Method for producing negative electrode material for lithium ion secondary battery and method for producing lithium ion secondary battery
By controlling the particle size distribution of the negative electrode material of lithium-ion secondary batteries and using dispersants, the problem of insufficient fast charging performance of lithium-ion secondary batteries is solved, achieving more efficient charging and discharging and extending battery life.
Patent Information
- Application Number
- CN201980099070.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-07-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-07-31
AI Technical Summary
Lithium-ion secondary batteries have insufficient fast charging performance in power supplies for electrical appliances, electric vehicles, and storage batteries, and it is necessary to improve battery performance to shorten charging time.
A method for manufacturing negative electrode materials for lithium ion secondary batteries is adopted, by obtaining a mixture containing a graphitizable aggregate and a binder, graphitizing and pulverizing it after shaping, and controlling the standard deviation of the particle size distribution of the aggregate to be less than or equal to 0.20 , use dispersants such as fatty acids to homogenize particle size and improve charging performance.
It achieves excellent fast charging performance of lithium-ion secondary batteries, improves the charge and discharge efficiency and cycle characteristics of the battery, and extends the battery life.
Smart Images

Figure GDA0004894675850000161
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a negative electrode material for a lithium ion secondary battery and a method for producing a lithium ion secondary battery. Background Art
[0002] Lithium-ion secondary batteries have a higher energy density than other secondary batteries such as nickel-cadmium batteries, nickel-hydrogen batteries, and lead-acid batteries, and are therefore widely used as power sources for portable electrical appliances such as notebook personal computers and mobile phones. In addition, lithium-ion secondary batteries are expected to be used not only in smaller electrical appliances, but also in electric vehicles, power sources for power storage, and the like.
[0003] Graphite is widely used as a negative electrode material (negative electrode material) for lithium ion secondary batteries. As a method for manufacturing a negative electrode material using graphite, for example, Patent Document 1 describes the following method: a mixture obtained by mixing a carbon material and a binder, etc., is crushed, the crushed material is graphitized in a state where it is formed using a mold, and the graphitized material is further crushed.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2015 / 147012 Summary of the invention
[0007] Problems to be solved by the invention
[0008] As the demand for lithium-ion secondary batteries in electrical appliances, electric vehicles, power sources for power storage, etc. increases, there is a demand for improved battery performance. As one of the battery performances of lithium-ion secondary batteries, it is required to shorten the charging time at the charging point, that is, to improve the rapid charging performance.
[0009] In view of the above, an object of the present invention is to provide a method for producing a negative electrode material for a lithium ion secondary battery capable of producing a lithium ion secondary battery having excellent rapid charging performance, and a method for producing a lithium ion secondary battery having excellent rapid charging performance.
[0010] Means for solving problems
[0011] Specific means for solving the above-mentioned problems include the following embodiments.
[0012] <1> A method for producing a negative electrode material for a lithium ion secondary battery, comprising: (a) obtaining a mixture containing a graphitizable aggregate and a graphitizable binder, (b) forming the mixture to obtain a formed product, (c) graphitizing the formed product to obtain a graphitized product, and (d) pulverizing the graphitized product to obtain a pulverized product.
[0013] The standard deviation of the particle size distribution of the above-mentioned aggregate is less than or equal to 0.20.
[0014] <2> The method for producing a negative electrode material for a lithium ion secondary battery according to <1>, wherein the mixture contains a dispersant.
[0015] <3> The method for producing a negative electrode material for a lithium ion secondary battery according to <2>, wherein the dispersant contains a fatty acid.
[0016] <4> The method for producing a negative electrode material for a lithium ion secondary battery according to any one of <1> to <3>, wherein the amount of the binder blended is 25% by mass or less based on the mixture.
[0017] <5> A method for producing a lithium ion secondary battery, comprising the step of producing a negative electrode using a negative electrode material, wherein the negative electrode material is obtained by the method for producing a negative electrode material for a lithium ion secondary battery according to any one of <1> to <4>.
[0018] <6> A method for producing a lithium ion secondary battery, comprising: a step of producing a negative electrode material for a lithium ion secondary battery by the method for producing a negative electrode material for a lithium ion secondary battery according to any one of <1> to <4>; and a step of producing a negative electrode using the negative electrode material for a lithium ion secondary battery.
[0019] Effects of the Invention
[0020] According to the present invention, a method for producing a negative electrode material for a lithium ion secondary battery capable of producing a lithium ion secondary battery having excellent rapid charging performance, and a method for producing a lithium ion secondary battery having excellent rapid charging performance can be provided. DETAILED DESCRIPTION
[0021] Hereinafter, the mode for implementing the present invention is described in detail. However, the present invention is not limited to the following embodiments. In the following embodiments, its constituent elements (including element steps, etc.) are not necessary except for the cases that are particularly clearly indicated, the cases that are considered to be obviously necessary in principle, etc. The same is true about numerical values and their ranges, and the present invention is not limited.
[0022] In the present disclosure, the term "process" includes processes that are independent of other processes and processes that cannot be clearly distinguished from other processes as long as the purpose of the process can be achieved.
[0023] In the present disclosure, in a numerical range represented by “to”, the numerical values described before and after including “to” are respectively regarded as the minimum value and the maximum value.
[0024] In the numerical range recorded in stages in the present disclosure, the upper limit or lower limit recorded in one numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in the present disclosure, the upper limit or lower limit of the numerical range can also be replaced by the value shown in the embodiment.
[0025] In the present disclosure, each component may include a plurality of substances corresponding to each component. When a plurality of substances corresponding to each component are present in the composition, the content or content of each component refers to the total content or content of the plurality of substances present in the composition unless otherwise specified.
[0026] In the present disclosure, multiple types of particles corresponding to each component may be included. When multiple types of particles corresponding to each component exist in the composition, unless otherwise specified, the particle size of each component refers to the value for the mixture of the multiple types of particles present in the composition.
[0027] In the present disclosure, the term "layer" includes not only a case where the layer is formed in the entire region when the region where the layer exists is observed, but also a case where the layer is formed in only a part of the region.
[0028] <Method for producing negative electrode material for lithium-ion secondary battery>
[0029] The method for producing a negative electrode material for a lithium ion secondary battery (hereinafter, also referred to as a negative electrode material) disclosed in the present invention comprises:
[0030] (a) a step of obtaining a mixture comprising a graphitizable aggregate and a graphitizable binder,
[0031] (b) forming the mixture to obtain a formed product,
[0032] (c) a step of graphitizing the molded product to obtain a graphitized product, and
[0033] (d) a step of crushing the graphitized material to obtain a crushed material,
[0034] The standard deviation of the particle size distribution of the above-mentioned aggregate is less than or equal to 0.20.
[0035] In the above method, an aggregate having a standard deviation of particle size distribution less than or equal to 0.20 is used as a graphitizable aggregate to manufacture a negative electrode material. That is, in the method, an aggregate having an uneven particle size distribution is used, a mixture comprising the aggregate and a graphitizable binder is modulated, a formed object obtained from the modulated mixture is graphitized, and then the graphitized object is crushed. Thus, compared with the case where a graphitized object obtained by crushing an aggregate having an uneven particle size distribution, a crushed object with a small uneven particle size can be obtained. By using a negative electrode material comprising a crushed object with a small uneven particle size for the manufacture of a lithium ion secondary battery, the resistance distribution in the negative electrode can be uniformized, and as a result, a lithium ion secondary battery with excellent fast charging performance can be manufactured.
[0036] Each step of the above method can be carried out continuously or discontinuously. In addition, each step of the above method can be carried out in the same place or in different places.
[0037] In step (a), a mixture containing a graphitizable aggregate and a graphitizable binder is obtained. The method for obtaining the mixture is not particularly limited, and a kneader or the like may be used. The mixing is preferably performed at a temperature at which the graphitizable binder softens. Specifically, when the graphitizable binder is asphalt, coal tar, etc., the temperature may be 50°C to 300°C, and when the graphitizable binder is a thermosetting resin, the temperature may be 20°C to 100°C.
[0038] The graphitizable aggregate is not particularly limited as long as it is an aggregate that can be graphitized by graphitization treatment. Specifically, cokes such as fluidized coke, needle coke, and mosaic coke can be cited, and needle coke is preferably used. The graphitizable aggregate is preferably in a particle form.
[0039] The average particle size of the graphitizable aggregate is, for example, preferably 5 to 40 μm, more preferably 10 to 30 μm, and even more preferably 10 to 25 μm. The average particle size is, for example, a volume average particle size (D50) measured by a laser diffraction-scattering method described below.
[0040] The standard deviation of the particle size distribution of the graphitizable aggregate is less than or equal to 0.20, preferably less than or equal to 0.18, and more preferably less than or equal to 0.16. By the standard deviation of the particle size distribution of the above-mentioned aggregate being less than or equal to 0.20, the uneven particle size of the aggregate can be reduced, and the uneven particle size of the obtained crushed material can also be suppressed. As a result, the fast charging performance of the lithium ion secondary battery is improved. Further, by reducing the uneven particle size of the aggregate, even if the content or content of the graphitizable adhesive is reduced, the function as an adhesive can be appropriately ensured. The standard deviation of the particle size distribution is, for example, a value (volume basis) measured by the laser diffraction-scattering method described later.
[0041] The lower limit of the standard deviation of the particle size distribution of the graphitizable aggregate is not particularly limited, and may be, for example, 0.05 or more, or 0.10 or more.
[0042] Examples of methods for adjusting the average particle size of the graphitizable aggregate and the standard deviation of the particle size distribution of the graphitizable aggregate to the above ranges include classification using a sieve, wind classification, wet classification, and the like.
[0043] The graphitizable binder is not particularly limited as long as it is a binder that can be graphitized by graphitization treatment, and specific examples thereof include coal-based, petroleum-based, and artificial asphalt and coal tar, thermoplastic resins, and thermosetting resins.
[0044] The proportion of each material in the mixture is not particularly limited. For example, the content of the graphitizable binder can be 10 to 30 parts by mass, 12 to 25 parts by mass, or 14 to 20 parts by mass relative to 100 parts by mass of the graphitizable aggregate. If the amount of the binder is greater than or equal to 10 parts by mass, it tends to function as a binder for the graphitizable aggregate. If the amount of the binder is less than or equal to 30 parts by mass, the amount of fixed carbon in the mixture can be fully ensured, and there is a tendency for excellent yield.
[0045] The content of the graphitizable binder relative to 100 mass % of the mixture is preferably 25 mass % or less, more preferably 20 mass % or less, further preferably 10 mass % to 19 mass %, particularly preferably 12 mass % to 18 mass %.
[0046] The graphitizable aggregate and the graphitizable binder contained in the mixture may be only one kind, or may be two or more kinds. In addition, the mixture may also contain components other than these. As components other than the graphitizable aggregate and the graphitizable binder, graphite, dispersant, graphitization catalyst, etc. may be cited.
[0047] The mixture may contain graphite. Examples of graphite include natural graphite and artificial graphite. The graphite is preferably in the form of particles. The mixture may contain only one type of graphite or two or more types of graphite.
[0048] From the viewpoint of easily dispersing the components in the mixture in step (b), the mixture preferably contains a dispersant. By including a dispersant in the mixture, it is possible to suppress the uneven particle size of the pulverized product obtained by pulverizing the graphitized product, and it is easy to obtain a pulverized product with a uniform particle size. As a result, there is a tendency for the rapid charging performance of the lithium ion secondary battery to be improved.
[0049] Furthermore, when the mixture contains a dispersant, it contributes to suppressing the amount of the graphitizable binder, and can also be expected to improve battery characteristics such as the initial charge and discharge efficiency of the negative electrode material.
[0050] There is no particular restriction on the type of dispersant. Specifically, there can be listed: hydrocarbons such as liquid paraffin, solid paraffin, polyethylene wax; fatty acids such as stearic acid, oleic acid, erucic acid, 12-hydroxystearic acid; fatty acid metal salts such as zinc stearate, lead stearate, aluminum stearate, calcium stearate, magnesium stearate; fatty acid amides such as stearic acid amide, oleic acid amide, erucic acid amide, methylene bis stearic acid amide, ethylene bis stearic acid amide; fatty acid esters such as monoglyceride of stearic acid, stearyl stearate, hydrogenated oil; higher alcohols such as stearyl alcohol, etc. Among them, fatty acids are not easy to affect the performance of negative electrode materials, are solid at room temperature and are therefore easy to handle, melt at the temperature of step (a) and are therefore evenly dispersed, disappear in the process until graphitization, and are cheap, so they are preferred, and more preferably stearic acid.
[0051] When the mixture contains a dispersant, the amount thereof is not particularly limited. For example, the content of the dispersant relative to the entire mixture may be 0.1% to 20% by mass, 0.5% to 10% by mass, or 0.5% to 5% by mass.
[0052] From the viewpoint of promoting graphitization of the graphitizable aggregate or binder, the mixture preferably contains a graphitization catalyst. The type of graphitization catalyst is not particularly limited. Specifically, materials having a graphitization catalyst function such as silicon, iron, nickel, titanium, boron, and carbides, oxides, nitrides, etc. of these materials can be cited.
[0053] When the mixture contains a graphitization catalyst, the amount thereof is not particularly limited. For example, the content of the graphitization catalyst relative to the entire mixture may be 0.1% to 50% by mass, 0.5% to 40% by mass, or 0.5% to 30% by mass.
[0054] In step (b), the mixture obtained in step (a) is formed to obtain a formed product. Preferably, the formed product is formed into a predetermined shape by uniaxial pressing or the like. By forming the formed product in this way, the amount of the mixture to be filled into the graphitization furnace can be increased when the mixture is graphitized, thereby improving productivity or enhancing the effect of the graphitization catalyst.
[0055] In step (b), there is no particular limitation on the method for molding the mixture. Examples include: a molding method in which the mixture is placed in a container such as a mold and pressurized in a uniaxial direction; a vibration molding method in which the mixture is placed in a container such as a mold and a weight is placed on the upper surface to impart vibration and impact to the mold frame; an extrusion molding method in which the mixture is extruded from a nozzle or the like by lateral pressing and pressing to form the mixture.
[0056] In step (b), the density of the obtained molded product is not particularly limited, but is preferably less than or equal to 1.3 g / cm from the viewpoint of productivity of the negative electrode material and cycle characteristics of the lithium ion secondary battery. 3 , more preferably 0.8 g / cm 3 ~1.2g / cm 3 , more preferably 0.9 g / cm 3 ~1.1g / cm 3 .
[0057] The molded product obtained in step (b) is preferably subjected to heat treatment before graphitizing the molded product in step (c). By performing heat treatment, organic components contained in the mixture that do not contribute to graphitization can be removed, and there is a tendency to suppress gas generation during graphitization.
[0058] The temperature of the heat treatment is not particularly limited, but is preferably a temperature lower than the heat treatment temperature in step (c), and can be performed, for example, in the range of 500°C to 1000°C.
[0059] In step (c), the molded product obtained in step (b) is graphitized. As long as the conditions under which the graphitizable components contained in the mixture can be graphitized are met, the method of graphitizing the molded product is not particularly limited. For example, a method of heat treating the mixture in an atmosphere that is difficult to oxidize can be cited. The atmosphere that is difficult to oxidize the mixture is not particularly limited, and can be cited as an inactive atmosphere such as nitrogen, argon, vacuum, etc.
[0060] The heat treatment temperature for graphitization may be, for example, greater than or equal to 1500°C, greater than or equal to 2000°C, greater than or equal to 2500°C, or greater than or equal to 2800°C. There is no particular limit to the upper limit of the heat treatment temperature, and for example, it may be less than or equal to 3200°C. If the heat treatment temperature is greater than or equal to 1500°C, changes in crystallization will occur, and graphitization tends to be easy to perform. If the sintering temperature is greater than or equal to 2000°C, the crystal growth of graphite tends to become better. On the other hand, if the heat treatment temperature for graphitization is less than or equal to 3200°C, there is a tendency to suppress the sublimation of part of the graphite.
[0061] In step (d), the graphitized product obtained in step (c) is pulverized to obtain a pulverized product. The pulverization method is not particularly limited, and it can be carried out using a jet mill, a vibration mill, a pin mill, a hammer mill, etc. using a known method. The pulverized product can be adjusted in a manner to have a desired size. The method for adjusting the particle size is not particularly limited, and examples thereof include a method using the above-mentioned pulverization device, a method using a sieve, and the like.
[0062] If necessary, the pulverized product obtained in step (d) may be subjected to steps such as (e) disposing low-crystalline carbon on at least a portion of the surface of the pulverized product, (f) mixing the pulverized product with other negative electrode active materials, and the like.
[0063] As a method for configuring low-crystalline carbon on at least a portion of the surface of the pulverized product in step (e), for example, a method of mixing a substance (resin, etc.) that can become low-crystalline carbon by heat treatment with the pulverized product and performing heat treatment can be cited. If low-crystalline carbon is configured on at least a portion of the surface of the pulverized product, the input-output characteristics such as the rapid charge and discharge characteristics of a lithium ion secondary battery using it as a negative electrode material are sometimes improved.
[0064] There is no particular limitation on the method of mixing the pulverized material with other negative electrode active materials in step (f). By mixing the pulverized material with other negative electrode active materials, the desired properties of the lithium ion secondary battery can sometimes be improved compared to the case where the pulverized material is used alone as a negative electrode active material. As other negative electrode active materials, graphite particles such as natural graphite and artificial graphite, particles containing elements that can absorb and release lithium ions, etc. can be listed, but they are not limited to them. As elements that can absorb and release lithium ions, there are no particular limitations, for example, Si, Sn, Ge, In, etc. can be listed.
[0065] The pulverized material obtained in step (f) may include particles in which a plurality of flat graphite particles are aggregated or combined, or may include particles in which a plurality of flat graphite particles are aggregated or combined in a manner in which the main surfaces of the graphite particles are not parallel to each other (hereinafter also referred to as graphite secondary particles).
[0066] If the pulverized product is in the form of graphite secondary particles, the negative electrode material particles are suppressed from being oriented along the current collector during pressing for increasing the density of the negative electrode, and paths for lithium ions entering and exiting the negative electrode material tend to be sufficiently ensured.
[0067] Furthermore, by including particles in a state where a plurality of flat graphite particles are aggregated or combined, the voids between the plurality of flat graphite particles can be utilized to reduce the effect of the pressure applied during pressing on the individual graphite particles, and there is a tendency to suppress the destruction of the graphite particles, the generation of cracks, etc.
[0068] In the present disclosure, "flat graphite particles" refer to non-spherical graphite particles having anisotropy in shape. Examples of flat graphite particles include graphite particles having shapes such as scales, flakes, and partial blocks.
[0069] For flat graphite particles, when the length in the long axis direction is A and the length in the short axis direction is B, the aspect ratio represented by A / B is preferably 1.2 to 20, and more preferably 1.3 to 10. If the aspect ratio is greater than or equal to 1.2, the contact area between the particles increases, and there is a tendency for the conductivity to be further improved. If the aspect ratio is less than or equal to 20, there is a tendency for the input and output characteristics such as the rapid charge and discharge characteristics of the lithium ion secondary battery to be further improved.
[0070] The aspect ratio is obtained by observing the graphite particles under a microscope, randomly selecting 100 graphite particles to measure their respective A / B, and taking the arithmetic mean of these measured values. In the observation of the aspect ratio, the length A in the major axis direction and the length B in the minor axis direction are measured as follows. That is, in the projected image of the graphite particles observed using a microscope, the tangent a1 and the tangent a2 are selected as two parallel tangents circumscribed to the periphery of the graphite particles and the distance between the two tangents is the largest, and the distance between the tangent a1 and the tangent a2 is set as the length A in the major axis direction. In addition, the tangent b1 and the tangent b2 are selected as two parallel tangents circumscribed to the periphery of the graphite particles and the distance between the two tangents is the smallest, and the distance between the tangent b1 and the tangent b2 is set as the length B in the minor axis direction.
[0071] In the present disclosure, the so-called "non-parallel principal surface" of the graphite secondary particles refers to that the surface (principal surface) with the largest cross-sectional area of a plurality of flat graphite particles is not aligned in a certain direction. Whether the principal surfaces of a plurality of flat graphite particles are non-parallel to each other can be confirmed by microscopic observation. By a plurality of flat graphite particles being assembled or combined in a state where the principal surfaces are not parallel to each other, the orientation of the principal surfaces of the flat graphite particles in the negative electrode can be suppressed, the expansion of the negative electrode accompanying charging can be suppressed, and the cycle characteristics of the lithium-ion secondary battery tend to be further improved.
[0072] In addition, the graphite secondary particles may partially include a structure in which a plurality of flat graphite particles are aggregated or bonded so that their main surfaces are parallel to each other.
[0073] In the present disclosure, the so-called "aggregate or bonded state" of a plurality of flat graphite particles refers to a state in which two or more flat graphite particles are aggregated or bonded. The so-called "bonding" refers to a state in which the particles are chemically bonded to each other directly or via a carbon substance. The so-called "aggregation" refers to a state in which the particles are not chemically bonded to each other, but maintain a shape as an aggregate due to their shape, etc. The flat graphite particles may also be aggregated or bonded via a carbon substance. As the carbon substance, for example, graphitized materials of graphitizable adhesives can be cited. From the viewpoint of mechanical strength, it is preferred that two or more flat graphite particles are bonded via a carbon substance. Whether the flat graphite particles are aggregated or bonded can be confirmed, for example, by observation using a scanning electron microscope.
[0074] From the viewpoint of the ease of aggregation or combination, the average particle size of the flat graphite particles is, for example, preferably 1 μm to 50 μm, more preferably 1 μm to 25 μm, and further preferably 1 μm to 15 μm. As a method for measuring the average particle size of the flat graphite particles, a method for measuring by a scanning electron microscope can be cited, and the average particle size of the flat graphite particles is, for example, the arithmetic mean of the particle sizes of 100 flat graphite particles.
[0075] The flat graphite particles and their raw materials are not particularly limited, and examples thereof include artificial graphite, scaly natural graphite, flaky natural graphite, coke, resin, coal tar, asphalt, etc. Among them, graphite obtained from artificial graphite, natural graphite, or coke has a tendency to easily densify the negative electrode due to its high crystallinity and soft particles.
[0076] The negative electrode material may include spherical graphite particles. When the negative electrode material includes spherical graphite particles, since the spherical graphite particles themselves have a high density, there is a tendency that the pressing pressure required to obtain a desired electrode density can be reduced.
[0077] As spherical graphite particles, spherical artificial graphite, spherical natural graphite, etc. can be cited. From the viewpoint of high density of the negative electrode, the spherical graphite particles are preferably high-density graphite particles. Specifically, it is preferably spherical natural graphite that can be high-density by implementing particle spheroidization treatment. Furthermore, the negative electrode material layer containing spherical natural graphite has excellent peel strength and tends to be difficult to peel off from the collector even with strong pressure.
[0078] When the negative electrode material includes spherical graphite particles, the flat graphite particles and spherical graphite particles may be included. When the negative electrode material includes the flat graphite particles and spherical graphite particles, the ratio of the two is not particularly limited and can be set according to the desired electrode density, the pressure conditions during pressing, the desired battery characteristics, etc.
[0079] In the case where the negative electrode material includes flat graphite particles and spherical graphite particles, there can be cited a state where flat graphite particles are mixed with spherical graphite particles, a state where flat graphite particles are combined with spherical graphite particles (hereinafter also referred to as composite particles), etc. As composite particles, for example, there can be cited particles in a state where flat graphite particles and spherical graphite particles are combined via carbides of organic matter.
[0080] The composite particles can be produced, for example, by using a mixture containing flat graphite particles or a raw material thereof and spherical graphite particles as the mixture in the step (a).
[0081] The average particle size of the negative electrode material manufactured by the above method is not particularly limited. For example, it is preferably 5 μm to 40 μm, more preferably 10 μm to 30 μm, and further preferably 10 μm to 25 μm. The average particle size can be measured by a scanning electron microscope in the same manner as the average particle size of the flat graphite particles, or it can be a volume average particle size (D50) measured by a laser diffraction-scattering method.
[0082] As a method for measuring the average particle size when using a negative electrode material to manufacture an electrode (negative electrode), the following methods can be cited, namely: making a sample electrode, burying the electrode in an epoxy resin, mirror polishing, and observing the electrode cross section by a scanning electron microscope (e.g., Keyence Co., Ltd., "VE-7800"); using an ion polishing device (e.g., Hitachi High-Tech Co., Ltd., "E-3500") to make an electrode cross section, and measuring it by a scanning electron microscope (e.g., Keyence Co., Ltd., "VE-7800"), etc. The average particle size in this case is the median value of 100 particle sizes arbitrarily selected from the observed particles.
[0083] The above-mentioned sample electrode can be prepared, for example, by the following method: a mixture of 98 parts by mass of negative electrode material, 1 part by mass of styrene butadiene resin as a binder, and 1 part by mass of carboxymethyl cellulose as a thickening agent is used as a solid component, water is added to prepare a dispersion, the above-mentioned dispersion is applied on a copper foil with a thickness of 10 μm to a thickness of about 70 μm (when applied), and then dried at 105°C for 1 hour.
[0084] The orientation of the negative electrode material when it is made into a negative electrode (when the negative electrode is produced with a pressing step, it is the pressed negative electrode) may be less than or equal to 40, less than or equal to 20, or less than or equal to 15. In addition, the orientation may be greater than or equal to 10.
[0085] The orientation of the negative electrode material is an indicator of the degree of orientation of the particles of the negative electrode material contained in the negative electrode. A low orientation means that the particles of the negative electrode material are oriented in random directions. In other words, it means that the orientation of the graphite particles along the surface of the collector due to the pressure during pressing is suppressed.
[0086] In the present disclosure, the orientation of the negative electrode is determined by measuring the surface of the sample electrode using an X-ray diffraction device using CuKα rays as an X-ray source. Specifically, the X-ray diffraction pattern of the sample electrode surface is measured and the orientation is determined by the following formula (1) based on the intensity of the carbon (004) plane diffraction peak detected near the diffraction angle 2θ = 53° to 56° and the carbon (110) plane diffraction peak detected near the diffraction angle 2θ = 70° to 80°.
[0087] (004) plane diffraction peak intensity / (110) plane diffraction peak intensity····Formula (1)
[0088] From the viewpoint of cycle characteristics and storage characteristics, the specific surface area of the negative electrode material is preferably less than or equal to 3.0 m 2 / g, more preferably 0.5m 2 / g~2.5m 2 / g, more preferably 0.7m 2 / g~2.0m 2 / g.
[0089] Regarding the specific surface area of the negative electrode material, it is sufficient to use a specific surface area / pore distribution measuring device (for example, Flowsorb III 2310, Shimadzu Corporation), use a mixed gas of nitrogen and helium (nitrogen:helium = 3:7), and measure the nitrogen adsorption at liquid nitrogen temperature (77K) by the one-point method at a relative pressure of 0.3, and calculate it by the BET method.
[0090] <Method for producing lithium-ion secondary battery]
[0091] A first embodiment of a method for producing a lithium ion secondary battery disclosed herein includes a step of producing a negative electrode using a negative electrode material obtained by the method for producing a negative electrode material described above.
[0092] A second embodiment of the method for producing a lithium ion secondary battery of the present disclosure includes a step of producing a negative electrode material by the method for producing a negative electrode material, and a step of producing a negative electrode using the negative electrode material.
[0093] There is no particular limitation on the method for preparing the negative electrode using the negative electrode material. For example, the following method can be mentioned, namely, forming a negative electrode material layer on a current collector using a composition containing a negative electrode material, a binder and a solvent, and performing heat treatment, pressing treatment and the like as needed.
[0094] The adhesive contained in the composition is not particularly limited. For example, it can be listed as follows: styrene-butadiene rubber, a polymer compound using ethylenically unsaturated carboxylic acid esters (methyl (meth) acrylate, ethyl (meth) acrylate, butyl (meth) acrylate, hydroxyethyl (meth) acrylate, etc.) as a polymerization component, a polymer compound using ethylenically unsaturated carboxylic acids (acrylic acid, methacrylic acid, itaconic acid, fumaric acid, maleic acid, etc.) as a polymerization component, polyvinylidene fluoride, polyethylene oxide, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polyimide, polyamide-imide and other polymer compounds. In the present disclosure, (meth) acrylate refers to either or both of methacrylate and acrylate.
[0095] The solvent contained in the composition is not particularly limited, and specifically, organic solvents such as N-methylpyrrolidone, dimethylacetamide, dimethylformamide, and γ-butyrolactone, and water can be used.
[0096] The composition may contain a thickener for adjusting the viscosity as necessary. Examples of the thickener include carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, polyacrylic acid and salts thereof, oxidized starch, phosphorylated starch, and casein.
[0097] The composition may contain a conductive additive as required. Examples of the conductive additive include carbon black, graphite, acetylene black, conductive oxides, and conductive nitrides.
[0098] The material and shape of the current collector used to make the negative electrode are not particularly limited. For example, materials such as strip foils containing metals or alloys such as aluminum, copper, nickel, titanium, and stainless steel; strip perforated foils; and strip meshes can be used. In addition, porous materials such as porous metals (foamed metals) and carbon paper can also be used.
[0099] The method for forming the negative electrode material layer on the current collector using the composition is not particularly limited, and can be carried out by known methods such as metal mask printing, electrostatic coating, dip coating, spraying, roller coating, scraper method, gravure coating, screen printing, etc. In the case of integrating the above-mentioned negative electrode material layer with the current collector, it can be carried out by known methods such as roller, pressing, combinations thereof, etc.
[0100] After the negative electrode material layer is formed on the current collector, heat treatment (drying) can be performed. By performing heat treatment, the solvent contained in the negative electrode material layer can be removed, and the high strength caused by the solidification of the binder can be promoted, which can improve the adhesion between particles and between particles and the current collector. In order to prevent oxidation of the current collector during the treatment process, the heat treatment can be carried out in an inactive atmosphere such as helium, argon, nitrogen, or a vacuum atmosphere.
[0101] After the negative electrode material layer is formed on the current collector, a pressing process may be performed. By performing the pressing process, the electrode density of the negative electrode can be adjusted. The electrode density of the negative electrode is not particularly limited and may be 1.5 g / cm 3 ~1.9g / cm 3 , can also be 1.6g / cm 3 ~1.8g / cm 3 The higher the electrode density, the higher the volume capacity of the negative electrode, the better the adhesion of the negative electrode material layer to the current collector, and the better the cycle characteristics. The pressing treatment is preferably performed before the heat treatment.
[0102] The lithium ion secondary battery manufactured by the above method may include a negative electrode, a positive electrode and an electrolyte manufactured by the above method. The lithium ion secondary battery may be configured, for example, in which a negative electrode and a positive electrode are arranged to face each other with a separator interposed therebetween and an electrolyte solution containing an electrolyte is injected.
[0103] Similar to the negative electrode, the positive electrode can be prepared by forming a positive electrode layer on the surface of a current collector. As the current collector, a strip-shaped foil containing a metal or alloy such as aluminum, titanium, stainless steel, etc.; a strip-shaped perforated foil; a strip-shaped mesh, etc. can be used.
[0104] There is no particular limitation on the positive electrode material contained in the positive electrode layer. For example, metal compounds, metal oxides, metal sulfides, and conductive polymer materials that can be doped or embedded with lithium ions can be listed. Furthermore, the following substances can be used alone or in combination of two or more: lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2), and their composite oxides (LiCo x Ni y Mn z O2, x+y+z=1, 0<x, 0<y; LiNi 2-x Mn x O4, 0<x≤2), lithium manganese spinel (LiMn2O4), lithium vanadium compounds, V2O5, V6O 13 , VO2, MnO2, TiO2, MoV2O8, TiS2, V2S5, VS2, MoS2, MoS3, Cr3O8, Cr2O5, olivine-type LiMPO4 (M: Co, Ni, Mn, Fe), polyacetylene, polyaniline, polypyrrole, polythiophene, polyacene and other conductive polymers, porous carbon, etc. Among them, lithium nickel oxide (LiNiO2) and its composite oxide (LiCo x Ni y Mn z O2, x+y+z=1, 0<x, 0<y; LiNi 2-x Mn x O4, 0<x≤2) is suitable as a positive electrode material due to its high capacity.
[0105] Examples of the separator include nonwoven fabrics, fabrics, microporous films, and combinations thereof, which are mainly composed of polyolefins such as polyethylene and polypropylene. In addition, when the lithium ion secondary battery has a structure in which the positive electrode and the negative electrode are not in contact, a separator is not required.
[0106] As the electrolyte, the so-called organic electrolyte solution can be used, which is prepared by dissolving lithium salts such as LiClO4, LiPF6, LiAsF6, LiBF4, LiSO3CF3 in a non-aqueous solvent such as ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, cyclopentanone, sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolin-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, butyl ethyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, ethyl acetate, etc., alone or as a mixture of two or more components. Among them, an electrolyte solution containing fluoroethylene carbonate is preferred because it tends to form a stable SEI (solid electrolyte interface) on the surface of the negative electrode material and the cycle characteristics are significantly improved.
[0107] The form of the lithium ion secondary battery is not particularly limited, and examples thereof include paper type batteries, button type batteries, coin type batteries, laminated type batteries, cylindrical type batteries, square type batteries, etc. In addition, the above-mentioned negative electrode material for lithium ion secondary batteries can also be applied to all electrochemical devices such as hybrid capacitors that use the insertion and extraction of lithium ions as a charging and discharging mechanism, in addition to lithium ion secondary batteries.
[0108] Example
[0109] Hereinafter, the above-mentioned embodiment will be described in more detail based on examples, but the above-mentioned embodiment is not limited to the following examples.
[0110] [Examples 1 to 3 and Comparative Example 1]
[0111] (1) Modification of negative electrode materials
[0112] For the needle coke as a raw material, the coke was finely pulverized using a free pulverizer manufactured by Nara Machinery Manufacturing Co., Ltd., and then air-classified using Turboplex (registered trademark) manufactured by Hosokawa Micron Co., Ltd., thereby preparing the aggregate shown below, and further using the materials shown below as raw materials. In addition, the average particle size of the aggregate and the negative electrode material, and the standard deviation of the particle size distribution of the aggregate were measured using a particle size distribution measuring device (SALD-3000 manufactured by Shimadzu Corporation) using a laser diffraction-scattering method. The standard deviation of the particle size distribution of the aggregate is a standard deviation defined on a logarithmic scale.
[0113] Aggregate 1 Needle coke with an average particle size of 14 μm and a standard deviation of particle size distribution of 0.15
[0114] Aggregate 2: Needle coke with an average particle size of 12 μm and a standard deviation of particle size distribution of 0.22
[0115] ·Binder···Coal tar pitch
[0116] ·Dispersant···Stearic acid
[0117] The raw materials shown in Table 1, i.e., aggregates, binders, etc., are mixed in the amounts (parts by mass) described in Table 1 using a kneader to obtain a mixture. Next, the obtained mixture is molded by uniaxial pressing at room temperature to obtain a molded product. Next, the obtained molded product is heat treated at 800°C to 850°C in a nitrogen atmosphere for 8 hours, and then graphitized at 2600°C to 3100°C for 30 hours to obtain a graphitized product. The obtained graphitized product is crushed to obtain graphite powders (negative electrode materials for lithium ion secondary batteries) of Examples 1 to 3 and Comparative Example 1.
[0118] The density (g / cm 3 ), density of graphite (g / cm 3 ) and the average particle size (μm) and specific surface area (m 2 / g), saturated tap density (g / cm 3 ) are shown in Table 1 respectively.
[0119] It should be noted that the pulverized product obtained in each example includes secondary particles in a state where graphite particles, which are graphitized materials of aggregates, are aggregated or bonded so that their main surfaces are not parallel to each other.
[0120] (2) Preparation of negative electrode and evaluation of its orientation
[0121] 96 parts by mass of the prepared negative electrode material, 1.5 parts by mass of styrene butadiene rubber (BM-400B, manufactured by Nippon Zeon Co., Ltd.), 1.5 parts by mass of carboxymethyl cellulose (CMC1380, manufactured by Daicel Corporation), and 1.0 parts by mass of carbon black (SuperP, manufactured by Imerys GC) were mixed, and water was added to adjust the viscosity to obtain a composition. The obtained composition was applied in an amount of 10 mg / cm 2 The composition layer was coated on the current collector (copper foil with a thickness of 10 μm) in a manner to form a composition layer. The composition layer was pressurized to form a pressurized electrode, and then dried at 130°C for 8 hours using a vacuum dryer. The density after vacuum drying was 1.60 g / cm 2 The orientation of the negative electrode produced by the above method was evaluated.
[0122] (3) Preparation of evaluation batteries
[0123] The negative electrode obtained above was punched into an electrode area of 1.54 cm 2 A 2016-type coin cell was prepared by using metallic lithium as a positive electrode, a mixed solution of ethylene carbonate / ethyl methyl carbonate (3 / 7 volume ratio) and vinylene carbonate (0.5 mass %) containing 1.0M LiPF6 as an electrolyte, a polyethylene microporous membrane with a thickness of 25 μm as a separator, and a copper plate with a thickness of 230 μm as a spacer. The 2016-type coin cell was used as an evaluation battery.
[0124] (4) Evaluation of battery characteristics
[0125] Using the produced evaluation battery, the initial discharge capacity (Ah / kg) and the initial charge and discharge efficiency (%) were measured. Specifically, the evaluation battery was placed in a thermostatic chamber maintained at 25°C, and a constant current charge was performed at 0.53 mA until 0 V, and then further charged at a constant voltage of 0 V until the current decayed to a value equivalent to 0.026 mA, and the initial charge capacity was measured. After charging, the battery was discharged after a rest of 30 minutes. The initial discharge capacity was measured at 0.53 mA until 1.5 V. At this time, the capacity was converted to the unit mass of the negative electrode material used. The value obtained by dividing the initial discharge capacity by the initial charge capacity was multiplied by 100 to obtain the initial charge and discharge efficiency (%). The results are shown in Table 1.
[0126] (5) Evaluation of fast charge capacity maintenance rate
[0127] The negative electrode obtained above was punched into an electrode area of 2.00 cm 2A 2016-type coin cell was prepared by coating lithium cobalt oxide on aluminum foil as a positive electrode, a mixed solution of ethylene carbonate / ethyl methyl carbonate (3 / 7 volume ratio) and vinylene carbonate (0.5 mass %) containing 1.0M LiPF6 as an electrolyte, a polyethylene microporous film with a thickness of 25 μm as a separator, and a spring spacer as a spacer. The 2016-type coin cell was used as an evaluation battery.
[0128] The evaluation battery was used to perform an aging treatment before the rapid charge test. Specifically, the evaluation battery was placed in a thermostatic chamber maintained at 25°C, and charged at a constant current of 0.92 mA until 4.2 V, and then further charged at a constant voltage of 4.2 V until the current decayed to a value equivalent to 0.046 mA. After charging, the battery rested for 10 minutes, and then discharged at 0.92 mA until 2.75 V. This charging and discharging was repeated for 5 cycles.
[0129] A rapid charging test was performed using the aged evaluation battery. Specifically, the evaluation battery was placed in a thermostatic chamber maintained at 25°C, and constant current charging was performed at 0.92 mA until 4.2 V was reached, and the charge capacity (1) was measured. After charging, the battery was discharged after a 10-minute break. The discharge was performed at 4.6 mA until 2.75 V. Furthermore, constant current charging was performed at 6.9 mA until 4.2 V was reached, and the charge capacity (2) was measured. After charging, the battery was discharged after a 10-minute break at 4.6 mA until 2.75 V was reached.
[0130] The value obtained by dividing the charge capacity (2) by the charge capacity (1) was multiplied by 100 to obtain the rapid charge capacity maintenance rate (%). The results are shown in Table 1.
[0131] (6) Evaluation of battery life
[0132] The evaluation battery is prepared and aged in the same manner as in (5) above. The aged evaluation battery is used to perform a cycle test and evaluate the battery life. Specifically, the evaluation battery is placed in a thermostatic chamber maintained at 25°C, and is charged at a constant current of 4.6 mA until it reaches 4.2 V, and then further charged at a constant voltage of 4.2 V until the current decays to a value equivalent to 0.046 mA. After charging, rest for 10 minutes, and then discharge at 4.6 mA until it reaches 2.75 V, and measure the initial discharge capacity. The charge and discharge are further repeated for 299 cycles, and the discharge capacity of the 300th cycle is measured.
[0133] The value obtained by dividing the discharge capacity at the 300th cycle by the initial discharge capacity was multiplied by 100 to obtain the battery life maintenance rate (%). The results are shown in Table 1.
[0134] [Table 1]
[0135]
[0136] As shown in Table 1, the evaluation battery made using the negative electrode material (Example) made by the method disclosed in the present invention has good evaluation results for the fast charge capacity retention rate and the battery life retention rate compared with the evaluation battery made using the negative electrode material (Comparative Example) made by the conventional manufacturing method (the density of the formed product is high).
Claims
1. A method for producing a negative electrode material for a lithium ion secondary battery, comprising: (a) a step of obtaining a mixture comprising a graphitizable aggregate and a graphitizable binder, (b) forming the mixture to obtain a formed product, (c) a step of graphitizing the formed product to obtain a graphitized product, and (d) a step of crushing the graphitized material to obtain a crushed material, The standard deviation of the particle size distribution of the aggregate is less than or equal to 0.
20. 2 . The method for producing a negative electrode material for a lithium ion secondary battery according to claim 1 , wherein the mixture contains a dispersant. 3 . The method for producing a negative electrode material for a lithium ion secondary battery according to claim 2 , wherein the dispersant contains a fatty acid. 4 . The method for producing a negative electrode material for a lithium ion secondary battery according to claim 1 , wherein the amount of the binder blended is 25% by mass or less relative to the mixture. 5 . A method for producing a lithium ion secondary battery, comprising the step of producing a negative electrode using a negative electrode material, wherein the negative electrode material is obtained by the method for producing a negative electrode material for a lithium ion secondary battery according to claim 1 .
Citation Information
Patent Citations
Negative electrode material for lithium-ion secondary cell, method for manufacturing negative electrode material for lithium-ion secondary cell, negative electrode material slurry for lithium-ion secondary cell, negative electrode for lithium-ion secondary cell, and lithium-ion secondary cell
WO2015147012A1
Negative electrode material for lithium-ion secondary cell, method for manufacturing negative electrode material for lithium-ion secondary cell, negative electrode material slurry for lithium-ion secondary cell, negative electrode for lithium-ion secondary cell, and lithium-ion secondary cell
CN106104871A
Negative electrode material for lithium-ion secondary cell, method for manufacturing negative electrode material for lithium-ion secondary cell, negative electrode material slurry for lithium-ion secondary cell, negative electrode for lithium-ion secondary cell, and lithium-ion secondary cell
CN108565463A