A low-transmittance film and its preparation method and battery

By designing a three-layer structure film and using polyolefin materials with different melt indexes, the problems of high transmittance and inappropriate pore size of lithium-ion battery separators are solved, achieving low transmittance and excellent battery performance, ensuring battery winding Tidiness and performance improvements.

CN114188661BActive Publication Date: 2024-10-25SHENZHEN ZHONGXING NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111260414.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-28
Publication Date
2024-10-25
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

The high transmittance of the existing lithium-ion battery separators causes the deflection corrector to be unable to detect the edges of the separators, which affects the orderliness of the battery winding. In addition, the unsuitable aperture size leads to problems with charging and discharging efficiency and safety.

Method used

It adopts a three-layer structure film. The middle layer and surface layer are made of polyolefin materials with different melt indexes. Through extrusion, annealing and stretching pore forming processes, a "small size" pore structure is designed to reduce light transmittance and improve Battery performance.

Benefits of technology

It effectively reduces the transmittance of the film, improves the process capability and performance of the battery, ensures that the correction device can detect the edge of the separator, avoids correction failure, and takes into account the charging and discharging efficiency and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114188661B_ABST
    Figure CN114188661B_ABST
Patent Text Reader

Abstract

A low-transmittance film, a preparation method thereof, and a battery, wherein the film comprises polyolefin, wherein the polyolefin comprises at least one of polyethylene, polypropylene, poly-1-butene, and polypentene. The film effectively reduces transmittance and solves the problem of poor induction in the battery separator process in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a low-transmittance film and a preparation method thereof, and a battery. Background Art

[0002] Lithium-ion batteries are mainly composed of four basic parts: positive and negative electrode materials, electrolyte, isolation membrane and battery container. Among them, the lithium battery separator is one of the key internal components of the lithium battery. The performance of the separator determines the interface structure and internal resistance of the battery, and directly affects the battery's capacity, cycle performance and safety performance. Excellent performance separators play an important role in improving the comprehensiveness of the battery. Its most important function is to separate the positive and negative electrodes of the battery to prevent the two electrodes from contacting and short-circuiting. In addition, it also has the function of allowing electrolyte ions to pass through.

[0003] The diaphragm pore size is a key indicator of diaphragm performance. If the pore size is large, the charge and discharge efficiency is high, but the self-discharge is large, which affects the battery capacity; if the pore size is small, the safety is high, but the transmittance is high, and the induction process is poor. Given that the refractive index of the polymer body is the largest, all light is transmitted without reflection. If the diaphragm has high transmittance and the film is transparent or close to transparent, the deviation corrector (a device for correcting the neatness of the diaphragm winding) will not be able to detect the edge of the diaphragm, resulting in deviation correction failure. In the battery winding, the diaphragm will be wound unevenly. Polymer materials have stress whitening phenomenon, and the holes on the membrane will affect the refractive index, resulting in differences in transmittance. At present, the pore size of pp (polypropylene) diaphragms is generally distributed in the range of 20 to 60nm. When the pore size is 20 to 30nm, the diaphragm transmittance is high, and the induction process is difficult. At the same time, the small pore size affects the efficiency of lithium ion passage and cannot achieve fast charging and discharging; when the diaphragm pore size is 50 to 60nm, the battery self-discharge is large and the short circuit rate increases. Summary of the invention

[0004] According to the first aspect, in one embodiment, a film is provided, comprising polyolefin, wherein the polyolefin comprises at least one of polyethylene, polypropylene, poly-1-butene, and polypentene. The film has a relatively low light transmittance, thus solving the problem of poor induction in the manufacturing process of battery separators in the prior art.

[0005] According to the second aspect, in one embodiment, there is provided a method for preparing the film of the first aspect, comprising:

[0006] The extrusion step comprises melting and plasticizing the two polyolefin raw materials respectively, and then casting and extruding them to obtain a three-layer co-extruded cast film;

[0007] An annealing step, comprising annealing the three-layer co-extruded cast film;

[0008] The stretching and hole forming process comprises cold drawing, hot drawing and heat setting the annealed film to obtain the film.

[0009] According to the third aspect, in one embodiment, a battery is provided, wherein the battery comprises the film according to the first aspect.

[0010] According to the low-transmittance film and its preparation method and battery of the above-mentioned embodiments, the transmittance of the film is effectively reduced and the battery performance is improved by adjusting the pore structure of the film. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 This is the SEM image of the separator of Example 2.

[0012] Figure 2 This is a light transmission diagram of the diaphragm of Example 2.

[0013] Figure 3 This is a light transmission diagram of the diaphragm of Example 4. DETAILED DESCRIPTION

[0014] The present invention is further described in detail below by specific embodiments in conjunction with the accompanying drawings. Wherein similar elements in different embodiments adopt associated similar element numbers. In the following embodiments, many detailed descriptions are for making the present application better understood. However, those skilled in the art can easily recognize that some features can be omitted in different situations, or can be replaced by other elements, materials, methods. In some cases, some operations related to the present application are not shown or described in the specification, this is to avoid the core part of the present application being overwhelmed by too much description, and for those skilled in the art, it is not necessary to describe these related operations in detail, and they can fully understand the related operations according to the description in the specification and the general technical knowledge in the art.

[0015] In addition, the features, operations or characteristics described in the specification can be combined in any appropriate manner to form various implementations. At the same time, the steps or actions in the method description can also be interchanged or adjusted in a manner that is obvious to those skilled in the art. Therefore, the various sequences in the specification and the drawings are only for the purpose of clearly describing a certain embodiment and are not meant to be a required sequence, unless otherwise specified that a certain sequence must be followed.

[0016] The serial numbers assigned to the components herein, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The "connection" or "coupling" mentioned in this application include direct and indirect connections (couplings) unless otherwise specified.

[0017] According to the first aspect, in one embodiment, a film is provided, the film comprising polyolefin, the polyolefin comprising at least one of polyethylene, polypropylene, poly-1-butene, and polypentene. The film effectively reduces light transmittance, solving the problem of poor induction in the battery separator process in the prior art.

[0018] In one embodiment, the light transmittance of the film is ≤10%, including but not limited to 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% and the like.

[0019] In one embodiment, the light transmittance of the film is 4-10%, preferably 5-10%.

[0020] In one embodiment, the film is a three-layer structure, including two surface layers and an intermediate layer located between the two surface layers, the two surface layers include a first surface layer and a second surface layer, and the intermediate layer and the two surface layers independently contain the polyolefin.

[0021] In one embodiment, the melt index of the polyolefin contained in the middle layer is less than the melt index of the polyolefin contained in any of the surface layers.

[0022] In one embodiment, the present invention uses polyolefins with different melt indexes as the surface layer and middle layer materials, and the cross-sectional pore size of the obtained film presents a "small-size" structure, which effectively reduces the transmittance. The obtained diaphragm has the characteristic of low transmittance, and therefore has a better process capability in battery winding.

[0023] In one embodiment, the film is used as a battery separator. The separator has low light transmittance, so that the deviation corrector can smoothly detect the edge of the separator, effectively avoiding deviation correction failure. During battery winding, the separator winding will be more neat.

[0024] In one embodiment, the melt index of the polyolefin contained in the middle layer is 0.3-2.0 g / 10 min, preferably 0.3-1.5 g / 10 min. The melt index of the polyolefin contained in the middle layer includes but is not limited to 0.3 g / 10 min, 0.4 g / 10 min, 0.5 g / 10 min, 0.6 g / 10 min, 0.7 g / 10 min, 0.8 g / 10 min, 0.9 g / 10 min, 1.0 g / 10 min, 1.1 g / 10 min, 1.2 g / 10 min, 1.3 g / 10 min, 1.4 g / 10 min, 1.5 g / 10 min, 1.6 g / 10 min, 1.7 g / 10 min, 1.8 g / 10 min, 1.9 g / 10 min, 2.0 g / 10 min, and the like.

[0025] In one embodiment, the melt index of the polyolefin contained in the first surface layer and the second surface layer is independently 3.0 to 6.0 g / 10 min, preferably 3.0 to 5.0 g / 10 min. The melt index of the polyolefin contained in the first surface layer and the second surface layer includes but is not limited to 3.0 g / 10 min, 3.1 g / 10 min, 3.2 g / 10 min, 3.3 g / 10 min, 3.4 g / 10 min, 3.5 g / 10 min, 3.6 g / 10 min, 3.7 g / 10 min, 3.8 g / 10 min, 3.9 g / 10 min, 4.0 g / 10 min, 4.1 g / 10 min, 4.2 g / 10 min, 4.3 g / 10 min, 4.4 g / 10 min. / 10min, 4.5g / 10min, 4.6g / 10min, 4.7g / 10min, 4.8g / 10min, 4.9g / 10min, 5.0g / 10min, 5.1g / 10min, 5.2g / 10min, 5.3g / 10min, 5.4g / 10min, 5.5g / 10min, 5.6g / 10min, 5.7g / 10min, 5.8g / 10min, 5.9g / 10min, 6.0g / 10min and so on.

[0026] In one embodiment, the present invention uses polyolefins with different melt indexes as surface layer and middle layer materials, combined with high temperature stretching and large cold drawing speed ratio, to produce a low-transmittance film, thereby effectively improving the process capability.

[0027] In one embodiment, the mass of the raw material of the middle layer accounts for 20-50% of the total mass of the raw materials of the middle layer and the two surface layers, including but not limited to 20%, 25%, 30%, 35%, 40%, 45%, 50% and the like.

[0028] In one embodiment, the average pore size of the first surface layer and the second surface layer are both smaller than the average pore size of the middle layer.

[0029] In one embodiment, the average pore diameters of the first surface layer and the second surface layer are independently 10 to 30 nm, preferably 15 to 17 nm.

[0030] In one embodiment, the average pore size of the intermediate layer is 30-40 nm, preferably 35-38 nm.

[0031] In one embodiment, the first surface layer and the second surface layer have the same average pore size.

[0032] In one embodiment, the mass ratio of the raw materials of the first surface layer and the second surface layer is 1:1.

[0033] In one embodiment, the polyolefins contained in the first skin layer and the second skin layer have the same melt index.

[0034] In one embodiment, the first surface layer and the second surface layer contain the same polyolefin.

[0035] In one embodiment, the film has a thickness of 10 to 18 μm, a porosity of 38 to 45%, an air permeability of 100 to 350 s / 100 mL, and a longitudinal (MD) tensile strength of 1800 to 2500 kgf / cm 2 , transverse (TD direction) tensile strength is 120~160kgf / cm 2 The puncture strength is 220-500g, the longitudinal heat shrinkage rate is ≤5%, and the transverse heat shrinkage rate is ≤1%.

[0036] In one embodiment, the ratio of the thickness of the intermediate layer to the thickness of any surface layer is 1:(1-3).

[0037] In one embodiment, the first surface layer and the second surface layer have the same thickness.

[0038] According to the second aspect, in one embodiment, there is provided a method for preparing the film of the first aspect, comprising:

[0039] The extrusion step comprises melting and plasticizing the two polyolefin raw materials respectively, and then casting and extruding them to obtain a three-layer co-extruded cast film;

[0040] An annealing step, comprising annealing the three-layer co-extruded cast film;

[0041] The stretching and hole forming process comprises cold drawing, hot drawing and heat setting the annealed film to obtain the film.

[0042] In one embodiment, in the annealing step, the annealing temperature is 100° C. to 145° C.

[0043] In one embodiment, in the annealing step, the annealing time is 0.1 to 24 hours, including but not limited to 0.1 h, 0.2 h, 0.3 h, 0.4 h, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, 5 h, 10 h, 15 h, 20 h, 21 h, 22 h, 23 h, 24 h and the like.

[0044] In one embodiment, the cold drawing temperature is room temperature, and the cold drawing speed ratio is 0.8 to 1.5.

[0045] In one embodiment, the hot drawing temperature is 100° C. to 130° C., and the hot drawing speed ratio is 1.8 to 2.48.

[0046] In one embodiment, the heat setting temperature is 110° C. to 130° C., and the heat setting speed ratio is 0.3 to 0.9.

[0047] According to the third aspect, in one embodiment, a battery is provided, wherein the battery comprises the film according to the first aspect.

[0048] In one embodiment, the film can be used as a battery separator to isolate the positive and negative electrodes of the battery and prevent the positive and negative electrodes from short circuiting.

[0049] In one embodiment, the battery includes but is not limited to a lithium ion battery and a sodium ion battery.

[0050] In one embodiment, an ABA three-layer structure membrane (A is the surface layer, B is the middle layer) is provided. The three-layer co-extruded lithium-ion battery membrane uses polyolefins with different melt indexes as the middle layer and the surface layer materials on the basis of the existing process, so as to realize the pore structure design of the three-layer film with "small size" pore size, so as to take into account the battery performance and process requirements. As a lithium-ion battery separator material, it has a microporous structure. The size and uniformity of the pore size have a direct impact on the performance of the lithium-ion battery. The large pore size means high charge and discharge efficiency, but the self-discharge is large, which affects the battery capacity; the small pore size means high safety, but the light transmittance is high and the process induction is poor. The ABA three-layer structure has a large pore size in the middle layer and a small pore size in the surface layer. The raw material mass ratio of the middle layer and the surface layer can be adjusted.

[0051] In one embodiment, the present invention uses three-layer extrusion to design a three-layer structure with a small pore size on the surface layer and a large pore size on the middle layer, thereby effectively solving the problems of poor film performance and poor process induction in the existing industry.

[0052] Examples 1 to 5

[0053] The polyolefins used to prepare the surface layer (ie, layer A) and the middle layer (ie, layer B) are both polypropylene.

[0054] The diaphragm preparation method is as follows:

[0055] Extrusion: Take material A used to prepare layer A and material B used to prepare layer B, add them into two different extruders according to different mass ratios for melting and plasticization, press them into a uniform melt through a mold, and extrude them through a casting die to obtain a three-layer co-extruded cast film. The three-layer structure specifically includes two surface layers and an intermediate layer, and the intermediate layer is located between the two surface layers.

[0056] Annealing: The three-layer co-extruded cast film is annealed at a temperature of 100°C to 145°C for a time of 0.1 to 24 hours to further improve the crystallization.

[0057] Stretching pores: The samples after annealing treatment are processed in three steps, including cold drawing, hot drawing and heat setting. Cold drawing is performed at room temperature (23±2°C), the cold drawing speed ratio is 0.8-1.5, the hot drawing temperature is 100°C-130°C, the hot drawing speed ratio is 1.8-2.48, the heat setting temperature is 110°C-130°C, and the heat setting speed ratio is 0.3-0.9. A three-layer co-extruded film with good pores is obtained, with a pore size of 18nm-30nm, a thickness of 10μm-18μm, a porosity of 38-45%, an air permeability of 100-350s / 100mL, and a tensile strength in the MD direction of 1800-2500kgf / cm 2 , TD direction tensile strength is 120~160kgf / cm 2 The puncture strength is 220-500g, the longitudinal heat shrinkage rate is ≤5%, and the transverse heat shrinkage rate is ≤1%.

[0058] In Examples 1 to 5, the melt index of the polyolefin raw material of the middle layer was 1.5 g / 10 min, and the thickness of the middle layer of the film obtained was 4 μm. The melt index of the polyolefin raw material of the surface layer was 3.8 g / 10 min, and the thickness of the surface layer of the film obtained was 5 μm.

[0059] The process parameters of each embodiment are shown in Table 2.

[0060] The specific process conditions of each embodiment are as follows:

[0061] Table 1

[0062]

[0063]

[0064] Table 2

[0065]

[0066] In Table 2, "A layer pore size" refers to the average pore size of one of the surface layers. The average pore size of the two surface layers is the same.

[0067] The “A:B mass ratio” refers to the ratio of the total mass of the raw materials of the two surface layers to the mass of the raw materials of the middle layer.

[0068] The thickness test method refers to "GB / T 6672-2001 Mechanical measurement method for thickness of plastic films and sheets". The measurement is carried out using a Mahr thickness gauge with a flat contact head. The instrument is calibrated and reset before measurement, and the contact surface is kept clean. A point is measured every 5 cm along the TD direction of the film, and the average value of the five points is the thickness.

[0069] Air permeability test: refer to GB / T 458-2008 Determination of air permeability of paper and paperboard, take 5 samples and test them with an air permeability meter, and take the average value of the measurement as the air permeability value of the sample to be tested.

[0070] The porosity test method is as follows: After the membrane is completely immersed in the electrolyte for 1 hour, it is taken out, the electrolyte on the surface of the membrane is absorbed with absorbent paper, and then weighed. The porosity p is calculated as follows: p = (ρ c -ρ e ) / ρ c *100%.ρ c is the density of the diaphragm after being soaked in the electrolyte, ρ e It is the density of the diaphragm when it is not soaked in electrolyte.

[0071] The electrolyte is composed of LiPF6, EC (ethylene carbonate), EMC (ethyl methyl carbonate), and DMC (dimethyl carbonate), with EC, EMC, and DMC being solvents. The concentration of LiPF6 in the electrolyte is 1 mol / L, and by volume, EC:EMC:DMC=1:1:1.

[0072] The pore size test method is as follows: the capillary flow analyzer is used for testing. The capillary flow analyzer uses the bubble point method, that is, an inert gas is used to break through the wetted diaphragm, and the pressure of the gas outflow is measured. The pore size parameters are obtained by calculation, referring to "GB / T14041.1-2007 Verification of structural integrity of hydraulic filter elements and determination of initial bubbling point" and "GB / T24219-2009 Determination of bubble point and pore size of woven filter cloth".

[0073] The test method of transmittance is as follows: put the sample into the test tank, use purple light source, red light source and visible light source to illuminate the transparent material to be tested, the sensor detects the incident light intensity of the three light sources and the light intensity after passing through the transparent material to be tested respectively, the ratio of the transmitted light intensity to the incident light intensity is the transmittance, expressed as a percentage. The instrument has three displays, and during the test, the instrument will display the values ​​of the three light sources at the same time. Examples 1 to 5 are the values ​​of the visible light source.

[0074] As can be seen from Table 2, the diaphragm has a high porosity, and the obtained low-transmittance film has good properties, and the transmittance is preferably 5-10%.

[0075] Since the three-layer co-extruded separator can adjust the microporous structure more flexibly, different pore distributions have different optical properties and battery performance. The surface layer (layer A) is small pores, the battery is safe, the film has extremely high light transmittance, and the film surface is transparent. The middle layer (layer B) is large pores, the battery rate performance is good, the film surface is white, and the picture contrast is obvious.

[0076] Figure 1This is the SEM picture of the diaphragm of Example 2, and a three-layer structure can be seen, showing a "small-size" pore structure, that is, the surface layer has a smaller pore structure, and the middle layer has a larger pore structure.

[0077] Figure 2 This is a light transmission diagram of the diaphragm of Example 2.

[0078] Figure 3 This is a light transmission diagram of the diaphragm of Example 4.

[0079] The above specific examples are used to illustrate the present invention, which is only used to help understand the present invention and is not intended to limit the present invention. For those skilled in the art, according to the concept of the present invention, some simple deductions, modifications or substitutions can be made.

Claims

1. A film with low light transmittance, characterized in that: The film is used for a battery separator; the film contains polyolefin, and the polyolefin is polypropylene; the film has a three-layer structure, including two surface layers and an intermediate layer located between the two surface layers, the two surface layers include a first surface layer and a second surface layer, and the intermediate layer and the two surface layers independently contain the polyolefin; The melting index of the polyolefin contained in the middle layer is 1.1-2.0 g / 10 min, and the melting index of the polyolefin contained in the first surface layer and the second surface layer is independently 3.0-6.0 g / 10 min; the average pore size of the first surface layer and the second surface layer is smaller than the average pore size of the middle layer, the average pore size of the first surface layer and the second surface layer is independently 10-30 nm, and the pore size of the middle layer is 30-40 nm; the transmittance of the film is ≤10%; the thickness of the film is 10-18 μm, and the porosity is 38-45%; the ratio of the thickness of the middle layer to the thickness of any surface layer is 1:(1-3).

2. The film according to claim 1, characterized in that The light transmittance of the film is 4-10%.

3. The film according to claim 2, characterized in that The light transmittance of the film is 5-10%.

4. The film according to claim 1, characterized in that The polyolefin contained in the middle layer has a melt index of 1.5 g / 10 min; The melt index of the polyolefin contained in the first skin layer and the second skin layer is independently 3.0 to 5.0 g / 10 min.

5. The film according to claim 1, characterized in that The first surface layer and the second surface layer have the same average pore diameter; and / or, the mass ratio of the raw materials of the first surface layer to the second surface layer is 1:1; and / or, the mass of the raw material of the middle layer accounts for 20-50% of the total mass of the raw materials of the middle layer and the two surface layers; And / or, the first surface layer and the second surface layer have the same thickness.

6. The film according to claim 5, characterized in that The average pore diameters of the first surface layer and the second surface layer are independently 15 to 17 nm.

7. The film according to claim 5, characterized in that The pore size of the intermediate layer is 35-38 nm.

8. The film according to claim 1, characterized in that The film has an air permeability of 100 to 350 s / 100 mL and a longitudinal tensile strength of 1800 to 2500 kgf / cm 2 , transverse tensile strength is 120~160kgf / cm 2 The puncture strength is 220-500g, the longitudinal heat shrinkage rate is ≤5%, and the transverse heat shrinkage rate is ≤1%.

9. The method for preparing a thin film according to any one of claims 1 to 8, characterized in that: include: The extrusion step comprises melting and plasticizing the two polyolefin raw materials respectively, and then casting and extruding them to obtain a three-layer co-extruded cast film; An annealing step, comprising annealing the three-layer co-extruded cast film; The stretching and hole forming process comprises cold drawing, hot drawing and heat setting the annealed film to obtain the film.

10. The preparation method according to claim 9, characterized in that: In the annealing step, the annealing temperature is 100°C to 145°C; and / or, in the annealing step, the annealing time is 0.1 to 24 hours; and / or, the cold drawing temperature is room temperature, and the cold drawing speed ratio is 0.8 to 1.5; and / or, the hot drawing temperature is 100° C. to 130° C., and the hot drawing speed ratio is 1.8 to 2.48; And / or, the heat setting temperature is 110° C. to 130° C., and the heat setting speed ratio is 0.3 to 0.

9.

11. A battery, characterized in that: The battery comprises the film according to any one of claims 1 to 8.

12. The battery according to claim 11, characterized in that The film is used to isolate the positive and negative electrodes of a battery, and the battery includes a lithium ion battery and a sodium ion battery.