to claim 13, characterized in that: During the reaction, the reaction pressure is controlled at 0.5-0.9 MPa.
16. The method for preparing a low-carbon carboxylic acid alkenyl ester according to claim 13, characterized in that: The molar ratio of olefin: organic acid: oxygen: water is 1: (0.1-0.3): (0.1-0.2): (0.2-0.4).
17. The method for preparing a low-carbon carboxylic acid alkenyl ester according to claim 12, characterized in that: The olefin is an olefin with a carbon number less than 6; the organic acid is an aliphatic organic acid with a carbon number less than 4.
18. The method for preparing a low-carbon carboxylic acid alkenyl ester according to claim 17, characterized in that: The olefin is an unsaturated hydrocarbon having 2 to 4 carbon atoms.
19. The method for preparing a low-carbon carboxylic acid alkenyl ester according to claim 18, characterized in that: The olefin is ethylene or propylene.
20. The method for preparing a low-carbon carboxylic acid alkenyl ester according to claim 17, characterized in that: The organic acid is a straight-chain organic acid having 1 to 4 carbon atoms.
21. The method for preparing a low-carbon carboxylic acid alkenyl ester according to claim 20, characterized in that: The organic acid is acetic acid or propionic acid.