A positive electrode material and preparation method thereof, a positive electrode sheet and a sodium ion battery
By combining lattice doping and surface doping in the sodium-ion battery cathode material, and using the synergistic effect of electrochemically active and inactive elements, a stable O3 phase structure is formed, which solves the problem that the sodium-ion battery cathode material is prone to change during the charge and discharge process. The problem of harmful phase changes occurs and the stability and performance of the material are improved.
Patent Information
- Application Number
- CN202111450796.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-11-30
AI Technical Summary
Existing sodium-ion battery cathode materials are prone to harmful phase changes during the charge and discharge process, leading to lattice distortion and performance degradation, and improper selection and amount of doping elements will affect capacity and cycle life.
The manganese-based layered cathode material uses Mn element as the basic framework. By combining lattice doping and surface doping, harmful phase changes during charge and discharge are suppressed. Electrochemically active elements such as Fe, Ni, Cr, and Cu are used with Li, The synergistic effect of inactive elements such as Na, K, and Mg forms a stable O3 phase structure and improves the material's specific capacity and cycle life.
It effectively suppresses harmful phase changes during the charge and discharge process, improves the stability, specific capacity and rate performance of the material, extends the cycle life, and optimizes the operating voltage and capacity retention rate.
Smart Images

Figure CN114204004B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Background Art
[0002] With the rapid advancement of automobile electrification, the demand for lithium-ion power batteries is huge, resulting in an increasingly tight supply of lithium resources and high prices. On the other hand, it is imperative to develop clean energy, mainly wind and solar. In order to improve the utilization efficiency of clean energy, energy storage batteries must be configured. Given that lithium-ion batteries currently dominate energy storage batteries, the rapid development of the energy storage industry has also exacerbated the rapid consumption of lithium resources. Therefore, it is urgent to develop new energy storage batteries after lithium-ion batteries. Sodium-ion batteries have comprehensive advantages such as good safety, low cost, abundant resources, and environmental friendliness, and are very suitable for large-scale energy storage. For the development of sodium-ion batteries, obtaining suitable positive electrode materials is a key factor. Layered materials have the advantages of high capacity, good rate performance, and long cycle life, and are suitable as positive electrode materials for sodium-ion batteries.
[0003] The layered materials used for sodium-ion batteries have certain similarities with the layered positive electrode materials of lithium-ion batteries, but the situation is more complicated, such as richer phases, easy phase change at lower charging voltage, easy lattice oxygen loss, and stronger surface alkalinity caused by reaction with air. At present, the layered materials used for the positive electrode of sodium-ion batteries generally use Mn elements as the basic framework, and contribute to capacity by doping electrochemically active elements such as Ni, Fe, Co, Cr, etc. Among the layered materials, O3-type materials have the advantage of high capacity, but complex phase changes will occur during the cycle process, causing the lattice to be distorted and thus causing poor cycle performance. The lattice is stabilized by doping with inactive elements, but excessive doping will cause a decrease in capacity, and even cause lattice oxygen loss and performance degradation, and high-valent ion doping will cause a decrease in the sodium content in the sodium layer. Therefore, it is necessary to optimize the doping elements, doping amount, and doping position. Summary of the invention
[0004] One of the purposes of the present invention is to provide a positive electrode material with a stable lattice structure and a surface doping structure coated with doping elements to address the deficiencies of the prior art, which effectively inhibits harmful phase changes during the charge and discharge process, has good stability, high specific capacity, good rate performance and cycle life.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A positive electrode material with the general chemical formula Na n-m A m Mn 1-x-y M1 x M2y O 2-z F z , the material is in O3 phase, wherein M1 is at least one of Fe, Ni, Cr, Cu, and Co, M2 is at least one of Li, Na, K, Mg, Ca, and Sr, A is at least one of Nb, Ta, Zr, Mo, and W, wherein 0.2≤x≤0.7, 0.01≤y≤0.1, x / (1-xy)≥0.5, 0 <z≤0.1,0<m≤0.05,0.85≤n≤1。
[0007] The manganese-based positive electrode material of the present invention uses Mn as the basic framework, combines lattice doping and surface doping to inhibit harmful phase changes during charge and discharge, and keeps the O3 phase. The elements Mn, M1, and M2 in the lattice particles are orderly distributed, and the A-type elements and the element F are gradiently distributed on the surface of the material particles. Through the bulk doping of the elements M1 and M2 and the surface gradient doping of the A-type elements and the element F, as well as the synergistic effect between them, the harmful phase changes of the material during charge and discharge are inhibited, and the cracking of the active particles is inhibited, thereby improving the electrochemical performance of the material. The lattice of the material during charge and discharge is stabilized, and its stability in the electrolyte and air is improved, thereby improving the specific capacity, rate performance, and cycle life of the material. The cathode material of the present invention is electrically neutral as a whole, and electrical neutrality means (nm) + m × K1 + (1-xy) × K2 + x × K3 + y × K4 = (2-z) × 2 + z, where K1, K2, K3, K4 are the valences of elements A, Mn, M1, and M2 in the cathode material, respectively. When the A-type elements, M1, and M2 have two or more elements, according to the electrical neutrality principle of the cathode material, the number of positive charges is equal to the number of negative charges, and a relationship can be obtained.
[0008] The doping element M1 is an electrochemically active element, and electrochemical activity means that the element can contribute to capacity by changing valence during the charge and discharge process.
[0009] Among them, the doping element M2 is an electrochemically inactive element, which means that the element cannot contribute to capacity by changing valence during the charge and discharge process. The advantages of this type of metal doping are: (1) This type of metal easily forms ionic bonds with oxygen and fluorine in the lattice, which is conducive to the formation of O3-type layered structure; (2) The ionic radius of this type of metal is large (Li + 、Na + , K + Mg 2+ , Ca 2+ , Sr 2+ The radii are ), which is much larger than the ionic radius of the active metal M1 when charged (Fe 2+ 、Ni 2+, Cu 2+ Cr 3+ 、Co 3+ The radius is ), which can compensate for the lattice distortion caused by the rapid decrease in the radius of the active metal M1 ion during charging, inhibit the slip of the transition metal layer, and thus inhibit harmful phase changes; (3) The doping of low-valent elements is beneficial to promote Mn to reach the most stable tetravalent state and increase the Na content, thereby inhibiting the John-Teller effect of trivalent manganese and increasing the capacity. (4) This type of ion doping can promote the redox reaction of M1, thereby activating the deintercalation of sodium ions in the sodium layer. (5) Although these elements belong to alkali metals and alkaline earth metals, according to the diagonal principle, Li + and Mg 2+ 、Na + and Ca 2+ , K + and Sr 2+ It has similar physical and chemical properties. Preferably, 0.01 ≤y≤0.1, and more preferably, 0.03≤y≤0.09. Within this range, an optimal balance among capacity, operating voltage and cycle life can be achieved. Too high a doping amount will cause voltage drop, capacity reduction and lattice oxygen loss.
[0010] Preferably, the positive electrode material comprises lattice particles and a surface doping layer coated on the surface of the lattice particles. The present invention combines lattice doping and surface doping to suppress harmful phase changes during charging and discharging, stabilize the lattice of the material during charging and discharging, and improve its stability in electrolyte and air, thereby improving the specific capacity, rate performance and cycle life of the material. The layered positive electrode material of the present invention is lattice doped and surface modified, and the surface modification includes doping of type A elements on the surface sodium side and doping of fluorine on the surface oxygen side.
[0011] Preferably, the surface doping layer comprises at least one of fluorine element or Group A elements. The surface doping includes at least one of surface fluorine element doping or Group A element doping. Among them, the doping of element F is located within 5 to 50 atomic layers on the surface of lattice particles, and the content of F element gradually decreases from outside to inside. The effects of surface gradient fluorine doping are as follows: (1) stabilizing the surface structure and suppressing harmful phase transitions usually initiated by the material surface; (2) a small amount of surface doping does not affect the diffusion of sodium ions inside the lattice and does not affect the specific capacity of the material; (3) the F-rich surface is beneficial to improving the stability of the material in air, and the F-rich surface is prone to in-situ formation of surface fluorides to improve the stability of the material in the electrolyte; (4) fluorine with a larger electronegativity than oxygen forms a stronger ionic bond with metal M2 with a smaller electronegativity, thereby stabilizing the surface structure of the material, further improving the stability of the material in the electrolyte and in air, and suppressing surface phase transitions. Preferably, 0 < z ≤ 0.1, and more preferably, 0.001 ≤ z ≤ 0.02. Within this range, an optimized balance of specific capacity, cycle life, and rate performance can be achieved, and stability in air can be realized.
[0012] Among them, for the gradient doping of Group A elements, where Group A elements are at least one of Nb, Ta, Zr, Mo, and W, the doping of Group A elements is located within 5 to 50 atomic layers on the particle surface, and the content of element A gradually decreases from outside to inside. The effects of surface gradient Group A element doping are as follows: (1) Element A plays a supporting role, suppressing the lattice distortion of the sodium layer during sodium deintercalation, stabilizing the surface structure, and suppressing harmful phase transitions usually starting from the material surface; (2) a small amount of surface doping does not affect the diffusion of sodium ions inside the lattice and does not affect the specific capacity of the material; (3) by doping, an appropriate amount of sodium vacancies are formed in the sodium layer, thereby accelerating the diffusion of sodium ions on the lattice surface and promoting the diffusion of bulk-phase sodium ions; (4) it is beneficial to improving the stability of the material in air and in the electrolyte. Preferably, 0 < m ≤ 0.05, and more preferably, 0.001 ≤ m ≤ 0.005. Within this range, an optimized balance of specific capacity, cycle life, and rate performance can be achieved, and stability in air can be realized.
[0013] Preferably, the fluorine content and / or the content of Group A elements in the surface doping layer gradually decrease from outside to inside. The surface gradient doping of fluorine element and Group A elements can controllably suppress harmful phase transitions and improve stability.
[0014] Preferably, the particle size of the positive electrode material is 0.5 μm to 20 μm. Within this particle size range, it is beneficial to improve the tap density of the electrode and improve the processing performance of the electrode.
[0015] The second object of the present invention is to provide a preparation method of a positive electrode material, which has the advantages of simple and controllable process, low cost, short cycle, low energy consumption, and being suitable for industrial production in view of the deficiencies of the prior art.
[0016] In order to achieve the above object, the present invention adopts the following technical solutions:
[0017] A method for preparing a positive electrode material comprises the following steps:
[0018] Step S1: Prepare lattice particles Na by synthesis method n Mn 1-x-y M1 x M2 y O 2 ;
[0019] Step S2: lattice particles Na n Mn 1-x-y M1 x M2 y O 2 Fluorine doping and A-type element doping were performed to obtain Na n- m A m Mn 1-x-y M1 x M2 y O 2-z F z .
[0020] The process of the present invention is simple and controllable, low cost, short cycle, low energy consumption and suitable for industrial production. The surface doping process of type A elements is generally to add Na n Mn 1-x-y M1 x M2 y O 2 Or surface F-doped Na n Mn 1-x-y M1 x M2 y O 2 The method comprises dispersing the organic salt of the class A element in an organic solvent, adding the organic salt of the class A element, stirring and drying, and finally calcining in air or oxygen to achieve surface gradient doping of the class A element, wherein the calcination temperature is 500° C. to 700° C., and the calcination time is 2 to 10 hours. The organic solvent is selected from ethanol, and the organic salt of the class A element is selected from ethanolate. The surface gradient doping of the element A is achieved by adjusting the amount of the organic salt of the class A element, the calcination temperature and the calcination time. The surface doping process of the element F is generally to add Na n Mn 1-x-y M1 x M2 y O 2 Or surface A-doped Na n Mn 1-x-y M1 x M2 y O 2 With NH 4F are mixed evenly, and then calcined in air or oxygen atmosphere to perform surface doping of F element. The calcination temperature is 300°C to 500°C, and the calcination time is 2 to 10 hours. The mixing method is preferably dry ball milling. By adjusting NH 4 The amount of F used, the calcination temperature and time achieve surface gradient doping of element F.
[0021] Preferably, the synthesis method in step S1 includes a solid phase method, a coprecipitation method, a spray drying method, or a sol-gel method.
[0022] Among them, the solid phase reaction method refers to the synthesis of Na n-m A m Mn 1-x-y M1 x M2 y O 2-z F z In the process, the compound containing the elements Na, Mn, M1 and M2 is mixed uniformly by sand milling, ball milling or high mixing, and then solid phase reaction is carried out, wherein the compound is selected from but not limited to nitrates, acetates, carbonates, oxalates, hydroxides, oxides, oxyhydroxyls or hydrates thereof containing these elements. Preferably, the solid phase reaction temperature is 600° C. to 1100° C., the reaction time is 3 to 24 hours, and the reaction atmosphere is selected from air, oxygen or compressed air.
[0023] The coprecipitation method refers to the synthesis of Na n-m A m Mn 1-x-y M1 x M2 y O 2-z F z In the process, a soluble salt containing Mn and M1 is dissolved in deionized water to prepare a salt solution, and a precipitant solution and a complexing agent solution are prepared, and then the salt solution, the precipitant solution and the complexing agent solution are simultaneously injected into a reaction container to obtain a precipitate. Preferably, the salt solution is selected from chloride, sulfate, nitrate, or a hydrate thereof, the complexing agent solution is selected from ammonia water, and the precipitant solution is selected from an aqueous solution of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium oxalate, and potassium oxalate; preferably, the coprecipitation reaction temperature is 40°C to 60°C, and the pH value of the reaction solution depends on the precipitant. When NaOH solution is selected as the precipitant, the pH value is generally about 11. After the coprecipitation reaction, the precipitate is washed and dried, mixed evenly with a compound containing Na and M2, and then subjected to a solid phase reaction.
[0024] The spray drying method adopts direct spray drying method to synthesize Na n-m A m Mn 1-x-y M1 x M2y O 2-z F z In the process, soluble compounds of Na, Mn, M1 and M2 are dissolved in deionized water, mixed thoroughly, spray dried to obtain a precursor, and then subjected to a solid phase reaction.
[0025] The sol-gel method is to synthesize Na n-m A m Mn 1-x-y M1 x M2 y O 2-z F z In the process, nitrates or sulfates of Na, Mn, M1, and M2 are dissolved in water and mixed to form a sol, and a complexing agent such as citric acid is added, and the mixture is stirred at 60°C to 90°C to obtain a gel, and then a solid phase reaction is carried out.
[0026] Preferably, after step S2, the step further comprises adding 1 to 10 parts by weight of a sodium supplement to 100 to 110 parts by weight of Na n-m A m Mn 1-x-y M1 x M2 y O 2-z F z During the synthesis reaction, high temperature easily leads to sodium burnout, and sodium needs to be supplemented to make the sodium excess 1% to 10%. The sodium supplement includes Na 2 S, a conductive agent and a catalyst, wherein the conductive agent is selected from at least one of acetylene black, carbon nanotubes, carbon fibers, and graphene, and the catalyst is a transition metal oxide selected from but not limited to CuO, MnO 2 , Mn 3 O 4 , NiO, wherein the Na 2 The weight ratio of S, conductive agent and catalyst is 1-2:0.01-0.1:0.01-0.1; preferably, the weight ratio of the sodium supplement agent to the layered active material is 1:100-10:100. By supplementing sodium, the sodium loss at the negative electrode during the first charge can be effectively compensated, thereby improving the first coulombic efficiency.
[0027] Preferably, the sodium supplement comprises sodium sulfide, a conductive agent and a catalyst in a weight ratio of 1 to 2: 0.01 to 0.1: 0.01 to 0.1.
[0028] The third object of the present invention is to provide a positive electrode sheet with good electrochemical performance, stable structure and long service life in view of the shortcomings of the prior art.
[0029] In order to achieve the above object, the present invention adopts the following technical solutions:
[0030] A positive electrode sheet includes a positive electrode current collector and a positive electrode active material disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material includes the above-mentioned positive electrode material. Preferably, the positive electrode active material can be disposed on one surface of the positive electrode current collector or on both surfaces of the positive electrode current collector.
[0031] The fourth object of the present invention is to provide a sodium ion battery with high capacity, excellent rate performance and long cycle life in view of the deficiencies of the prior art.
[0032] In order to achieve the above object, the present invention adopts the following technical solutions:
[0033] A sodium ion battery comprises the above-mentioned positive electrode sheet. Specifically, a sodium ion battery comprises a positive electrode sheet, a negative electrode sheet, a diaphragm, an electrolyte and a shell, wherein the diaphragm separates the positive electrode sheet and the negative electrode sheet, and the shell encapsulates and wraps the positive electrode sheet, the negative electrode sheet, the diaphragm and the electrolyte. Among them, the negative electrode sheet comprises a negative electrode current collector and a negative electrode active layer provided with at least one surface of the negative electrode current collector, and the negative electrode active layer comprises at least one negative electrode active material selected from soft carbon, hard carbon, or hard carbon / soft carbon composite materials. An organic solution containing an organic solvent, a sodium salt and an additive is used as an organic electrolyte. Among them, the organic solvent is selected from but not limited to at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate. The sodium salt comprises at least one of sodium hexafluorophosphate, sodium perchlorate, sodium trifluoromethanesulfonate, sodium bistrifluoromethanesulfonyl imide, sodium bisfluorosulfonyl imide, sodium tetrafluoroborate and sodium bisoxalatoborate.
[0034] Compared with the prior art, the beneficial effects of the present invention are: a positive electrode material of the present invention can effectively inhibit harmful phase changes of the material during the charge and discharge process through uniform doping of M1 and M2 elements in the material bulk phase, and surface doping of elements A and F, and the synergistic effect of the two, and improve the stability of the material in the electrolyte and air, and the obtained material has high capacity, excellent rate performance and long cycle life. The positive electrode material of the present invention has a stable lattice structure and a surface doping structure coated with doping elements, which effectively inhibits harmful phase changes during the charge and discharge process, has good stability, high specific capacity, good rate performance and cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the X-ray diffraction pattern of the O3-phase manganese-based positive electrode material prepared in Example 1 of the present invention.
[0036] Figure 2 It is a charge and discharge curve diagram of the O3 phase manganese-based positive electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0037] The present invention will be described in further detail below in conjunction with specific implementation modes and the accompanying drawings, but the implementation modes of the present invention are not limited thereto.
[0038] Example 1
[0039] Step S1: Press Na 0.91 Nb 0.004 [Mn 0.44 Fe 0.24 Ni 0.26 Li 0.06 ]O 1.99 F 0.01 The material was prepared by direct solid phase reaction and surface doping. 2 CO 3 , Mn 2 O 3 , Fe 2 O 3 、NiO、Li 2 CO 3 The mixture was mixed evenly and ball-milled to obtain a precursor, wherein the ball-milling time was 10 hours at a rotation speed of 400 rpm. The precursor was then placed in a muffle furnace and calcined at 820° C. in an air atmosphere for 10 hours to obtain a manganese-based layered material without surface doping.
[0040] Step S2: Mix the above product with a certain amount of niobium ethoxide in ethanol, stir and dry at 60°C, and then calcine in air at 600°C for 5 hours to perform surface Nb doping. 4 F was mixed evenly and calcined at 400℃ in air for 5 hours to perform surface F doping. The product was analyzed by XRD and was O3 phase. Figure 1 . According to elemental analysis, the elements Mn, Fe, Ni, and Li are evenly distributed in the bulk phase of the material, and the elements Nb and F are gradient-graded on the surface of the material, with the content gradually decreasing from the outside to the inside. The material prepared in this example is used as the positive electrode, metallic sodium is used as the negative electrode, and glass fiber is used as the separator. NaPF 6 The propylene carbonate (PC) / ethyl methyl carbonate (EMC) solution was used as the electrolyte, and 4% by weight of the above electrolyte was added to fluorinated ethylene carbonate (FEC), and a button cell was assembled and charged and discharged. The current density was 12 mA / g, the voltage range was 1.5 to 3.9 V, and the charge and discharge curve was as shown in FIG. Figure 2 As shown, the specific capacity is 125 mAh / g, and the material has a capacity retention rate of 91% after 400 cycles.
[0041] Example 2
[0042] Step S1: Press Na 0.86 Nb 0.002[Mn 0.47 Fe 0.24 Ni 0.24 Li 0.05 ]O 1.995 F 0.005 The material was prepared by coprecipitation method combined with solid phase reaction and surface doping. 4 、 MnSO 4 、FeSO 4 Place in deionized water and mix evenly to obtain a salt solution with a total concentration of 1 mol / L, prepare 0.5 mol / L ammonia solution and 2 mol / L NaOH solution as complexing agent and precipitating agent respectively, then inject the salt solution, complexing agent and precipitating agent into the reaction container at the same time to carry out coprecipitation reaction. The coprecipitation reaction temperature is 50 ° C, and the pH value is controlled at 11.0 by adjusting the flow rate of NaOH solution. The obtained precipitate is centrifuged and dried, and then mixed with Na 2 CO 3 and Li 2 CO 3 The mixture is mixed according to a stoichiometric ratio, and then placed in a muffle furnace, and calcined at 820° C. in an air atmosphere for 10 hours to obtain a manganese-based layered material without surface doping.
[0043] Step S2: Mix the above product with a certain amount of niobium ethoxide in ethanol, stir and dry at 60°C, and then calcine in air at 600°C for 5 hours to perform surface Nb doping. 4 F was mixed evenly and calcined at 400°C in air for 5 hours to perform surface F doping. The product was analyzed by XRD and was O3 phase. Elemental analysis showed that the elements Mn, Fe, Ni, and Li were evenly distributed in the bulk phase of the material, and the elements Nb and F were graded on the surface of the material, with the content gradually decreasing from the outside to the inside. The material prepared in this example was used as the positive electrode, metallic sodium as the negative electrode, glass fiber as the separator, and NaPF 6 The PC / EMC solution was used as the electrolyte, and 4% FEC by weight of the above electrolyte was added to assemble button batteries. The charge and discharge tests were carried out with a current density of 12 mA / g and a voltage range of 1.5 to 3.9 V. After 400 cycles, the capacity retention rate was 90%.
[0044] Example 3
[0045] Step S1: Press Na 0.87 Nb 0.002 [Mn 0.44 Fe 0.24 Ni 0.26 Li 0.05 ]O 1.995 F 0.005The material was prepared by sol-gel method combined with solid phase reaction and surface doping. 3 , LiNO 3 、Mn(NO 3 ) 2 ,Ni(NO 3 ) 2 、Fe(NO 3 ) 2 The mixture was mixed in deionized water and stirred to obtain a sol, and then citric acid was added and stirred at 60°C to obtain a gel, which was then placed in a muffle furnace and calcined at 810°C in an air atmosphere for 15 hours to obtain a non-surface-doped manganese-based layered material.
[0046] Step S2: Mix the above product with a certain amount of niobium ethoxide in ethanol, stir and dry at 60°C, and then calcine in air at 600°C for 5 hours to perform surface Nb doping. 4 F was mixed evenly and calcined at 400°C in air for 5 hours to perform surface F doping. The product was analyzed by XRD and had an O3 phase. Elemental analysis showed that the elements Mn, Fe, Ni, and Li were evenly distributed in the bulk phase of the material, and the elements Nb and F were graded on the surface of the material, with the content gradually decreasing from the outside to the inside. The material prepared in this example was used as the positive electrode, metallic sodium as the negative electrode, glass fiber as the separator, and NaPF 6 The PC / EMC solution was used as the electrolyte, and 4% FEC by weight of the above electrolyte was added to assemble button batteries. The charge and discharge tests were carried out with a current density of 12 mA / g and a voltage range of 1.5 to 3.9 V. After 400 cycles, the capacity retention rate was 93%.
[0047] Example 4
[0048] Step S1: Press Na 0.88 Nb 0.002 [Mn 0.43 Fe 0.31 Cu 0.20 Li 0.06 ]O 1.997 F 0.003 The material was prepared by coprecipitation method combined with solid phase reaction and surface doping. 4 、 MnSO 4 、FeSO 4Place in deionized water and mix evenly to obtain a salt solution with a total concentration of 1 mol / L, prepare 0.5 mol / L ammonia solution and 2 mol / L NaOH solution as complexing agent and precipitating agent respectively, then inject the salt solution, complexing agent and precipitating agent into the reaction container at the same time to carry out coprecipitation reaction. The coprecipitation reaction temperature is 50 ° C, and the pH value is controlled at 11.0 by adjusting the flow rate of NaOH solution. The obtained precipitate is centrifuged and dried, and then mixed with Na 2 CO 3 and Li 2 CO 3 The mixture is mixed according to a stoichiometric ratio, and then placed in a muffle furnace, and calcined at 820° C. in an air atmosphere for 10 hours to obtain a manganese-based layered material without surface doping.
[0049] Step S2: Mix the above product with a certain amount of niobium ethoxide in ethanol, stir and dry at 60°C, and then calcine in air at 600°C for 5 hours to perform surface Nb doping. 4 F was mixed evenly and calcined at 400°C in air for 5 hours to perform surface F doping. The product was analyzed by XRD and was O3 phase. Elemental analysis showed that the elements Mn, Fe, Cu, and Li were evenly distributed in the bulk phase of the material, and the elements Nb and F were graded on the surface of the material, with the content gradually decreasing from the outside to the inside. The material prepared in this example was used as the positive electrode, metallic sodium as the negative electrode, glass fiber as the separator, and NaPF 6 The PC / EMC solution was used as the electrolyte, and 4% FEC by weight of the above electrolyte was added to assemble button batteries. The charge and discharge tests were carried out with a current density of 12 mA / g and a voltage range of 1.5 to 3.9 V. After 400 cycles, the capacity retention rate was 91%.
[0050] Example 5
[0051] Step S1: Press Na 0.88 Ta 0.002 [Mn 0.43 Fe 0.27 Cr 0.04 Ni 0.20 Li 0.06 ]O 1.997 F 0.003 The material was prepared by coprecipitation method combined with solid phase reaction and surface doping. 4 、 MnSO 4 、FeSO 4 Cr 2 (SO 4 ) 3Place in deionized water and mix well to obtain a salt solution with a total concentration of 1 mol / L. Prepare 0.5 mol / L ammonia solution and 2 mol / L NaOH solution as complexing agent and precipitating agent respectively. Then inject the salt solution, complexing agent and precipitating agent into the reaction vessel at the same time to carry out coprecipitation reaction. The coprecipitation reaction temperature is 50 ° C. The pH value is controlled at 11.0 by adjusting the flow rate of NaOH solution. The obtained precipitate is centrifuged and dried, and then mixed with Na 2 CO 3 and Li 2 CO 3 The mixture is mixed according to a stoichiometric ratio, and then placed in a muffle furnace and calcined at 820° C. in an air atmosphere for 12 hours to obtain a manganese-based layered material without surface doping.
[0052] Step S2: Mix the above product with a certain amount of tantalum ethoxide in ethanol, stir and dry at 60°C, and then calcine at 600°C in air for 5 hours to perform surface Ta doping. 4 F was mixed evenly and calcined at 400°C in air for 5 hours to perform surface F doping. The product was analyzed by XRD and was O3 phase. Elemental analysis showed that the elements Mn, Fe, Cr, Ni, and Li were evenly distributed in the bulk phase of the material, and the elements Ta and F showed gradient distribution on the surface of the material, with the content gradually decreasing from the outside to the inside. The material prepared in this example was used as the positive electrode, metallic sodium as the negative electrode, and glass fiber as the separator. NaPF 6 The PC / EMC solution was used as the electrolyte, and 4% FEC by weight of the above electrolyte was added to assemble button batteries. The charge and discharge tests were carried out with a current density of 12 mA / g and a voltage range of 1.5 to 3.9 V. After 400 cycles, the capacity retention rate was 90%.
[0053] Example 6
[0054] Step S1: Press Na 0.85 Ta 0.004 [Mn 0.42 Fe 0.28 Ni 0.13 Cu 0.12 Mg 0.05 ]O 1.99 F 0.01 The material was prepared by direct solid phase method combined with surface doping. 3 , Mn 3 O 4 , Fe 3 O 4 、Ni(OH) 2, MgO and CuO are evenly mixed and ball-milled to obtain a precursor, wherein the ball-milling time is 10 hours and the rotation speed is 400 rpm. The precursor is then placed in a muffle furnace and calcined at 820° C. in an air atmosphere for 15 hours to obtain a non-surface doped manganese-based layered material.
[0055] Step S2: Mix the above product with a certain amount of tantalum ethoxide in ethanol, stir and dry at 60°C, and then calcine at 600°C in air for 5 hours to perform surface Ta doping. 4 F was mixed evenly and calcined at 400°C in air for 5 hours to perform surface F doping. The product was analyzed by XRD and had an O3 phase. Elemental analysis showed that the elements Mn, Fe, Ni, Cu, and Mg were evenly distributed in the bulk phase of the material, and the elements Ta and F showed a gradient distribution on the surface of the material, with the content gradually decreasing from the outside to the inside. The material prepared in this example was used as the positive electrode, metallic sodium as the negative electrode, and glass fiber as the separator. NaPF 6 The PC / EMC solution was used as the electrolyte, and 4% FEC by weight of the above electrolyte was added to assemble button batteries. Charge and discharge tests were carried out with a current density of 12 mA / g and a voltage range of 1.5 to 3.9 V. After 400 cycles, the capacity retention rate was 92%.
[0056] Example 7
[0057] Step S1: Press Na 0.88 Zr 0.003 [Mn 0.42 Fe 0.31 Ni 0.11 Cu 0.11 Li 0.05 ]O 1.996 F 0.004 The material was prepared by direct solid phase method combined with surface doping. 3 , Mn 3 O 4 , Fe 3 O 4 、Ni(OH) 2 、LiNO 3 , CuO are mixed evenly, and deionized water is used as the medium, and a precursor slurry is obtained after sand grinding, wherein the ball milling time is 3 hours, and the rotation speed is 2000rpm. The slurry obtained by sand grinding is spray dried to obtain a precursor, wherein the inlet temperature of the spray dryer is 180°C, and the outlet temperature is 110°C. The precursor is then placed in a muffle furnace and calcined at 820°C in an air atmosphere for 15 hours to obtain a non-surface doped manganese-based layered material.
[0058] Step S2: Mix the above product with a certain amount of zirconium ethoxide in ethanol, stir and dry at 60°C, and then calcine in air at 600°C for 5 hours to perform surface Zr doping. 4 F was mixed evenly and calcined at 400°C in air for 5 hours to perform surface F doping. The product was analyzed by XRD and had an O3 phase. Elemental analysis showed that the elements Mn, Fe, Ni, Cu, and Li were evenly distributed in the bulk phase of the material, and the elements Zr and F showed a gradient distribution on the surface of the material, with the content gradually decreasing from the outside to the inside. The material prepared in this example was used as the positive electrode, metallic sodium as the negative electrode, and glass fiber as the separator. NaPF 6 The PC / EMC solution was used as the electrolyte, and 4% FEC by weight of the above electrolyte was added to assemble button batteries. The charge and discharge tests were carried out with a current density of 12 mA / g and a voltage range of 1.5 to 3.9 V. After 400 cycles, the capacity retention rate was 90%.
[0059] Example 8
[0060] Step S1: Press Na 0.89 Zr 0.002 [Mn 0.42 Fe 0.31 Ni 0.05 Cu 0.16 Li 0.05 Mg 0.01 ]O 1.996 F 0.004 The material was prepared by direct solid phase method combined with surface doping. 2 CO 3 , MnO 2 , Fe 2 O 3 、NiO、CuO、Li 2 CO 3 , and MgO are mixed evenly, and deionized water is used as the medium, and a precursor slurry is obtained after sand grinding, wherein the ball milling time is 4 hours, and the rotation speed is 2000rpm. The slurry obtained by sand grinding is spray dried to obtain a precursor, wherein the inlet temperature of the spray dryer is 180°C, and the outlet temperature is 110°C. The precursor is then placed in a muffle furnace and calcined at 830°C in an air atmosphere for 10 hours to obtain a non-surface doped manganese-based layered material.
[0061] Step S2: Mix the above product with a certain amount of zirconium ethoxide in ethanol, stir and dry at 60°C, and then calcine in air at 600°C for 5 hours to perform surface Zr doping. 4F was mixed evenly, and calcined at 400°C in air for 5 hours to perform surface F doping. The product was analyzed by XRD and had an O3 phase. Elemental analysis showed that the elements Mn, Fe, Ni, Cu, Li, and Mg were evenly distributed in the bulk phase of the material, and the elements Zr and F showed a gradient distribution on the surface of the material, with the content gradually decreasing from the outside to the inside. The material prepared in this example was used as the positive electrode, metallic sodium as the negative electrode, glass fiber as the separator, and NaPF 6 The PC / EMC solution was used as the electrolyte, and 4% FEC by weight of the above electrolyte was added to assemble button batteries. The charge and discharge tests were carried out with a current density of 12 mA / g and a voltage range of 1.5 to 3.9 V. After 400 cycles, the capacity retention rate was 92%.
[0062] Example 9
[0063] Step S1: Press Na 0.85 Zr 0.002 [Mn 0.51 Fe 0.19 Ni 0.08 Cu 0.15 Li 0.07 ]O 1.996 F 0.004 The material was prepared by direct solid phase method combined with surface doping. 2 CO 3 , MnO 2 , Fe 2 O 3 、NiO、CuO、Li 2 CO 3 The mixture was mixed evenly, and a precursor slurry was obtained after sand grinding with deionized water as the medium, wherein the ball milling time was 4 hours and the rotation speed was 2000 rpm. The slurry obtained by sand grinding was spray dried to obtain a precursor, wherein the inlet temperature of the spray dryer was 180°C and the outlet temperature was 110°C. The precursor was then placed in a muffle furnace and calcined at 810°C in an air atmosphere for 15 hours to obtain a non-surface doped manganese-based layered material.
[0064] Step S2: Mix the above product with a certain amount of zirconium ethoxide in ethanol, stir and dry at 60°C, and then calcine in air at 600°C for 5 hours to perform surface Zr doping. 4 F was mixed evenly and calcined at 400°C in air for 5 hours to perform surface F doping. The product was analyzed by XRD and had an O3 phase. Elemental analysis showed that the elements Mn, Fe, Ni, Cu, and Li were evenly distributed in the bulk phase of the material, and the elements Zr and F showed a gradient distribution on the surface of the material, with the content gradually decreasing from the outside to the inside. The material prepared in this example was used as the positive electrode, metallic sodium as the negative electrode, and glass fiber as the separator. NaPF 6The PC / EMC solution was used as the electrolyte, and 4% FEC by weight of the above electrolyte was added to assemble button batteries. Charge and discharge tests were carried out with a current density of 12 mA / g and a voltage range of 1.5 to 3.9 V. After 400 cycles, the capacity retention rate was 91%.
[0065] Example 10
[0066] Step S1: Press Na 0.93 Zr 0.005 [Mn 0.46 Cr 0.18 Ni 0.14 Cu 0.16 Li 0.06 ]O 1.996 F 0.004 The material was prepared by direct spray drying combined with solid phase reaction and surface doping. 3 ,Mn(NO 3 ) 2 Cr(NO 3 ) 3 ,Ni(NO 3 ) 2 、Cu(NO 3 ) 2 、LiNO 3 The obtained precursor was placed in a muffle furnace and calcined at 820°C in an air atmosphere for 15 hours to obtain a non-surface doped manganese-based matrix material.
[0067] Step S2: Mix the above product with a certain amount of zirconium ethoxide in ethanol, stir and dry at 60°C, and then calcine in air at 600°C for 5 hours to perform surface Zr doping. 4 F was mixed evenly and calcined at 400°C in air for 5 hours to perform surface F doping. The product was analyzed by XRD and had an O3 phase. Elemental analysis showed that the elements Mn, Cr, Ni, Cu, and Li were evenly distributed in the bulk phase of the material, and the elements Zr and F showed a gradient distribution on the surface of the material, with the content gradually decreasing from the outside to the inside. The material prepared in this example was used as the positive electrode, metallic sodium as the negative electrode, and glass fiber as the separator. NaPF 6 The PC / EMC solution was used as the electrolyte, and 4% FEC by weight of the above electrolyte was added to assemble button batteries. The charge and discharge tests were carried out with a current density of 12 mA / g and a voltage range of 1.5 to 3.9 V. After 400 cycles, the capacity retention rate was 90%.
[0068] Embodiment 11
[0069] The difference from Example 1 is that no lithium is doped during the preparation process, and the lithium is partially replaced by the electrochemically active element Ni, i.e., Na 0.75 Nb 0.004 [Mn 0.44 Fe 0.24 Ni 0.32 ]O 1.99 F 0.01 Under the same test conditions as in Example 1, after 400 cycles, the capacity retention rate was 82%.
[0070] The rest is the same as Example 1 and will not be described again here.
[0071] Comparative Example 1
[0072] The difference from Example 1 is that: during the preparation process, no Nb was doped on the Na side surface to obtain Na 0.93 [Mn 0.44 Fe 0.24 Ni 0.26 Li 0.06 ]O 1.99 F 0.01 Under the same test conditions as in Example 1, after 400 cycles, the capacity retention rate was 80%
[0073] The rest is the same as Example 1 and will not be described again here.
[0074] Comparative Example 2
[0075] The difference from Example 1 is that: no surface doping with F is performed during the preparation process, and Na 0.92 Nb 0.004 [Mn 0.44 Fe 0.24 Ni 0.26 Li 0.06 ]O 2 Under the same test conditions as in Example 1, after 400 cycles, the capacity retention rate was 79%.
[0076] The rest is the same as Example 1 and will not be described again here.
[0077] Comparative Example 3
[0078] The difference from Example 1 is that: no surface doping with F and Nb is performed during the preparation process, and the obtained Na 0.94 [Mn 0.44 Fe 0.24 Ni 0.26 Li 0.06 ]O 2 Under the same test conditions as in Example 1, after 400 cycles, the capacity retention rate was 75%.
[0079] The rest is the same as Example 1 and will not be described again here.
[0080] Comparative Example 4
[0081] The difference from Example 1 is that no lithium is doped during the preparation process, and the lithium is partially replaced by the electrochemically active element Ni, i.e., Na 0.75 Nb 0.004 [Mn 0.44 Fe 0.24 Ni 0.32 ]O 1.99 F 0.01 O 2 .
[0082] The rest is the same as Example 1 and will not be described again here.
[0083] Comparative Example 5
[0084] The difference from Example 1 is that during the preparation process, the sodium side surface is doped with titanium to obtain Na 0.91 Ti 0.004 [Mn 0.44 Fe 0.24 Ni 0.26 Li 0.06 ]O 1.99 F 0.01 Under the same test conditions as in Example 1, after 400 cycles, the capacity retention rate was 78%.
[0085] The rest is the same as Example 1 and will not be described again here.
[0086] Performance test: The positive electrode materials prepared in Examples 1-10 and Comparative Examples 1-5 and the sodium ion batteries prepared from the positive electrode materials were tested. The test results are recorded in Table 1.
[0087] 1. Discharge rate test:
[0088] (1) In an environment of 25°C, discharge at a constant current of 0.2C to 1.5V, and let it stand for 5 minutes; (2) Charge at a constant current of 0.5C to 3.9V, charge at a constant voltage of 3.9V to a current lower than 0.05C, and let it stand for 5 minutes; (3) Discharge at a rate of 0.2C to 1.5V to obtain the discharge capacity at a discharge rate of 0.2C; (4) Repeat the above steps (2)-(3) and adjust the discharge rate in step (3) to 0.5C, 1C, 1.5C and 2.0C to obtain the discharge capacity at different discharge rates. The discharge capacity obtained at each rate is compared with the discharge capacity obtained at a rate of 0.2C to compare the rate performance.
[0089] 2. Cycle performance test:
[0090] At 25°C, the sodium ion secondary battery is charged to 3.9V at 1C constant current, then charged to 0.05C at 3.9V constant voltage, left to stand for 5 minutes, and then discharged to 1.5V at 1C constant current. This is a charge and discharge cycle process, and the discharge capacity this time is the discharge capacity of the first cycle. The sodium ion secondary battery is subjected to 400 cycles of charge and discharge tests according to the above method, and the discharge capacity of each cycle is recorded. Cycle capacity retention rate (%) = discharge capacity of the 400th cycle / discharge capacity of the first cycle × 100%
[0091] Table 1
[0092]
[0093]
[0094] It can be concluded from Table 1 that the positive electrode material prepared by the present invention has better electrochemical properties than the positive electrode material of the prior art, and the prepared sodium ion battery has good specific capacity, rate performance and cycle life. After 400 charge and discharge cycles, the capacity retention rate is as high as 93%, and the 2C discharge capacity / 0.2C discharge capacity is as high as 90.5%.
[0095] From the comparison of Examples 1-3, it can be concluded that when the material is prepared by a sol-gel method combined with a solid phase reaction and surface doping, the prepared positive electrode material has better electrochemical performance.
[0096] By comparing Examples 2, 4, and 5, it is found that Na 0.88 Nb 0.002 [Mn 0.43 Fe 0.31 Cu 0.20 Li 0.06 ]O 1.997 F 0.003 Stoichiometric ratio, when the material is prepared by co-precipitation method combined with solid phase reaction and surface doping, the prepared positive electrode material has better electrochemical performance.
[0097] By comparison with Examples 6-9, Na 0.89 Zr 0.002 [Mn 0.42 Fe 0.31 Ni 0.05 Cu 0.16 Li 0.05 Mg 0.01 ]O 1.996 F 0.004 The positive electrode material prepared according to the above stoichiometric ratio has better performance.
[0098] From the comparison between Examples 1 and 10, it can be concluded that the solid phase method is better than the spray drying method, and the prepared positive electrode material has better electrochemical performance.
[0099] By comparing Example 1 and Comparative Example 1, it can be seen that the material prepared without doping with Class A elements has poor performance and a decreased capacity retention rate, which indicates that doping with Class A elements can improve the electrochemical properties of the material and improve the capacity retention rate.
[0100] By comparing Example 1 and Comparative Example 2, it can be seen that the material prepared without doping with F element has worse performance and a significantly decreased capacity retention rate, which indicates that F element doping can improve the capacity retention rate of the material, and the impact is greater than that of Class A elements.
[0101] By comparing Example 1 and Comparative Example 3, it can be concluded that the material prepared without doping with F element and A-type element has the worst performance and the capacity retention rate decreases the most, indicating that both F element and A-type element have an impact on the capacity retention rate of the material, and doping with the two can help play a role and improve the capacity retention rate.
[0102] By comparing Example 1 and Comparative Example 4, it can be concluded that the material prepared without doping with the inactive element M2 has poor performance and a decreased capacity retention rate. This is because doping with the inactive element M2 can form a stronger ionic bond, thereby stabilizing the surface structure of the material, further improving the stability of the material in the electrolyte and air, and inhibiting surface phase change, thereby improving the capacity retention rate of the material.
[0103] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A positive electrode material, characterized in that: Its chemical general formula is Na n-m A m Mn 1-x-y M1 x M2 y O 2-z F z , the material is in the O3 phase. In the formula, M1 is at least one of Fe, Ni, Cr, Cu, and Co; M2 is at least one of Li, Na, K, Mg, and Ca; A is at least one of Nb, Ta, Zr, Mo, and W, where 0.2 ≤ x ≤ 0.7, 0.01 ≤ y ≤ 0.1, x / (1 - x - y) ≥ 0.5, 0 < z ≤ 0.1, 0 < m ≤ 0.05, 0.85 ≤ n ≤ 1; the positive electrode material includes lattice particles and a surface doping layer coated on the surface of the lattice particles. The surface doping layer includes fluorine elements and A-type elements. The fluorine content and the content of A-type elements in the surface doping layer decrease in sequence from the outside to the inside. The doping of A-type elements is located within 5 to 50 atomic layers on the particle surface, and the doping of element F is located within 5 to 50 atomic layers on the particle surface.
2. The positive electrode material according to claim 1, characterized in that The particle size of the positive electrode material is 0.5 micrometer to 20 micrometers.
3. A method for preparing a positive electrode material according to any one of claims 1 to 2, characterized in that: The following steps are involved: Step S1: Prepare lattice particles Na by synthesis method n Mn 1-x-y M1 x M2 y O2; Step S2: lattice particles Na n Mn 1-x-y M1 x M2 y O2 is doped with type A elements and then doped with fluorine to obtain Na n- m A m Mn 1-x-y M1 x M2 y O 2-z F z .
4. The method for preparing a positive electrode material according to claim 3, characterized in that: The synthesis method in step S1 includes solid phase method, coprecipitation method, spray drying method and sol-gel method.
5. The method for preparing a positive electrode material according to claim 3, characterized in that: The step S2 further comprises adding 1 to 10 parts by weight of a sodium supplement to 100 to 110 parts by weight of Na n-m A m Mn 1-x-y M1 x M2 y O 2-z F z Sodium supplementation was performed.
6. The method for preparing a positive electrode material according to claim 5, characterized in that: The sodium supplement comprises sodium sulfide, a conductive agent and a catalyst in a weight ratio of 1-2:0.01-0.1:0.01-0.
1.
7. A positive electrode sheet, characterized in that: The invention comprises a positive electrode current collector and a positive electrode active material arranged on at least one surface of the positive electrode current collector, wherein the positive electrode active material comprises the positive electrode material according to any one of claims 1 to 2.
8. A sodium ion battery, characterized in that: Including the positive electrode sheet as described in claim 7.