Method for preparing thermoplastically processable polyurethane polymers

By controlling the component reaction of TPU through a solvent-free method, the problem of mechanical properties and processing properties of TPU within the hardness range is solved, rapid curing and good coupling are achieved, and the mechanical properties and environmental compatibility of TPU are improved.

CN114174369BActive Publication Date: 2024-10-18COVESTRO DEUTSCHLAND AG
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202080056027.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-04
Publication Date
2024-10-18
Estimated Expiration
2040-08-04

AI Technical Summary

Technical Problem

Existing thermoplastically processable polyurethane (TPU) is difficult to achieve good mechanical and processing properties in the hardness range of 40 to 85 Shore A/D, especially the poor coupling between the hard and soft phases resulting in slow curing speed , strong incompatibility, it is difficult to prepare hard TPU with good low-temperature impact toughness.

Method used

TPU is prepared using a solvent-free method and controls the properties of NCO/OH functional prepolymers and OH functional prepolymers through component reactions of basic linear polyols, organic polyisocyanates, linear diols, catalysts, additives and monofunctional chain terminators. molar ratio to achieve the reaction of components A, B, and C to form thermoplastically processable polyurethane. The reaction is preferably carried out at 160°C to 240°C to reduce the oxidation process and improve the mechanical properties of TPU.

Benefits of technology

Achieved TPU in the hardness range of approximately 40 to 85 Shore A/D with good processing properties and mechanical properties, especially fast curing without the use of plasticizers, and good balance between hard and soft phases Coupling, improves high molecular weight and mechanical properties, and solvent-free methods improve environmental compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004932397300000041
    Figure GDA0004932397300000041
  • Figure GDA0004932397300000131
    Figure GDA0004932397300000131
  • Figure GDA0004932397300000141
    Figure GDA0004932397300000141
Patent Text Reader

Abstract

The present invention relates to a novel process for preparing thermoplastically processable polyurethanes, to thermoplastically processable polyurethanes obtainable by said process, to compositions, articles and uses of these polyurethanes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a novel process for preparing thermoplastically processable polyurethanes, to thermoplastically processable polyurethanes obtainable by said process, to compositions, articles and uses of these polyurethanes. Background Art

[0002] Thermoplastic processable polyurethane polymers (TPU) have long been known. Due to the combination of high-quality mechanical properties with the known advantages of cost-effective thermoplastic processability, they are very important in industry. By using different chemical building components, a very wide range of mechanical property changes can be achieved. An overview of TPU, their properties and applications is described, for example, in Kunststoffe 68 (1978), pages 819 to 825 or Kautschuk, Gummi, Kunststoffe 35 (1982), pages 568 to 584. TPU is formed by linear polyols (usually polyethers or polyesters), organic diisocyanates and short-chain diols (chain extenders). TPU can be prepared continuously or discontinuously. The most famous industrial production methods also used in industry are the belt process (GB1057018A) and the extruder process (DE 1964834A-1 and DE2059570A-1).

[0003] In order to adjust the properties, the building components can be varied within relatively wide molar ratios. Molar ratios of macrodiol / chain extender of 1:1 to 1:12 have proven useful. The hardness of the TPU can be adjusted within a wide range via the amount of chain extender. This produces products in the hardness range of about 40 Shore A to about 85 Shore D.

[0004] In order to improve the processing behavior, in particular the cycle time, those TPUs which have a very high curing speed after the processing process in the case of injection-molded articles are of particular interest in the entire hardness range of about 40 Shore A to about 85 Shore D. In the case of hard and soft TPUs in particular, the chemical coupling of hard and soft segments often presents problems due to the excessively high polarity difference between these phases. As a result, the overall potential of mechanical and processing properties is often not fully exploited. There is no lack of attempts to eliminate these disadvantages by specific methods.

[0005] W. et al. (EP-A 1757632) describe a process for preparing thermoplastically processable polyurethanes. The homogeneity of the TPU is improved by a multistage OH prepolymer process. However, the improved homogeneity slows down the curing speed of the TPU.

[0006] W. et al. (EP-A 1338614) describe a method for preparing a soft thermoplastic polyurethane elastomer with low shrinkage that can be demoulded well. The demoulding behavior of TPUs between 45 Shore A and 65 Shore A is improved by pre-expansion of the soft segments. At very high hardnesses, this method has significant disadvantages, since incompatibilities between hard and soft phases occur, so that good coupling between these phases can no longer be achieved. Therefore, the high molecular weight of the TPU required for good mechanical properties is not achieved. In fact, due to the excessively high and fluctuating viscosity of the prepolymer stage, this method is also very unstable and no longer works satisfactorily below 60 Shore A, so that extruder shutdowns often occur.

[0007] W. et al. (EP-A 1932863) likewise describe further soft thermoplastic polyurethane elastomers, their preparation and use. By combining different polyester polyols and chain extenders, TPUs with good demouldability are obtained. However, polyether-based TPUs are not described here. In the case of plasticizer-free TPUs according to this method with a hardness of less than 60 Shore A, only very slow curing after processing by injection molding has been achieved so far.

[0008] In order to improve the low-temperature impact toughness of polyester-based TPUs, for example for ski boot applications, polyether polyols with a molecular weight of more than 1600 g / mol, such as polytetramethylene ether glycol (US4980445A) and polypropylene glycol ether (WO / 2018 / 158327), are used as modifiers. Due to the incompatibility of the hard and soft phases in the TPU, which leads to poor coupling between these phases, such polyethers can only be incorporated into TPUs with a hardness of more than 60 Shore D as a pure soft phase with difficulty. It is difficult to prepare hard TPUs with good low-temperature impact toughness without modifiers. Summary of the invention

[0009] It was therefore an object of the present invention to provide a novel process for preparing TPU which enables the preparation of thermoplastic polyurethanes having good processing properties and good mechanical properties over a very large hardness range of about 40 Shore A to about 85 Shore D.

[0010] Surprisingly, this object is achieved by a solvent-free process for preparing thermoplastically processable polyurethane polymers by reacting components (A), (B), (C) optionally in the presence of (D), optionally in the presence of (E) and optionally in the presence of (F):

[0011] (A) one or more essentially linear polyols, wherein the total amount of component (A) has an average molecular weight Mn in the range from 500 g / mol to 5000 g / mol, wherein Mn is calculated from the OH number determined in accordance with DIN 53240,

[0012] (B) one or more organic polyisocyanates, preferably organic diisocyanates,

[0013] (C) one or more linear diols having a molecular weight of 62 g / mol to 500 g / mol,

[0014] (D) one or more catalysts,

[0015] (E) one or more additives, adjuvants and / or admixtures, and

[0016] (F) one or more monofunctional chain terminators,

[0017] The method is characterized in that it comprises or consists of the following steps:

[0018] 1) providing a mixture consisting of the total amount of component (A), a partial amount of component (B) and optionally a partial amount or the total amount of component (D), component (E) and / or component (F) and reacting it to provide an NCO-functional prepolymer, wherein in process step 1) the molar ratio of component (B) to component (A) is in the range from 1.1:1.0 to 5.0:1.0,

[0019] 2) reacting the NCO-functional prepolymer from process step 1) with the total amount of component (C), optionally in the presence of further partial amounts of component (D), component (E) and / or component (F) to obtain an OH-functional prepolymer,

[0020] 3) reacting the OH-functional prepolymer from process step 2) with the remaining amount of component (B) and optionally remaining amounts of component (D), component (E) and / or component (F) to obtain a thermoplastically processable polyurethane, wherein the molar ratio of component (B) to the sum of component (A) and component (C) in all process steps is in the range from 0.9:1.0 to 1.2:1.0.

[0021] The process according to the invention makes it possible to produce thermoplastic polyurethanes with good processing properties and good mechanical properties in the hardness range of about 40 Shore A to about 85 Shore D. In addition, in particular, TPUs with a hardness of less than 60 Shore A and a fast curing speed after injection molding without the use of plasticizers are also successfully provided. According to this method, very hard TPUs with a hardness of up to 85 Shore D can also be produced and good coupling between the hard phase and the soft phase of the TPU is achieved, which leads to an optimally high molecular weight and thus to very good mechanical properties of the finished workpiece. The process is solvent-free, which contributes to significantly better environmental compatibility in the production and use of polyurethane polymers.

[0022] "Solvent-free" is understood in the present invention to mean the reaction of components A, B and C without substantially additional diluents, such as organic solvents or water, which means that components A, B and C preferably react with each other in undiluted form. Components D, E and / or F may optionally be present in a suitable diluent and added to components A, B and / or C as a solution. In the present invention, the method is still considered to be solvent-free when the solvent content is at most 1% by weight based on the total weight of the reaction mixture, preferably at most 0.1% by weight, more preferably at most 0.01% by weight, and most preferably 0% by weight. Here, solvent is understood to mean a substance in which at least one of components A, B and C and optionally D, E and / or F can be dissolved, dispersed, suspended or emulsified, but not with any of components A, B and C and optionally D, E and / or F or with polymers and one or more prepolymers. In this article, "substantially" means that the proportion of solvent is at most 10% by weight based on the total weight of the reaction mixture, preferably at most 5% by weight, particularly preferably at most 1% by weight, more preferably at most 0.1% by weight, more preferably at most 0.01% by weight, and most preferably 0% by weight.

[0023] In the present invention, the word "a" or "an" in relation to countable parameters is to be understood as an index only when explicitly stated (e.g. by the expression "exactly one"). When referring to, for example, "a polyol" hereinafter, the word "a" is to be understood as referring only to the indefinite article and not to the number, which therefore also covers the embodiment comprising a mixture of at least two polyols.

[0024] In this context, "essentially" means that at least 95 mol%, preferably at least 98 mol%, particularly preferably at least 99 mol%, even more preferably at least 99.5 mol%, even more preferably at least 99.8 mol%, and most preferably 100 mol% of the total amount of polyols of component A) consists of linear polyols.

[0025] According to the present invention, the term "comprising" or "containing" preferably means "consisting essentially of", particularly preferably means "consisting of.

[0026] The hardness of the thermoplastically processable polyurethane can be adjusted from 40 Shore A to 85 Shore D by selecting the molar ratio of component A) to component C).

[0027] The amounts of the reaction components used for the NCO-functional prepolymer formation in step 1) are selected so that the NCO / OH ratio of the polyisocyanate to the polyol in step 1) is from 1.1:1 to 5.0:1.

[0028] The components are intimately mixed and the NCO prepolymer in step 1) is preferably reacted to complete conversion (based on the polyol component).

[0029] At least component (C) is then admixed as a chain extender (step 2) to provide an OH-functional prepolymer.

[0030] Thereafter, in step 3), the remaining amount of component (B) is added, wherein an NCO / OH ratio of 0.9:1 to 1.2:1 is maintained. Preferably, the same component (B) as in step 1) is used in step 3).

[0031] In a preferred embodiment of the process according to the invention, in process step 2), the molar ratio of NCO-functional prepolymer to component (C) is less than 1.0. Component (C) is therefore present in a molar excess.

[0032] The solvent-free process according to the invention can be carried out either by manual casting or in a reaction extruder at a temperature of 160 to 240° C., preferably 170 to 240° C., particularly preferably 180 to 240° C.

[0033] It has proven to be advantageous to carry out the process according to the invention in the presence of nitrogen. The advantage here is that oxidation processes during the preparation of the TPU at high temperatures, for example 180° C. to 240° C., are minimized, thereby obtaining significantly lower color values ​​for the TPU pellets. In the manual pouring method, it is sufficient to fill the reaction vessel with nitrogen and apply a nitrogen blanket of 1 to 10 liters of nitrogen per hour during the metering of the components. In the extruder method, it is advantageous to feed a nitrogen stream into the initial barrel of the extruder, for example barrel 1 to barrel 3. Here, the amount of nitrogen fed in is in the range of 10 to 1000 liters / hour, preferably 100 to 750 liters / hour, particularly preferably 100 to 500 liters / hour.

[0034] Suitable components (A) include all linear polyols known to those skilled in the art and having an average molecular weight Mn greater than 500 g / mol. According to the invention, the total amount of component A has an average molecular weight Mn in the range of 500 g / mol to 5000 g / mol, wherein Mn is calculated by the OH value determined according to DIN 53240. It is therefore possible that some of the polyols have an Mn greater than 5000 g / mol, as long as the Mn of the total amount of component A is in the range of 500 g / mol to 5000 g / mol. Particularly suitable linear polyols as component (A) include:

[0035] a) polyester polyols,

[0036] b) polyether polyols,

[0037] c) polyetheresters,

[0038] d) polycarbonate polyols,

[0039] e) polyether carbonates,

[0040] Or any mixture of polyols a) to e). As known to the person skilled in the art, the molecular weight Mn of these polyols is usually calculated via their OH number (hydroxyl number). The OH number is determined titrimetrically according to DIN 53240. The molar weight of the polyol can be calculated from the OH number (OHZ) by the following formula:

[0041]

[0042] Here, z is the number of OH groups in the macromolecule. For linear diols, z=2. For production reasons, these usually contain small amounts of nonlinear compounds.

[0043] Suitable polyester diols a) can be prepared, for example, from dicarboxylic acids having 2 to 12 carbon atoms, preferably 2 to 6 carbon atoms, and polyols. Examples of available dicarboxylic acids include aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid and sebacic acid, dodecanedioic acid and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid and terephthalic acid. Dicarboxylic acids can be used alone or as a mixture, for example in the form of a mixture of succinic acid, glutaric acid and adipic acid. For the preparation of polyester polyols, it may be advantageous to use the corresponding dicarboxylic acid derivatives instead of dicarboxylic acids, such as carboxylic acid diesters, carboxylic anhydrides or acid chlorides having 1 to 4 carbon atoms in the alcohol group. Examples of polyols are diols having 2 to 12, preferably 2 to 6, carbon atoms, such as ethylene glycol, diethylene glycol, butane-1,4-diol, pentane-1,5-diol, hexane-1,6-diol, decane-1,10-diol, dodecane-1,12-diol, 2,2-dimethylpropane-1,3-diol, propane-1,3-diol, propane-1,2-diol and dipropylene glycol. Depending on the desired properties, these polyols can be used alone or optionally mixed with one another. Condensation products of hydroxycarboxylic acids, for example hydroxycaproic acid, and polymerization products of lactones, for example optionally substituted caprolactones, are also suitable. Polyester polyols preferably used are ethylene glycol polyadipate, butane-1,4-diol polyadipate, hexane-1,6-diol polyadipate, ethylene glycol butane-1,4-diol polyadipate, hexane-1,6-diol neopentyl glycol polyadipate, hexane-1,6-diol butane-1,4-diol polyadipate and polycaprolactone. The polyester diols have a molecular weight Mn in the range of 500 to 5000 g / mol, preferably in the range of 600 to 3500 g / mol, particularly preferably in the range of 800 to 3000 g / mol. They can be used alone or in a mixture with one another.

[0044] Suitable polyether diols b) can be prepared by reacting one or more alkylene oxides having 2 to 4 carbon atoms in the alkylene group with a starter molecule containing two active hydrogen atoms in bonded form. Examples of alkylene oxides include: ethylene oxide, 1,2-propylene oxide, epichlorohydrin and 1,2-butylene oxide and 2,3-butylene oxide. Preferably, ethylene oxide, propylene oxide and a mixture of 1,2-propylene oxide and ethylene oxide are used. These alkylene oxides can be used alone, alternately in succession or as a mixture. Considerable starter molecules include, for example: water, amino alcohols, such as N-alkyldiethanolamines, such as N-methyldiethanolamine, and diols, such as ethylene glycol, 1,3-propylene glycol, butane-1,4-diol and hexane-1,6-diol. Optionally, mixtures of starter molecules can also be used. Suitable polyether diols are also hydroxyl-containing polymerization products of tetrahydrofuran. It is also possible to use trifunctional polyethers in proportions of 0 to 30% by weight, based on the difunctional polyether, but at most in amounts which form thermoplastically processable products. Suitable polyether diols have a number average molecular weight Mn in the range from 500 to 5000 g / mol, preferably from 750 to 5000 g / mol, very particularly preferably from 900 to 4200 g / mol. They can be used both individually and in mixtures with one another.

[0045] Suitable polyetheresters c) can be prepared, for example, by reacting short-chain polyetherdiols, for example polytetrahydrofuran having a molecular weight Mn in the range of 250 to 1000 g / mol, with organic dicarboxylic acids, for example succinic acid or adipic acid. The polyetheresterdiols have a molecular weight Mn in the range of 600 to 5000 g / mol, preferably 700 to 4000 g / mol, particularly preferably 800 to 3000 g / mol. They can be used alone or in a mixture with one another.

[0046] Suitable polycarbonate diols d) can be prepared, for example, by reacting short-chain diols, for example butane-1,4-diol or hexane-1,6-diol with diphenyl carbonate or dimethyl carbonate, with the aid of a catalyst and with elimination of phenol or methanol. The polycarbonate diols have a number average molecular weight Mn in the range of 500 to 5000 g / mol, preferably 750 to 5000 g / mol, particularly preferably 1000 to 4500 g / mol.

[0047] Suitable polyether carbonate diols e) can be prepared, for example, by the reaction of short-chain polyether diols, such as polytetrahydrofuran with a molecular weight of 250 to 1000 g / mol, with diphenyl carbonate or dimethyl carbonate, with the aid of a catalyst and elimination of phenol or methanol. In addition, polyether carbonate diols can be prepared by copolymerization of alkylene oxides, such as ethylene oxide or propylene oxide or mixtures thereof with carbon dioxide, with the aid of a suitable catalyst, such as a double metal cyanide catalyst. The polyether carbonate diols have a number average molecular weight Mn in the range of 500 to 8000 g / mol, preferably 750 to 6000 g / mol, particularly preferably 1000 to 4500 g / mol.

[0048] In a further preferred embodiment of the process according to the invention, component (A) used is one or more polyols selected from polyester diols, polyether diols, polycarbonate diols or a mixture of at least two thereof, preferably wherein the one or more polyols each have an average molecular weight Mn in the range of 500 g / mol to 5000 g / mol, wherein Mn is calculated from the OH number determined in accordance with DIN 53240.

[0049] In a further preferred embodiment of the process according to the invention, component (A) used is one or more polyester diols having an average molecular weight Mn in the range from 500 g / mol to 5000 g / mol, preferably in the range from 600 g / mol to 3500 g / mol, particularly preferably in the range from 800 g / mol to 3000 g / mol, wherein Mn is calculated from the OH number determined in accordance with DIN 53240.

[0050] In another preferred embodiment of the process according to the invention, component (A) used is one or more polycarbonate diols having an average molecular weight Mn in the range of 500 g / mol to 5000 g / mol, preferably in the range of 750 g / mol to 5000 g / mol, particularly preferably in the range of 1000 g / mol to 4500 g / mol, wherein Mn is calculated from the OH number determined in accordance with DIN 53240.

[0051] In another preferred embodiment of the process according to the invention, component (A) used is one or more polyether diols having an average molecular weight Mn in the range of 500 g / mol to 5000 g / mol, preferably in the range of 750 g / mol to 5000 g / mol, particularly preferably in the range of 900 g / mol to 4200 g / mol, wherein Mn is calculated from the OH number determined in accordance with DIN 53240.

[0052] In a further preferred embodiment of the process according to the invention, the one or more polyether diols are, independently of one another, polyethers based on polymers of ethylene oxide or propylene oxide or mixtures of different polymers of these raw materials.

[0053] In a further preferred embodiment of the process according to the invention, the one or more polyether diols are independently of one another polyethers of polymers based on tetrahydrofuran.

[0054] Suitable organic polyisocyanates for component (B) used in steps 1) and 3) include aliphatic, cycloaliphatic, araliphatic, heterocyclic and aromatic polyisocyanates as described, for example, in Justus Liebigs Annalen der Chemie, 562, pages 75-136.

[0055] Specific examples include, for example, aliphatic diisocyanates such as 1,5-pentane diisocyanate, 1,6-hexane diisocyanate and 1,10-decane diisocyanate, alicyclic diisocyanates such as isophorone diisocyanate, 1,4-cyclohexane diisocyanate, 1-methyl-2,4-cyclohexane diisocyanate and 1-methyl-2,6-cyclohexane diisocyanate and corresponding isomer mixtures, 4,4'-dicyclohexylmethane diisocyanate, 2,4'-dicyclohexylmethane diisocyanate and 2,2'-dicyclohexylmethane diisocyanate and corresponding isomer mixtures, aromatic diisocyanates such as 1,5-pentane diisocyanate, 1,6-hexane diisocyanate and 1,10-decane diisocyanate, alicyclic diisocyanates such as isophorone diisocyanate, 1,4-cyclohexane diisocyanate, 1-methyl-2,4-cyclohexane diisocyanate and 1-methyl-2,6-cyclohexane diisocyanate and corresponding isomer mixtures, Isocyanates such as 2,4-toluene diisocyanate, a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate and 2,2'-diphenylmethane diisocyanate, a mixture of 2,4'-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate, urethane-modified liquid 4,4'-diphenylmethane diisocyanate and 2,4'-diphenylmethane diisocyanate, 4,4'-diisocyanato-1,2-diphenylethane and 1,5-naphthalene diisocyanate. Preference is given to using hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, diphenylmethane diisocyanate isomer mixtures having a 4,4'-diphenylmethane diisocyanate content of >96% by weight, in particular 4,4'-diphenylmethane diisocyanate and 1,5-naphthalene diisocyanate. The diisocyanates mentioned can be used alone or in a mixture with one another. They can also be used together with up to 15% by weight (based on the total amount of diisocyanates) of polyisocyanates, for example triphenylmethane 4,4',4"-triisocyanate and polyphenylpolymethylene polyisocyanates.

[0056] In another preferred embodiment of the process according to the invention, component (B) used is a diphenylmethane diisocyanate isomer mixture having a 4,4′-diphenylmethane diisocyanate content of more than 96% by weight, based on the total weight of component (B), component (B) used is preferably 4,4′-diphenylmethane diisocyanate.

[0057] In a further preferred embodiment of the process according to the invention, component (B) used is hexamethylene diisocyanate.

[0058] Suitable components (C) (chain extenders) are all linear diols known to the person skilled in the art and having a molecular weight of 62 g / mol to 500 g / mol. The diols and / or their precursor compounds can be obtained from fossil or biological sources. Suitable diols are preferably aliphatic diols having 2 to 14 carbon atoms, for example ethylene glycol, butane-1,4-diol, hexane-1,6-diol, octan-1,8-diol, decan-1,10-diol, dodecane-1,12-diol, diethylene glycol and dipropylene glycol. However, diesters of terephthalic acid with diols having 2 to 4 carbon atoms, for example bis-ethylene glycol terephthalate or bis-butane-1,4-diol terephthalate, hydroxyalkylene ethers of hydroquinone, for example 1,4-bis(hydroxyethyl)hydroquinone, and ethoxylated bisphenols are also suitable. Ethylene glycol, butane-1,4-diol, hexane-1,6-diol and 1,4-di(hydroxyethyl)hydroquinone are particularly preferably used as short-chain diols. Mixtures of the aforementioned chain extenders can also be used. In addition, small amounts of diamines and / or triols can also be added.

[0059] In another preferred embodiment of the method according to the present invention, the component (C) used is one or more diols selected from ethane-1,2-diol, butane-1,4-diol, hexane-1,6-diol, 1,4-di(β-hydroxyethyl)hydroquinone or a mixture of at least two thereof, the component (C) used is preferably ethane-1,2-diol, butane-1,4-diol or a mixture thereof, and the component (C) used is particularly preferably ethane-1,2-diol.

[0060] Useful catalysts (D) include conventional catalysts known in polyurethane chemistry. Suitable catalysts are conventional tertiary amines known per se, such as triethylamine, dimethylcyclohexylamine, N-methylmorpholine, N,N'-dimethylpiperazine, 2-(dimethylaminoethoxy)ethanol, diazabicyclo[2.2.2]octane, etc., and in particular organometallic compounds, such as titanates, iron compounds, bismuth compounds, zirconium compounds, tin compounds, such as tin diacetate, tin dioctoate, tin dilaurate, or dialkyltin salts of aliphatic carboxylic acids, such as dibutyltin diacetate, dibutyltin dilaurate, etc. Preferred catalysts are organometallic compounds, in particular titanates, iron compounds or tin compounds. Very particularly preferred are dibutyltin dilaurate, tin dioctoate and titanates.

[0061] Useful additives, auxiliaries and admixtures (E) are, for example, lubricants, such as fatty acid esters, their metal soaps, fatty acid amides and silicone compounds, antiblocking agents, inhibitors, stabilizers against hydrolysis, light, heat and discoloration, flame retardants, dyes, pigments, inorganic or organic fillers, nucleating agents and reinforcing agents. Reinforcing agents are in particular fiber reinforcements, such as inorganic fibers, which are prepared according to the prior art and may also be sized. Further descriptions of the auxiliary and additive substances mentioned can be found in the special literature, for example JH Saunders, KC Frisch: "High Polymers", Volume XVI, Polyurethane, Parts 1 and 2, Interscience Publishers 1962 and 1964, R. H. Müller (editor): Taschenbuch der Kunststoff-Additive, 3rd edition, Hanser Verlag, München 1989 or DE-A2901774.

[0062] Useful monofunctional chain terminators (F) include monoalcohols such as 1-butanol, 1-hexanol, 1-octanol and stearyl alcohol, or monoamines such as 1-butylamine, di-n-butylamine and stearylamine to adjust to a specific TPU molecular weight.

[0063] In a further preferred embodiment of the method according to the invention, the thermoplastically processable polyurethane polymer has a hardness of less than 60 Shore A or greater than 80 Shore D, preferably in the range of 35 Shore A to 60 Shore A or in the range of 70 Shore D to 95 Shore D, particularly preferably in the range of 40 Shore A to 55 Shore A or in the range of 75 Shore D to 90 Shore D, in each case determined in accordance with DIN ISO 7619-1 (2012-02-01).

[0064] In a further preferred embodiment of the method according to the invention, the thermoplastically processable polyurethane polymer has a hardness of less than 60 Shore A, preferably in the range of 35 Shore A to 60 Shore A, particularly preferably in the range of 40 Shore A to 55 Shore A, in each case determined in accordance with DIN ISO 7619-1 (2012-02-01).

[0065] In a further preferred embodiment of the method according to the invention, the thermoplastically processable polyurethane polymer has a hardness of more than 70 Shore D, preferably in the range of 70 Shore D to 95 Shore D, particularly preferably in the range of 75 Shore D to 90 Shore D, in each case determined in accordance with DIN ISO 7619-1 (2012-02-01).

[0066] The TPU having a hardness of 40 Shore A to 60 Shore A produced by the process according to the invention is particularly preferably produced from the following main components:

[0067] Component (A):

[0068] i) butane-1,4-diol polyadipates, hexane-1,6-diol polyadipates, ethylene glycol butane-1,4-diol polyadipates, hexane-1,6-diol neopentyl glycol polyadipates, hexane-1,6-diol butane-1,4-diol polyadipates and mixtures thereof, having a molecular weight Mn of 500 to 5000 g / mol, wherein Mn is calculated from the OH number determined in accordance with DIN 53240, or ii) polypropylene oxide or polyethylene oxide / polypropylene oxide and / or tetrahydrofuran polymers and mixtures thereof, having a molecular weight Mn of 500 to 5000 g / mol, wherein Mn is calculated from the OH number determined in accordance with DIN 53240,

[0069] Component (B):

[0070] iii) diphenylmethane 4,4'-diisocyanate, dicyclohexylmethane 4,4'-diisocyanate and / or hexamethylene diisocyanate, component (C):

[0071] iv) ethylene glycol, butane-1,4-diol, hexane-1,6-diol and / or 1,4-bis(hydroxyethyl)hydroquinone,

[0072] It is also possible to use mixtures of the components within i) to iv) and mixtures between i) and ii), the Shore hardness being determined in each case in accordance with DIN ISO 7619-1 (2012-02-01).

[0073] Thermoplastically processable polyurethane polymers can be prepared discontinuously (manual casting process) or continuously using the method according to the invention. The most famous industrial production methods for preparing TPU are the belt method (GB-A 1057018) and the extruder method (DE-A 1964834, DE-A 2059570 and US-A 5795948). Known mixing devices, preferably those operating with high shear energy, are suitable for preparing thermoplastically processable polyurethane polymers. For continuous preparation, for example, co-kneaders, preferably extruders, such as twin-screw extruders and Buss kneaders can be mentioned.

[0074] Thermoplastically processable polyurethane polymers can be prepared, for example, in a twin-screw extruder by preparing a prepolymer in the first section of the extruder and then chain extending and adding the polyisocyanate in the second section. According to the invention, the metering of the chain extender (component (C)) must be carried out before the metering of the further polyisocyanate. The chain extender and the polyisocyanate must never be added in parallel to the same metering port of the extruder.

[0075] However, the NCO and OH prepolymers can also be prepared outside the extruder in a separate upstream prepolymer reactor—discontinuously in a tank or continuously in a tube or stirred tube (tubular mixer) with static mixers.

[0076] However, the OH prepolymer prepared in a separate prepolymer reactor can also be mixed with the diisocyanate by means of a first mixing device, such as a static mixer, and with the remaining amount of polyisocyanate by means of a second mixing device, such as a mixing head. Analogously to the known belt process, this reaction mixture is then applied continuously to a carrier, such as a conveyor belt, where it is reacted until the material solidifies, the belt being optionally heated, to provide the TPU.

[0077] In a preferred embodiment, the process is carried out at a reaction temperature of 140° C. to 240° C. In another preferred embodiment, the process is carried out in an extruder at a reaction temperature of 140° C. to 240° C.

[0078] Another subject of the present invention is a thermoplastically processable polyurethane polymer obtainable or obtained by the method according to the invention. The polyurethane polymers made by the method according to the invention have better properties than those made by methods known in the prior art. In particular, the polyurethane polymers according to the invention cure more rapidly and have a higher Shore hardness and improved tensile strength.

[0079] Another subject of the present invention is a thermoplastically processable polyurethane polymer having a thermal conductivity of ≥15 kJ / m at -30° C., measured in accordance with DIN EN ISO 179 / 1eA. 2 The Charpy impact toughness of 500 g / cm2 is obtainable or obtained by reacting components (A), (B), (C) optionally in the presence of (D), optionally in the presence of (E) and optionally in the presence of (F):

[0080] (A) one or more essentially linear polyether diols based on tetrahydrofuran polymers, wherein the total amount of component (A) has an average molecular weight Mn of more than 1450 g / mol, preferably an average molecular weight Mn in the range of 1450 g / mol to 3500 g / mol, particularly preferably an average molecular weight Mn in the range of 1450 g / mol to 3000 g / mol, even more preferably an average molecular weight Mn in the range of 1500 g / mol to 3000 g / mol, wherein Mn is calculated from the OH number determined in accordance with DIN 53240,

[0081] (B) one or more organic polyisocyanates, preferably organic diisocyanates,

[0082] (C) one or more linear diols having a molecular weight of 62 g / mol to 500 g / mol,

[0083] (D) one or more catalysts,

[0084] (E) one or more additives, adjuvants and / or admixtures, and

[0085] (F) one or more monofunctional chain terminators,

[0086] It is characterized in that the reaction of these components is carried out in a solvent-free manner and comprises or consists of the following steps:

[0087] 1) providing a mixture consisting of the total amount of component (A), a partial amount of component (B) and optionally a partial amount or the total amount of component (D), component (E) and / or component (F) and reacting it to provide an NCO-functional prepolymer, wherein in process step 1) the molar ratio of component (B) to component (A) is in the range from 1.1:1.0 to 5.0:1.0,

[0088] 2) reacting the NCO-functional prepolymer from process step 1) with the total amount of component (C), optionally in the presence of further partial amounts of component (D), component (E) and / or component (F) to obtain an OH-functional prepolymer,

[0089] 3) reacting the OH-functional prepolymer with the remaining amount of component (B) and optionally the remaining amount of component (D), component (E) and / or component (F) to obtain a thermoplastically processable polyurethane, wherein the molar ratio of component (B) to the sum of component (A) and component (C) in all process steps is in the range from 0.9:1.0 to 1.2:1.0, preferably the molar ratio of component (B) to the sum of component (A) and component (C) in all process steps is in the range from 0.95:1.0 to 1.1:1.0.

[0090] In a preferred embodiment of the thermoplastically processable polyurethane polymer according to the invention, it has a thermal conductivity of at least 30 kJ / m 2 measured at -30° C. according to DIN EN ISO 179 / 1eA (2010). 2 , preferably at least 70KJ / m 2 Charpy impact toughness.

[0091] Another subject of the present invention is a composition containing at least one thermoplastically processable polyurethane polymer according to the invention or having a heat release rate of ≥ 15 kJ / m at -30°C, measured according to DIN EN ISO 179 / 1eA. 2 Thermoplastically processable polyurethane polymers according to the present invention, and additives having a Charpy impact toughness of 1.5 %.

[0092] Another subject of the present invention is an article which comprises or contains the thermoplastically processable polyurethane polymer according to the invention or has a heat release rate at -30°C of ≥15 kJ / m 2 Thermoplastically processable polyurethane polymers according to the invention or compositions according to the invention having a Charpy impact toughness of 50 Å.

[0093] Another subject of the present invention is a thermoplastically processable polyurethane polymer according to the invention or a polyurethane having a thermal conductivity of ≥ 15 kJ / m at -30°C, measured according to DIN EN ISO 179 / 1eA. 2 Use of the thermoplastically processable polyurethane polymer according to the invention having a Charpy impact toughness of 1000 Å or the composition according to the invention for producing injection molded articles, extruded articles and coatings. Extruded articles include, for example, sheets, films or hoses. DETAILED DESCRIPTION

[0094] The present invention is explained in more detail with reference to the following examples.

[0095] Measurement method:

[0096] Tensile test:

[0097] Measured in a tensile test according to ISO 53504 (2009-10) at a tensile speed of 200 mm / min.

[0098] Shore hardness:

[0099] The Shore hardness was measured according to DIN ISO 7619-1 (2012-02-01).

[0100] Curing speed (hardness at 0s / 60s):

[0101] To determine the curing speed, the hardness development of round moldings (diameter 30 mm, height 6 mm) was measured after processing by injection molding (injection molding machine settings: 25 s cooling time and 25 s pressure holding time). Here, the hardness of the test specimens was measured immediately after ejection from the mold (0 s) and after 60 s according to DIN 7619-1 (2012-02-01).

[0102] Charpy impact toughness test

[0103] The Charpy impact toughness test was carried out on injection molded specimens at -30°C according to DIN EN ISO 179 / 1eA: (2010). The specimens had the following dimensions: 80 ± 2 mm length, 10.0 ± 0.2 mm width and 4.0 ± 0.2 mm thickness. The test had a notch. The notch base circle radius r N 0.25±0.05mm.

[0104] Solution viscosity:

[0105] The TPU sample was dissolved in a 0.4% solution of N-methylpyrrolidone + 0.1% dibutylamine at room temperature with stirring. At the same time, a so-called blank sample consisting of N-methylpyrrolidone and 0.1% dibutylamine solution but without TPU was also prepared. The solution was allowed to stand overnight and measured the next day. The solution was briefly stirred again and subsequently measured at 25°C using a SVM3000 / G2 Stabinger viscometer. The kinematic viscosity of the blank value and the solution was measured.

[0106] Raw materials used:

[0107] (commercial product from Covestro Deutschland AG, polyester, molecular weight Mn about 2000 g / mol)

[0108] (commercial product from Covestro Deutschland AG, polypropylene glycol ether, molecular weight Mn about 2000 g / mol)

[0109] (Commercial product from Invista: polytetramethylene glycol; molecular weight Mn about 1000 g / mol)

[0110] (Commercial product from Invista: polytetramethylene glycol; molecular weight Mn about 2000 g / mol)

[0111] (commercial product from Covestro Deutschland AG, polycarbonate diol, molecular weight Mn about 2000 g / mol)

[0112] (Commercial product from Invista: polytetramethyl glycol; molecular weight Mn about 1400 g / mol)

[0113] (Commercial product from Invista, polytetramethyl glycol, molecular weight Mn about 2900 g / mol)

[0114] BDO = butane-1,4-diol (BDO, purity ≥ 99 wt%) from Ashland.

[0115] MEG = ethane-1,2-diol (MEG, purity ≥ 99 wt%) from OQEMAAG.

[0116] MDI = diphenylmethane 4,4'-diisocyanate (MDI, purity ≥ 99 wt%) from Covestro AG.

[0117] HDI = 1,6-hexamethylene diisocyanate (HDI, purity ≥ 99 wt%) from Covestro AG.

[0118] 1010 comes from BASF SE (DE).

[0119] 2-Butanone (purity ≥ 99.5%) was obtained from Merck KGaA (DE).

[0120] AA105 comes from DorfKetal (US) Company.

[0121] Polyether LP 112 originates from Covestro AG (polypropylene glycol ether, molecular weight Mn about 1000 g / mol).

[0122] Example

[0123] The invention is illustrated with the aid of some examples in Table 1. The preparation methods used are described below.

[0124] Method 1*: Soft segment pre-extension (according to EP-A 1 338 614), not according to the invention

[0125] Stage 1: A portion of 1 MDI is reacted with 1 mol of a polyol or polyol mixture at about 140° C. with stirring until a conversion of >90 mol %, based on the polyol.

[0126] Stage 2: Part 2 of MDI and subsequently the chain extender are added to the stirred reaction mixture, which is poured onto a metal plate after vigorous mixing (approximately 20 s) and subsequently heat treated at 120° C. for 30 minutes.

[0127] Method 2*: One-step process with HDI as diisocyanate, not according to the invention

[0128] Stage 1: 1 mol of polyol or polyol mixture is pre-loaded with chain extender and heated to a reaction temperature of about 120°C. The entire amount of HDI is then added. After vigorous mixing (about 60 s), the reaction mixture is poured onto a metal plate and subsequently heat treated at 80°C for 30 minutes.

[0129] Method 3: MDI multi-stage pre-expansion method according to the present invention

[0130] Stage 1: A portion of 1 MDI is reacted with 1 mol of a polyol or polyol mixture at about 140° C. with stirring until a conversion of >90 mol %, based on the polyol.

[0131] Stage 2: The chain extender was added to the stirred reaction mixture and stirred vigorously for approximately 10 seconds.

[0132] Stage 3: Partial amount 2 of MDI is added to the stirred reaction mixture. The reaction mixture is stirred for a further 20 seconds, then poured onto a metal plate and heat treated at 120° C. for 30 minutes.

[0133] Method 4: HDI multi-stage pre-expansion method according to the present invention

[0134] Stage 1: A portion of 1 HDI is reacted with 1 mol of a polyol or polyol mixture at about 160° C. with stirring to a conversion of >90 mol %, based on the polyol.

[0135] Stage 2: The chain extender was added to the stirred reaction mixture and stirred vigorously for approximately 60 seconds.

[0136] Stage 3: Partial amount 2 of HDI is added to the stirred reaction mixture. The reaction mixture is stirred for a further 20 seconds, then poured onto a metal plate and heat treated at 80° C. for 30 minutes.

[0137] The resulting TPU cast plaques were chopped and pelletized. The pellets were injected into the mold using an Arburg Allrounder 470S model injection molding machine at a temperature range of 180° C. to 230° C. and a pressure range of 650 to 750 bar in a range of 10 to 35 cm 3 The mold was processed at an injection flow rate of 2000 g / s to produce rods (mold temperature: 40°C; rod dimensions: 80 x 10 x 4 mm) or plates (mold temperature: 40°C; dimensions: 125 x 50 x 2 mm).

[0138] The mechanical values ​​(100% modulus, 300% modulus, breaking strength, breaking elongation and Shore A / D hardness) and curing speed of the prepared TPU products were measured.

[0139] Table 1: Examples 1-18: Measurement results of soft to hard TPU

[0140]

[0141]

[0142] *Comparative example not according to the present invention, **Cannot be processed

[0143] ***Total HDI amount (one-step method), # Theoretical hardness is the ratio of hard segments in TPU: for example TH = n(BDO+MDI) / (n(BDO+MDI)+m(polymer+MDI)).

[0144] In the examples listed in Table 1 (Experiments 3, 4, 6, 7, 16, 17 and 18) in which the same raw material was produced by different methods at the same theoretical hardness, it is obvious that the TPU materials produced by the multistage method according to the invention (Methods 3 and 4) solidify significantly faster, i.e. the measured hardness after 0 seconds and after 60 seconds after removal from the injection molding machine is higher than in the respective comparative experiments. In Experiments 1, 2, 8 and 9 (very soft, polyester-based TPU and polyether-based TPU), it is obvious that the TPU based on monoethylene glycol (MEG) solidifies faster than those based on butane-1,4-diol (BDO). Hard and very hard TPU materials that could not be produced by the method 1 not according to the invention (Experiments 10 and 12) could be produced without problems by the method 3 according to the invention (Experiments 11, 13 and 15).

[0145] Table 2: Examples 19-26: Improvement of Charpy impact toughness by means of the method according to the invention

[0146]

[0147] +) Fracture type: s = brittle and z = ductile

[0148] *Comparative example not according to the present invention

[0149] **Cannot be processed

[0150] #Theoretical hardness is the ratio of hard segments in TPU. TH = n(BDO+MDI) / (n(BDO+MDI)+m(polymer+MDI)).

[0151] It is evident from the examples given in Table 2 that in the TPU according to method 3 of the invention, the low-temperature impact toughness improves as the molecular weight of the polyol increases. When the average molecular weight of the polyol is greater than 1450 g / mol, the TPU material is no longer brittle at -30°C. In the case of the preparation of the respective TPU by method 1 not according to the invention, no suitable TPU material was obtained. Either the low-temperature impact toughness was poor (experiment 19) or worse than in the method according to the invention (experiment 20), or the TPU was not processable (experiments 23 and 25).

[0152] Comparative Example with Solvent Addition

[0153] In Comparative Examples 8A and 24A, the polyol used was Polyether 2200N (Polyol 2) and T2000 (polyol 4) and was operated according to the experimental description in US Pat. No. 3,915,923. The products obtained were then compared with Examples 8 and 24 (both prepared according to process 3 of the invention). For this purpose, the same theoretical hardness was set in each case.

[0154] Experiment 8A:

[0155] 260 g of 2200N (OH value 56.1, equivalent to 1 mole) and 1.3 g 1010 is dissolved in 650.03 g of 2-butanone. 64.79 g (2 mol) of MDI are then slowly metered in. Thereafter, 0.69 g of Tyzor AA105 (0.5% solution in Polyether LP 112, equivalent to 10 ppm) is added. The reaction mixture is stirred for about 30 minutes and the temperature should be maintained at 60° C. Thereafter, 11.05 g (1.373 mol) of monoethylene glycol (MEG) are slowly added dropwise to the reaction mixture and stirred at 60° C. for another 30-60 minutes. Finally, 12.13 g (0.373 mol) of MDI are metered in at 60° C. and stirred further at 60° C. until the NCO content no longer changes, which can therefore be considered to be completely converted. Thereafter, the solvent 2-butanone is removed as much as possible by vacuum distillation.

[0156] Experiment 24A:

[0157] 58.89 g of 2000 (OH value 54, equivalent to 1 mole) and 0.28 g 1010 is dissolved in 294.44 g of 2-butanone. Then 27.48 g (4 mol) of MDI are slowly metered in. The reaction mixture is stirred for about 30 minutes and the temperature should be maintained at 60°C. Then 23.56 g (9.524 mol) of butane-1,4-diol (BDO) are slowly added dropwise to the reaction mixture and stirred at 60°C for another 30-60 minutes. Finally, 45.34 g (6.598 mol) of MDI are metered in at 60°C and stirred further at 60°C until the NCO content no longer changes and can therefore be considered to be completely converted. Thereafter, the solvent 2-butanone is removed as much as possible by vacuum distillation.

[0158] Table 3: Comparative Examples 8A and 24A compared with Examples 8 and 24 of the present invention

[0159]

[0160]

[0161] Experiments 8A and 24A were prepared according to the method of US 3915923. After the addition of the chain extender, stirring had to be carried out for as long as 3 hours to obtain complete conversion or to a constant NCO content. After the solvent had been distilled off, the reaction mixture was still very viscous and not solid at room temperature. The reaction time was very long compared to the reaction time of the method according to the invention (maximum 3 minutes). Due to the extremely low solution viscosity corresponding to the low molecular weight and the plasticity at room temperature, both products could not be processed thermoplastically in an injection molding machine for further mechanical measurements. The method with added solvent cannot be used economically in TPU production, because the solvent must be completely removed after the reaction, which is extremely expensive.

Claims

1. A solvent-free process for preparing thermoplastically processable polyurethane polymers by reacting components (A), (B), (C) optionally in the presence of (D), optionally in the presence of (E) and optionally in the presence of (F): (A) one or more essentially linear polyols, wherein the total amount of component (A) has an average molecular weight Mn in the range from 500 g / mol to 5000 g / mol, wherein Mn is calculated from the OH number determined in accordance with DIN 53240, wherein "essentially" means that at least 95 mol % of the total amount of polyols of component A) consists of linear polyols, (B) one or more organic polyisocyanates, (C) one or more linear diols having a molecular weight of 62 g / mol to 500 g / mol, (D) one or more catalysts, (E) one or more additives, and (F) one or more monofunctional chain terminators, Features The method comprises the following steps: 1) providing a mixture consisting of the total amount of component (A), a partial amount of component (B) and optionally a partial amount or the total amount of component (D), component (E) and / or component (F) and reacting it to provide an NCO-functional prepolymer, wherein in process step 1) the molar ratio of component (B) to component (A) is in the range from 1.1:1.0 to 5.0:1.0, 2) reacting the NCO-functional prepolymer from process step 1) with the total amount of component (C) to obtain an OH-functional prepolymer, optionally in the presence of further partial amounts of component (D), component (E) and / or component (F), 3) reacting the OH-functional prepolymer from process step 2) with the remaining amount of component (B) and optionally remaining amounts of component (D), component (E) and / or component (F) to obtain a thermoplastically processable polyurethane, wherein the molar ratio of component (B) to the sum of component (A) and component (C) in all process steps is in the range from 0.9:1.0 to 1.2:1.

0.

2. The method as claimed in claim 1, characterized in that In process step 2), the molar ratio of NCO-functional prepolymer to component (C) is less than 1.

0.

3. The method according to claim 1 or 2, characterized in that The component (A) used is one or more polyols selected from polyester diols, polyether diols, polycarbonate diols or a mixture of at least two thereof.

4. The method according to claim 1, characterized in that Component (A) used is one or more polyester diols having an average molecular weight Mn in the range from 500 g / mol to 5000 g / mol, Mn being calculated from the OH number determined in accordance with DIN 53240.

5. The method according to claim 1, characterized in that Component (A) used is one or more polycarbonate diols having an average molecular weight Mn in the range from 500 g / mol to 5000 g / mol, where Mn is calculated from the OH number determined in accordance with DIN 53240.

6. The method according to claim 1, characterized in that Component (A) used is one or more polyether diols having an average molecular weight in the range from 500 g / mol to 5000 g / mol, where Mn is calculated from the OH number determined in accordance with DIN 53240.

7. The method as claimed in claim 6, characterized in that The one or more polyether diols are independently of one another polyethers based on polymers of ethylene oxide or propylene oxide or mixtures of different polymers of these raw materials.

8. The method as claimed in claim 6, characterized in that The one or more polyether diols are independently of one another polyethers of polymers based on tetrahydrofuran.

9. The method according to claim 1 or 2, characterized in that The component (B) used is a diphenylmethane diisocyanate isomer mixture having a 4,4′-diphenylmethane diisocyanate content of more than 96% by weight, based on the total weight of component (B).

10. The method according to claim 1 or 2, characterized in that The component (B) used was hexamethylene diisocyanate.

11. The method according to claim 1 or 2, characterized in that The component (C) used is one or more diols selected from ethane-1,2-diol, butane-1,4-diol, hexane-1,6-diol, 1,4-di(β-hydroxyethyl)hydroquinone or a mixture of at least two thereof.

12. The method according to claim 1 or 2, characterized in that The thermoplastically processable polyurethane polymer has a hardness of less than 60 Shore A or greater than 80 Shore D, determined in each case in accordance with DIN ISO 7619-1, version 2012-02-01.

13. Thermoplastically processable polyurethane polymer obtainable by a process as claimed in any one of claims 1 to 12.

14. Thermoplastically processable polyurethane polymers having a thermal conductivity of ≥ 15 kJ / m at -30°C, measured according to DIN EN ISO 179 / 1eA. 2 The Charpy impact toughness of 500 % is obtained by reacting components (A), (B), (C) optionally in the presence of (D), optionally in the presence of (E) and optionally in the presence of (F): (A) one or more essentially linear polyether diols based on tetrahydrofuran polymers, wherein the total amount of component (A) has an average molecular weight Mn of more than 1450 g / mol, wherein Mn is calculated from the OH number determined in accordance with DIN 53240, wherein "essentially" means that at least 95 mol % of the total amount of polyols of component A) consists of linear polyols, (B) one or more organic polyisocyanates, (C) one or more linear diols having a molecular weight of 62 g / mol to 500 g / mol, (D) one or more catalysts, (E) one or more additives, and (F) one or more monofunctional chain terminators, Features The reaction of these components is carried out in a solvent-free manner and comprises the following steps: 1) providing a mixture consisting of the total amount of component (A), a partial amount of component (B) and optionally a partial amount or the total amount of component (D), component (E) and / or component (F) and reacting it to provide an NCO-functional prepolymer, wherein in process step 1) the molar ratio of component (B) to component (A) is in the range from 1.1:1.0 to 5.0:1.0, 2) reacting the NCO-functional prepolymer from process step 1) with the total amount of component (C) to obtain an OH-functional prepolymer, optionally in the presence of further partial amounts of component (D), component (E) and / or component (F), 3) reacting the OH-functional prepolymer from process step 2) with the remaining amount of component (B) and optionally remaining amounts of component (D), component (E) and / or component (F) to obtain a thermoplastically processable polyurethane, wherein the molar ratio of component (B) to the sum of component (A) and component (C) in all process steps is in the range from 0.9:1.0 to 1.2:1.

0.

15. Thermoplastically processable polyurethane polymer according to claim 14, characterized in that The thermoplastically processable polyurethane polymer has a thermal conductivity of at least 30 kJ / m 2 measured at -30°C according to DIN EN ISO 179 / 1eA, 2010 edition. 2 Charpy impact toughness.

16. Composition comprising at least one thermoplastically processable polyurethane polymer as claimed in claim 13 or a thermoplastically processable polyurethane polymer as claimed in claim 14 or 15, and additives.

17. An article comprising a thermoplastically processable polyurethane polymer as claimed in claim 13 or a thermoplastically processable polyurethane polymer as claimed in claim 14 or 15 or a composition as claimed in claim 16.

18. Use of a thermoplastically processable polyurethane polymer as claimed in claim 13 or a thermoplastically processable polyurethane polymer as claimed in claim 14 or 15 or a composition as claimed in claim 16 for producing injection-moulded articles, extruded articles or coatings.

Citation Information

Patent Citations

  • Polyurethane elastomers mfr by direct reac - tion in extruder

    DE1964834A1

  • process for the continuous single-stage production of polyurethane

    DE2059570A1

  • Polyurethane elastomer free running dyestuff or auxiliary concentrate - is resistant to microbes and stable, and mixes well with elastomer

    DE2901774A1

  • Method for the production of soft, easily demouldable thermoplastic polyurethane elastomers with a low shrinkage

    EP1338614A1

  • Process for preparing thermoplastic polyurethanes

    EP1757632A2