Opaque non-pearlescent polyester products

By using incompatible polymers of COC and hydrogenated styrene-based polymers in polyester products for hot melt blending and orientation, the degradation and processing problems caused by mineral fillers are solved, and high brightness, low density and non-pearded light are achieved Polyester products with a horn-like color properties have excellent opacity and recyclability.

CN114269850BActive Publication Date: 2024-11-01PENN COLOR
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080058747.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-15
Filing Date
2020-08-21
Publication Date
2024-11-01
Estimated Expiration
2040-08-21

AI Technical Summary

Technical Problem

When existing polyester products achieve opacity and non-pearl appearance, mineral fillers such as TiO2 are often used, resulting in degradation, changes in processing characteristics, weight increase and recycling difficulties. The lack of mineral-free filler solutions can achieve both whiteness and light barriers. sex.

Method used

Incompatible polymers containing COC, partially or completely hydrogenated styrene-based polymers and copolymers are formed by hot melt blending and oriented at a temperature below the softening point of the incompatible polymer Vika to form High opacity and non-pearl-looking polyester products that reduce or eliminate mineral filler loads.

Benefits of technology

In the absence of mineral fillers or low mineral fillers, the high brightness, low incompatible polymer loading, easy recovery and low density of polyester products, with the desired opacity and non-pearl-like heterochromatic properties, avoiding Degradation and processing difficulties caused by mineral fillers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114269850B_ABST
    Figure CN114269850B_ABST
Patent Text Reader

Abstract

The present disclosure generally relates to opaque, non-pearlescent polyester articles and methods of making the same, the articles having at least one layer formed from a polymer blend composition comprising a polyester base polymer, an incompatible polymer, and little to no mineral filler.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims the benefit of priority to U.S. Provisional Patent Application No. 62 / 890,266, filed on August 22, 2019, and U.S. Provisional Patent Application No. 62 / 936,131, filed on November 15, 2019, the entire disclosures of which are hereby incorporated by reference in their entirety. Technical Field

[0002] The present disclosure relates generally to polyester articles, such as bottles or other containers, sheets, films or fibers, having an opaque, non-pearlescent appearance and made from compositions containing little to no mineral fillers. Background Art

[0003] In the field of packaging, plastics have replaced other materials such as glass. This substitution minimizes breakage, reduces weight and reduces energy consumed in manufacturing and transportation. Attracting consumers to buy single-size or family-size containers includes trademark and trade dress considerations about the appearance of product containers. Modern consumer products require eye-catching attention. One of the elements of valuable appearance is the color of the container. Color can be described mathematically. For example, the CIELAB L*, a*, b* color space mathematically describes all visible colors in three dimensions: L* is used for brightness, a* is used for green-red, and b* is used for blue-yellow. See Hunter Lab, Applications Note, "Insight on Color", Vol. 8, No. 7 (2008). In the CIELAB color space, the L* axis extends from top to bottom. The maximum L* value is 100, which represents a perfect reflecting diffuser (perfect reflecting diffuser) (i.e., the brightest white). The minimum L* value is 0, which represents a perfect absorber (i.e., the darkest black). Positive a* is red. Negative a* is green. Positive b* is yellow. Negative b* is blue. Figure 1 . A CIELAB a* value or b* value equal to 0 indicates that there is no red-green or blue-yellow appearance, in which case the article will appear pure white. In contrast, a* values ​​or b* values ​​that are far away from 0 indicate that light is unevenly absorbed or reflected. When the a* value or b* value deviates from 0, the color may no longer appear bright white. One of the most important properties of the CIELAB model is device independence, which means that the color is defined without relying on the nature of the color's generation or the device that displays the color.

[0004] The L*, a*, and b* values ​​of the CIELAB color scale can be obtained using any CIELAB color measuring instrument and calculated from known formulas. See Hunter Lab, Applications Note, "Insight on Color", Vol. 8, No. 7 (2008). Using the L* value, the CIELAB model allows quantification of how bright a product actually is. Brightness is usually increased by adding highly reflective and minimally absorbing components such as titanium dioxide (TiO 2 )) to achieve it.

[0005] One aspect of the outward appearance of goods is whiteness, which can be desirable in some applications.For example, bright white can advantageously reflect almost all light, thereby protecting the product inside the goods from degradation caused by light.In order to obtain bright white containers, some packagers add colorants or sunscreens.However, other colorants or sunscreens increase the cost of the container and may cause vortex appearance (i.e., colorants and / or sunscreens do not seem to be fully dispersed in the composition), which may have a negative impact on consumer's product perception.Sunscreens may also cause undesirable physical properties due to high pigment content, reduced recycling capacity and lower glossiness.For bottles or thermoplastic parts of blow molding, due to the high reflectivity of infrared light, high-level sunscreens may also cause difficulties when reheating.Therefore, it is necessary to have an improved goods of whiteness realized in the absence of one or more of the above shortcomings related to colorants and sunscreens.

[0006] Another aspect of the appearance of the product is opacity or light barrier, which may be desirable if the contents of the package need to be shielded or the quality of the packaged product needs to be prevented from deteriorating during the period between packaging and consumption, because light exposure may cause undesirable changes to certain packaged items. For example, milk may be damaged by the photochemical and ionizing effects of light. Specifically, riboflavin photodegrades when exposed to light from 200nm to 520nm. This degradation may adversely affect the taste and smell of milk. Light barrier limits the passage of certain wavelengths of light through the container wall. Such barrier or opacity can be achieved by reflection or absorption, which prevents the contents contained in the container from being harmfully affected. However, some methods for achieving light barrier are associated with undesirable compromises in the performance and other characteristics of the container.

[0007] For example, light blocking can be achieved by incorporating mineral fillers such as TiO 2To achieve this, it has been found that there are several disadvantages. In polyester plastics, mineral fillers may cause degradation of the polyester, which may change the processing characteristics and adversely affect the physical properties, resulting in stress cracking, yellowing and / or reduced maximum load. Mineral fillers may also agglomerate and cause stress concentration points, resulting in loss of structural integrity and filter deposits that cause problems during recycling. Mineral fillers also add weight and increase density, which in turn increases costs. In addition, mineral fillers may be highly abrasive to processing equipment (e.g., extruders, stretching rollers) and internal processing parts (e.g., valves, pins, and molds). Articles containing mineral fillers may also be difficult to sort and recycle. In addition, TiO 2 (one of the most common mineral fillers used in plastic applications) has come under scrutiny regarding its potential carcinogenicity. Masterbatches of polymers containing mineral fillers may also result in an uneven distribution of the mineral filler, which results in a swirling or color-streaked appearance. Mineral fillers also tend to release degradation components, such as ethacrylaldehyde and other non-intentionally added substances (NIAS), and may have an adverse effect on the natural aging characteristics of the article. Therefore, there is a need for improved articles having light barrier properties or opacity that are less than that of articles containing little to no mineral fillers (e.g., TiO 2 ) and / or reduce or eliminate the use of mineral fillers (e.g. TiO 2 ) is achieved without any one or more of the above disadvantages associated with it.

[0008] Another aspect of the appearance of an article is gonioappearance, which is related to the appearance of the article when it is subjected to changes in illumination or viewing angle. For example, an article with non-pearlescent gonioappearance maintains uniform color and appearance across all viewing angles. Therefore, non-pearlescent articles can be beneficial because they can provide uniform color consistency and brand recognition regardless of the consumer's viewing position. In contrast, gonioapparent (e.g., pearlescent or metallic) articles show color differences across viewing angles. Sometimes a gonioapparent appearance is desirable because pearlescent and metallic effects can be eye-catching. However, such an effect can also be disadvantageous because reduced color uniformity can also reduce brand recognition.

[0009] Goniochromaticity can be measured with a multi-angle spectrophotometer such as the MA-T12 from X-Rite. ASTM E2175 describes the standard practice for specifying the geometry of multi-angle spectrophotometers. Color differences can be measured using CIELABDE CMC A calculation that indicates how much a color differs from a reference (e.g., a pure white standard). CMCThe higher the value, the more obvious the difference in color. For example, when the reference is pure white, a smaller DE CMC A value of 0 indicates a color that is closer to white. Angular flop can also show directionality based on the orientation of light relative to the internal voids (or pearlescent particles). For example, if the internal voids of a PET bottle are elongated in the axial direction (from the top to the bottom of an injection stretch blow molded bottle) rather than in the circumferential direction, the angular flop can be non-pearlescent when the light source is aligned orthogonally relative to the internal voids, but can be angularly variable (e.g., pearlescent or metallic) when the light source is aligned parallel relative to the internal voids. Therefore, because non-pearlescent flop can be advantageous, there is a need for improved articles having non-pearlescent flop that is angularly variable in the presence of little to no mineral fillers (e.g., TiO 2 ) and / or reduce or eliminate the use of mineral fillers (e.g. TiO 2 ) is achieved without any one or more of the above disadvantages associated with it. Summary of the invention

[0010] In one aspect, the disclosed technology relates to an oriented opaque, non-pearlescent article comprising one or more layers, wherein at least one layer is a composition comprising: a polyester; an incompatible polymer selected from COC, partially or fully hydrogenated styrenic polymers and copolymers, and combinations thereof; and 0 wt % to 8 wt % of a light scattering pigment based on the total weight of the composition; wherein the article is oriented, opaque, and non-pearlescent. In some embodiments, the layer has a DE of less than 15 units when measured from a 45° light source between a viewing angle of 15° and a viewing angle of 110°. CMC In some embodiments, the layer has a DE of less than 10 units when measured between 15° viewing angle and 110° viewing angle from a 45° light source. CMC In some embodiments, the incompatible polymer has a Vicat Softening Point that is higher than the orientation temperature of the article. In some embodiments, the layer is white and has a CIELAB a* value within a range of ±10 units and a CIELAB b* value within a range of ±10 units. In some embodiments, the polyester is polyethylene terephthalate (PET). In some embodiments, the composition comprises at least 85% by weight of the polyester based on the total weight of the composition. In some embodiments, the incompatible polymer comprises a hydrogenated styrenic polymer. In some embodiments, the incompatible polymer comprises COC.

[0011] In some embodiments, the composition comprises about 15 wt % or less of incompatible polymers based on the total weight of the composition. In some embodiments, the composition does not comprise titanium dioxide. In some embodiments, the composition comprises no more than 1 wt % of mineral filler based on the total weight of the composition. In some embodiments, the light scattering pigment comprises zinc sulfide present in an amount of about 4 wt % or less based on the total weight of the composition. In some embodiments, the composition further comprises titanium dioxide. In some embodiments, the composition comprises no more than 0.1 wt % of light scattering pigment based on the total weight of the composition.

[0012] In some embodiments, the composition further comprises an additive or a colorant. In some embodiments, the composition comprises an additive selected from the following: anti-blocking agent, antioxidant, antistatic agent, slip agent, chain extender, cross-linking agent, flame retardant, IV reducer (IV reducer), laser marking additive, release agent, optical brightener, flow aid, colorant, plasticizer, pigment, dye, nucleating agent, oxygen scavenger, antimicrobial agent, UV stabilizer and combination thereof. In some embodiments, the composition comprises a colorant selected from the following: dye, organic pigment, inorganic pigment and combination thereof. In some embodiments, the colorant includes aluminum. In some embodiments, the colorant includes a combination of dyes. In some embodiments, the layer has an average light transmittance of about 20% or less for light with a wavelength in the range of 400nm to 700nm. In some embodiments, the article is a container.

[0013] In another aspect, the disclosed technology relates to a method for making an opaque, non-pearlescent article, the method comprising the steps of: (a) hot melt blending a polyester with an incompatible polymer selected from COC, partially or fully hydrogenated styrenic polymers and copolymers, and combinations thereof to produce a composition comprising about 15 wt% or less of the incompatible polymer based on the total weight of the composition; (b) subjecting the composition to an orientation stress at a temperature below the Vicat softening point of the incompatible polymer; and (c) producing an article that is visually non-pearlescent and has a percent transmittance of less than 20% for light with a wavelength in the range of 400 nm to 700 nm. In some embodiments, at least one additive or colorant is added to the composition during step (a).

[0014] In another aspect, the disclosed technology relates to an oriented opaque, non-pearlescent, white article comprising one or more layers, wherein at least one layer is a composition comprising, based on the total weight of the composition: at least 91.5 wt % of polyethylene terephthalate (PET); less than 4 wt % of an incompatible polymer selected from COC and hydrogenated styrenic polymers; less than 4 wt % of a polymer selected from titanium dioxide (TiO 2) and zinc sulfide (ZnS); and less than 0.5% by weight of additional components selected from colorants and additives; wherein the article is oriented; the article has a percent transmittance of less than 20% for light with a wavelength in the range of 400 nm to 700 nm; when measured from a 45° light source at a viewing angle between 15° and 110°, the layer has a DE of less than 10 units CMC The layer has a CIELAB a* value within a range of ±10 units and a CIELAB b* value within a range of ±10 units. In some embodiments, the composition comprises less than 1 wt % TiO 2 and less than 3 wt% ZnS.

[0015] In another aspect, the disclosed technology relates to an oriented opaque, non-pearlescent article comprising one or more layers, wherein at least one layer is a composition comprising, based on the total weight of the composition: at least 91.5 wt% polyethylene terephthalate (PET); less than 4 wt% of an incompatible polymer selected from COC and hydrogenated styrenic polymers; less than 4 wt% zinc sulfide (ZnS); and less than 0.5 wt% of an additional component selected from colorants and additives; wherein the composition does not contain titanium dioxide; the article is oriented; the article has a percent transmittance of less than 20% for light having a wavelength in the range of 400 nm to 700 nm; and the layer has a DE of less than 10 units when measured from a 45° light source between a viewing angle of 15° and a viewing angle of 110°. CMC Non-pearlescent angular flop.

[0016] In another aspect, the disclosed technology relates to an oriented opaque, non-pearlescent article comprising one or more layers, wherein at least one layer is a composition comprising, based on the total weight of the composition: at least 91.5 wt% polyethylene terephthalate (PET); about 1 wt% to about 5 wt% of an incompatible polymer selected from COC and hydrogenated styrenic polymers; about 1 wt% to about 3 wt% polymethylpentene (PMP); and less than 0.5 wt% of an additional component selected from colorants and additives; wherein the composition does not contain titanium dioxide or zinc sulfide; the article is oriented; the article has a percent transmittance of less than 20% for light having a wavelength in the range of 400 nm to 700 nm; and the layer has a DE of less than 10 units when measured from a 45° light source between a viewing angle of 15° and a viewing angle of 110°. CMC In some embodiments, the additional components include non-mineral ingredients selected from aluminum and organic dyes. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1This is a diagram of the CIELAB L*, a*, b* color space.

[0018] Figure 2 is a graph of exemplary multi-angle color measurements for determining the goniochromaticity of an article using a 45° incident light source and measuring color at near specular (15°) and far specular (110°) angles.

[0019] Figure 3 is a graph of a mixture of immiscible polymers (matrix polymer and incompatible polymers).

[0020] Figure 4 is a graph of a mixture of immiscible polymers (matrix polymer and incompatible polymer) after orientation stress.

[0021] Figure 5 This is an optical microscopy image of a non-pearlescent product.

[0022] Figure 6 This is an optical microscopy image of a pearlescent product. DETAILED DESCRIPTION

[0023] The present disclosure relates to polyester articles having improved opacity (light barrier), non-pearlescent appearance across a range of viewing angles, and reduced or eliminated mineral filler loading. In some embodiments, the opaque, non-pearlescent polyester articles have a brighter, whiter appearance (higher L* value) and / or low loading levels of incompatible polymers.

[0024] The following discussion includes multiple embodiments that do not limit the scope of the attached claims. Any examples set forth herein are intended to be non-restrictive and only illustrate some of the many possible embodiments of the present disclosure. In addition, the specific features described herein can be used in combination with other described features in each of various possible combinations and arrangements. Unless otherwise specifically defined herein, all terms will be given their broadest reasonable interpretation, including the meaning implied from the specification and the meaning understood by those skilled in the art and / or the meaning defined in dictionaries, papers, etc. It must also be noted that, as used in the specification and claims, unless otherwise stated, nouns that are not modified with quantifiers include plural objects, and when used in this specification, the terms "include" and / or "comprise" specify the presence of the features, steps, elements and / or components, but do not exclude the presence or addition of one or more other features, steps, elements, components and / or combinations thereof.

[0025] The disclosed articles are made from phase separated mixtures or compositions comprising immiscible polymers, wherein the incompatible polymers are mixed with a matrix polymer, such as Figure 3As shown. Without being bound by any particular theory, it is believed that when the composition of these phase-separated mixtures is subjected to orientation stress (e.g., blow molding, biaxial sheet orientation, uniaxial stretching, thermoforming, fiber spinning, etc.), the droplets of the less immiscible components (incompatible polymers) can elongate and form a plate-like structure. If the incompatible polymers and the matrix polymer have different refractive indices, the plate-like structure results in an appearance that varies with angle (e.g., pearlescent or metallic). In addition, if the incompatible polymers remain rigid during the orientation stress, the incompatible components may not be completely flattened. Instead, the incompatible polymers may separate from the matrix, thereby creating internal voids that elongate as the matrix polymer is stretched and oriented. If the incompatible polymer is sufficiently rigid, it can support the expanded internal void structure. Therefore, a large number of dispersed incompatible polymer domains create internal overlapping voids within the matrix polymer, such as Figure 4 These voids create a large light scattering surface that reflects light in a non-uniform manner, resulting in an angle-dependent (eg, pearlescent or metallic) effect in which the color difference across viewing angle varies significantly.

[0026] Articles disclosed herein may include one or more layers, wherein at least one layer comprises a composition comprising: a polymer blend of a matrix polymer and an incompatible polymer and optionally another component. The disclosed articles may include various forms, including but not limited to a finished product, a multilayer structure, or a layer (e.g., an outer layer) in a multilayer structure. For example, an injection stretch blow molded article (e.g., a bottle) may include a transparent polyester skin or another colorant or functional surface layer to enhance the aesthetics of the product. When one or more of the skin or layer comprises a composition disclosed herein, such an article may have a desired opaque non-pearlescent appearance. For films or other injection stretch blow molded articles, nylon may be added to the layer of the disclosed composition as an oxygen barrier layer or added to the layer of the disclosed composition as a reactive oxygen scavenger. In some embodiments, incompatible polymers may be used in one layer, and colorants may be used in another separate layer. In some embodiments, the outer layer containing incompatible polymers may hide the layer containing a light absorbing colorant to enhance light blocking in a multilayer structure and still maintain a white appearance. In other words, a layer having a composition disclosed herein that exhibits certain advantageous properties (eg, opacity, non-pearl, optional whiteness) will impart those advantageous properties to the article when used as an outer layer (eg, but not necessarily, the outermost layer) of the article.

[0027] The compositions disclosed herein reduce or eliminate mineral fillers (e.g., TiO 2 ) use. Thus, the disclosed articles can be more easily recycled into bottles, fibers or thermoformed parts.

[0028] Polyester polymer

[0029] The disclosed compositions include a major polymer component that is a polyester matrix resin (also interchangeably referred to herein as a polyester polymer or matrix polymer), which can be any polyester suitable for making bottles or other containers, sheets, films, thermoformed parts, or other types of articles. Non-limiting examples of suitable polyester polymers for use in the compositions for making the disclosed articles include polyester terephthalate (PET), PET homopolymers, copolymers of PET with glycols, copolymers of PET with cyclohexanedimethanol (CHDM), copolymers of PET with isophthalic acid (IPA), polylactic acid (PLA), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polycyclohexanedimethylene terephthalate (PCT), polyethylene naphthalate (PEN), polyethylene furanoate (PEF), and combinations thereof.

[0030] The polyester polymer comprises the majority of the composition. In some embodiments, the composition comprises a polyester polymer (e.g., PET) in an amount of at least 85%, at least 88%, at least 89%, at least 90%, at least 91%, at least 91.5%, at least 92%, at least 93%, at least 94%, at least 95%, at least 96%, at least 97%, or at least 98% by weight, based on the total weight of the composition (e.g., a layer of a final article, as described further below).

[0031] Incompatible polymers

[0032] The disclosed composition includes "incompatible polymers", which refer to the secondary polymer components that form phase separation domains in the matrix polymer under the heat and shear conditions of the extruder. The incompatibility and size of the phase separation domain can be driven by the differences in molecular weight, rheology, chemical composition, surface energy and processing conditions (such as shear, temperature, humidity), etc. Non-limiting examples of suitable incompatible polymers used in the composition for the manufacture of the disclosed article include polymethylpentene (PMP), cycloolefin copolymers, cycloolefin polymers, partially or completely hydrogenated styrene polymers and combinations thereof. As used herein, the term "COC" refers to both cycloolefin copolymers and cycloolefin polymers. In some embodiments, the incompatible polymer is not PMP, or PMP is not the only incompatible polymer in the composition. In other words, in some embodiments, PMP is only included in the composition in combination with another incompatible polymer such as COC or hydrogenated styrene polymers.

[0033] While incompatible polymers can be added to improve opacity, it is generally expected that incompatible polymers will produce a glossy or pearlescent appearance after orientation and require light scattering mineral fillers such as TiO 2 to mitigate such effects. However, the incompatible polymers for use in the disclosed compositions are selected based on their physical properties of being able to achieve both high opacity and a non-pearlescent appearance when biaxially stretched. Thus, the disclosed compositions can be prepared with reduced or eliminated mineral fillers, thereby providing one or more significant benefits, such as lower density, improved recyclability, improved regulatory compliance, and less degradation due to shear or moisture.

[0034] In some embodiments, the incompatible polymers used in combination with the disclosed technology have low surface energy and high Vicat softening point. The Vicat softening point (also referred to as Vicat hardness) is the softening point temperature of a material without a definite melting point, and can be considered an indication of rigidity. In some embodiments, the incompatible polymers have a Vicat softening point greater than the orientation temperature of the polymer blend (i.e., a composition comprising both a matrix polymer and an incompatible polymer). Since the Vicat softening point of the incompatible polymer affects pearlescence and opacity, different grades of incompatible polymers can be combined to adjust both opacity and non-pearlescence to a desired level.

[0035] In some embodiments, hot melt mixing a small amount of an incompatible polymer with a large amount of a polyester in an extruder and orienting the polymer blend composition at a temperature below the Vicat softening point of the incompatible polymer produces an opaque white article that unexpectedly does not require additional light scattering pigments such as TiO 2 The case has a non-pearlescent appearance.

[0036] Advantageously, it has been discovered that, unlike other olefin polymers, COC and hydrogenated styrenic plastics can dissolve dyes and act as carrier polymers for the masterbatch without allowing the dye to bleed or migrate out of the masterbatch.

[0037] Cyclic olefin copolymers include copolymers of ethylene and norbornene or ethylene and tetracyclodecene. For example, some of these polymers are available from Polyplastics as (COC), available from Zeonex as (COC) and available from Mitsui as APEL TM (COC) is commercially available. Due to differences in the polymerization and subsequent hydrogenation processes, the grades available from Zeonex are referred to as cycloolefin polymers. Other examples of COC include grades available from Polyplastics 5013F-04, which can be used in some embodiments in a polyester terephthalate (PET) matrix for injection stretch blow molding (ISBM) because The Vicat softening point of 5013F-04 is 133°C, which is higher than the PET orientation temperature of about 95°C to 120°C during the ISBM process. 8007F-04, another COC available from Polyplastics, has a relatively low Vicat softening point of 80°C and fails to produce opacity or a non-pearlescent appearance under the same orientation conditions.

[0038] Hydrogenated styrenic plastics include, for example, those available from Mitsui under the trade name VIVION TM Commercially available fully hydrogenated styrene butadiene copolymer. Grade VIVION TM VIVION 1325 is a fully hydrogenated styrene-butadiene copolymer available from Mitsui and has a Vicat softening point of 123°C, which is suitable for producing opaque articles with a non-pearlescent appearance from PET oriented by ISBM. Other non-limiting examples of suitable hydrogenated styrenic plastics include fully hydrogenated polystyrene (also known as polycyclohexylethylene or polyvinylcyclohexane), fully or partially hydrogenated styrene-isoprene copolymers, other partially or fully hydrogenated styrenic copolymers, and combinations thereof. TM 8210 is a fully hydrogenated styrenic cyclic block copolymer with a relatively low Vicat softening point of 105°C, which falls within the range of PET orientation temperatures during ISBM and can therefore produce angle-dependent (pearlescent) articles with higher light transmittance.

[0039] In some embodiments, the degree of hydrogenation of the hydrogenated polystyrenic copolymer is adjusted to increase the Vicat softening point to form an article having greater opacity and / or a non-pearlescent appearance. The hydrogenated polystyrenic copolymer is also stable in hot melt processing, thereby improving the repeated recyclability of polyester articles made therefrom. Furthermore, as shown in Example 4 below, unlike PMP, which exhibits a stable transmittance at about 4.5% without further decreasing with increasing PMP loading, the hydrogenated polystyrenic copolymer does not experience a plateau of opacity even at very high loading levels. Furthermore, the hydrogenated polystyrenic copolymer has color stability over time, even after multiple extrusion passes and UV exposure.

[0040] Suitable incompatible polymers can be added to the polyester polymer by dry blending the pellets and feeding them into the hopper of an extruder. Alternatively, the incompatible polymer can be pre-blended with other additives or colorants in the form of a masterbatch that is added to the polyester polymer.

[0041] In the disclosed articles, opacity and whiteness can be achieved with relatively small loadings of incompatible polymers in the composition—e.g., about 1 wt % or less, about 2 wt % or less, about 3 wt % or less, about 4 wt % or less, about 5 wt % or less, about 6 wt % or less, about 7 wt % or less, about 8 wt % or less, about 9 wt % or less, about 10 wt % or less, about 11 wt % or less, about 12 wt % or less, about 13 wt % or less, about 14 wt % or less, about 15 wt % or less, about 1 wt % to about 15 wt %, about 1 wt % to about 10 wt %, about 1 wt % to about 5 wt %, about 1 wt % to about 3 wt %, about 2 wt % to about 15 wt %, about 2 wt % to about 10 wt %, or about 2 wt % to about 5 wt %, based on the total weight of the composition (e.g., the total weight of a layer comprising the disclosed composition as provided in a bottle or other article). Producing an article with a relatively small amount of an incompatible polymer can result in a reduced density of the article, thereby advantageously reducing the overall weight and cost of the article. In some embodiments, the density of the article or its layer is about 1.3 g / cm 3 or smaller, about 1.2g / cm 3 or less, or about 1.1 g / cm 3 Or smaller, which reduces the weight of the product and saves costs and material consumption.

[0042] In some embodiments, the composition does not include any one or more of the following, which may otherwise be considered incompatible polymers: polypropylene, high density polyethylene, low density polyethylene, or linear low density polyethylene. Such polymers typically require high loading levels (e.g., greater than 15 wt %) to produce opacity; and higher loadings may have a negative impact on physical properties and result in higher costs.

[0043] In some embodiments, the composition does not include any one or more of the following, which may otherwise be considered incompatible polymers: polystyrene, polymethyl methacrylate, polyvinyl chloride, or polymethylpentene. Such polymers may degrade at some polyester processing temperatures to produce unintended substances such as styrene monomer or valeric acid, which may be toxic or alter the taste and / or odor of the product (e.g., food or beverage) contained within the article.

[0044] Factors that may affect the dispersion of incompatible polymers can be related to material properties such as refractive index difference, viscosity ratio and interfacial tension. These properties can be adjusted with additives such as internal lubricants, compatibilizers or crosslinkers.

[0045] Cyclic olefin copolymers and hydrogenated styrene plastics both have high barrier properties and very low absorption to water vapor. This can result in enhanced barrier properties to water vapor loss. In addition, incompatible polymers have little to no effect on deoxygenation capacity (i.e., the ability of the product to absorb oxygen from the surrounding environment and prevent it from diffusing through the product) or deoxygenation catalysts (e.g., cobalt). Without being bound by a particular theory, incompatible polymers can serve as degradable polymers in deoxygenation systems. In addition, in some embodiments, the incompatible polymers used in the disclosed compositions will not degrade under PET processing conditions, in which case little to no non-intentionally added substances (NIAS) are produced.

[0046] Barrier properties to gases such as oxygen and carbon dioxide are also important for content protection. In the case of insufficient gas barrier properties, carbonated beverages may lose carbon dioxide and become flat. Oxygen can degrade food products and cause rancidity. Methods for improving the oxygen barrier properties of polyesters such as PET can include using a cobalt catalyst as an active barrier in the presence of a degradable polymer. Active barriers such as oxygen scavengers are consumed and eventually fail. Passive barriers may be more beneficial because they are generally not consumed and can be used in combination with active barriers. Mixtures of polyesters and incompatible polymers as disclosed herein can improve passive barriers to oxygen, carbon dioxide or other gases. Adding incompatible polymers disclosed herein can also improve one or more physical properties of the final product, such as bursting strength, maximum load, stress cracking, tensile modulus, tensile strength, anti-delamination, fiber toughness, crushing strength and bending resistance.

[0047] Additional components

[0048] One or more additional components (e.g., additives, colorants) may optionally be included in the disclosed compositions for making opaque, non-pearlescent polyester articles. Non-limiting examples of suitable additives include anti-blocking agents (e.g., silica), antioxidants (e.g., primarily phenolic antioxidants), 1010), antistatic agents (e.g., glyceryl monostearate), slip agents (e.g., erucamide), chain extenders (e.g., carbonyl dicaprolactam), crosslinking agents (e.g., pyromellitic dianhydride), flame retardants (e.g., alumina trihydrate), IV reducers (e.g., AMP-95 TM ), laser marking additives (e.g. 8835), mold release agents (e.g. calcium stearate), optical brighteners (e.g. optical brightener OB-1), flow aids (e.g. DAIKIN PPA DA-310ST), plasticizers (e.g. polyester copolymers), nucleating agents (e.g. talc), oxygen scavengers (e.g. ), antimicrobial agents (e.g. triclosan), UV stabilizers (e.g. TINUVIN234), acetaldehyde scavengers (e.g. anthranilamide), coupling agents (e.g. 18507), extenders (e.g. CA 100), non-mineral fillers (e.g. cross-linked silicone (e.g. TOSPEARL 1110A), cross-linked polystyrene (TECHPOLYMERSBX-8) or cross-linked PMMA (GANZPEARL GMX-0610)), mineral fillers (e.g. TiO 2 ), and combinations thereof.

[0049] In some embodiments, the composition may contain little to no mineral fillers, such as TiO 2 For example, the composition may include a mineral filler (e.g., TiO ) in an amount of about 4 wt % or less, about 3 wt % or less, about 2 wt % or less, about 1 wt % or less, about 0.5 wt % or less, or 0 wt %, based on the total weight of the composition. 2 or ZnS).

[0050] One or more colorants may be optionally included in the disclosed composition for making an opaque non-pearlescent polyester article. Non-limiting examples of suitable colorants include dyes (e.g., Solvent Red 135), organic pigments (Pigment Blue 15:1), inorganic pigments (e.g., Iron Oxide Pigment Red 101), effect pigments (e.g., aluminum flakes), and combinations thereof. Pigments such as TiO 2 Alternatively, other inorganic or organic pigments may also be used in the composition to color the article or its layer. Colorants may increase the opacity of the article or its layer by creating additional scattering sites and / or by absorbing light of specific wavelengths (e.g., visible, UV, and IR).

[0051] In some embodiments, the composition may contain impurities such as polymers that degrade under the processing conditions of polyesters in a small amount of 0 wt % to 1.0 wt % (e.g., 0 wt % to 0.5 wt %) based on the total weight of the composition. For example, expected impurities include polystyrene (PS), styrene acrylonitrile (SAN), acrylonitrile butadiene styrene (ABS), polyvinyl chloride (PVC), thermoplastic polyurethane (TPU), inert mineral fillers (e.g., calcium carbonate (CaCO 3)), catalyst residues (e.g., antimony or titanium), or combinations thereof. Impurities are not preferred, but small amounts are acceptable. For purposes of this disclosure, miscible polyester blends, such as PET and PBT, PET and PETG, or PET and PTT are not considered impurities.

[0052] Products

[0053] Articles disclosed herein may include one or more layers, wherein at least one layer comprises the disclosed composition. As used herein, "layer" refers to a layer of the macroscopic scale of the material forming the article. In some embodiments, the thickness of the layer is from about 0.05 mm to about 5 mm, from about 0.1 mm to about 3 mm, or from about 0.2 mm to about 2 mm. In some embodiments, the layer comprises the sidewall of the article. The weight percentage of the components included in the disclosed composition is described as being based on the gross weight of the composition, which is identical to the gross weight based on the layer in which the composition is present, rather than based on the gross weight of the entire article (of course, unless the entire article is formed by a monolayer).

[0054] Non-limiting examples of suitable articles include bottles and other containers, sheets, films, thermoformed parts, fibers, and packaging for holding various consumer products. In some embodiments, the internal volume of the article can be from about 10 ml to about 5000 ml, from about 50 ml to about 4000 ml, from about 100 ml to about 2000 ml, from about 200 ml to about 1000 ml, or from about 10 ml to about 250 ml.

[0055] After the composition is oriented, the resulting article (or its layer) is opaque and has a non-pearlescent appearance. Additional components (e.g., pigments and / or dyes) may be included in the article without interfering with its non-pearlescent appearance. Therefore, the article may be produced to have a desired color and opacity without including any mineral filler or only including a minimum of mineral fillers in the composition. In some embodiments, dyes are used in the composition but pigments are not used, and the article exhibits desired color, opacity, and non-pearlescence.

[0056] In some embodiments, the disclosed articles have an opaque, non-pearlescent appearance and are free of pigments. 2 Or other pigments can lead to improved recyclability due to less polyester degradation and no pigment agglomeration. In addition, articles that do not contain mineral fillers or particles have a lower density and a lower overall weight, which leads to lower costs.

[0057] Manufacturing method

[0058] The present disclosure also relates to methods for manufacturing articles from the compositions disclosed herein. Some such methods include "blow molding," which refers to a manufacturing process by which an article including a hollow cavity is formed. The blow molding process begins by hot-melting or at least partially hot-melting or heat-softening a thermoplastic composition (e.g., masterbatch pellets, pellets containing the disclosed composition, etc.) and forming it into a preform, which can then be formed into an article by a molding or forming step (e.g., extrusion through a die, injection molding, etc.). Typically, a preform is a test tube-shaped plastic piece with a hole at one end through which compressed gas can pass. The preform can be clamped in a mold while air is pumped into it, sometimes combined with mechanical stretching of the preform (called "stretch blow molding"). Before air is pumped into the preform, the preform can be preheated. The air pressure pushes the thermoplastic outward to conform to the shape of the mold in which the preform is contained. After the plastic cools and hardens, the mold is opened and the expansion component (article) is removed. Generally, there are three main types of blow molding: extrusion blow molding (EBM), injection blow molding (IBM) and injection stretch blow molding (ISBM).

[0059] In some embodiments, the disclosed articles can be made by a method comprising the steps of hot melt blending a polyester polymer and an incompatible polymer by an extruder to form a preformed part or preform, and then orienting the preform at a temperature below the Vicat softening point of the incompatible polymer to form a final article having an opaque and non-pearlescent appearance. Without being limited by a particular theory, it is believed that the incompatible polymer forms a separate and distinct phase within the polyester matrix. When the polyester is oriented below the Vicat softening point of the incompatible polymer, the dispersed phase (incompatible polymer) remains rigid and produces internal voids within the polyester. These voids scatter light, resulting in whiteness and opacity. It is possible that some dispersed domains of the incompatible polymer have no voids and act as light scattering centers that broaden light reflections and minimize the angularly variable (e.g., pearlescent or metallic) appearance caused by the voids. In addition, the effect of orientation can change the color characteristics of the article in the oriented position. That is, it is believed that orientation produces internal voids that act as light scattering regions that change the appearance of the article, so that different stretch ratios will result in different color appearances.

[0060] As used herein, "oriented" refers to an article that has been subjected to a processing method for orientation. Non-limiting examples of suitable orientation processing methods include: single-state injection stretch blow molding (wherein the preform is injection molded, equilibrated to a target temperature, and then stretched), two-stage injection stretch blow molding (wherein the preform is injection molded, completely cooled and stored, and then completely reheated before being blown and oriented into a bottle or other shape), extrusion blow molding (wherein the polymer blend composition is hot melted and formed into a parison or preform in the hot melt phase, and then oriented before completely cooling), unidirectional film orientation (wherein a sheet is formed and stretched using clips in a tenter frame or by using differential speed rolls and roll gaps), biaxial sheet orientation (wherein a sheet is formed and then stretched sequentially on diverging tracks using different roll speeds and then using tenter frame clips), biaxial tubular orientation (wherein an annular die forms a temperature-regulated tube, which is then supported by gas pressure to expand the tube to a larger size), amorphous or crystalline thermoforming (wherein a sheet is produced and then formed in a mold using, for example, pressure or vacuum assistance), fiber orientation (wherein a hot melt extruded polymer is passed through a spinarette to form a yarn, which can be partially or fully oriented).

[0061] Orientation can be performed in a single direction (uniaxial) or in multiple directions (biaxial). In some embodiments involving uniaxial orientation, the orientation is about 3x or higher. In some embodiments involving biaxial orientation, the total area stretch ratio (first direction multiplied by the second direction) is about 7.0x 2 or higher, about 8.0x 2 or higher, about 9.0x 2 or higher, about 10.0x 2 or higher, or about 7x 2 to about 12x 2 In general, higher orientations give rise to higher opacity due to void generation and void growth.

[0062] Similar to the pearlescent particles (e.g., coated with TiO 2 The flop of the article may be affected by the effects caused by the mica of the matrix (e.g., mica of the matrix), and the flop of the article may be affected by the reflection and refraction from the internal inclusions with high aspect ratio. The effect on the flop of the article due to the pearlescent particles depends on the size effect, shape effect, orientation effect, reflection effect, absorption effect, refraction effect and / or scattering effect of these particles. Incompatible polymers may behave in a similar manner, except that instead of plate-like polymer domains, orientation can cause the dispersed incompatible polymer to form internal voids with high aspect ratio, which can produce a pearlescent appearance. In contrast, the low aspect ratio voids and small size domains of the dispersed incompatible polymer can scatter light and cause a non-pearlescent appearance. The properties of both the matrix polymer and the incompatible polymer can affect the size and shape of the voids, which can thereby affect the flop of the article.

[0063] The temperature of orientation can be adjusted, but generally falls within a range suitable for the base polymer. For example, a typical bottle grade PET having an intrinsic viscosity (IV) of about 0.80 dl / g can undergo orientation at a temperature in the range of 90°C to 130°C, preferably in the range of 95°C to 120°C. Orientation at too low a temperature may result in stress-induced cracking, and orientation at too high a temperature may result in premature crystallization. For multilayer articles, processing conditions may be separated and tailored for one or more layers to independently affect the flop properties of each layer.

[0064] In addition, due to the way of reheating, there may be temperature differences in different parts of the preform or pre-stretched product. If the preform is heated with infrared (IR) light, the amount of reflection or absorption at the surface facing the IR light may be higher than the surface not facing the IR light. Undesirable crystallization may occur in the part of the preform that absorbs too much IR light. Therefore, uniform temperature throughout the preform or pre-stretched product is advantageous and allows a wider processing window. Therefore, the disclosed technology is particularly beneficial for manufacturing methods that require reheating, especially IR reheating. Mineral fillers scatter and reflect light, thereby reducing the effectiveness of IR reheating. Such problems can be avoided by minimizing or eliminating the amount of mineral fillers used to manufacture the disclosed products. In addition, since opacity is not achieved until after orientation, the preform formed before orientation has significantly less light scattering and lower reflectivity. Therefore, before orientation, IR light will more effectively penetrate the preform.

[0065] Furthermore, it was unexpectedly found that the mineral filler zinc sulfide (ZnS) is particularly advantageous because, in contrast to the conventional mineral fillers (TiO 2 ), allows IR light to penetrate deeper into the article. ZnS exhibits a lower refractive index than TiO 2 Less light is reflected. Less reflection, while detrimental to opacity, allows for improved reheat performance. Thus, in applications requiring IR reheat, such as two-stage injection stretch blow molding, preforms (i.e., pre-oriented structures) comprising the ZnS-containing compositions disclosed herein can be reheated more easily because the IR light is not reflected prior to orientation, and the ZnS allows the IR light to penetrate deeper into the pre-oriented structure.

[0066] Aluminum flakes are also an advantageous additional component because they provide not only light reflection, but also a small amount of IR absorption. In contrast, carbon black is generally disadvantageous because it absorbs both visible and IR light without reflection, which can result in excessive absorbance at the surface, little IR penetration, and a large temperature difference between the surface and the interior of the reheated material. In some embodiments, the composition does not include carbon black.

[0067] Whiteness / Opacity

[0068] The whiteness of the article (or its layer) can be evaluated by measuring the a* value and b* value of the CIELAB color scale using a CIELAB color measuring instrument and a known formula. In some embodiments, the a* value and / or b* value of the advantageous white article layer of the present disclosure is 0 or within the range of ±2, ±4, ±6, ±8 or ±10. In any single article layer, the a* value and b* value may be the same or different. As used herein, "±" with respect to the listed values ​​refers to the entire range between negative and positive values. For example, an a* value of ±10 means an a* value within the range of -10 to +10.

[0069] Whiteness and / or opacity of oriented polyester (e.g., PET) articles can be achieved by incorporating mineral fillers into the polyester, for example, via a masterbatch. Non-limiting examples of suitable such mineral fillers include anatase TiO 2 , rutile TiO 2 , zinc sulfide (ZnS), barium sulfate, calcium carbonate (CaCO 3 ), mica, coated with TiO 2 Mica (pearlescent particles), borosilicate glass, ceramic beads, talc, zinc oxide, and combinations thereof. The mineral filler or a masterbatch containing the mineral filler can be hot melt mixed with an incompatible polymer and a matrix polymer in an extruder to form a composition that is later formed into an article.

[0070] In some embodiments, the disclosed compositions include TiO 2 , TiO 2 It can provide both an effective barrier to light and a highly white appearance. Compared with other mineral fillers, TiO 2 It is also readily available and fairly cheap. The combination of light blocking, whiteness, and low cost makes TiO 2 The high TiO 2 The significant disadvantages associated with loading mean that, if present for any reason, its content should be minimized.

[0071] In order to reduce the concentration of mineral fillers, but further improve light blocking, absorbing pigments and / or dyes can be included in the composition. However, adding absorbing colorants can reduce the whiteness of the product. When total reflection produces a white appearance, traditional reflective colorants can be included at a relatively high loading level to achieve higher opacity. Absorbing colorants such as carbon black can be used in combination with reflective pigments to increase light blocking, thereby preventing further degradation of the product contained in the product interior. However, absorbing colorants such as carbon black may also absorb too much IR light, as in the case of injection stretch blow molded PET bottles, if the product is heated before orientation, this may be problematic.

[0072] Opacity can be assessed as a measure of light transmittance, which is the average amount of light that passes through the article in the visible light range (400 nm to 700 nm). In some embodiments, the average light transmittance of an opaque article (or layer thereof) of the present disclosure is about 20% or less, about 15% or less, about 10% or less, about 5% or less, about 4% or less, about 3% or less, about 2.5% or less, about 2% or less, about 1.5% or less, about 1% or less, or about 0.5% or less.

[0073] Although incompatible polymers produce opacity, opacity production may not be preferred for some recyclable materials. Therefore, in some embodiments, opacity can be reduced by adding polyethylene or another polymer having a Vicat softening point lower than the orientation temperature of the polyester polymer in the composition. This is counterintuitive because adding polymers usually increases light scattering. However, without being bound by a specific theory, it is believed that the Vicat softening point of incompatible polymers can be reduced by blending with miscible incompatible polymers with lower Vicat softening points, which reduces the total Vicat softening point of the blend of incompatible polymers. The Vicat softening point is reduced to a temperature lower than the orientation temperature of the composition (comprising matrix polymer and incompatible polymer blend) to obtain an article with significantly less opacity. On the contrary, it is believed that the Vicat softening point of incompatible polymers can be improved by blending with miscible incompatible polymers with higher Vicat softening points, which raises the total Vicat softening point of the blend of incompatible polymers. Raising the Vicat softening point to a temperature above the orientation temperature of the composition (comprising the matrix polymer and the incompatible polymer blend) can result in a significantly more opaque article.

[0074] Non-pearlescent

[0075] As used herein, the term "non-pearlescent" refers to the phenomenon in which the color of a material does not change significantly with changes in the angle of illumination or observation. To assess whether an article (or a layer thereof) is non-pearlescent, a multi-angle spectrophotometer (e.g., MA-T12 from X-Rite) can be used to calculate the CIELAB DE between near and far specular viewing angles. CMC The value is used to quantify the magnitude of the appearance change of an article. Using a 45° incident light source and measuring the color at a near specular (15°) angle and a far specular (110°) angle, the color difference indicates the appearance change across the two viewing angles. Figure 2 .DE CMC Large differences in the values ​​indicate a pearlescent or metallic appearance. CMC An insignificant difference in the values ​​indicates a non-pearlescent appearance. For the purposes of this disclosure, the color change observed between a 15° viewing angle and a 110° viewing angle from a 45° illuminant is considered insignificant, and thus if the color change difference is less than 15 units DE CMC , less than 10 units DE CMC , less than 8 units DE CMC or less than 6 units DE CMC , then it shows non-pearlescence, among which DE CMC Measure both parallel to the orientation direction and perpendicular to the orientation direction. For bottles, there are two orientation directions - circumferential and axial. Choose the highest measured DE CMC The value is used as a measure of angular flop. The principle is that highly pearlescent and metallic materials reflect most of the light at angles close to the specular surface and very little light at angles far from the specular surface.

[0076] Even when the orientation is not uniform, the appearance of the disclosed articles formed using incompatible polymers can have a uniform non-pearlescent appearance. It is believed that this occurs because both the unoriented preform and the oriented article are non-pearlescent.

[0077] Example

[0078] Next, the disclosed technology is described by the following examples. The use of these examples and other examples anywhere in the specification is illustrative only and in no way limits the scope and meaning of the present disclosure or any illustrative form. Likewise, the present disclosure is not limited to any particular preferred embodiment described herein. Indeed, modifications and variations of the present disclosure may be apparent to those skilled in the art upon reading this specification, and may be made without departing from its spirit and scope. Therefore, the present disclosure is limited only by the terms of the claims and the full scope of equivalents authorized by the claims. All bottles described in the following examples are considered representative articles, and comparable results are expected for other types of articles—e.g., other containers, sheets, films, thermoformed parts, fibers, etc.

[0079] For purposes of the present disclosure and the following examples, various parameters (eg, goniochromaticity, visual pearlescence, opacity / transmittance, whiteness / color value, density, Vicat softening point, gloss) were measured as described below.

[0080] Angular flop: To measure angular flop, a method was developed to quantify the extent to which the color of a material changes over a range of viewing angles. As defined above, an insignificant color change indicates non-pearlescent angular flop. A multi-angle spectrophotometer (MA-96 from X-Rite) was used to measure the spectral reflectance of a sample placed on a black Leneta card. The MA-96 uses a 45° light source and measures the reflection at six different angles - 15°, 15°, 25°, 45°, 70°, and 110°, where 0° is the direct specular reflection of the 45° light source. Using a D65 light source and a 10° standard observer, the CIELAB L* value, a* value, and b* value were calculated for each measured reflection angle. Since the MA-96 uses a directional light source, six measurements using a light source aligned in the circumferential orientation direction were recorded and averaged together. Six measurements using a light source aligned in the axial orientation direction were then recorded and averaged together. The color difference between the reflection at 15° and the reflection at 110° (as measured by DE CMC The average DE of two CMC The higher of the values ​​is taken as an indication of the goniochromaticity.

[0081] Visual Pearlescence: A visual assessment of pearlescence is made and recorded as No or Yes in most cases. "No" means that the sample does not appear to be pearlescent visually. See for example Figure 5 "Yes" means that the sample visually appears to be pearlescent. See for example Figure 6Visual evaluation can determine a quantitative measurement of the goniochromaticity. In some cases, the presence or absence of a pearlescent appearance is ambiguous, in which case the visual evaluation is recorded as Not Determinable (ND).

[0082] Opacity / Light Transmission (LT): Light transmission was measured using an X-Rite Ci7800 spectrophotometer. The average light transmittance from 400 nm to 700 nm was calculated as percent transmittance. Each light transmittance value presented in the following samples represents the average of six measurements.

[0083] Whiteness / L*, a*, b*: Color values ​​were measured in reflection using an X-Rite Ci7800 spectrophotometer. L*, a*, and b* values ​​were calculated assuming a D65 illuminant and a 10° standard observer. Each L*, a*, and b* color value presented in the following examples represents an average of six measurements.

[0084] Density: Density is measured using the displacement method according to ASTM D792. Density is an indication of the amount of voids present. The specific gravity of PET is about 1.36 g / cm 3 Adding 4 wt% of olefin will reduce the specific gravity of the composite blend by a small amount. For example, adding 4.0 wt% of olefin will have a specific gravity of 1.02 g / cm 3 Adding COC to PET reduces the composite specific gravity to 1.34g / cm 3 A measured density lower than the calculated composite density indicates the presence of voids.

[0085] Vicat softening point (VSP): The Vicat softening point is measured as the 2 The temperature at which a flat-bottomed needle of circular or square cross-section penetrates a test specimen to a depth of 1 mm. For the purposes of this disclosure, the Vicat softening point is determined according to the method of ASTM D1525 (1 kg, 50° C. / hour).

[0086] Gloss: Gloss was measured at incident angles of 20°, 60°, and 85° using a BYK micro-tri-gloss meter according to the method of ASTM D523.

[0087] The materials used in the following examples are identified in Table 1.

[0088] Table 1: Materials

[0089]

[0090] Example 1

[0091] Samples 1 to 9 were prepared in which a minor amount of an incompatible polymer was added to a major amount of dry PET (PQB7 manufactured by Polyquest). In one sample (Sample 8), no incompatible polymer was included, but TiO 2 As a control. In the absence of incompatible polymer, the TiO 2 The composition will be non-pearlescent. 2 Each mixture of PET and PET pellets was fed into the extruder of a Nissei ASB-50 single-stage blow molding machine operating at 280°C to produce 29.7 g preforms, which were injection molded and stretched into bottles. The overall orientation of each preform was estimated to be 3.38x axial and 2.63x circumferential for a total area stretch ratio of 8.9x2. The orientation temperature was estimated to be in the range of 95°C to 110°C. The oriented bottles were evaluated for angular color flop and visual pearlescence, and the results are shown in Table 2.

[0092] Table 2

[0093]

[0094] *4 wt% TiO added via 50 wt% masterbatch (MB) 2

[0095] Samples 1 and 9 unexpectedly showed favorable results, including a non-pearlescent visual appearance and a DE of 9.3 CMC Units (Sample 1) and 9.1 DE CMC Non-pearlescent flop of unit (Sample 9). Samples 1 and 9 each comprise an incompatible polymer having a Vicat softening point (VSP) above the estimated 95°C to 110°C orientation temperature—i.e., in Sample 1, the selected COC has a VSP of 137°C; and in Sample 9, the selected HSB has a VSP of 126°C.

[0096] Example 2

[0097] Samples 10 to 17 were prepared using the same materials and processing conditions as Samples 1 to 8 of Example 1, except that the overall orientation of each preform of Samples 10 to 17 was estimated to be 10.9x 2 The total area stretch ratio was 3.3x axial and 3.3x circumferential. The oriented bottles were evaluated for goniochromaticity and visual pearlescence, and the results are shown in Table 3.

[0098] Table 3

[0099]

[0100] *4 wt% TiO added via 50 wt% masterbatch (MB) 2

[0101] Sample 10 unexpectedly showed favorable results including a non-pearlescent visual appearance and a DE of 12.8 CMC Sample 10 contains an incompatible polymer with a VSP above the estimated orientation temperature of 95°C to 110°C - ie, the VSP of the selected COC is 137°C.

[0102] Example 3

[0103] Preparation of a mixture in which a minor amount of incompatible polymer pellets (PMP (grade TPX TM RT-31) or PMP (Grade TPX TM RT-31) and COC (Grade Samples 18 to 21 were hand mixed with a major amount of PET pellets (PQB7 manufactured by Polyquest). TiO was not included in any of these samples. 2 The mixture of pellets was fed into the extruder of a Nissei ASB-50 single-stage blow molding machine under the following processing conditions: PET dryer temperature (300°F); PET dryer dew point (-42°F); bag shaking; recovery (175RPM); back pressure (0MPa to 2MPa); extruder barrel temperature (280°C); injection time (9 seconds); injection speed (40% to 80%); injection pressure (4MPa to 10.5MPa); hot runner temperature (280°C); holding pressure (7MPa); cooling time (5.5 seconds); preform cooling temperature (64°F); conditioning tank temperature (180°C); and conditioning time (12 seconds). Each of the resulting bottles had a 10.9x 2 The total area stretch ratio is 3.3x for the estimated axial orientation and 3.3x for the estimated circumferential orientation.

[0104] The samples were evaluated for whiteness / color value, light transmittance, density, goniochromaticity, and viewing angle pearlescence, and the results are shown in Table 4.

[0105] Table 4

[0106] Sample 18 Sample 19 Sample 20 Sample 21 PMP (wt%) 2.0 2.0 2.0 2.0 COC (weight %) 5.0 0.0 5.0 5.0 PET (weight %) 93.0 98.0 93.0 93.0 L* 97.38 97.37 97.36 97.54 a* -0.12 -0.17 -0.06 -0.06 b* -0.40 0.18 -0.33 -0.38 Light transmittance (%) 3.52 13.30 3.38 2.74 <![CDATA[Density (g / cm 3 )]]> 1.18 1.29 1.17 1.11 <![CDATA[Circumferential DE CMC > 11.5 25.1 13.8 13.1 <![CDATA[Axial DE CMC > 9.5 7.5 6.9 7.7 Pearlescent No Yes No No Preform weight (g) 57.4 58.3 58.1 57.8

[0107] Samples 18, 20, and 21 unexpectedly showed favorable results including: non-pearlescent visual appearance; 11.5 DE CMC Unit (sample 18), 13.8 DE CMC Units (sample 20) and 13.1 DE CMCand low light transmittance of 3.52% (Sample 18), 3.38% (Sample 20), and 2.74% (Sample 21). Sample 19 contained PMP as the only incompatible polymer and resulted in an article having a non-pearlescent visual appearance.

[0108] Example 4

[0109] Preparation of fully hydrogenated styrene butadiene (HSB) copolymers (VIVION from Mitsui) where the loading was increased TM 1325) and the balance of bottle-grade PET (0.80 dl / g IV, grade PQB7 from Polyquest) were hot melt blended. Each mixture was extruded at 280°C and formed into preforms on an ASB MB50 single-stage blow molding machine. The resulting bottles had a 10.9x 2 The total area stretch ratio of 1000 nm was 3.3x with an estimated axial orientation of 3.3 and an estimated circumferential orientation of 3.3. The opacity was measured on an X-Rite Ci7800 spectrophotometer, where the % transmittance is defined as the average transmittance from 400 nm to 700 nm. The samples were evaluated for transmittance and density, and the results are shown in Table 5. The data show that the HSB copolymer continues to reduce transmittance (i.e., increase opacity) even at higher loadings, and shows that the benefit of increased opacity does not plateau.

[0110] Table 5

[0111]

[0112] The PET was melt blended with the remaining bottle-grade PET (0.80 dl / g IV, grade PQB7 from Polyquest) to increase the loading of PMP (grade TPX from Mitsui). TM RT-31) was used to prepare comparative samples 1 to 6. Each mixture was extruded at 280°C and formed into preforms on an ASB MB50 single-stage blow molding machine. The resulting bottles had a 10.9x 2 The total area stretch ratio was 3.3x with an estimated axial orientation of 3.3 and an estimated circumferential orientation of 3.3x. Opacity was measured on an X-Rite Ci7800 spectrophotometer, where % transmittance is defined as the average transmittance from 400nm to 700nm. The samples were evaluated for transmittance and density, and the results are shown in Table 6. The data show that, unlike HSB (see Table 5 above), increasing loading of PMP achieved only a limited reduction in transmittance, reaching a plateau at about 4.5% transmittance. Therefore, even at comparable loadings, compositions with PMP as the only incompatible polymer did not achieve the same favorable degree of opacity as compositions containing HSB.

[0113] Table 6

[0114] sample Comparison 1 Comparison 2 Comparison 3 Comparison 4 Comparison 5 Comparison 6 PMP (wt%) 1.00 3.00 4.00 5.00 6.00 8.00 % Light Transmittance 15.82 5.28 5.57 4.46 4.05 4.29 Density(g / cm3) 1.34 1.24 1.18 1.20 1.15 1.15

[0115] Example 5

[0116] Bottles were prepared from a mixture of masterbatch pellets, incompatible polymer pellets and pre-dried PET (grade PQB7) pellets. MB pellets were prepared by mixing additives or colorants with PET (grade PQB4), then extruding the mixture on a twin screw extruder at 260°C, stranding and cutting into pellets. The composition of these masterbatch pellets is shown in Table 7. The incompatible polymer used in this example was PMP (TPX TM RT-31)、HSB(VINION TM 1325) and COC( 5013F-04).

[0117] Table 7

[0118]

[0119] Samples 30 to 37 and comparative samples 7 to 9 are preform compositions prepared by mixing masterbatch pellets, incompatible polymer pellets and PET pellets in a bag and then feeding the mixture into the feed inlet of a Nissei ASB-50M single-stage blow molding machine. The contents of the preforms of samples 30 to 37 and comparative samples 7 to 9 are shown in Table 8.

[0120] Table 8

[0121]

[0122] The preforms of samples 30 to 37 and comparative samples 7 to 9 were stretch oriented under the following processing conditions to form two types of bottles (bottle form A and bottle form B): PET dryer temperature (300°F); PET dryer dew point (-42°F); bag shaking; recovery (175RPM); extruder barrel temperature (280°C); injection time (9 seconds); hot runner temperature (280°C); cooling time (5.5 seconds); preform cooling temperature (64°F); conditioning tank temperature (180°C); and conditioning time (12 seconds). The back pressure, holding pressure and injection speed were varied as shown in Table 9.

[0123] Table 9

[0124] sample 30 31 32 33 34 35 36 37 Comparison 7 Comparison 8 Comparison 9 Back pressure(MPa) 2 2 2 2 2 0 2 2 0 2 2 Maintaining pressure (MPa) 4 4 4 4 4 7 4 4 7 4 4 Injection speed (%) 70 70 70 75 80 40 75 75 50 70 75

[0125] The compositions of the final bottles (as identified as Samples 30' to 37' and Comparative Samples 7' to 9') are shown in Table 10. For clarity, it is noted that, for example, Sample 30 is a preform composition, while Sample 30' is an article formed from the preform composition of Sample 30. This terminology applies similarly to other similarly identified samples disclosed herein.

[0126] Table 10

[0127]

[0128] Bottle Form A has an estimated value of 8.9x 2 The total area stretch ratio of 3.38x axial and 2.63x circumferential orientation was evaluated for whiteness / color value, light transmittance, density, goniochromaticity, visual pearlescence, and gloss of Bottle A samples, and the results are shown in Table 11.

[0129] Table 11

[0130]

[0131] Bottle Form B has an estimated value of 10.9x 2 The Bottle B samples were evaluated for whiteness / color value, light transmittance, density, goniochromaticity, visual pearlescence, and gloss, and the results are shown in Table 12.

[0132] Table 12

[0133]

[0134] Samples 30' to 33' unexpectedly showed favorable results, including demonstrating that the presence or absence of a colorant such as TiO 2 In the case of ZnS or ZnS, the use of incompatible polymers based on COC can produce articles that are white, opaque and non-pearlescent.

[0135] Samples 34' and 35' show that varying select process conditions can produce very different gloss values, yet still produce a bottle having a white, opaque, non-pearlescent appearance.

[0136] Sample 36' unexpectedly exhibited favorable results, including demonstrating that the use of a hydrogenated styrenic block copolymer as an incompatible polymer can produce an article that is white, opaque, and non-pearlescent.

[0137] Sample 37' unexpectedly exhibits favorable results, including demonstrating that blending a PMP with another incompatible polymer can produce an article that is non-pearlescent even when the ratio of PMP to light scattering pigment is high, such as 10 to 1.

[0138] Comparative Samples 7' to 9' show that the use of PMPs can produce articles having a pearlescent visual appearance even in the presence of about 1 wt% to 3 wt% of other colorants and even when the a* and b* values ​​are each within the range of ±3 units.

[0139] Example 6

[0140] Bottles were prepared from a mixture of the same masterbatch pellets, incompatible polymer pellets, and predried PET (grade PQB7) pellets as those described in Example 5. See Table 7. Samples 38 to 41 and Comparative Samples 10 to 12 were compositions made by mixing the masterbatch pellets, incompatible polymer pellets, and PET pellets in a bag and then feeding the mixture into a Nissei ASB-50M single-stage blow molding machine to produce preforms. The contents of the preform compositions of Samples 38 to 41 and Comparative Samples 10 to 12 are shown in Table 13.

[0141] Table 13

[0142]

[0143] The preform compositions of samples 38 to 41 and comparative samples 10 to 12 were stretch oriented under the following processing conditions to form two types of bottles (bottle form A and bottle form B): PET dryer temperature (300°F); PET dryer dew point (-42°F); bag shaking; recovery (175RPM); extruder barrel temperature (280°C); injection time (9 seconds); hot runner temperature (280°C); cooling time (5.5 seconds); preform cooling temperature (64°F); conditioning tank temperature (180°C); conditioning time (12 seconds); back pressure (2MPa); holding pressure (4MPa to 7MPa); and injection speed (65% to 70%). The composition of the final bottles (as identified by samples 38' to 41' and comparative samples 10' to 12') is shown in Table 14.

[0144] Table 14

[0145]

[0146] Bottle Form A has an estimated value of 8.9x 2 The total area stretch ratio of 3.38x axial and 2.63x circumferential orientation was evaluated for whiteness / color value, light transmittance, density, goniochromaticity, visual pearlescence, and gloss of Bottle A samples, and the results are shown in Table 15.

[0147] Table 15

[0148]

[0149] Bottle Form B has an estimated value of 10.9x 2 The Bottle B samples were evaluated for whiteness / color value, light transmittance, density, goniochromaticity, visual pearlescence, and gloss, and the results are shown in Table 16.

[0150] Table 16

[0151]

[0152] Samples 38' to 40' unexpectedly showed favorable results, including demonstrating that in the absence of TiO 2 In some cases, the use of incompatible COC-based polymers can produce white, opaque, non-pearlescent articles with transmittance values ​​less than 1.0%, and even less than 0.5%.

[0153] Sample 41' unexpectedly exhibited favorable results, including demonstrating that the use of hydrogenated styrenic incompatible polymers can produce articles that are white, opaque, and non-pearlescent. Comparative Sample 10' had the same composition as Sample 41' but with the addition of 0.1 wt% yellow dye. Thus, the Comparative Sample 10' bottle had a pearlescent appearance and was not white, with CIELAB a* color values ​​and b* color values ​​outside the range of ±10 units.

[0154] Comparative Sample 11' shows that pearlescence does not necessarily correspond to a non-white appearance. The bottle of Comparative Sample 11' is opaque due to the presence of TiO 2 Comparative Sample 12' also demonstrates the pearlescent appearance produced by the composition comprising PMP and dye.

[0155] Example 7

[0156] Bottles were prepared from a mixture of masterbatch pellets and pre-dried PET (grade PQB7) pellets. For samples 42 to 43 and comparative samples 13 to 16, the masterbatch pellets contained an incompatible polymer (COC, grade 5013F-04) and TiO 2 The contents of these masterbatches are shown in Table 17.

[0157] Table 17

[0158]

[0159] For each of Samples 42 to 43 and Comparative Samples 13 to 16, 5.1 wt% of the corresponding masterbatch pellets were added to 94.9 wt% of dry PET (grade PQB7) pellets using a Plastrac volumetric dosing system, which was then fed into the feed inlet of a Nissei ASB-50M single-stage blow molding machine.

[0160] The compositions of samples 42 to 43 and comparative samples 13 to 16 were stretch oriented under the following processing conditions to form two types of bottles (bottle form A and bottle form B): PET dryer temperature (300°F); PET dryer dew point (-42°F); bag shaking; recovery (175RPM); extruder barrel temperature (280°C); injection time (9 seconds); hot runner temperature (280°C); cooling time (5.5 seconds); preform cooling temperature (64°F); conditioning tank temperature (180°C); conditioning time (12 seconds); back pressure (2MPa); holding pressure (4MPa); and injection speed (65% to 70%). The compositions of the final bottles of samples 42 to 43 and comparative samples 13 to 16 are shown in Table 18.

[0161] Table 18

[0162]

[0163] Bottle Form A has an estimated value of 8.9x 2 The Bottle A samples were evaluated for whiteness / color value, light transmittance, density, goniochromaticity, visual pearlescence, and gloss, and the results are shown in Table 19.

[0164] Table 19

[0165]

[0166] Bottle Form B has an estimated value of 11.0x 2 The Bottle B samples were evaluated for whiteness / color value, light transmittance, density, goniochromaticity, visual pearlescence, and gloss, and the results are shown in Table 20.

[0167] Table 20

[0168]

[0169] Sample 42 unexpectedly showed favorable results, including demonstrating that the inclusion of an incompatible polymer and TiO 2 The masterbatch can produce a white, opaque and non-pearlescent product.

[0170] Sample 43 unexpectedly exhibited favorable results, including demonstrating that the addition of another incompatible polymer can improve properties such as light transmittance and gloss while maintaining a white, opaque, non-pearlescent article.

[0171] Comparative Samples 13 to 16 show that adding a small amount of colorant such that the CIELAB a* value or b* value falls outside the range of ±10 units changes the appearance of the article to pearlescent. In contrast, Samples 39 and 40 combine zinc sulfide with an incompatible polymer and colorant such that both the CIELAB a* value or b* value are within the range of ±10 units, and the appearance of the article is non-pearlescent.

[0172] Example 8

[0173] Samples 44 to 45 and Comparative Sample 17 are multi-layer stretch-oriented bottles made on a Nissei ASB-50M equipped with two extruders and designed to make bottles with the following three layers: outer skin (A layer), core (B layer) and inner skin (A layer). The bottles were made to have a three-layer ABA structure, where the A layer composition was the same in both the outer skin and the inner skin. The A layer contained an incompatible polymer (COC, grade 5013F-04), inorganic fillers (ZnS, HDS), optional colorant, and pre-dried PET. The B layer is a different composition used only in the core. The B layer is completely encapsulated by the outer A layer skin and the inner A layer skin. The B layer core composition includes 5 wt% of a dye-based black colorant masterbatch containing a blend of solvent dyes in a polyester carrier and 95 wt% of dry PET. The compositions of the A and B layers used in samples 44 to 45 and comparative sample 17 are shown in Table 21.

[0174] Table 21

[0175]

[0176] The compositions of Samples 44 to 45 and Comparative Sample 17 were stretched to an estimated total area stretch ratio of 11.0 x 2 Samples 44 to 45 and Comparative Sample 17 were evaluated for whiteness / color value, light transmittance, angle-of-view color flop, gloss, and layer thickness, and the results are shown in Table 22.

[0177] Table 22

[0178]

[0179] Samples 44-45 unexpectedly show favorable results, including demonstrating that only one layer of the multilayer structure needs to contain an incompatible polymer to produce an article that is white, opaque, and non-pearlescent. Comparative Sample 17 shows that adding a colorant such that the CIELAB a* value or b* value is no longer within the range of ±10 units causes the article to appear pearlescent.

[0180] Example 9

[0181] By mixing 13.33 wt% of 60 wt% TiO 2 ( A-100) and a masterbatch of a polyester carrier, 0.10 wt% yellow dye ( YELLOW 3G, SY-93), and 86.57 wt. % dry PET (PQB7) were hand mixed in a bag and the mixture was then fed into the feed inlet of a Nissei ASB-50M single-stage blow molding machine under the following processing conditions to prepare Comparative Sample 18 (stretch oriented bottle): PET dryer temperature (300°F); PET dryer dew point (-42°F); bag shaking; recovery (175RPM); extruder barrel temperature (280°C); injection time (9 seconds); hot runner temperature (280°C); cooling time (5.5 seconds); preform cooling temperature (64°F); conditioning tank temperature (180°C); and conditioning time (12 seconds).

[0182] The orientation of Comparative Sample 18 was estimated to be 2 The total area stretch ratio is 3.3x axial and 3.3x circumferential.

[0183] Sample 40 (above), Comparative Sample 9 (above), and Comparative Sample 18 were tested for the presence of volatile non-intentionally added substances (NIAS). See Franz et al., "Investigation of non-intentionally added substances (NIAS) in PET bottles and closures," Fraunhofer Institute for Process Engineering and Packaging (IVV) (poster presentation at the 4th International Food Packaging Symposium (November 2008)). 1 g of each sample removed from the fully oriented sidewall (specifically, the sidewall of bottle B for each of Sample 40 and Comparative Sample 9) was transferred to a 20 ml headspace vial and incubated at 200° C. for 1 hour to release any volatile components. Identification of volatile organic compounds was performed by headspace GC combined with MS and FID spectroscopy (MS-Agilent 7890B gas chromatograph with FID and 5977A mass selective detector). Analysis of the mass spectra was completed by comparison with the NIST17 spectral library. The results of the headspace chemical characterization showed that the presence of various NIAS was detected in each of Sample 40, Comparative Sample 9, and Comparative Sample 18.

[0184] Sample 40 unexpectedly showed favorable results, as only 11 volatile compounds were detected. In comparison, 21 volatile compounds were detected in Comparative Sample 9, and 19 volatile compounds were detected in Comparative Sample 18. Therefore, the data indicate that the TiO-containing 2 Compared to compositions comprising an incompatible polymer and zinc sulfide without TiO 2 The composition significantly reduced the amount of NIAS produced.

[0185] Example 10

[0186] This example demonstrates that by 2 The significant improvement in infrared (IR) reheat performance achieved by representative articles made from the composition of the present invention. To compare the IR reheat performance, a series of flat rectangular samples were made using an injection molding machine using conditions similar to those used in an injection stretch blow molding machine. Flat samples were made in a range of thicknesses from 0.15 mm to 2.9 mm. The spectral reflectance and transmittance of each thickness were measured using a Cary 5000 UV-Vis-IR spectrophotometer. The spectral absorbance values ​​were calculated using the following equation:

[0187] absorb% λ =100%-reflection% λ-transmission% λ

[0188] Multiply the spectral absorption curve by the theoretical spectral emission (E) of the IR reheat lamp. λ ) and integrated over all measurable wavelengths (λ) to calculate the expected absorption for a given depth / thickness (t) using the following formula:

[0189]

[0190] By calculating the absorption at each thickness, the depth of absorption was estimated.

[0191] Samples 46 and 47 each contained 93 to 95 wt% PET, less than 0.5 wt% colorant, 3 to 5 wt% COC, and 1 to 2 wt% PMP.

[0192] Comparative Sample 19 contained 93.78 wt% dry PET, 6.10 wt% TiO 2 , 0.04 wt% aluminum flakes and 0.08 wt% other colorants.

[0193] The absorption depth curve for each of Samples 46 to 47 and Comparative Example 19 was calculated as shown above, and the results are shown in Table 23, which identifies the percentage of IR light absorbed at various thicknesses.

[0194] Table 23

[0195] Thickness(mm) Sample 46 Sample 47 Comparison 19 0.15 25.2% 9.3% 55.5% 0.25 31.4% 14.8% 65.0% 0.41 52.0% 22.3% 82.2% 0.56 60.7% 56.8% 91.2% 0.76 69.6% 40.7% 92.1% 1.45 91.9% 67.0% 100.0% 2.26 98.6% 83.3% 97.7% 2.90 100.0% 100.0% 99.0%

[0196] Does not contain any TiO 2 Samples 46 to 47 unexpectedly showed favorable results, including demonstrating less than 33% absorption of IR light within the first (outermost) 0.25 mm. Therefore, most of the heat penetrates efficiently into the article, allowing for uniform heat distribution and a wider operating window for reheat stretch blow molding. 2 Comparative Sample 19 of 100% IR light absorption was shown to be greater than 50% within the first 0.15 mm. This can lead to overheating at the surface, non-uniform heat distribution and a narrow operating window for reheat stretch blow molding.

[0197] All references cited and / or discussed in this specification are herein incorporated by reference in their entirety and to the same extent as if each reference were incorporated by reference individually.

Claims

1. An oriented opaque non-pearlescent article comprising one or more layers, wherein at least one layer is a composition comprising: Polyester; an incompatible polymer selected from the group consisting of COC, partially or fully hydrogenated styrenic polymers and copolymers, and combinations thereof, wherein the incompatible polymer is present in an amount of 7 wt % or less based on the total weight of the composition, and wherein the incompatible polymer has a Vicat softening point above the orientation temperature of the article; and 0 wt % to 8 wt % of a light scattering pigment, based on the total weight of the composition; wherein the article is oriented, the layer has an average light transmittance of 20% or less for light having a wavelength in the range of 400 nm to 700 nm, and the layer has a DE between 15° near specular reflection and 110° far specular reflection with a 45° incident light source. CMC Non-pearlescent appearance measuring less than 15 units.

2. The article of claim 1, wherein the layer has a DE of less than 10 units when measured from a 45° illuminant at a viewing angle between 15° and 110°. CMC Non-pearlescent angular flop.

3. The article of claim 1, wherein the layer is white and has a CIELAB Ba* value within ±10 units and a CIELAB b* value within ±10 units.

4. The article of any one of claims 1 to 3, wherein the polyester is polyethylene terephthalate (PET).

5. The article of any one of claims 1 to 3, wherein the composition comprises at least 85 wt% polyester, based on the total weight of the composition.

6. The article of any one of claims 1 to 3, wherein the incompatible polymer comprises a hydrogenated styrenic polymer.

7. The article of any one of claims 1 to 3, wherein the incompatible polymer comprises COC.

8. The article of any one of claims 1 to 3, wherein the composition comprises 5 wt% or less of an incompatible polymer, based on the total weight of the composition.

9. The article of any one of claims 1 to 3, wherein the composition does not contain titanium dioxide.

10. The article of any one of claims 1 to 3, wherein the composition comprises no more than 1 wt% mineral filler, based on the total weight of the composition.

11. The article of any one of claims 1 to 3, wherein the light scattering pigment comprises zinc sulfide present in an amount of 4 wt% or less, based on the total weight of the composition.

12. The article of any one of claims 1 to 3, wherein the composition further comprises titanium dioxide.

13. The article of any one of claims 1 to 3, wherein the composition comprises no more than 0.1 wt% light scattering pigment, based on the total weight of the composition.

14. The article of any one of claims 1 to 3, wherein the composition further comprises an additive or a colorant.

15. The article of any one of claims 1 to 3, wherein the composition comprises an additive selected from the group consisting of antiblocking agents, antioxidants, antistatic agents, slip agents, chain extenders, crosslinkers, flame retardants, IV reducers, laser marking additives, mold release agents, optical brighteners, flow aids, colorants, plasticizers, pigments, dyes, nucleating agents, oxygen scavengers, antimicrobial agents, UV stabilizers, and combinations thereof.

16. The article of any one of claims 1 to 3, wherein the composition comprises a colorant selected from the group consisting of dyes, organic pigments, inorganic pigments, and combinations thereof.

17. The article of claim 14, wherein the colorant comprises aluminum.

18. The article of claim 14, wherein the colorant comprises a combination of dyes.

19. The article of any one of claims 1 to 3, wherein the article is a container.

20. A method for producing an opaque non-pearlescent product, comprising the steps of: (a) hot melt blending a polyester with an incompatible polymer selected from the group consisting of COC, partially or fully hydrogenated styrenic polymers and copolymers, and combinations thereof to produce a composition comprising the incompatible polymer in an amount of 7 wt % or less based on the total weight of the composition, wherein the incompatible polymer has a Vicat softening point above the orientation temperature of the article; (b) subjecting the composition to an orientation stress at a temperature below the Vicat softening point of the incompatible polymer; and (c) Producing an article that is visually non-pearlescent and has a percent transmittance of less than 20% for light having a wavelength in the range of 400 nm to 700 nm.

21. The method of claim 20, wherein at least one additive or colorant is added to the composition during step (a).

22. An oriented opaque non-pearlescent white article comprising one or more layers, wherein at least one layer is a composition comprising, based on the total weight of the composition: At least 91.5% by weight of polyethylene terephthalate (PET); Less than 4 weight percent of an incompatible polymer selected from COC and hydrogenated styrenic polymers, wherein the incompatible polymer has a Vicat softening point above the orientation temperature of the article; Less than 4% by weight of a mineral filler selected from titanium dioxide (TiO2) and zinc sulfide (ZnS); as well as Less than 0.5% by weight of additional components selected from colorants and additives; wherein the article is oriented; the article has a percent transmittance of less than 20% for light having a wavelength in the range of 400 nm to 700 nm; and the layer has a DE of less than 10 units when measured from a 45° light source at a viewing angle between 15° and 110°. CMC The layer has a CIELAB Ba* value within the range of ±10 units and a CIELAB b* value within the range of ±10 units.

23. The article of claim 22, wherein the composition comprises less than 1 wt% TiO2 and less than 3 wt% ZnS.

24. An oriented opaque, non-pearlescent article comprising one or more layers, wherein at least one layer is a composition comprising, based on the total weight of the composition: At least 91.5% by weight of polyethylene terephthalate (PET); Less than 4 weight percent of an incompatible polymer selected from COC and hydrogenated styrenic polymers, wherein the incompatible polymer has a Vicat softening point above the orientation temperature of the article; Less than 4% by weight of zinc sulfide (ZnS); as well as Less than 0.5% by weight of additional components selected from colorants and additives; wherein the composition does not contain titanium dioxide; the article is oriented; the article has a percent transmittance of less than 20% for light having a wavelength in the range of 400 nm to 700 nm; and the layer has a DE of less than 10 units when measured from a 45° light source at a viewing angle between 15° and 110°. CMC Non-pearlescent angular flop.

25. An oriented opaque, non-pearlescent article comprising one or more layers, wherein at least one layer is a composition comprising, based on the total weight of the composition: At least 91.5% by weight of polyethylene terephthalate (PET); 1 to 5 wt% of an incompatible polymer selected from COC and hydrogenated styrenic polymers, wherein the incompatible polymer has a Vicat softening point above the orientation temperature of the article; 1 to 3 wt % polymethylpentene (PMP); and Less than 0.5% by weight of additional components selected from colorants and additives; wherein the composition does not contain titanium dioxide or zinc sulfide; the article is oriented; the article has a percent transmittance of less than 20% for light having a wavelength in the range of 400 nm to 700 nm; and the layer has a DE of less than 10 units when measured from a 45° light source at a viewing angle between 15° and 110°. CMC Non-pearlescent angular flop.

26. The article of claim 25, wherein the additional component comprises a non-mineral ingredient selected from aluminum and an organic dye.

27. An oriented article comprising a layer as a composition comprising: A polyester base resin; and 7 wt% or less of COC, based on the total weight of the composition, wherein the COC has a Vicat softening point above the orientation temperature of the article; wherein the article is oriented, the layer has an average transmittance of less than 20% for light having a wavelength in the range of 400 nm to 700 nm, and the layer has a non-pearlescent flop of less than 10 units DECMC when measured from a 45° light source at viewing angles between 15° and 110°.

28. The article of claim 27, wherein the layer is white.

29. The article of claim 27, wherein the polyester is polyethylene terephthalate (PET).

30. The article of any one of claims 27 to 29, wherein the composition comprises less than 5 wt% COC, based on the total weight of the composition.

31. The article of any one of claims 27 to 29, wherein the composition does not comprise titanium dioxide.

32. The article of any one of claims 27 to 29, wherein the composition further comprises titanium dioxide.

33. The article of any one of claims 27 to 29, wherein the composition further comprises an additive or a colorant.

34. The article of any one of claims 27 to 29, wherein the composition comprises an additive selected from the group consisting of antiblocking agents, antioxidants, antistatic agents, slip agents, chain extenders, crosslinkers, flame retardants, IV reducers, laser marking additives, mold release agents, optical brighteners, flow aids, plasticizers, nucleating agents, oxygen scavengers, antimicrobial agents, and UV stabilizers.

35. The article of any one of claims 27 to 29, wherein the composition comprises a colorant selected from the group consisting of dyes, organic pigments, inorganic pigments, and combinations thereof.

36. The article of claim 33, wherein the colorant comprises a combination of dyes.

37. The article of any one of claims 27 to 29, wherein the article is selected from bottles, sheets, films, and fibers.

38. The article of any one of claims 27 to 29, wherein the COC has a glass transition temperature that is higher than an orientation temperature of the article.

39. A method for producing an opaque non-pearlescent product comprising the following steps: hot melt blending a polyester with COC to produce a composition comprising COC in an amount of 7 wt % or less based on the total weight of the composition, wherein the COC has a Vicat softening point above an orientation temperature of the article; subjecting the composition to an orientation stress at a temperature below the glass transition temperature of the COC; and An article is produced that is visually non-pearlescent and has a percent transmittance of less than 20% for light having a wavelength in the range of 400 nm to 700 nm.