Polyamide composite fibers and processed yarns

By using eccentric core-sheath composite fibers composed of crystalline polyamide (A) and polyamide (B), the water absorption rate and heat shrinkage stress are controlled, and the polyamide composite fibers in the prior art lose their elasticity in the processing step. The problem is to achieve the superior elasticity and curlability of the fabric.

CN114207200BActive Publication Date: 2024-11-05TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080053997.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-31
Filing Date
2020-07-27
Publication Date
2024-11-05
Estimated Expiration
2040-07-27

AI Technical Summary

Technical Problem

The existing polyamide composite fibers tend to lose their elasticity during processing steps, and they are difficult to fully exhibit crimping properties during wet or dry heat treatment, resulting in insufficient elasticity of fabrics.

Method used

The eccentric core-sheath composite fiber consisting of crystalline polyamide (A) and crystalline polyamide (B) was used to control the water absorption rate to be less than 5.0% by standing at 30°C and 90% RH for 72 hours, and the water absorption rate was controlled to be less than 5.0%. Processing was carried out under the condition that the heat shrinkage stress was 0.15 cN/dtex or above to form fibers with a hard straight amorphous amount of 40-60% and a stretching elongation of 30%.

Benefits of technology

After applying high tension in the warp direction, the fabric can fully demonstrate curlability and elasticity, and obtain a fabric with superior elasticity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114207200B_ABST
    Figure CN114207200B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a polyamide composite fiber or a processed yarn made of the polyamide composite fiber, which can obtain a fabric with excellent stretchability. The polyamide composite fiber of the present invention is an eccentric core-sheath type polyamide composite fiber composed of two crystalline polyamides (A) and crystalline polyamides (B) with different compositions, wherein the water absorption of the polyamide composite fiber after standing for 72 hours in an environment of 30°C and a relative humidity of 90RH% is 5.0% or less, and the heat shrinkage stress is 0.15cN / dtex or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an eccentric core-sheath type composite fiber composed of polyamide and a processed yarn composed of the same. Background Art

[0002] Polyamide fibers have been widely used for clothing applications because they are softer and have a better touch than polyester fibers. Single fiber yarns composed of a single type of polymer, such as nylon 6 or nylon 66, which are representative polyamide fibers for clothing, have almost no elasticity by themselves, so they are subjected to false twisting and other processes to impart elasticity and are used for stretchable fabrics (also called braids, including woven fabrics and knitted fabrics). However, it is still difficult to obtain fabrics with fully satisfactory elasticity by subjecting single fiber yarns to false twisting and other processes.

[0003] Therefore, there are proposals for obtaining a stretchable fabric by using a fiber having elasticity, or a method for obtaining a stretchable fabric by using two polymers having different properties together and preparing a composite fiber having a potential crimping property that exhibits crimping by heat treatment such as a dyeing step (see Patent Document 1). Furthermore, there are proposals for obtaining a polyamide composite fiber having a potential crimping property by arranging two polyamides having different viscosities in a parallel type or an eccentric core-sheath type (see Patent Document 2).

[0004] In addition, there is a proposal for a composite fiber and processed yarn, which is made by making a high heat shrinkage polyamide composite fiber containing amorphous polyamide or a processed yarn composed of it, and even when subjected to wet heat or dry heat treatment under high tension in the warp direction, it still shrinks with a stress higher than the restraint force of the fabric and can exhibit curling in the warp direction (see patent document 3).

[0005] [Prior art literature]

[0006] [Patent Document]

[0007] Patent Document 1: International Patent Publication No. 2018 / 110523

[0008] Patent Document 2: Japanese Patent Application Publication No. 2002-363827

[0009] Patent Document 3: International Patent Publication No. 2017 / 221713 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] However, when the composite fiber described in Patent Document 1 is obtained from two polyamides with different properties, the product may not be able to obtain sufficient stretchability due to the unique swelling property of polyamides and the loss of stretchability during processing steps such as scouring and dyeing. The same is true for the polyamide composite fiber described in Patent Document 2.

[0012] Furthermore, the composite fiber composed of polyamide described in Patent Document 2 has excellent crimping property in the state of raw yarn or processed yarn, but wrinkles unique to polyamide fiber are easily generated in the wet heat step of scouring or dyeing of fabric, or wrinkles generated in the wet heat step are difficult to remove in the dry heat step of the heat setting step, so in order to maintain the quality of the fabric, the fabric must be processed while applying tension in the wet heat step. As such, in the polyamide composite fiber described in Patent Document 2, since tension is applied to the fabric in the wet heat step, the crimp of the raw yarn or processed yarn cannot be fully expressed, resulting in a problem of a fabric lacking in elasticity.

[0013] Furthermore, in the highly heat-shrinkable polyamide composite fiber described in Patent Document 3, since the amorphous polyamide polymer absorbs moisture and crystallizes over time, the shrinkage characteristics also decrease over time, and the resulting fabric may have low stretchability.

[0014] Therefore, an object of the present invention is to solve the above-mentioned problems and to provide a polyamide conjugate fiber and a processed yarn made thereof, which can provide a fabric having excellent stretchability.

[0015] (Technical means to solve the problem)

[0016] The polyamide composite fiber of the present invention is an eccentric core-sheath type polyamide composite fiber composed of two crystalline polyamides (A) and crystalline polyamides (B) having different compositions from each other, wherein the water absorption of the polyamide composite fiber after being left to stand in an environment at a temperature of 30°C and a relative humidity of 90RH% for 72 hours is less than 5.0%, and the thermal shrinkage stress is greater than 0.15 cN / dtex.

[0017] According to a preferred embodiment of the polyamide composite fiber of the present invention, the polyamide composite fiber has a rigid amorphous content of 40 to 60% and a stretching elongation of 30% or more.

[0018] According to a preferred embodiment of the polyamide conjugate fiber of the present invention, the crystalline polyamide (A) is nylon 6 or a copolymer thereof.

[0019] According to a preferred embodiment of the polyamide conjugate fiber of the present invention, the crystalline polyamide (B) is nylon 610 or a copolymer thereof.

[0020] According to a preferred embodiment of the polyamide conjugate fiber of the present invention, the crystalline polyamide (A) is a core component, and the crystalline polyamide (B) is a sheath component.

[0021] In the present invention, a processed yarn made of the above-mentioned polyamide composite fiber can be obtained.

[0022] According to a preferred embodiment of the processed yarn of the present invention, the stretch elongation is 100% or more.

[0023] Effects of the Invention

[0024] According to the present invention, a polyamide composite fiber and processed yarn capable of producing a fabric having excellent stretchability can be obtained. Furthermore, according to the present invention, a polyamide composite fiber and processed yarn capable of producing a fabric having excellent stretchability can be obtained by shrinking with a stress higher than the restraining force of the fabric even when a high tension is applied in the warp direction and by applying wet heat or dry heat, thereby fully expressing crimp in the warp direction. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic cross-sectional view illustrating a cross section of the eccentric core-sheath type polyamide composite fiber of the present invention.

[0026] Figure 2 (A) to Figure 2 (C) is a schematic cross-sectional view illustrating the cross section of another eccentric core-sheath type polyamide composite fiber of the present invention. DETAILED DESCRIPTION

[0027] The polyamide conjugate fiber of the present invention and a processed yarn using the same will be described below.

[0028] In addition, in this specification, "mass" and "weight" have the same meaning.

[0029] The polyamide composite fiber of the present invention is an eccentric core-sheath type polyamide composite fiber composed of two types of crystalline polyamide (A) and crystalline polyamide (B) having different polymer compositions, and is characterized in that the water absorption of the polyamide composite fiber after being left to stand in an environment of a temperature of 30°C and a relative humidity of 90RH% for 72 hours is less than 5.0%, and the thermal shrinkage stress is greater than 0.15 cN / dtex.

[0030] The polyamide composite fiber of the present invention is an eccentric core-sheath composite fiber, which is composed of two crystalline polyamides (A) and crystalline polyamides (B) having different polymer compositions. The eccentric core-sheath polyamide composite fiber refers to a composite fiber in which two or more polyamides form an eccentric core-sheath structure.

[0031] The polyamide composite fiber of the present invention must have a composite cross section formed by joining two crystalline polyamides, and the two crystalline polyamides having different polymer compositions are substantially not separated but exist in a joined state. In the present invention, an eccentric core-sheath type in which the crystalline polyamide (A) is used as a core component and the crystalline polyamide (B) is used as a sheath component, and the crystalline polyamide (B) covers the crystalline polyamide (A).

[0032] Here, the term "eccentricity" in the present invention means that the position of the center of gravity of the core component in the cross section of the polyamide conjugate fiber is different from the center of the cross section of the conjugate fiber.

[0033] Figure 1 This is a schematic cross-sectional view illustrating a cross section of an eccentric core-sheath type polyamide composite fiber (hereinafter also referred to as a "polyamide eccentric core-sheath type composite fiber") of the present invention. Figure 1 In the eccentric polyamide core-sheath type composite fiber 10A, a core component (crystalline polyamide (A)) 1 and a sheath component (crystalline polyamide (B)) 2 are formed, and the center of gravity of the core component crystalline polyamide (A) is different from the center of the composite fiber cross section.

[0034] also, Figure 2 (A) to Figure 2 (C) is a schematic cross-sectional view illustrating the cross section of another polyamide eccentric core-sheath type composite fiber of the present invention. Figure 2 (A) Figure 2 (B) and Figure 2 (C) shows the morphology of polyamide eccentric core-sheath type composite fibers 10B to 10C having different shapes and arrangements of the core component (crystalline polyamide (A)) 1 and the sheath component (crystalline polyamide (B)) 2, respectively. Figure 1 Similarly, the position of the center of gravity of the crystalline polyamide (A) which is the core component is different from the center of the cross section of the conjugate fiber.

[0035] In addition, the composite ratio of crystalline polyamide (A) to crystalline polyamide (B) is preferably crystalline polyamide (A): crystalline polyamide (B) = 6:4 to 4:6 (mass ratio). By preferably setting the mass ratio to 6:4 to 4:6 in this manner, the water absorption of the polyamide composite fiber of the present invention can be controlled to 5.0% or less, and excellent stretchability can be imparted to the obtained fabric.

[0036] The polyamide composite fiber of the present invention is composed of two crystalline polyamides having different polymer compositions. Crystalline polyamide, i.e., polyamide that forms crystals and has a melting point, is also known as a polymer in which a hydrocarbon group is linked to the main chain via an amide bond. As crystalline polyamide, specifically, polycaproamide, polyhexamethylene adipamide, polyhexamethylene sebacamide, polybutylene adipamide, condensation polymerization type polyamide of 1,4-cyclohexanediamine and linear aliphatic dicarboxylic acid, and copolymers thereof or mixtures thereof can be cited. Among them, homopolymerized polyamide is preferably used from the viewpoint of easy reproduction of uniform silk and stable function.

[0037] Examples of the crystalline polyamide (A) include nylon 6, nylon 66, nylon 4, nylon 610, nylon 11, nylon 12, and copolymers thereof as main components, which are different types of polyamide from the crystalline polyamide (B). The crystalline polyamide (A) may contain components other than lactam, aminocarboxylic acid, diamine, and dicarboxylic acid in its repeating structure without hindering the effects of the present invention. However, elastomers containing polyols and the like in the repeating structure are excluded from the viewpoint of yarn forming properties or strength.

[0038] In addition, from the viewpoints of yarn forming properties, strength and anti-stripping properties, the crystalline polyamide (A) preferably has a repeating structure of 90% or more of a single lactam, a single aminocarboxylic acid, or a single combination of a diamine and a dicarboxylic acid, and more preferably 95% or more of the repeating structure. From the viewpoint of thermal stability, such a component is particularly preferably in the form of nylon 6 or a copolymer thereof.

[0039] In addition, the crystalline polyamide (B) can be obtained, for example, by combining a dicarboxylic acid unit and a diamine unit whose main components are sebacic acid units. Among them, nylon 610 and its copolymers, which have stable polymerization properties, little yellowing of the crimped yarn, and good dyeability, are most preferably used. Here, sebacic acid can be produced by, for example, refining castor oil, and is positioned as a plant-derived raw material.

[0040] Examples of the dicarboxylic acid constituting the dicarboxylic acid unit other than the sebacic acid unit include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, phthalic acid, isophthalic acid, and terephthalic acid, and these can be blended within a range not impairing the effects of the present invention.

[0041] The copolymerization amount of the dicarboxylic acid units other than the sebacic acid units is preferably 0 to 40 mol%, more preferably 0 to 20 mol%, and even more preferably 0 to 10 mol% in the total dicarboxylic acid units.

[0042] Examples of the diamine constituting the diamine unit include diamines having 2 or more carbon atoms, preferably diamines having 4 to 12 carbon atoms, and specific examples include butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, trimethylenediamine, nonanediamine, methylpentanediamine, phenylenediamine, and ethambutol, etc. In addition, among these diamines, plant-derived diamines are preferred.

[0043] Furthermore, pigments, heat stabilizers, antioxidants, weathering agents, flame retardants, plasticizers, mold release agents, lubricants, foaming agents, antistatic agents, moldability improvers, and reinforcing agents may be added to the crystalline polyamide (A) and the crystalline polyamide (B) as needed.

[0044] The water absorption of the polyamide composite fiber of the present invention after being left to stand for 72 hours at a temperature of 30°C and a relative humidity of 90RH% (temperature 30°C × relative humidity 90RH%) must be 5.0% or less. The water absorption here is a value measured in accordance with JIS L1013. By setting the water absorption when treated at a temperature of 30°C × relative humidity 90RH% for 72 hours to 5.0% or less, the swelling of the polyamide fiber under wet and hot conditions such as the scouring step or the dyeing step is small, and the stretching of the fabric during these steps becomes small. In this way, the scouring step or the dyeing step can be performed without applying excess tension to the fabric. As a result, a fabric with excellent stretchability can be obtained.

[0045] On the other hand, the higher the water absorption, the more the polyamide fiber tends to swell due to water. If the water absorption exceeds 5.0%, wrinkles or grains are easily generated during the scouring or relaxation treatment steps and the dyeing steps, and the stretchability is usually reduced due to the stretching process.

[0046] The water absorption rate is preferably 4% or less. In addition, the lower limit of the water absorption rate is not particularly limited, but is practically about 1.0%.

[0047] The water absorption rate can be controlled by the polymer selection of the crystalline polyamide (A) and the crystalline polyamide (B) and the core-sheath composite ratio.

[0048] The polyamide composite fiber of the present invention must have a heat shrinkage stress of 0.15 cN / dtex or more. Here, the so-called "heat shrinkage stress" refers to the use of a heat shrinkage stress measuring machine (for example, manufactured by Kanebo Engineering, model "KE-2"), where the fiber yarns to be measured are connected into a ring with a circumference of 16 cm, an initial load of 1 / 30 g of the fineness (detex) of the yarns is applied, and the temperature is increased from 40°C to 210°C at a heating rate of 100°C / min, and the peak value of the obtained heat stress curve is measured as the maximum heat stress (cN / dtex).

[0049] By setting the heat shrinkage stress to 0.15 cN / dtex or more, even when a high tension is applied in the warp direction and a wet heat treatment or a dry heat treatment is performed, the fabric shrinks with a stress higher than the restraining force of the fabric, and the curling property in the warp direction is fully exhibited, and a fabric with good stretchability can be obtained. When the heat shrinkage stress is less than 0.15 cN / dtex, the fabric does not exhibit sufficient curling in the wet heat step with high tension, and the stretchability is deteriorated.

[0050] The thermal shrinkage stress is preferably 0.20 cN / dtex or more, and more preferably 0.25 cN / dtex or more. In addition, if the thermal shrinkage stress is too high, the mesh at the interlaced point of the fabric is easily clogged, which hinders the stretchability, so the upper limit of the thermal shrinkage stress is preferably 0.50 cN / dtex. The thermal shrinkage stress can be controlled by using a high viscosity polymer and controlling the stiff amorphous amount of the fiber under the conditions of low spinning temperature, low spinning speed and high stretch ratio.

[0051] The polyamide composite fiber of the present invention preferably has a rigid amorphous content of 40 to 60%. Rigid amorphous is an amorphous substance whose content is obtained by the method described in the items of the examples, and is an intermediate state between crystal and mobile amorphous (complete amorphous in the past), and is an amorphous substance whose molecular motion is frozen even above the glass transition temperature (Tg), and becomes a fluid state at a temperature higher than Tg (for example, see Shi Shimin, "DSC (3) - Glass transition behavior of polymers -", ​​Journal of the Fiber Society (Fibers and Industry (Textiles and Industry)), Vol. 65, No. 10 (2009)).

[0052] The rigid amorphous content is represented by "100% - degree of crystallinity - movable amorphous content". In the present invention, the polyamide composite fiber contains a crystalline part, a rigid amorphous part and a movable amorphous part. The thermal shrinkage stress depends on the restraining force of the rigid amorphous chain when forming the fiber structure and the shrinkage of the amorphous chain having mobility when the heat treatment is performed. By setting the rigid amorphous content to the above range, the thermal shrinkage stress can be expressed.

[0053] The amount of rigid amorphous particles can be controlled by spinning. Similar to the thermal shrinkage stress, the amount of rigid amorphous particles can be controlled by using a high viscosity polymer and designing the production method.

[0054] By making the hard amorphous content 40% or more, the restraint of the hard amorphous chain is expressed, and the shrinkage of the movable amorphous chain is not damaged, and the desired thermal shrinkage stress can be obtained. In addition, by making the hard amorphous content 60% or less, the restraint of the hard amorphous chain is expressed, the shrinkage of the movable amorphous chain can be maintained, and the desired thermal shrinkage stress can be obtained. The hard amorphous content is preferably 45 to 55%.

[0055] The polyamide composite fiber of the present invention preferably has a stretching elongation of 30% or more. The stretching elongation is an index of the crimping property of the raw yarn, and a higher value indicates a higher crimping ability.

[0056] The polyamide composite fiber of the present invention exhibits a shrinkage difference and curling due to the orientation difference between the crystalline polyamide (A) and the crystalline polyamide (B) when the fiber is formed. However, in general, polyamide fibers are prone to wrinkles during the scouring or dyeing process of the fabric. In order to maintain the quality of the fabric, the fabric is processed under a high tension applied to the warp direction, so there is a possibility that the shrinkage difference is reduced due to the influence of external force (high tension). In order to maintain the shrinkage difference, the curling of the raw yarn can be maintained by having a certain thermal shrinkage stress in the raw yarn. If the stretch elongation is 30% or more, a fabric with better stretchability can be obtained. The stretch elongation is further preferably 100 to 200%. The stretch elongation is expressed by the shrinkage difference between the two components, the crystalline polyamide (A) and the crystalline polyamide (B), so the greater the shrinkage difference, the higher the stretch elongation.

[0057] The polyamide composite fiber of the present invention is preferably in a state where the total fineness of the filaments is 20 to 120 dtex. In particular, when used for sportswear, down jackets, outerwear and underwear, the total fineness is more preferably 30 to 90 dtex. In addition, the single fiber fineness of the polyamide composite fiber is not specific, and is usually used in the range of 1.0 to 5.0 dtex.

[0058] Next, the method for producing the polyamide conjugate fiber of the present invention by melt spinning will be described.

[0059] In the crystalline polyamide used in the present invention, the relative viscosity of the crystalline polyamide (A) is preferably 3.1 to 3.8. In addition, the relative viscosity of the crystalline polyamide (B) is preferably 2.6 to 2.8. The relative viscosity ratio (A / B) of the crystalline polyamide (A) to the crystalline polyamide (B) is preferably 1.2 to 1.4.

[0060] By selecting a crystalline polyamide with a relative viscosity in this range, after heat treatment, it shows differential shrinkage, forms a three-dimensional helical structure and shows curling. In addition, in the silk-making step, the polyamide is subjected to the heat of melting, and changes from amorphous to crystalline. At this time, since the molecular binding force of the crystalline polyamide (A) with a higher relative viscosity is higher, its speed of changing from amorphous to crystalline is also slower than that of the crystalline polyamide (B) with a lower relative viscosity. Therefore, after being extruded from the spinning nozzle, if the polyamide is cooled while changing from amorphous to crystalline, it is easy to generate a hard amorphous in the intermediate state, the hard amorphous amount of the composite fiber increases, and the thermal shrinkage stress and the stretching elongation are improved.

[0061] In addition, the polyamide composite fiber of the present invention has a composite cross-section formed by joining two kinds of crystalline polyamides, and has an eccentric core-sheath structure in which the crystalline polyamide (A) belonging to the core component is covered by the crystalline polyamide (B) belonging to the sheath component. In the case of the conventional parallel structure in which the crystalline polyamide (A) is not covered by the crystalline polyamide (B) belonging to the sheath component, the crystalline polyamides with relative viscosity differences are melted separately and formed into a composite cross-section in the spinning assembly. When the polymers are discharged from the spinning nozzle, the flow resistance is different, and the yarn is easily bent due to the difference in flow speed, which deteriorates the workability. Therefore, when manufacturing the crystalline polyamide (A) and the crystalline polyamide (B) with different melt viscosities, by adopting the eccentric core-sheath structure of the present invention, stable manufacturing can be carried out using conventional equipment.

[0062] Next, a method for producing the polyamide conjugate fiber of the present invention by melt spinning and conjugate spinning will be described.

[0063] First, the method for producing the polyamide conjugate fiber of the present invention by high-speed direct spinning of melt spinning will be described below by way of example.

[0064] The crystalline polyamide (A) and the crystalline polyamide (B) are melted separately, metered and conveyed by a gear pump, and directly formed into a composite flow in a core-sheath structure by a conventional method, and an eccentric core-sheath type composite fiber spinning nozzle is used to form a composite fiber. Figure 1 The polyamide composite fiber filaments are discharged from the spinning nozzle in the manner of the cross section shown in the example. The discharged polyamide composite fiber filaments are cooled to 30°C by blowing cooling air through a filament cooling device such as a chimney type. Then, the cooled filaments are oiled and bundled by an oiling device, and are pulled at 1500 to 4000 m / min by a pulling roller, and are passed through a pulling roller and a stretching roller. At this time, they are stretched at a ratio of 1.5 to 3.0 times the peripheral speed of the pulling roller and the stretching roller. Furthermore, the filaments are heat-set by a stretching roller and wound into a package at a winding speed of more than 3000 m / min.

[0065] Furthermore, a method for producing the polyamide conjugate fiber of the present invention by high-speed direct spinning of melt spinning is described below by way of example.

[0066] The crystalline polyamide (A) and the crystalline polyamide (B) are melted separately, metered and conveyed by a gear pump, and directly formed into a composite flow in a core-sheath structure by a conventional method, and an eccentric core-sheath type composite fiber spinning nozzle is used to form a composite fiber. Figure 1 The polyamide composite fiber filaments are discharged from the spinning nozzle in the manner of the cross section shown in the example. The discharged polyamide composite fiber filaments are cooled to 30°C by blowing cooling air through a filament cooling device such as a chimney type. Then, the cooled filaments are oiled and bundled by an oiling device, and are pulled at 3000 to 4500 m / min by a pulling roller, and are passed through the pulling roller and the stretching roller. At this time, micro-stretching is performed at a ratio of 1.0 to 1.2 times the peripheral speed of the pulling roller and the stretching roller. Furthermore, the filaments are wound into a package at a winding speed of more than 3000 m / min.

[0067] In particular, the spinning temperature is appropriately designed based on the melting point of the crystalline polyamide (A) with a relatively high relative viscosity. If the spinning temperature becomes higher, the crystalline part increases and the rigid amorphous amount decreases. If the spinning temperature becomes lower, the movable amorphous amount increases and there is a tendency for the rigid amorphous amount to decrease slightly. Therefore, the spinning temperature is preferably a temperature 35 to 70°C higher than the melting point of the crystalline polyamide (A), and more preferably a temperature 45 to 60°C higher. By appropriately setting the spinning temperature, the rigid amorphous amount of the polyamide composite fiber of the present invention can be controlled, and the desired thermal shrinkage stress and stretching elongation can be obtained.

[0068] Furthermore, by appropriately designing the traction stretching (pulling speed), the rigid amorphous content of the polyamide composite fiber of the present invention increases, and the thermal shrinkage stress and the tensile elongation are improved. The pulling speed is preferably 1500 to 4000 m / min.

[0069] When obtaining a drawn yarn, by performing heat drawing using the drawing roller as a heating roller, the stiff amorphous content of the polyamide composite fiber of the present invention is increased and the heat shrinkage stress is improved. The drawing ratio is preferably 1.5 to 3.0 times, more preferably 2.0 to 3.0 times. In addition, the heat drawing temperature is preferably 30 to 90°C, more preferably 40 to 60°C.

[0070] Furthermore, by performing heat setting using the stretching roller as a heating roller, the heat shrinkage stress of the polyamide composite fiber of the present invention can be appropriately designed. The heat setting temperature is preferably 130 to 180°C.

[0071] In addition, the step before winding can also be carried out by using a known interlacing device. If necessary, the number of interlacing can be increased by applying multiple interlacing. Furthermore, additional oil can be applied when winding is approaching.

[0072] The processed yarn made of the polyamide composite fiber of the present invention is obtained by using the eccentric core-sheath type polyamide composite fiber of the present invention in at least a part of the yarn. The manufacturing method of the processed yarn is not limited, and examples thereof include a fiber blending method or a false twisting method. As a fiber blending method, air fiber blending, combined twisting, and composite false twisting can be applied. Air fiber blending can easily control fiber blending and has a low manufacturing cost, so it can be preferably used. As a false twisting method, it is preferred to use a needle type, a friction type, a belt type, etc. to implement false twisting in accordance with the fineness or the number of twists.

[0073] The processed yarn made of the polyamide composite fiber of the present invention preferably has a stretch elongation of 100% or more. By setting the stretch elongation to 100% or more, sufficient crimping performance and the crimping of the false twisted yarn are multiplied to obtain a fabric with excellent stretchability. The higher the stretch elongation, the greater the crimping property, but processing wrinkles are more likely to occur. In order to suppress wrinkles, the fabric is manufactured in a state where high tension is applied in the warp direction, which easily hinders the stretchability of the fabric. Therefore, the stretch elongation is preferably 120 to 200%.

[0074] The processed yarn made of the polyamide composite fiber of the present invention preferably has a stretch elongation of 100% or more as described above. The stretch elongation fabric is formed by using the polyamide composite fiber or processed yarn of the present invention in at least a part. According to the present invention, crimp can be fully expressed even when a high tension is applied to the warp direction in the wet heat step, and a fabric with excellent stretchability can be provided.

[0075] The stretchable fabric made of the polyamide composite fiber or processed yarn of the present invention can be woven (knitted) or knitted (woven) by a known method. In addition, the structure of the fabric is not limited.

[0076] In the case of woven fabrics, the weave may be plain weave, twill weave, satin weave, or any of these modified weaves and mixed weaves, depending on the purpose of use. In order to obtain a fabric with a clear texture and a fluffy feel, a plain weave with more restraint points, or a combination of a plain weave and a stone pattern (stone mesh), and a ripstop weave is preferred.

[0077] In the case of knitted fabrics, the structure can be a plain stitch structure of circular knitted fabrics, a double rib structure of warp knitted fabrics, a half structure of warp knitted fabrics, a satin structure, a jacquard texture, or any of these variations and mixed structures, depending on the purpose of use; from the viewpoint that the knitted fabric is thinner, more stable, and has excellent elongation, a half structure of a single tricot knitted fabric is preferred.

[0078] In addition, the use of the fabric composed of the polyamide composite fiber or processed yarn of the present invention is not limited, but is preferably used for clothing, and more preferably for sports, casual clothing or women's and gentlemen's clothing represented by down jackets, windbreakers, golf clothing, raincoats, etc. It is particularly suitable for use in sportswear and down jackets.

[0079] [Example]

[0080] Next, the polyamide conjugate fiber and processed yarn of the present invention will be specifically described by way of examples.

[0081] A. Melting point

[0082] Thermal analysis was performed using Q1000 manufactured by TA Instruments, and data processing was performed using Universal Analysis 2000. Thermal analysis was performed under a nitrogen flow (50 mL / min) at a temperature range of -50 to 300°C, a heating rate of 10°C / min, and a fragment sample mass of about 5 g (calorific value was normalized using the mass after measurement). The melting point was determined based on the melting peak.

[0083] B. Relative viscosity

[0084] 0.25 g of a polyamide chip sample was dissolved in 25 ml of 98% by mass sulfuric acid to a concentration of 1 g / 100 ml, and the flow time (T1) at 25° C. was measured using an Ostwald viscometer. Next, the flow time (T2) of only 98% by mass sulfuric acid was measured. The ratio of T1 to T2, i.e., T1 / T2, was defined as the relative viscosity of sulfuric acid.

[0085] C.Total fineness

[0086] According to JIS L1013. The fiber sample is subjected to a tension of 1 / 30 (g) and a length measuring machine with a yarn frame circumference of 1.125m is used to make 200 turns of skein. Dry at 105°C for 60 minutes and move to a dryer. Cool for 30 minutes at 20°C and 55% RH. Measure the weight of the skein, calculate the mass per 10,000m from the obtained value, set the official regain to 4.5%, and calculate the total fineness of the fiber filaments. The measurement is carried out 5 times, and the average value is set as the total fineness.

[0087] D. Thermal shrinkage stress

[0088] Using a KE-2 thermal shrinkage stress measuring machine manufactured by Kanebo Engineering, the fiber samples were connected into a ring with a circumference of 16 cm, an initial load of 1 / 30 g of the total fineness of the yarn was applied, and the load was measured when the temperature was changed from 40°C to 210°C at a heating rate of 100°C / min. The peak value of the obtained thermal stress curve was set as the thermal shrinkage stress.

[0089] E. Telescopic elongation

[0090] The fiber sample was wound into a hank, immersed in boiling water at 90°C for 20 minutes and air-dried, and a load of 2 mg / d was applied for 30 seconds to determine the length A, and then a load of 100 mg / d was applied for 30 seconds to determine the length B. The stretching elongation was calculated using the following formula.

[0091] Telescopic elongation (%) = [(BA) / B] × 100

[0092] F. Hard amorphous amount

[0093] The hard amorphous amount is measured using Q1000 manufactured by TA Instruments as a measuring machine. The difference (△Hm-△Hc) between the heat of fusion (△Hm) and the heat of cold crystallization (△Hc) obtained by differential scanning calorimetry (hereinafter referred to as DSC), the specific heat difference (△Cp) obtained by temperature-modulated DSC measurement, and further the theoretical value of polyamide being 100% crystalline (completely crystalline) and the theoretical value of polyamide being 100% amorphous (completely amorphous) are used. Here, △Hm0 is the heat of fusion of polyamide (completely crystalline). In addition, △Cp0 is the specific heat difference before and after the glass transition temperature (Tg) of polyamide (completely amorphous).

[0094] The crystallinity (Xc) and the movable amorphous content (Xma) are obtained by the following equations (1) and (2). Furthermore, the rigid amorphous content (Xra) is calculated by the following equation (3). The rigid amorphous content is calculated by the average value of these two measurements.

[0095] (1) Xc(%)=(△Hm-△Hc) / △Hm0×100

[0096] (2) Xma(%)=△Cp / △Cp0×100

[0097] (3) Xra (%) = 100 - (Xc + Xma)

[0098] The measurement conditions of DSC and temperature-modulated DSC are shown below.

[0099] (DSC measurement)

[0100] Measurement device: Q1000 manufactured by TA Instruments

[0101] Data processing: Universal Analysis 2000 manufactured by TA Instruments

[0102] Environment: Nitrogen flow (50mL / min)

[0103] Sample amount: about 10 mg

[0104] Sample container: Aluminum standard container

[0105] Temperature and heat correction: high purity indium (Tm = 156.61 ° C, △ Hm = 28.71 J / g)

[0106] Temperature range: about -50~300℃

[0107] Heating rate: 10℃ / min. First run

[0108] (Temperature modulation DSC measurement)

[0109] Measurement device: Q1000 manufactured by TA Instruments

[0110] Data processing: Universal Analysis 2000 manufactured by TA Instruments

[0111] Environment: Nitrogen flow (50mL / min)

[0112] Sample amount: about 5 mg

[0113] Sample container: Aluminum standard container

[0114] Temperature and heat correction: high purity indium (Tm = 156.61 ° C, △ Hm = 28.71 J / g)

[0115] Temperature range: about -50~210℃

[0116] Heating rate: 2℃ / min

[0117] G. Strength and elongation

[0118] The fiber sample was measured using "TENSILON" (registered trademark) and UCT-100 manufactured by ORIENTEC under the constant speed elongation conditions shown in JIS L1013 (Testing methods for chemical fiber yarns, 2010). The elongation was obtained from the elongation at the point showing the maximum strength in the tensile strength-extension curve. In addition, the strength was the value obtained by dividing the maximum strength by the fineness. The measurement was performed 10 times, and the average values ​​were set as the strength and elongation.

[0119] H. Water absorption rate in an environment with a temperature of 30°C and a relative humidity of 90RH%

[0120] According to JIS-L-1013 (2010 edition), the mass was measured after leaving it to stand at 30° C. and 90 RH% in an absolutely dry state for 72 hours, and the moisture regain was measured.

[0121] I. Evaluation of woven fabrics

[0122] (a) Manufacturing of weft yarn

[0123] Polycaprolactam (N6) (relative viscosity 2.70, melting point 222°C) was used, and a spinning nozzle with 12 spinning nozzle discharge holes was used to perform melt extrusion at a temperature of 275°C. After melt extrusion, the obtained filaments were cooled and oiled, interlaced, and then pulled by a pulling roller at 2570m / min, then stretched to 1.7 times and heat-set at a temperature of 155°C, and 70dtex12 monofilament nylon 6 filaments were obtained at a winding speed of 4000m / min.

[0124] (b) Manufacture of woven fabrics

[0125] The eccentric core-sheath polyamide composite yarns obtained in Examples 4 to 11 and Comparative Examples 1 to 3 were used as warps (warp density 90 s / 2.54 cm), and the nylon 6 yarns obtained in (a) were used as wefts (weft density 90 s / 2.54 cm) to weave a plain weave (warp / composite fiber) (apparent density 40 g / cm 2 In addition, the eccentric core-sheath type polyamide composite false twisted textured yarn obtained in Examples 1 to 3 was used as the warp (warp density 90 s / 2.54 cm), and the nylon 6 yarn obtained in (a) was used as the weft (weft density 90 s / 2.54 cm), and a plain weave fabric (warp / textured yarn) (apparent density 40 g / cm 2 ).

[0126] The obtained fabric was scoured at 80°C for 20 minutes, then dyed at 100°C for 30 minutes using Kayanol Yellow N5G 1% owf and acetic acid to adjust the pH to 4, then subjected to a fixation treatment at 80°C for 20 minutes, and finally heat treated at 170°C for 30 seconds to improve the texture.

[0127] (c) Elongation (stretchability) in the warp direction of woven fabrics

[0128] The fabric samples of 50 mm x 300 mm in width obtained in Examples 1 to 10 and Comparative Examples 1 to 4 were measured using a tensile tester, and the elongation was measured when the fabric samples were stretched to 14.7 N at a tension speed of 200 mm / min with a gripping interval of 200 mm in the warp direction of the fabric, and the evaluation was performed according to the following three stages "A", "B" and "C". 15% or more was judged to have stretchability.

[0129] A (good): more than 20%

[0130] B (allowable): 15% or more but less than 20%

[0131] C (Not acceptable): Less than 15%

[0132] [Example 1]

[0133] Nylon 6 (N6) with a relative viscosity of 3.3 and a melting point of 222°C was used as the crystalline polyamide (A), and nylon 610 (N610) with a relative viscosity of 2.7 and a melting point of 225°C was used as the crystalline polyamide (B). The crystalline polyamide (A) was used as the core component, and the crystalline polyamide (B) was used as the sheath component, and they were melted separately, and an eccentric core-sheath type composite fiber spinning nozzle (12 holes, round holes) was used, and the composite ratio (mass ratio) of the crystalline polyamide (A) and the crystalline polyamide (B) was set to crystalline polyamide (A): crystalline polyamide (B) = 5:5, and melt-discharging was performed (spinning temperature 270°C). The filaments discharged from the spinning nozzle are cooled and solidified by the filament cooling device, supplied with water-containing oil by the oil supply device, interlaced by the fluid interlacing nozzle device, and then pulled at 3700 m / min by the pulling roller (room temperature 25°C), stretched to 1.1 times between the stretching rollers (room temperature 25°C), and then wound into a package at a winding speed of 4000 m / min. A polyamide composite fiber filament with 62 dtex12 monofilament, 49% stretching elongation, 3.8% water absorption, 0.16 cN / dtex heat shrinkage stress, and 41% hard amorphous content is obtained.

[0134] The obtained polyamide composite fiber yarn was used to perform a disk false twist at a twist number (D / Y) of 1.95 in a state of being stretched at a heater temperature of 190°C at a ratio of 1.25, to obtain a false twisted yarn having a stretch elongation of 130%. The obtained false twisted yarn was used as a warp to form a woven fabric. The obtained woven fabric has excellent stretchability. The results are shown in Table 1.

[0135] [Example 2]

[0136] Except for using nylon 6 (N6) with a relative viscosity of 3.6 and a melting point of 222°C as the crystalline polyamide (A), the same method as Example 1 was used to obtain a polyamide composite fiber yarn with 62dtex12 monofilament, tensile elongation of 53%, water absorption of 3.8%, thermal shrinkage stress of 0.21cN / dtex, and stiff amorphous content of 46%.

[0137] The obtained polyamide composite fiber yarn was subjected to disk false twisting in the same manner as in Example 1 to obtain a false twisted yarn having a stretch elongation of 150%. The obtained false twisted yarn was used as a warp to form a woven fabric. The obtained woven fabric had excellent stretchability. The results are shown in Table 1.

[0138] [Example 3]

[0139] Except for using a copolymer of nylon 6 and nylon 66 (N6 / N66) with a relative viscosity of 3.6 and a melting point of 200°C as the crystalline polyamide (A), a polyamide composite fiber yarn with 62dtex12 monofilament, tensile elongation of 67%, water absorption of 3.6%, thermal shrinkage stress of 0.25cN / dtex, and stiff amorphous content of 53% was obtained in the same manner as in Example 1.

[0140] The obtained polyamide composite fiber yarn was subjected to disk false twisting in the same manner as in Example 1 to obtain a false twisted yarn having a stretch elongation of 200%. The obtained false twisted yarn was used as a warp to form a woven fabric. The obtained woven fabric had a better stretchability than that of Examples 1 and 2. The results are shown in Table 1.

[0141] Table 1

[0142]

[0143] [Example 4]

[0144] A copolymer of nylon 6 and nylon 66 (N6 / N66) with a relative viscosity of 3.6 and a melting point of 200°C was used as the crystalline polyamide (A), and nylon 610 (N610) with a relative viscosity of 2.7 and a melting point of 225°C was used as the crystalline polyamide (B). The crystalline polyamide (A) was used as the core component, and the crystalline polyamide (B) was used as the sheath component, and they were melted separately, and an eccentric core-sheath type composite fiber spinning nozzle (12 holes, round holes) was used, and the composite ratio (mass ratio) of the crystalline polyamide (A) and the crystalline polyamide (B) was set to crystalline polyamide (A): crystalline polyamide (B) = 5:5, and melt-discharging was performed (spinning temperature 270°C). The filaments discharged from the spinning nozzle are cooled and solidified by the filament cooling device, and after the non-aqueous oil is supplied by the oil supply device, the filaments are interlaced by the fluid interlacing nozzle device, and then pulled at 1700m / min by a slightly heated pulling roller (temperature 50°C), stretched to 2.4 times between heated stretching rollers (heat setting temperature: 150°C), and then wound into a package at a winding speed of 4000m / min. A polyamide composite fiber filament with 62dtex12 single yarn, 117% stretch elongation, 3.6% water absorption, 0.29cN / dtex heat shrinkage stress, and 55% stiff amorphous content is obtained. The obtained polyamide composite fiber filaments are used as warps to form woven fabrics. The obtained woven fabric has better stretchability than Example 5. The results are shown in Table 2.

[0145] [Example 5]

[0146] Nylon 6 (N6) with a relative viscosity of 3.3 and a melting point of 222°C was used as the crystalline polyamide (A), and nylon 610 (N610) with a relative viscosity of 2.7 and a melting point of 225°C was used as the crystalline polyamide (B). The crystalline polyamide (A) was used as the core component, and the crystalline polyamide (B) was used as the sheath component, and they were melted separately, and an eccentric core-sheath type composite fiber spinning nozzle (12 holes, round holes) was used to melt-dispense the composite fiber at a composite ratio of crystalline polyamide (A) to crystalline polyamide (B) = 5:5 (spinning temperature 270°C). The filaments discharged from the spinning nozzle are cooled and solidified by the filament cooling device, and after the non-aqueous oil is supplied from the oil supply device, the filaments are interlaced by the fluid interlacing nozzle device, and then pulled at 1700m / min by a slightly heated pulling roller (temperature 50°C), stretched to 2.4 times between the heated stretching rollers (heat setting temperature: 150°C), and then wound into a package at a winding speed of 4000m / min. A polyamide composite fiber filament with 62dtex12 single filament, 83% stretch elongation, 3.8% water absorption, 0.20cN / dtex heat shrinkage stress, and 46% stiff amorphous content is obtained. The obtained composite fiber filaments are used as warps to form fabrics. The obtained fabric has excellent stretchability. The results are shown in Table 2.

[0147] [Example 6]

[0148] Except that the composite ratio of crystalline polyamide (A) to crystalline polyamide (B) is set to crystalline polyamide (A): crystalline polyamide (B) = 4:6, a polyamide composite fiber yarn with 62dtex12 monofilament, 81% stretch elongation, 3.3% water absorption, 0.18cN / dtex heat shrinkage stress, and 45% rigid amorphous content is obtained in the same manner as in Example 5. The obtained polyamide composite fiber yarn is used as a warp to form a fabric. The obtained fabric has excellent stretchability. The results are shown in Table 2.

[0149] [Example 7]

[0150] Except that the composite ratio of crystalline polyamide (A) to crystalline polyamide (B) is set to crystalline polyamide (A): crystalline polyamide (B) = 6:4, a polyamide composite fiber yarn with 62dtex12 monofilament, 87% stretch elongation, 4.3% water absorption, 0.23cN / dtex heat shrinkage stress, and 47% rigid amorphous content is obtained in the same manner as in Example 5. The obtained polyamide composite fiber yarn is used as a warp to form a fabric. The obtained fabric has excellent stretchability. The results are shown in Table 2.

[0151] [Example 8]

[0152] In addition to using nylon 6 (N6) with a relative viscosity of 3.6 and a melting point of 222°C as the crystalline polyamide (A), and using a copolymer of nylon 610 and nylon 510 (N610 / N510) with a relative viscosity of 2.7 and a melting point of 225°C as the crystalline polyamide (B), a polyamide composite fiber yarn with 62 dtex12 monofilament, a stretch elongation of 103%, a water absorption of 4.1%, a heat shrinkage stress of 0.20 cN / dtex, and a stiff amorphous content of 46% was obtained in the same manner as in Example 5. The obtained polyamide composite fiber yarn was used as the warp to form a fabric. The obtained fabric has a better stretchability than that of Example 5. The results are shown in Table 2.

[0153] [Example 9]

[0154] In addition to using a slightly heated pulling roller (50°C) to pull at 2050m / min, and stretching to 2.0 times between heated stretching rollers (heat setting temperature: 150°C), a polyamide composite fiber yarn with 62dtex12 monofilament, 82% stretch elongation, 3.8% water absorption, 0.18cN / dtex heat shrinkage stress, and 43% hard amorphous content was obtained in the same manner as in Example 5. The obtained polyamide composite fiber yarn was used as a warp to form a fabric. The obtained fabric has excellent stretchability. The results are shown in Table 2.

[0155] [Example 10]

[0156] In the same manner as in Example 5, except that the spinning temperature was set to 280°C, a polyamide composite fiber yarn having a 62 dtex 12 monofilament, a stretch elongation of 82%, a water absorption of 3.8%, a heat shrinkage stress of 0.18 cN / dtex, and a stiff amorphous content of 43% was obtained. The obtained polyamide composite fiber yarn was used as a warp to form a fabric. The obtained fabric had excellent stretchability. The results are shown in Table 2.

[0157] [Example 11]

[0158] In the same manner as in Example 5, except that the spinning temperature was set to 260°C, a polyamide composite fiber yarn having a 62 dtex 12 monofilament, a stretch elongation of 95%, a water absorption of 3.8%, a heat shrinkage stress of 0.22 cN / dtex, and a stiff amorphous content of 49% was obtained. The obtained polyamide composite fiber yarn was used as a warp to form a fabric. The obtained fabric had excellent stretchability. The results are shown in Table 2.

[0159] [Comparative Example 1]

[0160] A polyamide composite yarn of 62 dtex 12 monofilament was obtained in the same manner as in Example 5, except that nylon 6 (N6) with a relative viscosity of 2.7 and a melting point of 222°C was used as the crystalline polyamide (A). The composite yarn of Comparative Example 1, which has almost no relative viscosity difference, has a small shrinkage difference after heat treatment and a low elongation of 13%, a heat shrinkage stress of 0.13 cN / dtex, and a rigid amorphous content of 39%. The obtained polyamide composite fiber yarn was used as a warp to form a fabric, and the resulting fabric had deteriorated stretchability. The results are shown in Table 2.

[0161] [Comparative Example 2]

[0162] A polyamide composite yarn of 62 dtex 12 monofilaments was obtained in the same manner as in Example 5, except that the composite ratio of crystalline polyamide (A) to crystalline polyamide (B) was set to crystalline polyamide (A): crystalline polyamide (B) = 7:3. The polyamide composite yarn of Comparative Example 2, in which the ratio of polyamide (A) having a higher water absorption rate was increased, had a water absorption rate as high as 5.8%. The obtained polyamide composite fiber yarn was used as a warp to form a woven fabric in the same manner as in Example 5, but since wrinkles remained, the tension was increased in the warp direction to a level where wrinkles did not remain, and processing was performed, resulting in a fabric with deteriorated stretchability. The results are shown in Table 2.

[0163] [Comparative Example 3]

[0164] A polyamide composite fiber yarn of 62 dtex 12 monofilament was obtained in the same manner as in Example 5, except that nylon 6 (N6) with a relative viscosity of 3.3 and a melting point of 222°C was used as the crystalline polyamide (A), and nylon 6 (N6) with a relative viscosity of 2.7 and a melting point of 225°C was used as the crystalline polyamide (B). The polyamide composite fiber yarn of Comparative Example 3, which was made using a similar polyamide with a higher water absorption rate, had a water absorption rate as high as 6.2%. The obtained polyamide composite fiber yarn was used as the warp to form a fabric in the same manner as in Example 5, but because wrinkles remained, the tension was increased in the warp direction to a level where no wrinkles remained, and processing was performed, resulting in a fabric with deteriorated stretchability. The results are shown in Table 2.

[0165] [Comparative Example 4]

[0166] Except that the spinning temperature was set to 300°C, a polyamide composite fiber yarn with 62 dtex 12 monofilament, 53% stretch elongation, 3.8% water absorption, 0.13 cN / dtex heat shrinkage stress, and 36% rigid amorphous content was obtained in the same manner as in Example 5. The obtained polyamide composite fiber yarn was used as a warp to form a fabric. The obtained fabric had deteriorated stretchability. The results are shown in Table 2.

[0167]

[0168] The present invention is described in detail using specific forms above, but those skilled in the art know that various changes and modifications can be made to the present invention without departing from the intent and scope of the present invention. In addition, this application is based on Japanese patent application (Special Application 2019-141540) filed on July 31, 2019, and its entire contents are introduced herein.

[0169] Description of the accompanying drawings

[0170] 1: Core component (crystalline polyamide (A))

[0171] 2: Sheath component (crystalline polyamide (B))

[0172] 10A~10D: Polyamide eccentric core-sheath composite fiber

Claims

1. A polyamide composite fiber, which is an eccentric core-sheath type polyamide composite fiber composed of a crystalline polyamide (A) and a crystalline polyamide (B), wherein the crystalline polyamide (A) and the crystalline polyamide (B) are two polyamides having different compositions from each other, the crystalline polyamide (A) has a sulfuric acid relative viscosity of 3.1 to 3.8, and the crystalline polyamide (B) has a sulfuric acid relative viscosity of 2.6 to 2.8, The polyamide composite fiber has a water absorption rate of 5.0% or less after being left to stand for 72 hours in an environment with a temperature of 30° C. and a relative humidity of 90 RH%, and The polyamide composite fiber has a heat shrinkage stress of 0.15 cN / dtex or more, a rigid amorphous content of 45-55%, The crystalline polyamide (A) is nylon 6 or a copolymer thereof, the crystalline polyamide (B) is nylon 610 or a copolymer thereof, the crystalline polyamide (A) is a core component, and the crystalline polyamide (B) is a sheath component.

2. A processed yarn made from the polyamide composite fiber according to claim 1.

3. The processed yarn according to claim 2, which has a stretch elongation of 100% or more.