Method for producing a thin-walled plastic small part and thin-walled plastic small part
By using low-viscosity polyethylene furanoate to manufacture thin-walled plastic small parts in the plastic injection molding method, the problem of difficult recycling of multi-layer film manufacturing in the existing technology is solved, and efficient, low-cost single-layer structure manufacturing and Improved barrier properties.
Patent Information
- Application Number
- CN202111624519.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2016-01-20
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2036-01-20
AI Technical Summary
Existing thin-walled plastic small parts present difficulties in recycling because the way the multilayer film is thermoformed makes it difficult to separate and recycle.
Low-viscosity polyethylene furanoate (PEF) is used to manufacture thin-walled plastic small parts through plastic injection molding. Its low viscosity and high crystallinity characteristics are used to achieve the manufacturing of a single-layer structure, and the content is reduced through drying and foaming processes. The amount of water ensures the stability of the molecular structure.
It achieves low-cost and efficient manufacturing of thin-walled plastic small parts, improves its barrier properties and heat resistance, and makes it fully suitable for recycling, avoiding the complex process and high cost of thermoforming.
Abstract
Description
[0001] The present invention is a divisional application of an invention patent application with an application date of January 20, 2016, application number 201680008651.2 (PCT / EP2016 / 051129), and invention name “Method for manufacturing thin-walled plastic small parts and thin-walled plastic small parts”. Technical Field
[0002] The invention relates to a method for producing a thin-walled plastic small part. The invention also relates to a thin-walled plastic small part. Background Art
[0003] Plastic small parts for the purposes of the present invention relate to, for example, closures for beverage packages, parts of packages such as tube shoulders, entire packages such as cups, capsule-shaped containers and blister-shaped packages (pads) for coffee, cocoa or tea, etc. For the purposes of the present invention, plastic small parts are considered to be thin-walled if they have an average wall thickness of less than 1.5 mm.
[0004] Such thin-layer plastic small parts are usually made of general-purpose plastics (Massenkunststoffen), such as polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polystyrene (PS) or polyvinyl chloride (PVC). Since plastic small parts made of these general-purpose plastics have only relatively poor barrier properties with respect to oxygen, carbon dioxide and water vapor, especially due to their thin walls, additional barrier layers are usually provided when plastic small parts are produced from these materials, or the plastic must be mixed with barrier additives before it is processed into plastic small parts. Ethylene vinyl alcohol copolymer (EVOH), polyglycolic acid (PGA) or polyamide are used as barrier layers, for example. Plastic small parts with plasma coatings, such as carbon coatings (DLC) or thin titanium coatings, aluminum coatings or silicon oxide coatings are often used to achieve the required barrier properties.
[0005] The production of such thin-walled plastic small parts is usually achieved by thermoforming (deep drawing) of multilayer films. The production of multilayer films is relatively simple and widely used on the market. Thermoforming (deep drawing) represents a traditional field of application, especially for the production of packaging parts, for example in the food industry, and has been well proven.
[0006] However, the use of multi-layer films or sheets in thermoforming has proven to be disadvantageous for recycling, since the multi-layered plastic small parts are difficult to separate from the specific materials, if any. In the case of thermoforming, punching screens are often still required, which are difficult or impossible to feed to the recycling process. As a result, the recycling rates sought or specified are often not achieved. Summary of the invention
[0007] The object of the present invention is therefore to eliminate the disadvantages of the thin-walled plastic small parts of the prior art described. A method for producing such thin-walled plastic small parts should be realized, by means of which plastic small parts can be produced which can be easily recycled after their normal use.
[0008] The solution to this object is the method according to the invention for producing thin-walled plastic small parts. According to the invention, the object is also achieved by the thin-walled plastic small parts according to the invention. Improvements and / or advantageous embodiment variants of the invention are described below.
[0009] The invention provides a method for producing thin-walled plastic small parts with an average wall thickness of less than 1.5 mm, wherein the plastic small parts are produced in a plastic injection molding process from polyethylene furanoate (PEF), which has a viscosity of 0.4 dl / g to 0.7 dl / g, preferably less than 0.6 dl / g, measured according to a measurement method similar to ASTM D4603, which describes a test in PET materials, and has a water content of less than 100 ppm during injection molding of the plastic. Ideally, the water content during injection molding of the plastic is less than 30 ppm.
[0010] By using polyethylene furanoate (PEF) with a very low viscosity, it is possible to produce small plastic parts very economically in the plastic injection molding process. In this case, the viscosity is determined according to a measurement method similar to ASTM D4603. Although these standardized measurement methods have been developed for determining the viscosity of PET, they can also be applied to PEF in a similar manner. The measurement method for the viscosity of PEF, similar to ASTM D4603, was selected because there is no special standard for viscosity measurement for the material PEF.
[0011] The use of very fluid PEF as raw material reduces its production costs, since time-consuming and costly solid phase polymerization processes (or polycondensation processes) can be dispensed with or only have to be carried out to a limited extent in order to achieve the desired viscosity. In addition, the use of fluid PEF has advantages during plastic injection molding. During plastic injection molding, with the aid of fluid PEF, long, thin flow paths can be produced very easily without the risk of premature solidification of the PEF melt or of orientation of the molecular chains in the PEF melt. This allows the production of very thin-walled and low-distortion profiles in the plastic injection molding process.
[0012] The low viscosity of PEF used for plastic injection molding also has a positive effect on the barrier properties of PEF, because the fluid PEF is significantly more mobile due to its relatively short molecular chain, so that it can crystallize more to the desired crystallinity. Higher crystallinity is conducive to the barrier properties and heat resistance of injection-molded thin-walled plastic small parts. On the other hand, the higher amorphous state of plastic small parts is conducive to low-temperature impact resistance. For example, amorphous PEF has a 10-fold higher barrier property relative to oxygen compared to PET with similar wall thickness. Compared with PP, the barrier property of amorphous PEF relative to oxygen is even up to 300 times. Compared with PET with the same wall thickness, the barrier property of PEF relative to water vapor is also twice as much. Therefore, amorphous PEF has an advantage in maintaining the aroma of the product being transferred relative to the traditionally used plastics. As a result, thin-walled plastic small parts can be manufactured as a single-layer structure. The manufacture of multi-layer films or plates for thermoforming and the frequently used punching screens are omitted. Compared to thermal reforming, less plastic material must be heated and cooled again for plastic injection molding. The inherently more complex plastic injection molding method is therefore a more cost-effective alternative to hot forming (deep drawing). Plastic small parts injection molded from single-layer PEF can be completely fed to recycling processes, which can have a positive effect on the recycling rate to be achieved.
[0013] Here, the PEF processed in the plastic injection molding method has a water content of less than 100 ppm. Preferably, the water content of the PEF processed in the plastic injection molding method is less than 30 ppm. For this reason, the PEF is dried before its processing. Before the PEF is processed in the plastic injection molding method, setting its viscosity and water content helps to maintain the molecular structure of the PEF and especially its chain length. By drying the PEF, the hydrolytic decomposition of the chain is reduced, and the chain breakage of the PEF can be suppressed by the hydrolysis during the injection molding of the PEF. Here, the preparation of the PEF should be as close as possible to its further processing in the plastic injection molding method. For the purposes of the present invention, a time period of 0 to 2 hours is regarded as close in time. The PEF used to manufacture thin-walled plastic small parts in the plastic injection molding method can have a linear structure or contain smaller or larger branches. DETAILED DESCRIPTION
[0014] In one method variant, the PEF used for the plastic injection molding method can contain 10% to 100% bio-based PEF. For ecological reasons, the use of bio-based PEF is desirable, since only renewable substances are used for the production of the PEF.
[0015] In another method variant, the PEF used can contain up to 100% renewable materials. Due to the production method of PEF and the temperatures used for drying and further processing of PEF, possible small impurities with other substances, especially other polymers, are of minor importance. Thus, injection-molded plastic small parts containing renewable materials can come into direct contact with the packaging goods without restriction.
[0016] Another method variant can provide that the PEF is foamed physically or chemically until it has a degree of foaming of 0% to 30%. Here, the foaming of the PEF can be carried out inside the mold cavity of the injection molding mold used.
[0017] Another method variant can provide for the admixture of an easily oxidizable additional material which can react with oxygen with or without a catalyst and can thus protect the filler from oxygen. Cobalt salts come into consideration as catalysts, for example.
[0018] In order to set the desired moisture content, the PEF can be dried at a drying temperature which is greater than 100° C. and less than 200° C. The drying process serves to set the moisture content of the PEF and allows the PEF material to be partially purified or the viscosity to be increased to the desired level if necessary. The drying can be carried out in a conventional dryer. However, it can prove to be expedient to use a stirring tool or a corresponding device during the drying in order to avoid the PEF material from sticking. Depending on the initial wetness of the PEF material, a drying time of between 3 hours and 30 hours is sought in order to achieve a moisture content of less than 100 ppm. In addition, energy can also be introduced by infrared radiation or microwave radiation in order to further shorten the drying time. Finally, the drying of the PEF can also be carried out in a vacuum or in an inert gas environment, for example in a nitrogen environment, which does not react with the PEF.
[0019] In another method variant, the PEF can be admixed with a certain proportion of nucleating agents, which does not exceed 5%. The addition of nucleating agents can influence the crystallization in a targeted manner. Examples of nucleating agents used are: calcium carbonate, clay powder, silicates, alkali metal salts, alkaline earth metal salts, aluminum salts, titanium salts, organic salts (e.g. metal salts of polyesters), metal oxides, sorbitol derivatives, phosphate derivatives, talc, waxes, polyolefins (PE, TPE, PP), aliphatic polyamides.
[0020] In an alternative method variant, in order to suppress crystallization during the injection molding of the PEF, a proportion of a copolymer, for example diethylene glycol, which does not exceed 10% can be admixed to the PEF.
[0021] The thin-walled plastic small parts produced according to the invention by the plastic injection molding method have an average wall thickness of less than 1.5 mm. In this case, the plastic small parts consist essentially only of a single-layer PEF. The single-layer construction of the plastic small parts from PEF makes them completely recyclable, which is particularly desirable from an ecological point of view.
[0022] In one variant of the invention, the injection molded thin-walled plastic small parts have an average wall thickness of less than 1 mm. The low-viscosity PEF used is very fluid and allows very rapid filling of the mold cavity of the injection molding mold. Due to the very narrow mold gap width, a certain degree of desired crystallization of the injected PEF melt can still be induced.
[0023] One variant of the invention can provide that the thin-walled plastic small part at least partially has a crystallinity of up to 50%. A higher crystallinity can have a positive effect on the barrier properties, while the amorphous state of the PEF can have a favorable effect on the low-temperature impact resistance.
[0024] In a variant of the invention, the injection molding die can be not completely closed when the PEF material is injected and the injection molding die is completely closed only during or after the PEF material is injected. In this type of process control, thin-walled plastic small parts are formed by the injection molding process and the impact extrusion process. Depending on when the mold is just closed, the injection molding process or the impact extrusion process is dominant.
[0025] In another method variant, the thermoplastic PEF molding compound can be introduced into the mold cavity before the mold is closed. In this case, the production of the plastic small parts is no longer actually an injection molding process, but in this case it is called an impact extrusion method.
[0026] The injection-molded thin-walled plastic small parts according to the invention can be configured as closures for beverage packages, parts of packages, such as tube shoulders, entire packages, such as cups, capsule containers and blister packages (pads) for coffee, cocoa or tea. The plastic small parts can be configured in particular as packages for oxygen-sensitive fillers. The thin-walled plastic small parts can be, for example, cups or trays for oxygen-sensitive fillers. The configuration of the injection-molded thin-walled plastic small parts as capsule-shaped or blister-shaped packages for coffee, cocoa or tea allows storage with minimal loss of flavor. Here, the closing film for the capsule-shaped packages can also be made of PEF, which greatly improves the recyclability of such packages. Finally, the thin-walled plastic small parts according to the invention can also be used as cups for children's food, for the preservation of pesto, sauce or ketchup.
[0027] The use of low-viscosity PEF enables the cost-effective production of thin-walled plastic small parts by plastic injection molding. Plastic small parts injection-molded from PEF can be constructed in a single layer without negatively affecting their barrier properties. Here, the plastic small parts are at least equal to, and in many cases even superior to, plastic small parts constructed from films or plates in thermoforming (deep drawing) with regard to their barrier properties, the films or plates being composed of conventional general-purpose plastics such as PE, PP, PET, PS or PVC, the frame plastic being provided with a barrier layer consisting of EVOH, PGA or PA or also having a coating consisting of an amorphous carbon layer or a thin glass coating. Unlike the prior art plastic small parts that are multi-layered and constructed from a variety of different materials, are difficult to transport and cannot be completely transported to a recycling process, the thin-walled plastic small parts according to the present invention are single-material parts constructed from a single layer of PEF, which are very simple and completely recyclable.
[0028] According to an embodiment of the present disclosure, the following additional notes are also disclosed:
[0029] Note 1. A method for manufacturing thin-walled plastic small parts with an average wall thickness of less than 1.5 mm,
[0030] It is characterized in that
[0031] The plastic small parts are produced in a plastic injection molding process from polyethylene furanoate (PEF), which has a viscosity of 0.4 dl / g to 0.7 dl / g, preferably less than 0.6 dl / g, measured according to the measurement method according to ASTM D4603, and has a water content of less than 100 ppm, preferably less than 30 ppm during plastic injection molding.
[0032] Note 2. According to the method described in Note 1,
[0033] It is characterized in that
[0034] PEF is used for the plastic injection molding method, and the PEF includes 10% to 100% by mass of bio-based PEF.
[0035] Note 3. The method according to Note 1 or 2,
[0036] It is characterized in that
[0037] PEF is used for the plastic injection molding process, which PEF comprises up to 100% renewable materials.
[0038] Note 4. The method according to any one of Notes 1 to 3,
[0039] It is characterized in that
[0040] The PEF is physically or chemically foamed to have a foaming degree of 0% to 30%.
[0041] Note 5. According to any one of the above notes,
[0042] It is characterized in that
[0043] The PEF is dried at a drying temperature greater than 100°C but less than 200°C.
[0044] Note 6. According to the method described in Note 5,
[0045] It is characterized in that
[0046] The PEF is agitated during the drying process.
[0047] Note 7. The method according to Note 5 or 6,
[0048] It is characterized in that
[0049] The drying process of the PEF is assisted by delivering energy in the form of microwave radiation.
[0050] Note 8. The method according to any one of Notes 5 to 7,
[0051] It is characterized in that
[0052] The drying of the PEF is performed under vacuum conditions or in an inert gas environment.
[0053] Note 9. According to any one of the above notes,
[0054] It is characterized in that
[0055] The PEF is doped with a nucleating agent in a proportion not exceeding 5% by mass.
[0056] Note 10. The method according to any one of Notes 1 to 8,
[0057] It is characterized in that
[0058] The PEF is admixed with a copolymer in a proportion not exceeding 10% by mass.
[0059] Note 11. A thin-walled plastic small component with an average wall thickness of less than 1.5 mm, the plastic small component being manufactured by the injection molding method according to any one of Notes 1 to 10.
[0060] It is characterized in that
[0061] The plastic small part consists essentially of PEF in a single-layer configuration.
[0062] Note 12. A thin-walled plastic small part according to Note 10,
[0063] It is characterized in that
[0064] The plastic small part has an average wall thickness of less than 1 mm.
[0065] Note 13. A thin-walled plastic small part according to Note 11 or 12,
[0066] It is characterized in that
[0067] The plastic small component at least partially has a degree of crystallinity of up to 50%.
[0068] Note 14. A thin-walled plastic small part according to any one of Notes 11 to 13,
[0069] It is characterized in that
[0070] The plastic small parts constitute, for example, closures for beverage packages, parts of packages, such as tube shoulders, entire packages, such as cups, capsule-like containers and blister-like packages (pads), for example, for coffee, cocoa or tea.
[0071] Note 15. A thin-walled plastic small part according to any one of Notes 11 to 14,
[0072] It is characterized in that
[0073] The small plastic part is designed as a packaging for an oxygen-sensitive filler.
Claims
1. A method for producing thin-walled plastic small parts with an average wall thickness of less than 1.5 mm, It is characterized in that The plastic small part is produced from polyethylene furanoate (PEF) in a plastic injection molding process, wherein the viscosity of the polyethylene furanoate is set to 0.4 dl / g to 0.7 dl / g before the polyethylene furanoate is processed in the plastic injection molding process, the viscosity being measured according to the measuring method in accordance with ASTM D4603, and the water content of the polyethylene furanoate is set to less than 100 ppm by drying before the polyethylene furanoate is processed in the plastic injection molding process, and wherein the plastic small part consists of a single-layer PEF.
2. The method according to claim 1, characterized in that The viscosity of the polyethylene furanoate is set to less than 0.6 dl / g before processing the polyethylene furanoate in the plastic injection molding process.
3. The method according to claim 1, characterized in that: The water content of the polyethylene furanoate is set to less than 30 ppm by drying before processing the polyethylene furanoate in the plastic injection molding process.
4. The method according to claim 1, It is characterized in that PEF is used for the plastic injection molding method, and the PEF includes 10% to 100% by mass of bio-based PEF.
5. The method according to claim 1 or 4, It is characterized in that PEF is used for the plastic injection molding process, which PEF comprises up to 100% renewable materials.
6. The method according to any one of claims 1 to 4, It is characterized in that The PEF is physically or chemically foamed to have a foaming degree of 0% to 30%.
7. The method according to any one of claims 1 to 4, It is characterized in that The PEF is dried at a drying temperature greater than 100°C but less than 200°C.
8. The method according to claim 7, It is characterized in that The PEF is agitated during the drying process.
9. The method according to claim 7, It is characterized in that The drying process of the PEF is assisted by delivering energy in the form of microwave radiation.
10. The method according to claim 7, It is characterized in that The drying of the PEF is performed under vacuum conditions or in an inert gas environment.
11. The method according to any one of claims 1 to 4, It is characterized in that The PEF is doped with a nucleating agent in a proportion not exceeding 5% by mass.
12. The method according to any one of claims 1 to 4, It is characterized in that The PEF is admixed with a copolymer in a proportion not exceeding 10% by mass.
13. A thin-walled plastic small part with an average wall thickness of less than 1.5 mm, the plastic small part being produced by the method according to any one of claims 1 to 12, It is characterized in that The plastic small part consists essentially of PEF in a single-layer configuration.
14. The thin-walled plastic small part according to claim 13, It is characterized in that The plastic small part has an average wall thickness of less than 1 mm.
15. A thin-walled plastic small part according to claim 13 or 14, It is characterized in that The plastic small component at least partially has a degree of crystallinity of up to 50%.
16. A thin-walled plastic small part according to claim 13 or 14, It is characterized in that The small plastic part is formed as: a closure; a part of a packaging; or a whole packaging.
17. The thin-walled plastic small part according to claim 16, It is characterized in that The closure is a closure for a beverage package, a portion of the package is a tube shoulder, and the entire package is an entire package for cups, capsule-like containers and blister-like packages of coffee, cocoa or tea.
18. A thin-walled plastic small part according to claim 13 or 14, It is characterized in that The small plastic part is designed as a packaging for an oxygen-sensitive filler.
Citation Information
Patent Citations
Polyester compositions
CN103328569A
In-mould labelling process
CN104203537A
Plastic bottles for perfume compositions having improved crazing resistance
CN104271633A
Method for solid phase polymerization
CN1238790A
Copolymerized polyester suitable for extrusion
CN1244544A