Crystal chip mixed metallization method and crystal chip and electronic device

The high binding force metal layer is formed on the crystal chip by electroless plating method, which solves the problem of insufficient bonding force between metal and silicon in the prior art, and improves the mechanical strength and thermal resistance performance of the device.

CN114300351BActive Publication Date: 2024-11-01QINGDAO TIANYIN TEXTILE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111622524.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-11-01
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

In the prior art, the bonding force between metal and silicon during the metallization process of crystal chips is insufficient, resulting in the film being easily shedded, affecting product quality, and the high-temperature evaporation process has insufficient step coverage and adhesion.

Method used

Using a hybrid metallization method based on electroless plating, the nanopalladium particles are contacted by treating the surface of the silicon wafer with a modified alkali solution, followed by coating the nickel plating and gold plating solution, and drying at different temperatures to form a high The bonding metal layer.

Benefits of technology

High adhesion between the metal layer and silicon is achieved, hollowing during contact is reduced, mechanical strength and welding thermal resistance are improved, and thermal fatigue resistance and ohmic contact of the device are enhanced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a crystal chip mixed metallization method, a crystal chip and an electronic device. The metal deposition of the crystal chip of the present invention has good adhesion to silicon, and there are few voids when contact is formed, so that the mechanical strength of the bonding between the chip and the deposited metal is high, and the contact thermal resistance of the solder layer between the chips is small, thereby reducing the thermal resistance of the device, having good secondary breakdown performance, and high anti-thermal fatigue cycle times. In addition, after the metal of the present invention is deposited, it has good ohmic contact with silicon and a small series resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of integrated circuits, in particular to a method for hybrid metallization of a crystal chip, a metallized crystal chip obtained thereby and an electronic device containing the metallized crystal chip. Background Art

[0002] In the manufacturing process of crystal chips, it is required that there is no rectification effect between metals and semiconductors, that is, the voltage-current relationship conforms to Ohm's law. The purpose of crystal chip metallization is to make the contact electrodes form good ohmic contact. The metallized chip has the characteristics of small saturation voltage drop, reliable welding, small on-state source-drain resistance, good heat dissipation, and low working energy consumption. Crystal chip metallization is a very important technology in the manufacturing process of transistors, especially for transistor devices with high operating voltage and large current. The quality of metal deposition has very high requirements for reliability.

[0003] At present, the industry widely uses high-temperature evaporation processes to metallize crystal chips, mainly including single-gun multi-crucible electron beam evaporation coating and multi-target magnetron sputtering coating. Among them, the former has the advantages of forming metal deposition on the back of the wafer, such as simple equipment and easy operation, high purity of the prepared film, fast film formation rate, simple growth mechanism, etc.; the disadvantages are that the formed film has low adhesion to the substrate and poor step coverage. The advantage of the latter is that it is suitable for depositing alloys and has the ability to maintain the original components of complex alloys. It can improve step coverage and adhesion between the film and the substrate.

[0004] Although schemes for chemically plating metal on substrates have been disclosed, these chemical plating methods are rarely used for metallization of crystal chips. One reason is that chemical plating generally requires treating the substrate with an acidic solution, and the plated metal has a weak bond with silicon and is easily detached during the production or use of electronic devices, thereby causing problems such as product quality.

[0005] The information in the background technology is only for illustrating the general background of the present invention and should not be regarded as admitting or suggesting in any form that such information constitutes the prior art known to a person skilled in the art. Summary of the invention

[0006] In order to solve at least some of the technical problems in the prior art, the present invention improves the hybrid metallization method of crystal chips based on chemical plating, thereby obtaining a hybrid metallized crystal chip with strong bonding force that can meet actual production needs. Specifically, the present invention includes the following contents.

[0007] A first aspect of the present invention provides a method for hybrid metallization of a crystal chip, comprising the following steps:

[0008] (1) contacting at least a portion of the surface of the silicon wafer with a modified alkaline solution having a pH of 8-10 to obtain a treated surface;

[0009] (2) contacting the treated surface of the silicon wafer (i.e., the treated surface) with a dispersion of nano-palladium particles for 1-10 hours, and then taking it out and drying it;

[0010] (3) applying a nickel plating solution to the treated surface of the silicon wafer obtained in step (2) and reacting for 1-10 minutes, removing the nickel plating solution and drying;

[0011] (4) further coating the treated surface obtained in step (3) with a gold plating solution and reacting for 10-30 minutes, removing the gold plating solution and drying; and

[0012] (5) heating to 120-160° C. in an inert atmosphere or vacuum and drying for 10-20 minutes, then heating to 200-300° C. and drying for 25-35 minutes, and then further heating to 970-1000° C. and drying for 3-6 hours, thereby obtaining a metallized silicon crystal chip.

[0013] According to the crystal chip mixed metallization method of the present invention, preferably, the nickel plating solution contains 15-20 g / L nickel chloride, 20-30 g / L sodium hypophosphite and 10-20 g / L sodium acetate.

[0014] According to the crystal chip mixed metallization method of the present invention, preferably, the gold plating solution contains 0.5-5 g / L gold cyanide, 5-15 g / L sodium tetraborate, 1-5 g / L potassium cyanide and 10-20 g / L sodium thiosulfate.

[0015] According to the crystal chip hybrid metallization method of the present invention, preferably, the modified alkaline solution contains 1-10 mg / ml of dopamine.

[0016] According to the crystalline chip hybrid metallization method of the present invention, preferably, at least part of the surface is located on the back side of the silicon wafer.

[0017] According to the crystalline chip hybrid metallization method of the present invention, preferably, after step (5), a cleaning and drying step is further included, which includes cleaning the wafer with water for 10-30 minutes and then heating it to 150-250° C. for drying.

[0018] The second aspect of the present invention provides a mixed metallized crystal chip, which is obtained by the preparation method described in the first aspect of the present invention, wherein the thickness of the metal layer is 3-10 μm.

[0019] The third aspect of the present invention provides an electronic device comprising the hybrid metallization crystal chip described in the first aspect of the present invention.

[0020] The metal deposition of the crystal chip of the present invention has good adhesion to silicon, and there are few voids when contact is formed. In this way, the mechanical strength of the bonding between the wafer and the deposited metal can be high, and the contact thermal resistance of the solder layer between the wafers is small, thereby reducing the thermal resistance of the device, having good secondary breakdown performance, and a high number of thermal fatigue resistance cycles. In addition, after the metal of the present invention is deposited, it has good ohmic contact with silicon and a small series resistance. At the same time, the thermal matching between the wafer solder obtained by the present invention and the layers of the bottom layer is good, thereby improving the thermal fatigue resistance of the device. DETAILED DESCRIPTION

[0021] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0022] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that the upper and lower limits of the scope and each intermediate value therebetween are specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0023] Unless otherwise specified, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail. Unless otherwise specified, "%" is a percentage based on weight.

[0024] The term "mixed metallized crystal chip" herein refers to a chip with two or more different metals deposited on at least a portion of the surface of a silicon crystal chip. In particular, it refers to the plating of two or more different metals by chemical methods. Different metals can be deposited on the surface of the silicon crystal in a mixed form, or, for example, a certain metal first forms a first metal layer on at least a portion of the surface of the silicon crystal, and then another different metal is further deposited on this basis to form a second metal layer covering the first metal layer. In this case, the thickness of the first metal layer and the second metal layer is not particularly limited. For example, the thickness of the first metal layer is generally 500-2000nm, and the thickness of the second metal layer is generally 1000-3000nm. Preferably, the thickness of the first metal layer is less than the thickness of the second metal layer. The first metal is preferably nickel, and the second metal is preferably gold.

[0025] The term "modified alkaline solution" herein refers to a solution that can pre-treat the surface of a silicon crystal to activate its surface, and its pH is usually in the range of 8-10, preferably in the range of 8.5-9. The modified alkaline solution contains 0.5-10 mg / ml of dopamine, preferably its concentration is 1-8 mg / ml, more preferably 2-6 mg / ml, such as 3 mg / ml, 4 mg / ml, etc. An exemplary modified alkaline solution is a Tris solution with a pH of 8.5-9.0.

[0026] The term "palladium nanoparticles" herein refers to nano-scale palladium particles of metallic palladium, which are generally spherical or quasi-spherical particles. The size of the palladium particles is generally 1-100 nm, preferably 5-50 nm, and more preferably 5-20 nm. Nano-scale particles are more easily adsorbed to the crystal surface, thereby promoting the deposition of nickel metal ions on the silicon crystal surface as catalytic active sites.

[0027] The term "nickel plating solution" herein refers to a solution for chemically plating a nickel metal layer on a crystal chip, which generally contains nickel chloride, sodium hypophosphite and sodium acetate. Among them, the working concentration of nickel chloride is generally 15-20g / L, preferably 16-18g / L. The working concentration of sodium hypophosphite is generally 20-30g / L, preferably 22-28g / L, such as 25g / L. The working concentration of sodium acetate is generally 10-20g / L, preferably 12-17g / L, such as 14g / L, 16g / L, etc.

[0028] The term "gold plating solution" herein refers to a solution used to form a gold layer on the surface of a nickel metal layer, which generally comprises gold cyanide, sodium tetraborate, potassium cyanide and sodium thiosulfate. Among them, the working concentration of gold cyanide is generally 0.5-5g / L, preferably 1-4g / L, and more preferably 2-3g / L. The working concentration of sodium tetraborate is generally 5-15g / L, preferably 6-10g / L, and more preferably 7-8g / L. The working concentration of potassium cyanide is generally 1-5g / L, preferably 2-4g / L. The concentrations of potassium cyanide and gold cyanide are preferably the same. The concentration of sodium thiosulfate is generally 10-20g / L, preferably 12-18g / L, and more preferably 14-16g / L.

[0029] The term "heat drying" herein includes at least a strengthening treatment at a first temperature and a strengthening treatment at a second temperature. The strengthening treatment at the first temperature is used to strengthen the bonding between the nickel plating layer and the silicon wafer and between different metals. The first temperature is generally 200-300°C, preferably 250-280°C, and more preferably 160-270°C. The treatment time is generally 25-35 minutes, preferably 30 minutes. The strengthening treatment at the second temperature is used to decompose the residual nickel ions to further improve the compactness and bonding strength of the coating, and its temperature needs to be above 970°C. On the other hand, it is preferred that the second temperature is below 1000°C. The treatment time is generally 3-6 hours, such as 4 hours and 5 hours. The compactness of the metal coating and the conductivity and bonding strength of the obtained particles can be improved by strengthening treatment at different temperatures. In addition to the strengthening treatment at the first temperature and the second temperature mentioned above, the heating drying herein also includes drying treatment at a lower temperature, such as 120-160°C. The treatment time is generally 10-20 minutes, such as 12-18 minutes, such as 15 minutes. Drying treatment is usually carried out before the first temperature treatment and the second temperature treatment. The heating drying here is generally carried out in a vacuum or inert atmosphere.

[0030] The term "cleaning and drying" herein refers to further treatment after heating and drying. The temperature of cleaning and drying is not particularly limited, and is generally 150-250° C. The drying time is generally 10-30 minutes. Cleaning and drying can be carried out in an atmospheric environment or an inert atmosphere.

[0031] Example

[0032] In the following examples, the scratch test is performed by using a blade to scratch multiple "well" structures at different locations on the back of the chip, pasting the "well" structures with tape, and then peeling off the tape to evaluate the metal bonding strength of the plating by observing whether there is detached metal on the peeled tape.

[0033] Example 1

[0034] 1. Take a certain amount of palladium particles with a diameter of 6 nm, add them into a container containing anhydrous ethanol, stir for 1.5 hours, take them out by centrifugation, and dry them.

[0035] 2. After protecting the front side of the silicon wafer, immerse it in a container of anhydrous ethanol for 1.5 hours, take it out, dry it, wash it with water three times, and then immerse it in a 3mg / ml dopamine solution (pH8.5) for 8 hours.

[0036] 3. Add the palladium particles treated in step 1 to a proper amount of water for dispersion, then slowly put the chip obtained in step 2 into the dispersion, and stir and react at below 30° C. for 5 hours. Take out the chip and dry it at room temperature.

[0037] 4. Dissolve 18g nickel chloride, 25g sodium hypophosphite and 15g sodium acetate in 1L water to prepare a nickel plating solution. Apply the nickel plating solution evenly on the back of the chip treated in step 3 and react at room temperature for 5 minutes. After cleaning, dry in a vacuum oven for 1 hour.

[0038] 5. Dissolve 2g of gold cyanide, 10g of sodium tetraborate, 2g of potassium cyanide and 15g of sodium thiosulfate in 1L of water to obtain a gold plating solution. Apply the gold plating solution evenly on the back of the chip obtained in step 4 and react at 70°C for 15 minutes.

[0039] 6. After removing the protective layer, add argon gas to heat at 150℃ in a double cone vacuum rotary dryer for 15 minutes, then heat to 250℃ and dry for 30 minutes, and then heat to 980℃ in a double cone vacuum rotary dryer and dry for 5 hours. Wash with pure water for 20 minutes, and heat to 150-250℃ and dry for 1 hour.

[0040] The total thickness of the metal layer obtained in this embodiment is 4.5 μm, and no metal shedding is found in the scratch test, indicating that the plated metal has strong bonding strength.

[0041] Example 2

[0042] 1. Take a certain amount of palladium particles with a diameter of 6 nm, add them into a container containing anhydrous ethanol, stir for 1.5 hours, centrifuge and dry.

[0043] 2. After protecting the front side of the silicon wafer, immerse it in a container of anhydrous ethanol for 1.5 hours, take it out, dry it, wash it with water three times, and then immerse it in a 4 mg / ml dopamine solution (pH 8.5) for 8 hours.

[0044] 3. Add the palladium particles treated in step 1 to a proper amount of water for dispersion, then slowly put the chip obtained in step 2 into the dispersion, and stir and react at below 30° C. for 5 hours. Take out the chip and dry it at room temperature.

[0045] 4. Dissolve 20g of nickel chloride, 25g of sodium hypophosphite and 20g of sodium acetate in 1L of water to prepare a nickel plating solution. Apply the nickel plating solution evenly on the back of the chip treated in step 3, and react at room temperature for 10 minutes. Then, dry in a vacuum oven for 1 hour.

[0046] 5. Take 3g of gold cyanide, 10g of sodium tetraborate, 2g of potassium cyanide and 15g of sodium thiosulfate and dissolve them in 1L of water to obtain a gold plating solution. Apply the gold plating solution evenly on the back of the chip obtained in step 4 and react at 70°C for 20 minutes.

[0047] 6. After removing the protective layer, add argon gas to heat at 150℃ in a double cone vacuum rotary dryer for 15 minutes, then heat to 250℃ and dry for 30 minutes, and then heat to 980℃ in a double cone vacuum rotary dryer and dry for 5 hours. Wash with pure water for 20 minutes, and heat to 150-250℃ and dry for 1 hour.

[0048] The total thickness of the metal layer obtained in this embodiment is 5.4 μm, and no metal shedding is found in the scratch test, indicating that the plated metal has strong bonding strength.

[0049] Comparative Example 1

[0050] 1. After protecting the front side of the silicon wafer, immerse it in a container of anhydrous ethanol for 1.5 hours, take it out, dry it, wash it with water three times, and then immerse it in a 3mg / ml dopamine solution (pH8.5) for 8 hours.

[0051] 2. Dissolve 18g of nickel chloride, 25g of sodium hypophosphite and 15g of sodium acetate in 1L of water to prepare a nickel plating solution. Evenly apply the nickel plating solution on the back of the chip obtained in step 1, react at room temperature for 5 minutes, and then dry in a vacuum oven for 1 hour.

[0052] 3. Dissolve 2g of gold cyanide, 10g of sodium tetraborate, 2g of potassium cyanide and 15g of sodium thiosulfate in 1L of water to obtain a gold plating solution. Evenly apply the gold plating solution on the back of the chip obtained in step 4 and react at 70°C for 15 minutes.

[0053] 4. After removing the protective layer, add argon gas to heat at 150℃ in a double cone vacuum rotary dryer for 15 minutes, then heat to 250℃ and dry for 30 minutes, and then heat to 980℃ in a double cone vacuum rotary dryer and dry for 5 hours. Wash with pure water for 20 minutes, and heat to 150-250℃ and dry for 1 hour.

[0054] The total thickness of the metal layer obtained in this embodiment is 0.8 μm, and no metal shedding is found in the scratch test, indicating that the plated metal has strong bonding strength.

[0055] Comparative Example 2

[0056] 1. After protecting the front side of the silicon wafer, immerse it in a container of anhydrous ethanol for 1.5 hours, take it out, dry it, wash it with water three times, and then immerse it in a 3mg / ml dopamine solution (pH8.5) for 8 hours.

[0057] 2. Dissolve 18g nickel chloride, 10g palladium chloride, 25g sodium hypophosphite and 15g sodium acetate in 1L water to prepare a nickel plating solution. Evenly apply the nickel plating solution on the back of the chip obtained in step 1, react at room temperature for 5 minutes, and then dry in a vacuum oven for 1 hour.

[0058] 3. Dissolve 2g of gold cyanide, 10g of sodium tetraborate, 2g of potassium cyanide and 15g of sodium thiosulfate in 1L of water to obtain a gold plating solution. Evenly apply the gold plating solution on the back of the chip obtained in step 4 and react at 70°C for 15 minutes.

[0059] 4. After removing the protective layer, add argon gas to heat at 150℃ in a double cone vacuum rotary dryer for 15 minutes, then heat to 250℃ and dry for 30 minutes, and then heat to 980℃ in a double cone vacuum rotary dryer and dry for 5 hours. Wash with pure water for 20 minutes, and heat to 150-250℃ and dry for 1 hour.

[0060] The total thickness of the metal layer obtained in this embodiment is 2.4 μm, and no metal shedding is found in the scratch test, indicating that the plated metal has strong bonding strength.

[0061] Comparative Example 3

[0062] 1. Take a certain amount of palladium particles with a diameter of 6 nm, add them into a container containing anhydrous ethanol, stir for 1.5 hours, take them out by centrifugation, and dry them.

[0063] 2. After protecting the front side of the silicon wafer, immerse it in a container of anhydrous ethanol for 1.5 hours, take it out, dry it, wash it with water three times, and then immerse it in a 3mg / ml dopamine solution (pH8.5) for 8 hours.

[0064] 3. Add the palladium particles treated in step 1 to a proper amount of water for dispersion, then slowly put the chip obtained in step 2 into the dispersion, and stir and react at below 30° C. for 5 hours. Take out the chip and dry it at room temperature.

[0065] 4. Dissolve 18g of nickel chloride, 25g of sodium hypophosphite and 15g of sodium acetate in 1L of water to prepare a nickel plating solution. Apply the nickel plating solution evenly on the back of the chip treated in step 3, and react at room temperature for 5 minutes. Then, dry in a vacuum oven for 1 hour.

[0066] 5. Dissolve 2g of gold cyanide, 10g of sodium tetraborate, 2g of potassium cyanide and 15g of sodium thiosulfate in 1L of water to obtain a gold plating solution. Apply the gold plating solution evenly on the back of the chip obtained in step 4 and react at 70°C for 15 minutes.

[0067] 6. After removing the protective layer, add argon gas to a double cone vacuum rotary dryer and dry at 150°C for 15 minutes. Then heat to 250°C and dry for 30 minutes, and then heat to 450°C and dry for 5 hours in a double cone vacuum rotary dryer. Wash with pure water for 20 minutes, and dry at 150-250°C for 1 hour.

[0068] The total thickness of the metal layer obtained in this embodiment is 4.5 μm. The scratch test found that metal was peeled off, indicating that the bonding force of the plated metal was weak.

[0069] Although the present invention has been described with reference to exemplary embodiments, it should be understood that the present invention is not limited to the disclosed exemplary embodiments. Various adjustments or changes may be made to the exemplary embodiments of the present specification without departing from the scope or spirit of the present invention. The scope of the claims should be based on the broadest interpretation to cover all modifications and equivalent structures and functions.

Claims

1. A method for hybrid metallization of a crystal chip, characterized in that: The following steps are involved: (1) contacting at least a portion of the surface of a silicon wafer with a modified alkaline solution having a pH of 8-10 to obtain a treated surface, wherein the modified alkaline solution contains 0.5-10 mg / ml of dopamine; (2) contacting the treated surface of the silicon wafer with the dispersion of nano-palladium particles for 1-10 hours, and then drying the surface; (3) applying a nickel plating solution to the treated surface of the silicon wafer obtained in step (2) and reacting for 1-10 minutes, removing the nickel plating solution and drying, wherein the nickel plating solution comprises 15-20 g / L nickel chloride, 20-30 g / L sodium hypophosphite and 10-20 g / L sodium acetate; (4) further coating the treated surface obtained in step (3) with a gold plating solution and reacting for 10-30 minutes, removing the gold plating solution and drying, wherein the gold plating solution comprises 0.5-5 g / L gold cyanide, 5-15 g / L sodium tetraborate, 1-5 g / L potassium cyanide and 10-20 g / L sodium thiosulfate; and (5) heating to 120-160° C. in an inert atmosphere or vacuum and drying for 10-20 minutes, then heating to 200-300° C. and drying for 25-35 minutes, and then further heating to 970-1000° C. and drying for 3-6 hours, thereby obtaining a metallized silicon crystal chip.

2. The method for hybrid metallization of a crystal chip according to claim 1, characterized in that: The at least part of the surface is located on the back side of the silicon wafer.

3. The method for hybrid metallization of a crystal chip according to claim 2, characterized in that: After step (5), a cleaning and drying step is further included, which includes cleaning the silicon wafer with water for 10-30 minutes and then heating it to 150-250° C. for drying.

4. A hybrid metallized crystal chip, characterized in that: It is obtained by the crystal chip mixed metallization method according to any one of claims 1 to 3, wherein the thickness of the metal layer is 3-10 μm.

5. An electronic device, characterized in that: It comprises the mixed metallized crystal chip as claimed in claim 4.