A method for detecting eccentricity direction of round welding strip coating

By removing the round welding tape from the spool, fixing and marking the sample welding tape, and observing the thickness under a microscope after forming a fixed sample, the problem of being unable to accurately locate the eccentric direction of the round welding tape in the prior art is solved, and the product concentricity is improved The accuracy of the adjustment reduces the bad and scrap rate.

CN114280054BActive Publication Date: 2024-11-08NINGBO JIAMING METAL PROD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202111517897.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-13
Publication Date
2024-11-08
Estimated Expiration
2041-12-13

AI Technical Summary

Technical Problem

The prior art cannot accurately locate the eccentric direction of the round welding tape, resulting in poor batch size and scrapping of products during welding.

Method used

By removing the round welding tape from the spool, fixing and marking the sampling welding tape, putting it into the shaping solvent to form the shaping sample, and then observing the thickness under a microscope to determine the eccentric direction.

Benefits of technology

The accurate positioning of the eccentricity direction of the round welding tape is achieved, the defect rate and scrap rate are reduced, and the accuracy of concentricity adjustment is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114280054B_ABST
    Figure CN114280054B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for detecting the eccentric direction of a coating of a round welding strip, the steps of which include: taking the round welding strip to be detected from a bobbin, and selecting a fixed point on the round welding strip for fixing; obtaining a sampled welding strip according to the fixed point, and marking the sampled welding strip; preparing a setting solvent, and placing the sampled welding strip into the setting solvent to obtain a setting sample; and placing the setting sample under a microscope for observation to determine the eccentric direction of the sampled welding strip. The present invention realizes the detection of the eccentric direction of the round welding strip by taking a section of the round welding strip from the bobbin and placing it under a microscope to observe its thickness state, and determining the eccentric direction according to the thickness state. The staff can adjust the position of the production equipment according to the detection result, thereby reducing the defective rate and scrap rate caused by adjusting the concentricity of the product, and improving the accuracy of the staff in adjusting the concentricity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of detection technology, and in particular to a method for detecting the eccentricity direction of a round welding strip coating. Background Art

[0002] The welding ribbon is an important raw material in the welding process of photovoltaic modules. The quality of the welding ribbon will directly affect the current collection efficiency of the photovoltaic module and have a great impact on the power of the photovoltaic module.

[0003] For circular welding strips, there is currently no detection method that can accurately locate the eccentricity direction of the circular welding strip. For example, it is impossible to determine in which direction (front, back, left, right) the circular welding strip is thinner or thicker. As a result, the staff cannot make timely adjustments due to the unclear eccentricity direction of the coating, which can easily cause batch defects and scrapping of circular welding strip products. Summary of the invention

[0004] In view of the defects in the prior art, the present invention provides a method for detecting the eccentricity direction of a round welding strip coating, the steps comprising:

[0005] Take the round welding strip to be tested from the spool, and select a fixed point on the round welding strip for fixing;

[0006] Acquire a sampled welding strip according to the fixed point, and mark the sampled welding strip;

[0007] Preparing a setting solvent, and placing the sampling welding strip into the setting solvent to obtain a setting sample;

[0008] The shaped sample is placed under a microscope for observation to determine the eccentricity direction of the sampled welding strip.

[0009] Furthermore, before selecting a fixing point on the circular welding belt for fixing, the method further comprises: maintaining the circular winding state of the circular welding belt.

[0010] Furthermore, the fixing points are selected on the circular welding strip for fixing, specifically:

[0011] An arbitrary point on the curved section of the circular welding strip is selected as a fixed point, and the circular welding strip is fixed at the fixed point with an adhesive tape.

[0012] Furthermore, the sampling welding strip is a welding strip having a total length of 3 cm before and after the fixed point, and the sampling welding strip remains in a bent state.

[0013] Furthermore, the sampling welding strip is marked, specifically:

[0014] The inner curved surface of the sampled welding strip is marked as surface A, and the outer curved surface of the sampled welding strip is marked as surface B.

[0015] Furthermore, before the setting solvent is prepared, the method further includes: flattening the sampling welding strip and placing it horizontally.

[0016] Furthermore, the step of obtaining the finalized sample is as follows:

[0017] The sampling welding strip is vertically placed in a shaping solvent, and taken out after being cooled and shaped, so as to obtain a shaped sample, wherein the shaped sample is a solid sample comprising the sampling welding strip and the shaping solvent.

[0018] Furthermore, the shaped sample is placed under a microscope for observation to determine the eccentricity direction of the sampled welding strip, specifically:

[0019] When placing the finalized sample under a microscope, the A side of the sampled welding strip in the finalized sample faces the inspector;

[0020] Obtaining an imaging result through observation under the microscope, and obtaining an actual thick point of the sampled welding strip according to the imaging result;

[0021] The direction of the actual thick point of the sampled welding strip is determined as the eccentric direction.

[0022] The beneficial effects of the present invention are as follows: by taking a section of the circular welding strip from the spool and placing it under a microscope, observing its thickness state, and judging the eccentricity direction according to the thickness state, the eccentricity direction of the circular welding strip can be detected, and the staff can adjust the position of the production equipment according to the detection results, thereby reducing the defective rate and scrap rate caused by adjusting the concentricity of the product and improving the accuracy of the staff in adjusting the concentricity. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.

[0024] Figure 1 A flow chart of a method for detecting the eccentricity direction of a circular welding strip coating provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0025] The following embodiments of the technical solution of the present invention are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore only used as examples, and cannot be used to limit the protection scope of the present invention.

[0026] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in this application should have the common meanings understood by those skilled in the art to which the present invention belongs.

[0027] like Figure 1 As shown, a method for detecting the eccentricity direction of a round welding strip coating comprises the following steps:

[0028] S1: Take the round welding strip to be tested from the spool, and select a fixed point on the round welding strip for fixing;

[0029] Specifically, take a section of the round welding tape to be tested from the spool, the length of which is about 5-7 turns, and keep the round welding tape in a circular winding state after taking it off. After taking off the round welding tape, select any point on the curved section of the round welding tape as a fixed point, and then take a small section of tape and stick it on the fixed point to fix the round welding tape.

[0030] S2: Obtain a sampled welding strip according to the fixed point, and mark the sampled welding strip;

[0031] Specifically, after the round welding strip is fixed, use scissors to cut off the welding strip with a total length of about 3 cm before and after the fixing point as the sampling welding strip, and keep the cutting sampling welding strip in a bent state. After removal, the two sides of the sampling welding strip are divided into the inner side and the outer side according to the inner curved surface and the outer curved surface of the sampling welding strip, and the inner side of the sampling welding strip is marked as the A side and the outer side is marked as the B side with a marker pen, so as to distinguish them in the subsequent steps.

[0032] S3: preparing a setting solvent, and placing the sampled welding strip into the setting solvent to obtain a setting sample;

[0033] Specifically, after marking the sampling welding strip, before configuring the setting solvent, it is also necessary to place the sampling welding strip on a horizontal plane and flatten it. Since the marking has been done in step S2, the inner and outer sides of the sampling welding strip can be distinguished according to the mark at this time. When configuring the setting solvent, first take a fixed container, the size of which can be selected according to the actual situation, and pour resin powder into the fixed container to configure the setting solvent. After the setting solvent is slightly solidified, the flattened sampling welding strip is vertically placed in the setting solvent, that is, the A side and the B side of the sampling welding strip are both kept 90° vertical to the bottom of the fixed container. After the setting solvent to be inserted into the sampling welding strip is completely cooled and set, the set sample is taken out, and the set sample at this time is a solid sample containing the sampling welding strip and the setting solvent.

[0034] S4: placing the shaped sample under a microscope for observation to determine the eccentricity direction of the sampled welding strip;

[0035] Specifically, after taking out the finalized sample, enter the microscope observation stage. Preferably, after taking out the finalized sample, the cross section of the finalized sample can be ground and polished first, and the ground cross section is the observation surface, so that the image can be clearer when observed with a microscope. When placing the finalized sample, place the finalized sample with the sampling weld belt side A facing outward, that is, the sampling weld belt side A inside the finalized sample is facing the inspector. Since the sampling weld belt is vertically inserted into the finalized sample, the finalized sample is viewed from the perspective of the microscope at this time, and the A side is the bottom of the sampling weld belt, and the B side is the top of the sampling weld belt.

[0036] After placing, observe the finalized sample through a microscope to obtain the imaging result. The thickness of the sampled welding strip can be seen from the imaging result, so as to obtain the actual thick point of the sampled welding strip. The microscope includes a positive imaging microscope and a negative imaging microscope. If a positive imaging microscope is used for observation, the thickness of the imaging result is the actual thickness of the sampled welding strip, and the thick part is the actual thick point of the sampled welding strip. For example, if a positive imaging microscope is used for observation, if the bottom of the sampled welding strip is thicker in the microscope, then the actual object is also thicker in the bottom, that is, the A side of the sampled welding strip is thicker; if the top of the sampled welding strip is thicker in the microscope, then the actual object is also thicker in the top, that is, the B side of the sampled welding strip is thicker.

[0037] If an inverse imaging microscope is used for observation, according to the imaging principle, the thicker points presented in the imaging results are the actual thinner points of the sampled welding strip. Correspondingly, the thinner points presented in the imaging results are the actual thicker points of the sampled welding strip. For example, if an inverse imaging microscope is used for observation, if the bottom of the sampled welding strip is thinner and the top is thicker in the microscope, then the actual object is thinner at the top and thicker at the bottom, that is, the A side of the sampled welding strip is thicker; if the top of the sampled welding strip is thinner and the bottom is thicker in the microscope, then the actual object is thinner at the bottom and thicker at the top, that is, the B side of the sampled welding strip is thicker. The actual thickness state judgment process of the left and right directions of the sampled welding strip is similar.

[0038] After obtaining the actual thick point of the sampled welding strip according to the imaging result, the direction of the actual thick point of the sampled welding strip is determined as the eccentric direction. For example, if the actual sampled welding strip is observed to be thicker at the bottom, the center of the circle of the sampled welding strip is determined to be downward, that is, the eccentric direction is downward. The eccentric direction of the sampled welding strip is the eccentric direction of the circular welding strip, and the position is adjusted in combination with the corresponding production machine, thereby improving the accuracy of the product concentricity.

[0039] The eccentricity direction detection method provided by the present invention is also applicable to any round wire product with a coating on the outside, such as enameled wire, and has a wide range of applications and high practical value.

[0040] The present invention realizes the detection of the eccentricity direction of the circular welding strip by taking a section of the circular welding strip from the spool and placing it under a microscope to observe the thickness state thereof and judge the eccentricity direction according to the thickness state. The staff can adjust the position of the production equipment according to the detection result, thereby reducing the defective rate and scrap rate caused by adjusting the concentricity of the product and improving the accuracy of the staff in adjusting the concentricity.

[0041] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.

Claims

1. A method for detecting the eccentricity direction of a round welding strip coating, characterized in that the steps include: Take the round welding tape to be tested off the spool, keep the round welding tape in a circular winding state after taking it off, and select a fixed point on the round welding tape for fixing; The sampled welding strip is obtained according to the fixed point, the sampled welding strip is kept in a bent state after being cut, and the inner curved surface of the sampled welding strip is marked as surface A, and the outer curved surface is marked as surface B; Place the sampled welding strip on a horizontal surface and press it flat; Prepare a setting solvent, and vertically place the sampling welding strip into the setting solvent so that both the A side and the B side of the sampling welding strip are kept 90° vertical to the bottom of the fixed container to obtain a setting sample; The shaped sample is placed under a microscope for observation to determine the eccentricity direction of the sampled welding strip, specifically: When placing the finalized sample under a microscope, the A side of the sampled welding strip in the finalized sample faces the inspector; Obtaining an imaging result through observation under the microscope, and obtaining an actual thick point of the sampled welding strip according to the imaging result; The direction of the actual thick point of the sampled welding strip is determined as the eccentric direction.

2. A method for detecting the eccentricity direction of a round welding strip coating according to claim 1, characterized in that: The fixing point is selected on the circular welding strip for fixing, specifically: An arbitrary point on the curved section of the circular welding belt is selected as a fixed point, and the circular welding belt is fixed at the fixed point with an adhesive tape.

3. A method for detecting the eccentricity direction of a round welding strip coating according to claim 2, characterized in that: The sampling welding strip is a welding strip with a total length of 3 cm before and after the fixed point.

4. A method for detecting the eccentricity direction of a round welding strip coating according to claim 3, characterized in that: The obtaining of the finalized sample specifically comprises: The sampling welding strip is vertically placed in a shaping solvent, and taken out after being cooled and shaped, so as to obtain a shaped sample, wherein the shaped sample is a solid sample comprising the sampling welding strip and the shaping solvent.

Citation Information

Patent Citations

  • Non-contact welding rod eccentric value detecting device and method

    CN108145344A

  • Photovoltaic solder strip

    CN110890441A

  • Laser welding strip eccentricity detection device

    CN210321642U

  • Non-destructive evaluation and weld-to-weld adaptive control of metal resistance spot welds via topographical data collection and analysis

    WO2020205998A1