Coated tool and cutting tool equipped with the same
By adopting the structure of Ti intermediate layer and Al2O3 layer in the coated tool, combined with the design of multiple protrusions, the problem that the coated tool is easy to break during high-efficiency cutting processing is solved, and higher breakage resistance and cost are achieved. Film properties extend the service life of the tool.
Patent Information
- Application Number
- CN202080052804.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-07-28
AI Technical Summary
Existing coated tools are prone to coating chipping and peeling due to large impacts during high-efficiency cutting, making it difficult to meet the requirements for chipping resistance.
A coating structure with a Ti intermediate layer and an Al2O3 layer is adopted. The Al2O3 layer is located far away from the substrate and is connected to the intermediate layer. The intermediate layer has multiple protrusions, at least one of which is a composite protrusion. The average number of the second protrusions of the composite protrusions is 1.4. Hereinafter, it is formed by chemical vapor deposition method.
Significantly improves the chipping resistance and film-forming properties of the coating, extending the service life of the tool.
Smart Images

Figure CN114173968B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a coated tool having a coating on the surface of a substrate and a cutting tool having the same. Background Art
[0002] It is known that a substrate such as cemented carbide, cermet, or ceramic has Al laminated thereon via a bonding film. 2 O 3 Coated tools such as cutting tools made of a layer of coating.
[0003] With the recent high efficiency of cutting processing, cutting tools are increasingly used for heavy-duty intermittent cutting where the cutting edge is subjected to large impact. Under such harsh cutting conditions, the coating is subjected to large impact, which easily causes the coating to break and peel off. Therefore, in addition to wear resistance, the coating is also required to have improved breakage resistance.
[0004] In order to solve such a problem, Patent Document 1 describes a method for 2 O 3 The interface where the layers meet is provided with a protrusion whose front end is bent into a hook shape.
[0005] In addition, Patent Documents 2 and 3 describe that 2 O 3 A composite protrusion is arranged at the interface where the layers meet, and the composite protrusion has a plurality of second protrusions on the side of a first protrusion extending in the stacking direction of the coating layer.
[0006] Among them, the front ends of the protrusions and composite protrusions described in Patent Documents 1 and 2 are obtuse, forming a shape with poor film-forming properties. In addition, the composite protrusions described in Patent Documents 2 and 3 have a large number of second protrusions on the first protrusion, and are also formed into a shape with poor film-forming properties.
[0007] Prior Art Literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2004-74324
[0010] Patent Document 2: U.S. Patent Publication No. 2013 / 0149527
[0011] Patent Document 3: Japanese Patent Application Publication No. 2009-166216 Summary of the invention
[0012] Provided is a coated tool having excellent fracture resistance.
[0013] The coated tool of the present invention comprises a substrate and a coating layer located on the surface of the substrate. The coating layer comprises an intermediate layer containing Ti and Al 2 O 3 The Al 2 O 3 The layer is located at a position farther from the substrate than the intermediate layer and is in contact with the intermediate layer. 2 O 3 A plurality of first protrusions protruding from a layer. At least one of the plurality of first protrusions is a composite protrusion having a second protrusion protruding in a direction intersecting with the protruding direction of the first protrusion. In the composite protrusion, the average number of the second protrusions is 1.4 or less.
[0014] The cutting tool of the present invention comprises: a tool holder extending from a first end toward a second end and having a groove on the first end side; and the above-mentioned coated tool located in the groove. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a schematic perspective view showing an example of a coated tool according to the present invention.
[0016] Figure 2 It is used to illustrate Figure 1 Schematic diagram of the composition of the cross section of the coating in a coated tool.
[0017] Figure 3 The intermediate layer and Al 2 O 3 An enlarged view of the main structure near the layer.
[0018] Figure 4 The intermediate layer and Al 2 O 3 An enlarged view of the main structure near the layer.
[0019] Figure 5 The intermediate layer and Al 2 O 3 An enlarged view of the main structure near the layer.
[0020] Figure 6 It is a top view showing an example of the cutting tool of the present invention. DETAILED DESCRIPTION
[0021] <Coated tools>
[0022] The coated tool of the present invention has Figure 1In the example shown, the main surface is generally in the shape of a quadrilateral plate. However, it is not limited to this shape. The coated tool 1 has a first surface 2 and a second surface 3, and has a cutting edge 4 on at least a portion of the portion where the first surface 2 and the second surface 3 intersect. The first surface 2 is a surface called a rake face, and the second surface 3 is a surface called a flank face. Therefore, it can also be said that there is a cutting edge 4 on at least a portion of the portion where the rake face 2 and the flank face 3 intersect.
[0023] In addition, if Figure 2 As shown in the schematic diagram for explaining the cross-sectional structure of the coating layer 7 of the coated tool 1 , the coated tool 1 includes a base body 5 and a coating layer 7 located on the surface of the base body 5 .
[0024] The material of the substrate 5 constituting the coated tool 1 may be cemented carbide, ceramic or metal. As a cemented carbide, it may be a cemented carbide containing ferrous metals such as tungsten carbide (WC), cobalt (Co) and nickel (Ni). As another cemented carbide, it may be a Ti-based metal ceramic containing ferrous metals such as titanium carbonitride (TiCN), cobalt (Co) and nickel (Ni). Ceramics may be Si 3 N 4 、Al 2 O 3 , diamond, cubic boron nitride (cBN). The metal may be carbon steel, high speed steel, alloy steel. Among the above materials, when used as a coated tool 1, the substrate 5 is made of cemented carbide or metal ceramics, which has good fracture resistance and wear resistance.
[0025] The coating 7 has an intermediate layer 9 containing Ti and Al 2 O 3 Layer 11. Al 2 O 3 The layer 11 is in contact with the intermediate layer 9 at a position of the intermediate layer 9 that is remote from the base body 5 .
[0026] The intermediate layer 9 of the coated tool 1 of the present invention is a layer containing Ti, and may contain, for example, TiN, TiC, TiNO, etc. In addition, for example, it may contain Ti, C, and N. In other words, the intermediate layer 9 may contain TiCN crystals. In addition, the intermediate layer 9 may contain, for example, Ti, C, N, and O. In other words, the intermediate layer 9 may contain TiCNO crystals. If it has such a structure, Al 2 O 3 The layer 11 has excellent bonding properties with the intermediate layer 9 .
[0027] The coated tool 1 of the present invention, such as Figure 3 As shown, with an orientation toward Al 2 O 3 The layer 11 has a plurality of first protrusions 13 protruding therefrom.
[0028] The first protrusion 13 has a base 13a as a protruding start point of the first protrusion 13. In addition, the first protrusion 13 has a front end 13b at a position farthest from the base 5. The first protrusion 13 extends from the base 13a toward the front end 13b. The first protrusion 13 typically has a triangular shape.
[0029] The base portion 13a refers to a position of the first protrusion 13 close to the base 5. In other words, the base portion 13a may be the base of the triangle formed by the first protrusion 13.
[0030] Also, in the coated tool 1 of the present invention, the first protrusion 13, such as Figure 3 , 4 As shown, the tip 13 b is an acute angle and has a height of 10 nm or more, which means that the ratio of the average height of the plurality of first protrusions 13 to the average width of the bases 13 a of the plurality of first protrusions 13 is 0.6 or more.
[0031] like Figure 3 As shown, in the coated tool 1 of the present invention, at least one of the plurality of first protrusions 13 is a composite protrusion 17, and the composite protrusion 17 has a second protrusion 15 protruding in a direction intersecting with the protruding direction of the first protrusion 13. In the coated tool 1 of the present invention, all the first protrusions 13 may be composite protrusions 17. Hereinafter, the first protrusions 13 having the second protrusions 15 are referred to as composite protrusions 17.
[0032] In addition, the so-called second protrusion 15 in the coated tool 1 of the present invention has a height of 10 nm or more from the center of the base 15a of the second protrusion 15, which is the protrusion starting point of the second protrusion 15, to the tip 15b of the second protrusion 15. In other words, the minute concavoconvexities existing on the side surface of the first protrusion 13 are not treated as the second protrusion 15 in the coated tool 1 of the present invention.
[0033] In the coated tool 1 of the present invention, the average number of the second protrusions 15 of the composite protrusions 17 is less than 1.4. In addition, the average number of the second protrusions 15 of the composite protrusions 17 can be the average value of 50 composite protrusions 17. 2 O 3 The film forming property of the layer 11 is excellent, and the intermediate layer 9 and the Al 2 O 3 The bonding property of the layer 11 is excellent. In addition, since the composite protrusions 17 include the second protrusions 15, the lower limit of the average number does not include 1.
[0034] In the coated tool 1 of the present invention, the average number of the second protrusions 15 of the composite protrusions 17 may be 1.2 or less. 2 O 3The bonding property of layer 11 is more excellent.
[0035] The average number of the second protrusions 15 of the composite protrusions 17 can be measured, for example, by taking 30,000-fold photographs using a scanning electron microscope and a transmission electron microscope. The number of photographs taken can be appropriately determined according to the number of composite protrusions 17 present. In addition, the other components of the coated tool of the present invention can also be measured in the same manner.
[0036] The ratio of the average height of the second protrusions 15 to the average width of the base 15a of the second protrusions 15 in the coated tool 1 of the present invention may be greater than the ratio of the average height of the plurality of first protrusions 13 to the average width of the base 13a of the plurality of first protrusions 13. The ratio of the average height of the second protrusions 15 to the average width of the base 15a of the second protrusions 15 is the value obtained by dividing the average height from the center of the base 15a of the second protrusions 15 to the front end 15b of the second protrusions 15 by the average width of the base 15a of the second protrusions 15. If such a structure is provided, the intermediate layer 9 and the Al 2 O 3 The bonding property of layer 11 is more excellent.
[0037] In the coated tool 1 of the present invention, the ratio of the average height of the plurality of first protrusions 13 to the average width of the bases 13a of the plurality of first protrusions 13 may be 1.2 or less. 2 O 3 The layer 11 has excellent bonding properties.
[0038] The ratio of the average height of the plurality of first protrusions 13 to the average width of the bases 13 a of the plurality of first protrusions 13 may be 1.0 or less.
[0039] In the coated tool 1 of the present invention, the average width of the base 13a of the first protrusion 13 is greater than 10nm and less than 50nm, and the average height of the first protrusion 13 may be greater than 10nm and less than 60nm. 2 O 3 The bonding property of the layer 11 is excellent. In addition, the average width of the base 13a may be 25 nm or more and 45 nm or less. The average height of the first protrusions 13 may be 10 nm or more and 50 nm or less.
[0040] In the coated tool 1 of the present invention, the average angle of the front end 13b of the first protrusion 13 can be greater than 50° and less than 90°. 2 O 3 The film forming property of the layer 11 is excellent, and the intermediate layer 9 and the Al 2 O 3The bonding property of the layer 11 is excellent. In addition, the average angle of the front end 13b of the first protrusion 13 can also be 55° or more. In addition, the average angle of the front end 13b of the first protrusion 13 can also be 80° or less. If such a structure is provided, the Al 2 O 3 The film forming property of the layer 11 is excellent, and the intermediate layer 9 and the Al 2 O 3 The layer 11 has excellent bonding properties.
[0041] In addition, if Figure 4 As shown, the composite protrusion 17 in the coated tool 1 of the present invention may also have a third protrusion 19 protruding in a direction intersecting with the protruding direction of the second protrusion 15. If such a structure is provided, the intermediate layer 9 and the Al 2 O 3 The bonding property of the layer 11 is more excellent. In addition, the height of the third protrusion 19 is greater than 10 nm. In other words, the tiny concavo-convex on the side of the second protrusion 15 is not treated as the third protrusion 19 in the coated tool 1 of the present invention. Such tiny concavo-convex has a great influence on the bonding between the intermediate layer 9 and the Al 2 O 3 The bonding properties of layer 11 also do not help substantially.
[0042] In the coated tool 1 of the present invention, as Figure 5 As shown, the coating 7 may have a TiN layer 10a, a first TiCN layer 10b, a second TiCN layer, an intermediate layer 9, an Al 2 O 3 Layer 11. If it has such a structure, it becomes a coated tool 1 with a long life. The first TiCN layer 10b can be the MT-TiCN layer described later. The second TiCN layer can also be the HT-TiCN layer described later. In addition, as a surface layer (not shown), a TiN layer or the like can be provided. The surface layer can also be made of other materials other than titanium nitride, such as titanium carbonitride, titanium oxynitride, chromium nitride, etc. The surface layer is composed of a colored material, so that it has the function of easily distinguishing whether the cutting edge is used or not. The surface layer can be set to a thickness of 0.1μm to 3.0μm.
[0043] The first protrusion 13, the second protrusion 15 and the third protrusion 19 of the coated tool 1 of the present invention may all contain Ti, C and N and have a homogeneous composition. In addition, the first protrusion 13, the second protrusion 15 and the third protrusion 19 may all contain Ti, C, N and O and have a homogeneous composition. If the first protrusion 13, the second protrusion 15 and the third protrusion 19 have a homogeneous composition, cracks and damage are unlikely to occur between the first protrusion 13, the second protrusion 15 and the third protrusion 19, and the intermediate layer 9 and the Al2O3 layer may be more uniform than when the respective compositions are different. 2 O 3 The bonding property of the layer 11 becomes higher.
[0044] The phrase "the first protrusions 13 , the second protrusions 15 , and the third protrusions 19 have the same composition" means that the difference in the constituent components is 5% or less.
[0045] Furthermore, the deviation of each composition may be 3% or less. Furthermore, it may be 1% or less.
[0046] Such first protrusions 13 , second protrusions 15 , and third protrusions 19 can be obtained by using the same gas when forming the first protrusions 13 , second protrusions 15 , and third protrusions 19 .
[0047] In addition, the first protrusion 13 and the second protrusion 15 may have different compositions, and the second protrusion 15 and the third protrusion 19 may have different compositions.
[0048] In order to form the first protrusions 13 , the second protrusions 15 , and the third protrusions 19 having different compositions, gases having different compositions may be used during film formation.
[0049] In addition, the first protrusion 13 may not be formed perpendicularly to the first surface 2 of the base 5 , but may be formed inclined relative to the first surface 2 of the base 5 .
[0050] In addition, when the thickness of the intermediate layer 9 is 10 nm to 35 nm, the hardness of the intermediate layer 9 does not decrease, and the Al 2 O 3 The layer 11 has an α-type crystal structure. Here, the thickness of the intermediate layer 9 is the thickness excluding the first protrusions 13 , the second protrusions 15 , and the third protrusions 19 .
[0051] The intermediate layer 9 may contain, for example, 30 to 70 atomic % of titanium, 1 to 70 atomic % of carbon, 1 to 35 atomic % of nitrogen, and 3 to 20 atomic % of oxygen. In addition, it may also contain less than 10 atomic % of aluminum. In addition, it may also contain 1 to 10 atomic % of components such as chlorine and chromium. In addition, the intermediate layer 9 may also contain other trace components.
[0052] In the coated tool 1 of the present invention, the first protrusions 13 , the second protrusions 15 , and the third protrusions 19 may all have the same composition, or may have the composition within the above-mentioned range.
[0053] <Manufacturing method>
[0054] The intermediate layer having the first protrusions can be formed, for example, by forming a film on the surface of the substrate by chemical vapor deposition (CVD) under the following conditions.
[0055] First, the substrate is placed in the furnace of the film forming device, and the film forming temperature is set to 900°C to 990°C, the gas pressure is set to 15kPa to 40kPa, and the titanium tetrachloride (TiCl4 ) gas is 3% to 15% by volume, methane (CH 4 ) gas is 3% to 10% by volume, nitrogen (N 2 ) gas is 3% to 50% by volume, carbon monoxide (CO) gas is 0.2% to 1.0% by volume, and the balance is hydrogen (H 2 ) gas to form a film. For convenience, this process is called the pre-process of the film forming process of the intermediate layer. The film forming time of this pre-process can be more than 20 minutes and less than 40 minutes. 2 ) is 30 volume % to 50 volume %, the average width of the base of the first protrusion is easy to widen, and the average height of the first protrusion is easy to shorten. In other words, under such conditions, it is easy to obtain a thick, short, and unbreakable first protrusion. In addition, the film forming time of the previous process is set to be more than 20 minutes and less than 40 minutes. Under such film forming conditions, it is easy to form a first protrusion with an average base spacing of more than 70nm and less than 120nm.
[0056] In the later stage of forming the intermediate layer, if the film forming temperature is lowered to 900-940° C. without changing the raw material gas ratio, the second protrusions can be formed. The total film forming time and the previous steps can be 30-90 minutes.
[0057] In the later stage of film formation of the intermediate layer, that is, in the process of forming the second protrusions, if the film formation time is extended, the number of the second protrusions increases, and the width and height are likely to increase. In addition, it is easy to form a second protrusion extending toward the substrate. In addition, if the film formation time is extended, a third protrusion protruding from the second protrusion will be formed.
[0058] Al 2 O 3 After the intermediate layer is formed, the film forming temperature can be set to 900°C to 990°C, the gas pressure can be set to 5kPa to 20kPa, and aluminum chloride (AlCl 3 ) gas is 3.5 volume % to 15 volume %, hydrogen chloride (HCl) gas is 0.5 volume % to 2.5 volume %, carbon dioxide (CO 2 ) gas is 0.5 volume % to 5.0 volume %, hydrogen sulfide (H 2 S) gas is 0% to 1.0% by volume, and the balance is hydrogen (H 2 ) gas to form a film. 2 O 3 The layer may consist of α-aluminum oxide.
[0059] The above describes that the intermediate layer and the Al 2 O 3The coating may have a TiN layer, a first TiCN layer, and a second TiCN layer in order from the substrate. Furthermore, an intermediate layer, an Al 2 O 3 In addition, in Al 2 O 3 The Ti layer may further include a surface layer containing Ti and N.
[0060] When a TiN layer is formed on the surface of a substrate, the film forming temperature can be set to 800°C to 940°C, the gas pressure can be set to 8kPa to 50kPa, and the composition of the reaction gas can be made such that titanium tetrachloride (TiCl 4 ) gas is 0.5 volume % to 10 volume %, nitrogen (N 2 ) gas is 10% to 60% by volume, and the remainder is hydrogen (H 2 ) gas to form a film.
[0061] A first TiCN layer and a second TiCN layer may be provided on the TiN layer. The first TiCN layer may be a so-called MT (moderate temperature)-TiCN layer. The MT-TiCN layer may be formed by using, for example, a TiN layer containing titanium tetrachloride (TiCl 4 ) gas, nitrogen (N 2 ) gas and acetonitrile (CH 3 CN) gas, etc., the film forming temperature is 780°C to 880°C, and the film is formed at a relatively low temperature. If the thickness of the first TiCN layer is 2μm to 15μm, the wear resistance and fracture resistance of the first TiCN layer are high. The titanium carbonitride crystals contained in the first TiCN layer can also be elongated columnar crystals in the thickness direction of the coating.
[0062] The second TiCN layer may be a so-called HT (high temperature)-TiCN layer. For example, titanium tetrachloride (TiCl 4 ) gas, nitrogen (N 2 ) gas, methane (CH 4 ) gas, etc., does not contain acetonitrile (CH 3 CN) gas, and the film is formed at a film forming temperature in the range of 900° C. to 1050° C. Alternatively, the film may be formed at a higher temperature than that of the first TiCN layer. The thickness of the second TiCN layer may be 10 nm to 900 nm.
[0063] Here, an interface layer (not shown) may be disposed between the first TiCN layer and the second TiCN layer. The interface layer may contain 30-70 atomic % of titanium, 15-35 atomic % of carbon, 15-35 atomic % of nitrogen, and 2-10 atomic % of oxygen. The thickness of the interface layer may be 5 nm to 50 nm.
[0064] The following is an example of the film forming conditions of the first TiCN layer. The film forming temperature can be 780°C to 880°C, the gas pressure can be 5kPa to 25kPa, and the reaction gas composition can be, in volume %, titanium tetrachloride (TiCl 4 ) gas is 0.5 volume % to 10 volume %, nitrogen (N 2 ) gas is 5% to 60% by volume, acetonitrile (CH 3 CN) gas is 0.1 volume % to 3.0 volume %, and the balance is hydrogen (H 2 ) gas to form a film. At this time, acetonitrile (CH 3 The content ratio of the titanium carbonitride (TiCN) gas is increased in the later stage of film formation compared with the initial stage of film formation, thereby achieving a structure in which the average crystal width of the titanium carbonitride columnar crystals constituting the first TiCN layer is larger on the surface side than on the substrate side.
[0065] Next, the film forming conditions of the second TiCN layer are described. The film forming temperature can be 900°C to 990°C, the gas pressure can be 5 kPa to 40 kPa, and the composition of the reaction gas can be titanium tetrachloride (TiCl 4 ) gas is 1% to 4% by volume, nitrogen (N 2 ) gas is 5% to 20% by volume, methane (CH 4 ) gas is 0.1 volume % to 10 volume %, and the balance is hydrogen (H 2 ) gas to form a film.
[0066] Thereafter, at least the edge of the coating surface is ground as required. The grinding process makes the edge smooth, thereby suppressing the adhesion of the cut material and making the tool more resistant to chipping.
[0067] As mentioned above, the coated cutting tool of the present invention has been described, but the present invention is not limited to the above-mentioned embodiment, and various improvements and changes can be made without departing from the scope of the present invention.
[0068] <Cutting tools>
[0069] Next, the cutting tool of the present invention will be described with reference to the drawings.
[0070] The cutting tool 101 of the present invention, such as Figure 6 As shown, for example, from the first end ( Figure 6 ) toward the second end ( Figure 6 The cutting tool 101, such as Figure 6 As shown, the tool holder 105 has a groove 103 at the first end side (front end side) and the coated tool 1 is located in the groove 103. Since the cutting tool 101 includes the coated tool 1, stable cutting can be performed for a long time.
[0071] The clamping groove 103 is a portion where the coated tool 1 is mounted, and has a support surface parallel to the lower surface of the tool holder 105 and a limiting side surface inclined relative to the support surface. In addition, the clamping groove 103 opens at the first end side of the tool holder 105.
[0072] The coated tool 1 is located in the slot 103. At this time, the lower surface of the coated tool 1 can directly contact the slot 103. In addition, a spacer (not shown) can be sandwiched between the coated tool 1 and the slot 103.
[0073] The coated tool 1 is mounted on the tool holder 105 in such a manner that at least a portion of the portion used as the cutting edge 4 on the ridgeline where the first surface 2 and the second surface 3 intersect protrudes outward from the tool holder 105. In the present embodiment, the coated tool 1 is mounted on the tool holder 105 by the fixing bolt 107. That is, the fixing bolt 107 is inserted into the through hole 17 of the coated tool 1, and the front end of the fixing bolt 107 is inserted into a screw hole (not shown) formed in the slot 103 to tighten the bolt portions, thereby mounting the coated tool 1 on the tool holder 105.
[0074] Steel, cast iron, etc. can be used as the material of the shank 105. Among these members, steel with high toughness can also be used.
[0075] In this embodiment, a cutting tool 101 for so-called turning is exemplified. As turning, for example, inner diameter processing, outer diameter processing, and grooving processing can be cited. In addition, the cutting tool 101 is not limited to turning. For example, a cutting tool for hobbing can also use the coated tool 1 of the above-mentioned embodiment.
[0076] Example
[0077] First, according to the ratio of 6% by mass of metal cobalt powder with an average particle size of 1.2 μm, 0.5% by mass of titanium carbide powder with an average particle size of 2.0 μm, 5% by mass of niobium carbide powder with an average particle size of 2.0 μm, and the balance of tungsten carbide powder with an average particle size of 1.5 μm, the above powders are added and mixed, and molded into a tool shape (CNMG120408) by impact molding. Thereafter, dewaxing treatment is implemented, and sintering is performed at a temperature of 1450°C to 1600°C for 1 hour in a non-oxidizing atmosphere such as an argon atmosphere and a nitrogen atmosphere to produce a matrix composed of cemented carbide. Thereafter, the produced matrix is brushed, and R honing is performed on the portion serving as the cutting edge.
[0078] Next, a coating is formed on the above-mentioned cemented carbide substrate by chemical vapor deposition (CVD). In the example in Table 1, an intermediate layer, an Al 2 O 3 In the example of Table 2, a TiN layer is provided on the surface of the cemented carbide substrate, and a first TiCN layer, a second TiCN layer, an intermediate layer, an Al 2 O 3 The film forming conditions of the intermediate layer of each sample are described in Tables 1 and 2. In addition, TiCl 4 Gas, N 2 gas, CO gas and H 2 Gas. The column of raw material gas shown in Tables 1 and 2 shows the volume % of each gas. In Tables 1 and 2, the film formation is performed in the order of the early and late film formation conditions. In addition, for samples in which only the early stage is recorded but not the late stage, the film formation is performed only under the film formation conditions in the early stage without changing the film formation conditions.
[0079] Al 2 O 3 The film forming temperature of the layer was 950°C. The gas pressure was 7.5 kPa. The composition of the reaction gas was aluminum trichloride (AlCl 3 ) gas is 3.7% by volume, hydrogen chloride (HCl) gas is 0.7% by volume, and carbon dioxide (CO 2 ) gas is 4.3% by volume, hydrogen sulfide (H 2 S) gas is 0.3% by volume, and the balance is hydrogen (H 2 ) gas. 2 O 3 The film formation time of the layer was 380 minutes.
[0080] The film forming conditions of the TiN layer in the example of Table 2 are shown below. The film forming temperature of the TiN layer is 850 degrees. The gas pressure is 16 kPa. The composition of the reaction gas is titanium tetrachloride (TiCl 4) gas is 1.0% by volume nitrogen (N 2 ) gas is 38% by volume, and the remainder is hydrogen (H 2 The film forming time is 180 minutes.
[0081] The film forming conditions of the first TiCN layer in the example of Table 2 are shown below. The film forming temperature was 850°C and the gas pressure was 9.0 kPa. In the reaction gas composition, titanium tetrachloride (TiCl 4 ) gas is 4.0% by volume, nitrogen (N 2 ) gas is 23% by volume, acetonitrile (CH 3 CN) gas is 0.4% by volume, and the balance is hydrogen (H 2 The film forming time is 400 minutes.
[0082] The film forming conditions of the second TiCN layer in the example of Table 2 are shown below. The film forming temperature is 950°C. The gas pressure is 13 kPa. In the composition of the reaction gas, titanium tetrachloride (TiCl 4 ) gas is 4% by volume nitrogen (N 2 ) gas is 20% by volume, methane (CH 4 ) gas is 8% by volume, and the remainder is hydrogen (H 2 ) gas. The film forming time is 80 minutes.
[0083] The samples in Tables 1 and 2 were observed by SEM in the cross section including the coating layer to observe the morphology of the first protrusions and the composite protrusions. The results are shown in Tables 1 and 2.
[0084] The obtained samples were used to perform intermittent cutting tests under the following conditions to evaluate the fracture resistance. The test results are shown in Tables 1 and 2. The number of impacts (ratios) shown in Tables 1 and 2 are the ratios of the number of impacts of each sample to the number of impacts of sample No. 1. The larger the number of impacts (ratio), the better the fracture resistance.
[0085] <Interrupted cutting conditions>
[0086] Workpiece: Chrome-molybdenum steel 4-slot steel (SCM440)
[0087] Tool shape: CNMG120408
[0088] Cutting speed: 300m / min
[0089] Feed speed: 0.3mm / rev
[0090] Cutting depth: 1.5mm
[0091] Others: Use water-soluble cutting fluid
[0092] Evaluation items: Measurement up to Al2 O 3 The number of impacts that cause layer peeling.
[0093]
Table 1
[0094]
[0095]
Table 2
[0096]
[0097] In Table 1, the average number of second protrusions of the composite protrusions is 1.4 or less, and the coated tool fracture resistance of samples No. 3, 5 to 9 as examples of the present invention is excellent. Samples No. 1 and 2, in which the average number of second protrusions of the composite protrusions is higher than 1.4, are inferior to the fracture resistance of samples No. 3, 5 to 9. In addition, samples No. 4 and 10 without composite protrusions, and sample No. 10 are also inferior to the fracture resistance of samples No. 3, 5 to 9.
[0098] In Table 2, the average number of second protrusions of the composite protrusions is 1.4 or less, and the coated tool fracture resistance of samples No. 13, 15 to 19 as examples of the present invention is excellent. Samples No. 11 and 12, in which the average number of second protrusions of the composite protrusions is greater than 1.4, are inferior in fracture resistance to samples No. 13, 15 to 19. In addition, samples No. 14 and 20 without composite protrusions are inferior in fracture resistance to samples No. 13, 15 to 19.
[0099] Explanation of symbols
[0100] 1 Coated tools
[0101] 2 First side, rake face
[0102] 3 Second side, back face
[0103] 4 Cutting edge
[0104] 5 Matrix
[0105] 7 Coating
[0106] 9 Middle Layer
[0107] 10a TiN layer
[0108] 10b First TiCN layer
[0109] 11 Al 2 O 3 layer
[0110] 13. First protrusion
[0111] 13a Base of the first protrusion
[0112] 13b Front end of the first protrusion
[0113] 15 Second protrusion
[0114] 15a Base of the second protrusion
[0115] 15b Front end of the second protrusion
[0116] 17 Compound protrusion
[0117] 19 The third protrusion
[0118] 101 Cutting Tools
[0119] 103 Card slot
[0120] 105 Handle
[0121] 107 Fixing bolts.
Claims
1. A coated tool comprising a substrate and a coating located on the surface of the substrate, in, The coating has an intermediate layer containing Ti and Al 2 O 3 layer, The Al 2 O 3 The layer is located farther from the substrate than the intermediate layer and is in contact with the intermediate layer. The intermediate layer has a 2 O 3 A plurality of first protrusions protruding from the layer, At least one of the plurality of first protrusions is a composite protrusion having a second protrusion protruding in a direction intersecting with a protruding direction of the first protrusion, In the composite protrusion, the average number of the second protrusions is less than 1.2, The ratio of the average height of the second protrusions to the average width of the bases of the second protrusions is greater than the ratio of the average height of the plurality of first protrusions to the average width of the bases of the plurality of first protrusions. The ratio of the average height of the plurality of first protrusions to the average width of the bases of the plurality of first protrusions is 1.2 or less, An average width of bases of the plurality of first protrusions is greater than or equal to 10 nm and less than or equal to 50 nm, and an average height of the first protrusions is greater than or equal to 10 nm and less than or equal to 60 nm.
2. The coated tool according to claim 1, in, In the plurality of first protrusions, an average angle of the front ends is greater than or equal to 50° and less than or equal to 90°.
3. The coated tool according to claim 1, in, The composite protrusion has a third protrusion protruding in a direction intersecting with a protruding direction of the second protrusion.
4. The coated tool according to any one of claims 1 to 3, in, The coating layer includes, in order from the substrate, a first TiCN layer, a second TiCN layer, the intermediate layer, the Al 2 O 3 layer.
5. The coated tool according to any one of claims 1 to 3, in, The intermediate layer contains C and N.
6. The coated tool according to claim 5, in, The intermediate layer also contains O.
7. A cutting tool comprising: A knife handle extending from a first end toward a second end and having a slot on a side of the first end; and A coated cutting tool according to any one of claims 1 to 6 located in the groove.
Citation Information
Patent Citations
Aluminum oxide-coated tool
JP2004074324A
Coating layer for cutting tools
US20130149527A1
Coated tool
JP2009166216A
Surface coated cutting tool
JP2010173025A
Cutting tool
WO2017090765A1