A method for testing the weight of chromium-free passivation film on color-coated sheets

The membrane weight of the chromium-free passivation film is detected by an X-ray fluorescence analyzer, which solves the problems of large and complex errors of traditional methods, and achieves rapid and accurate membrane weight detection, which is suitable for the rapid detection needs of factory production lines.

CN114324431BActive Publication Date: 2024-11-19QINGDAO HEGANG NEW MATERIAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111474690.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-06
Publication Date
2024-11-19
Estimated Expiration
2041-12-06

AI Technical Summary

Technical Problem

The existing chromium-free passivation film thickness detection methods have large errors, complexity, dangers and are not suitable for rapid detection. In particular, the traditional chromium element determination methods are not suitable for chromium-free passivation films, and the inductively coupled plasma emission spectrometer is complex and consumed. The duration is difficult to meet the rapid testing needs of factory production lines.

Method used

The film weight of the chromium-free passivation film is detected by using an X-ray fluorescence analyzer. By preparing standard samples and drawing standard curves, the high accuracy and rapidity of the X-ray fluorescence analyzer can achieve damage-free detection, simplifying the detection process and reducing cost.

Benefits of technology

It realizes rapid and accurate detection of chromium-free passivation film weight, simplifies the detection process, reduces detection errors, is suitable for the rapid detection needs of factory production lines, and does not involve dangerous chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114324431B_ABST
    Figure CN114324431B_ABST
Patent Text Reader

Abstract

The present application relates to the field of characterization of the weight of the passivation film, and specifically discloses a method for testing the weight of the chromium-free passivation film of a color-coated plate. A method for testing the weight of the chromium-free passivation film of a color-coated plate comprises the following steps: S1, preparation of a standard sample; S2, drawing a standard curve with the content of the characteristic element in the standard sample as the horizontal coordinate and the intensity of the spectrum line corresponding to the content of the characteristic element in the standard sample as the vertical coordinate; S3, selecting a sample to be tested containing a chromium-free passivating agent with the characteristic element, and detecting the intensity of the spectrum line of the characteristic element in the sample to be tested with an X-ray fluorescence analyzer; S4, quantitatively analyzing the content of the characteristic element in the sample to be tested according to the standard curve and the intensity of the spectrum line of the characteristic element in the sample to be tested, and obtaining the content of the characteristic element per unit area in the passivation film; S5, determining the film weight of the passivation film according to the content of the characteristic element per unit area in the passivation film. The method for testing the weight of the chromium-free passivation film of the color-coated plate of the present application is simple, fast, does not damage the sample to be tested, and the measurement results are more accurate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of characterization of passive film weight, and more specifically, to a method for testing the film weight of a chromium-free passive film on a color-coated plate. Background Art

[0002] Color-coated steel sheets are made of cold-rolled steel sheets and galvanized steel sheets as substrates. After surface pretreatment, the paint is applied in a continuous manner, and then baked and cooled. The passivation treatment on the surface of color-coated steel sheets plays a vital role in the adhesion of the coating layer on the surface of the color-coated steel sheets. The thickness of the passivation film is small, usually less than 1 micron. Conventional thickness measurement tools are not precise enough and have large measurement errors.

[0003] Traditional passivation mostly uses hexavalent chromate for passivation treatment. For the thickness detection of the passivation film containing chromium, the hexavalent chromium in the coating of the test sample can be stripped by an alkaline solution containing a corrosion inhibitor. The stripping solution is used at a wavelength of 540nm and diphenylcarbazide is used as an indicator to detect the hexavalent chromium content using a spectrophotometer.

[0004] However, the chromium-containing passivation solution contains polar and carcinogenic hexavalent chromate, which has a mutagenic effect. The aerosol generated during the passivation treatment and the wastewater discharged during production have serious harm to the biomass environment. Therefore, the existing color-coated plates have begun to use chromium-free passivation in large quantities. Therefore, the traditional method of using chromium to measure the thickness of the passivation film is no longer applicable to chromium-free passivation films. In addition, since the content of characteristic elements in the chromium-free passivation coating is extremely low (such as zirconium content is not more than 50mg / m 2 , silicon content is not more than 150mg / m 2 ), the currently available measurement methods are limited and the measurement cycle is long, which has a great impact on product performance assurance and production line process stability evaluation.

[0005] At present, inductively coupled plasma emission spectrometer (ICP) is also commonly used to measure the thickness of the passivation film. It first needs to prepare more than 5 standard solutions containing the characteristic elements to be tested, and then dissolve the sample to be tested with the corresponding solution. Specifically: ① Take a coated steel plate of a certain size (area B); ② Use nitric acid to fully digest the coating, thereby separating it from the steel plate, and heat and evaporate to concentrate the digestion solution; ③ Use ICP test standard solution to establish a test range standard curve, and then use ICP to detect the characteristic elements (content C) in the digestion solution; ④ Calculate the weight of the characteristic element on a single square area D = C / B.

[0006] However, the operation of the inductively coupled plasma emission spectrometer is relatively complicated. The preparation of standards and test samples is difficult, requires high precision and a long time, and involves hazardous chemicals (nitric acid). It must be completed by professionals, and the equipment needs to be calibrated and maintained regularly. The detection process damages the test samples and is not suitable for the rapid detection rhythm in factory production lines. Summary of the invention

[0007] In order to achieve simple and rapid detection of the weight of the chromium-free passivation film without damaging the test sample and improving the accuracy of the test results, the present application provides a method for testing the weight of the chromium-free passivation film of the color-coated plate.

[0008] In the first aspect, the present application provides a method for testing the weight of a chromium-free passivation film of a color-coated plate, using the following technical solution:

[0009] A method for testing the weight of a chromium-free passivation film of a color-coated plate comprises the following steps:

[0010] S1. Preparation of standard samples:

[0011] (1) Select a galvanized sheet with a smooth and uniform surface, cut it into the same size and grind off the burrs as the substrate;

[0012] (2) mixing a chromium-free passivating agent containing characteristic elements with water in a weight ratio of 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, and 1:40, and coating the chromium-free passivating agent on a degreased substrate using a 3#RDS stainless steel wire rod and a 6#RDS stainless steel wire rod, respectively, at a PMT of 60-90° C., to obtain passivated plates of different thicknesses;

[0013] (3) The passivated plate is made into a disc with a diameter of 30-50 mm or a square with a side length of 30-35 mm, and the spectral line intensity corresponding to the characteristic elements in the samples of different thicknesses is detected by an X-ray fluorescence analyzer;

[0014] (4) Detect the content of characteristic elements in samples of different thicknesses;

[0015] (5) Select samples with increasing characteristic element contents as standard samples;

[0016] S2. Plotting a standard curve: plotting a standard curve with the characteristic element content in the standard sample as the abscissa and the spectral line intensity corresponding to the characteristic element content in the standard sample measured in step (3) as the ordinate;

[0017] S3. Selection of samples to be tested and detection of spectral line intensity: Select a chromium-free passivation agent coated sample containing characteristic elements, make a disc-shaped sample with a diameter of 30-50 mm or a square with a side length of 30-35 mm, and use an X-ray fluorescence analyzer to detect the spectral line intensity of the characteristic elements in the sample to be tested;

[0018] S4. Detection of characteristic element content in the sample to be tested: quantitatively analyze the characteristic element content in the sample to be tested according to the standard curve and the spectral line intensity of the characteristic element in the sample to be tested, and obtain the characteristic element content per unit area in the passivation film;

[0019] S5. Passivation film weight detection: Determine the passivation film weight based on the characteristic element content per unit area in the passivation film.

[0020] By adopting the above technical scheme, the burrs on the galvanized sheet are ground off after cutting to prevent the burrs on the surface of the galvanized sheet from affecting the uniformity and flatness of the surface of the passivation film; the passivator containing characteristic elements is coated on the galvanized sheet with different thicknesses, and after testing, standard plates with a gradient increasing content of characteristic elements are selected to prevent the product quality from being difficult to control when the manufacturer cannot provide standard plates.

[0021] Because X-rays have good penetrating power, ionization ability and phosphorescence fluorescence effect, they are widely used in many fields such as medicine, geology, detection, materials science and metallurgy. X-ray fluorescence analyzer consists of two parts: excitation source (X-ray tube) and detection system. X-ray fluorescence analyzer is used to detect the film weight of chromium-free passivation film. The X-ray tube generates primary X-rays (primary rays), which are irradiated to the surface of the sample to be tested. When the energy generated by the primary X-rays is at the same order of magnitude as the energy of the electron layer in the nucleus of the characteristic element, the inner electrons of the characteristic element absorb the radiation energy of the primary rays and are excited, resulting in transitions, thereby generating a "vacancy" in the inner electron orbit. The outer electrons will spontaneously fill these low-energy "vacancies". The outer electrons have higher energy and want to transition to lower energy levels. The excess energy will be released in the form of X-rays (secondary rays). The detection system collects these secondary rays and then draws fluorescence spectra. Each element has its own unique spectrum. According to the spectrum characteristics of the received secondary rays, qualitative analysis can be performed, and the intensity of the rays can be quantitatively analyzed.

[0022] First record the intensity of the spectrum line in the sample, and then detect the content of the characteristic elements in the sample. Even if the ICP method is used to test the characteristic content in the sample, it will not cause the problem of no standard sample later. When testing the content of characteristic elements in the sample to be tested, it is only necessary to perform X-ray analysis on the sample to be tested, and it will not damage the sample to be tested. In addition, X-ray detection has the advantages of high precision, good accuracy, and fast analysis speed. The standard curve is established with the standard sample to test the content of characteristic elements in the sample to be tested, and then the film weight of the chromium-free passivation film on the sample to be tested is obtained. The detection method is simple, fast, and the result is more accurate.

[0023] Preferably, in step S1, the characteristic element is silicon or zirconium.

[0024] By adopting the above technical scheme, the silicon-containing chromium-free passivator has good stability, is non-toxic, non-polluting, easy to use and has low processing cost; the zirconium-containing chromium-free passivator has excellent corrosion resistance to a variety of corrosive media, excellent physical properties, and can effectively improve the adhesion between the substrate and the coating and the durability of the coating.

[0025] Preferably, the test conditions of the silicon-containing sample and standard sample are as follows: the analytical spectrum is Ka, the detector is FPC, the light tube voltage is 40-45kV, the light tube current is 70-95mA, the spectroscopic crystal is PET, the peak position measurement time is 20-40s, and the PHA is 25-75.

[0026] By adopting the above technical solution, the spectral line intensity corresponding to the silicon element in the sample to be tested and the standard sample is detected under the test conditions, the detection speed is fast and the detection result is more accurate.

[0027] Preferably, in step S2, the standard curve equation of the silicon-containing standard sample is X1=1.7Y1-2.16, R 2 =0.999, where Y1 is the spectral line intensity of silicon in the standard sample, in kcps; X1 is the silicon content corresponding to the spectral line intensity of silicon in the standard sample, in mg / m 2 .

[0028] By adopting the above technical solution, the determination coefficient R of the standard sample curve equation containing silicon element 2 The value is close to 1, which means that the standard curve equation has a good fit to the relationship between the silicon content in the sample and the spectral line intensity, and the determination of the silicon content in the sample is more accurate.

[0029] Preferably, the test conditions of the sample to be tested and the standard sample containing zirconium in the step are: the analytical spectrum is Ka, the detector is SC, the light tube voltage is 40-45kV, the light tube current is 70-95mA, the spectroscopic crystal is LiF, the peak position measurement time is 20-40s, and the PHA is 25-75.

[0030] By adopting the above technical solution, the relationship between the spectral line intensities corresponding to the zirconium element in the standard sample and the sample to be tested is detected under this condition, the detection speed is fast, and the detection result is more accurate.

[0031] Preferably, in step S2, the standard curve of the zirconium-containing standard sample is X2=-4.37Y2 2 +14.35Y2-1.93, R 2 =0.996, where Y2 is the spectral line intensity of zirconium in the standard sample, in kcps; X2 is the zirconium content corresponding to the spectral line intensity of zirconium in the standard sample, in mg / m 2 .

[0032] By adopting the above technical solution, the zirconium content in the zirconium-containing standard sample and the spectral line intensity are in a quadratic function relationship. This is because the spectral line intensity measured by the X-ray fluorescence analyzer is not only determined by the element content in the standard sample, but also affected by many other factors, such as matrix effect, content range of analyzed elements, etc. However, the determination coefficient of the standard sample is 0.996, which is close to 1, indicating that the standard curve has a good fit with the zirconium content and spectral line intensity in the sample to be tested, and the determination of the zirconium content in the sample to be tested is relatively accurate.

[0033] Preferably, the method for determining the film weight of the passivation film of the sample to be tested in step S5 is: dividing the content of the characteristic element per unit area in the passivation film of the sample to be tested by the weight percentage of the characteristic element in the solid part of the passivator to calculate the film weight of the passivation film containing the characteristic element.

[0034] By adopting the above technical solution, the characteristic element content is divided by the weight percentage of the characteristic element in the solid part of the passivator, the calculation method is simple and the calculation result is accurate.

[0035] Preferably, in step S1, the content of the characteristic element in the standard sample is measured by an inductively coupled plasma optical emission spectrometer.

[0036] By adopting the above technical solution, the ICP method is used to detect the content of characteristic elements in the standard sample, ensuring the accuracy of the final XRF test results.

[0037] Preferably, the degreasing method of the substrate in step S1 is: immersing the substrate in a degreasing agent with a mass percentage of 2-4% and a temperature of 45-60° C., wiping it repeatedly with gauze for 3-5 minutes, taking it out, rinsing it with tap water for 2-3 minutes, then rinsing it with pure water for 1-2 minutes, and drying it.

[0038] By adopting the above technical solution, the substrate is degreased by immersing in a degreasing agent, which is simple, economical and reliable. After degreasing, the adhesion between the passivating agent and the substrate can be improved.

[0039] In summary, this application has the following beneficial effects:

[0040] 1. Since the present application adopts an X-ray fluorescence analyzer to detect the film weight of the chromium-free passivation film, and since X-rays are adaptable to a wide range of forms and have a wide range of analytical contents, it is an analysis method that can replace the ICP method and is fast, simple, and low-cost. The standard plate can be made according to the standard curve drawn from the relationship between the characteristic element content and the spectral line intensity in the homemade standard plate. The content of special elements in the re-made standard plate does not need to be detected by the ICP method. The re-made standard plate can be used for production line benchmarking, and the same sample can be re-tested, which is convenient for later result tracing, and has the advantages of good precision, good accuracy, and fast analysis speed.

[0041] 2. In this application, the standard curve is drawn with the characteristic element content in the standard sample as the horizontal axis and the spectral line intensity corresponding to the characteristic element content as the vertical axis. The characteristic element content with a low content in the chromium-free passivation film in the sample to be tested can be detected. The detection range of the characteristic element content is wider, the detection method is simple, the result error does not exceed 4%, and the measurement result is accurate. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 is the standard curve of the standard sample containing silicon in Example 1;

[0043] Figure 2 This is the standard curve of the standard sample containing zirconium element in Example 2. DETAILED DESCRIPTION

[0044] Example

[0045] Instruments and reagents used in the examples: Standard samples coated with silicon or zirconium passivating agent: provided by the passivating agent manufacturer, electric hydraulic punching machine (HUM GP-3S), desktop X-ray fluorescence analyzer (Shimadzu XRF-1800).

[0046] Embodiment 1: A method for testing the weight of a chromium-free passivation film of a color-coated plate, comprising the following steps:

[0047] S1. Preparation of standard samples:

[0048] (1) Select 16 galvanized sheets with smooth and uniform surfaces, cut them into the same size, and grind off the burrs to serve as substrates;

[0049] (2) A chromium-free passivating agent containing silicon element was mixed with water in a weight ratio of 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, and 1:40, and the chromium-free passivating agent was coated on the degreased substrate using a 3#RDS stainless steel wire rod and a 6#RDS stainless steel wire rod, respectively, with a PMT of 60°C, to obtain 16 passivated plates of different thicknesses; the degreasing method of the substrate was as follows: immersing the substrate in a degreasing agent with a mass percentage of 4% and a temperature of 45°C, wiping it repeatedly with gauze for 3 minutes, taking it out, rinsing it with tap water for 2 minutes, rinsing it with pure water for 1 minute, and drying it, and the degreasing agent was a sodium hydroxide solution;

[0050] (3) The passivated plate was made into a sample with a diameter of 40 mm, and the spectral line intensity corresponding to the silicon element in the samples of different thicknesses was detected by an X-ray fluorescence analyzer;

[0051] (4) Using inductively coupled plasma emission spectrometer to detect the content of silicon in samples of different thicknesses;

[0052] (5) Select 8 samples with increasing silicon content as standard samples;

[0053] S2. Plotting a standard curve: Plotting a standard curve with the silicon content in the eight standard samples as the horizontal axis and the intensity of the spectral line corresponding to the silicon content in the standard samples measured in step (3) as the vertical axis. Figure 1 As shown, Figure 1 The standard curve equation is X1 = 1.7Y1-2.16, R 2 =0.999, X1 is the content of silicon in the standard sample, the unit is mg / m 2 ; Y1 is the spectral line intensity of silicon in the standard sample, in kcps;

[0054] S3, selection of samples to be tested and detection of spectral line intensity: select a sample coated with a chromium-free passivation agent containing silicon element, make a disc-shaped sample to be tested with a diameter of 40 mm, put the sample to be tested into an X-ray fluorescence analyzer, and detect the spectral line intensity of the silicon element in the sample to be tested; the detection conditions of the spectral line intensity corresponding to the silicon element in the sample to be tested and the standard sample in step S1 are: the analysis spectrum is Ka, the detector is FPC, the light tube voltage is 40kV, the light tube current is 70mA, the spectroscopic crystal is PET, the peak position measurement time is 20s, the low PHA value is 25, and the high PHA value is 75;

[0055] S4. Detection of silicon content in the sample to be tested: According to the standard curve and the spectral line intensity of the silicon element in the sample to be tested, the silicon element content in the sample to be tested is quantitatively analyzed to obtain the characteristic element content per unit area in the passivation film, that is, the spectral line intensity corresponding to the silicon element in the sample to be tested is brought into the standard curve to calculate the silicon element content per unit area in the passivation film in the sample to be tested;

[0056] S5. Calculation of the weight of the passivation film of the sample to be tested: Determine the weight of the passivation film according to the silicon content per unit area in the passivation film of the sample to be tested, and the calculation method is: divide the silicon content per unit area in the passivation film of the sample to be tested by the weight percentage of silicon in the solid part of the passivator.

[0057] Example 2: A method for testing the film weight of a chromium-free passivation film on a color-coated plate. The difference from Example 1 is that in step S3, the test conditions for the silicon-containing sample to be tested are: the analysis spectrum is Ka, the detector is FPC, the light tube voltage is 20 kV, the light tube current is 70 mA, the spectroscopic crystal is PET, the peak position measurement time is 20 s, the low PHA value is 25, and the high PHA value is 75.

[0058] Example 3: A method for testing the film weight of a chromium-free passivation film on a color-coated plate. The difference from Example 1 is that in step S3, the analysis spectrum is Ka, the detector is FPC, the light tube voltage is 40 kV, the light tube current is 50 mA, the spectroscopic crystal is PET, the peak position measurement time is 20 s, the low PHA value is 25, and the high PHA value is 75.

[0059] Example 4: A method for testing the film weight of a chromium-free passivation film on a color-coated plate. The method differs from Example 1 in that, in step S3, the analysis spectrum is Ka, the detector is FPC, the light tube voltage is 40 kV, the light tube current is 70 mA, the spectroscopic crystal is PET, the peak position measurement time is 10 s, the low PHA value is 25, and the high PHA value is 75.

[0060] Example 5: A method for testing the film weight of a chromium-free passivation film on a color-coated plate. The method differs from Example 1 in that, in step S3, the analysis spectrum is Ka, the detector is FPC, the light tube voltage is 40 kV, the light tube current is 70 mA, the spectroscopic crystal is PET, the peak position measurement time is 60 s, the low PHA value is 25, and the high PHA value is 75.

[0061] Embodiment 6: A method for testing the weight of a chromium-free passivation film of a color-coated plate, comprising the following steps:

[0062] S1. Preparation of standard samples:

[0063] (1) Select 16 galvanized sheets with smooth and uniform surfaces, cut them into the same size, and grind off the burrs to serve as substrates;

[0064] (2) A chromium-free passivating agent containing zirconium element was mixed with water in a weight ratio of 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, and 1:40, and the chromium-free passivating agent was coated on the degreased substrate using a 3#RDS stainless steel wire rod and a 6#RDS stainless steel wire rod, respectively, with a PMT of 60°C, to obtain 16 passivated plates of different thicknesses; the degreasing method of the substrate was as follows: immersing the substrate in a degreasing agent with a mass percentage of 2% and a temperature of 45°C, wiping it repeatedly with gauze for 3 minutes, taking it out, rinsing it with tap water for 2 minutes, rinsing it with pure water for 1 minute, and drying it, and the degreasing agent was a sodium hydroxide solution;

[0065] (3) The passivated plate was made into a sample with a diameter of 40 mm, and the spectral line intensity corresponding to the zirconium element in the samples of different thicknesses was detected by an X-ray fluorescence analyzer;

[0066] (4) Using inductively coupled plasma optical emission spectrometry to detect the content of zirconium in samples of different thicknesses;

[0067] (5) Select five samples with increasing zirconium content as standard samples;

[0068] S2. Plotting a standard curve: Plotting a standard curve with the zirconium content in the five standard samples as the horizontal axis and the spectral line intensity corresponding to the zirconium content in the standard samples measured in step (3) as the vertical axis, such as Figure 2 As shown, Figure 2 The standard curve equation is X2 = -4.37Y2 2+14.35Y2-1.93, R 2 =0.996, X2 is the content of zirconium in the sample, the unit is mg / m 2 , Y2 is the spectral line intensity of zirconium element in the sample, in kcps;

[0069] S3, selection of samples to be tested and detection of spectral line intensity: select a sample coated with a chromium-free passivation agent containing zirconium element, make a disc-shaped sample to be tested with a diameter of 40 mm, put the sample to be tested into an X-ray fluorescence analyzer, and detect the spectral line intensity of the zirconium element in the sample to be tested; the detection conditions of the spectral line intensity corresponding to the zirconium element in the sample to be tested and the standard sample in step S1 are: the analysis spectrum is Ka, the detector is SC, the light tube voltage is 40kV, the light tube current is 95mA, the spectroscopic crystal is LiF, the peak position measurement time is 40s, the low PHA value is 25, and the high PHA value is 75;

[0070] S4. Detection of zirconium content in the sample to be tested: According to the standard curve and the spectral line intensity of the zirconium element in the sample to be tested, the zirconium content in the sample to be tested is quantitatively analyzed to obtain the characteristic element content per unit area in the passivation film, that is, the spectral line intensity corresponding to the zirconium element in the sample to be tested is brought into the standard curve to calculate the zirconium content per unit area in the passivation film in the sample to be tested;

[0071] S5. Calculation of the weight of the passivation film of the sample to be tested: Determine the weight of the passivation film according to the content of zirconium per unit area in the passivation film of the sample to be tested, and the calculation method is: divide the content of zirconium per unit area in the passivation film of the sample to be tested by the weight percentage of zirconium in the solid part of the passivator.

[0072] Example 7: A method for testing the film weight of a chromium-free passivation film on a color-coated plate. The method differs from Example 5 in that, in step S3, the test conditions for the zirconium-containing sample are as follows: the analytical spectrum is Ka, the detector is SC, the light tube voltage is 20 kV, the light tube current is 95 mA, the spectroscopic crystal is LiF, the peak position measurement time is 40 s, the low PHA value is 25, and the high PHA value is 75.

[0073] Example 8: A method for testing the film weight of a chromium-free passivation film on a color-coated plate. The method differs from Example 1 in that, in step S3, the test conditions for the zirconium-containing sample are as follows: the analytical spectrum is Ka, the detector is SC, the light tube voltage is 40 kV, the light tube current is 50 mA, the spectroscopic crystal is LiF, the peak position measurement time is 40 s, the low PHA value is 25, and the high PHA value is 75.

[0074] Example 9: A method for testing the film weight of a chromium-free passivation film on a color-coated plate. The method differs from Example 1 in that, in step S3, the test conditions for the zirconium-containing sample are as follows: the analytical spectrum is Ka, the detector is SC, the light tube voltage is 40 kV, the light tube current is 95 mA, the spectroscopic crystal is LiF, the peak position measurement time is 10 s, the low PHA value is 25, and the high PHA value is 75.

[0075] Example 10: A method for testing the film weight of a chromium-free passivation film on a color-coated plate. The method differs from Example 1 in that, in step S3, the test conditions for the zirconium-containing sample are as follows: the analytical spectrum is Ka, the detector is SC, the light tube voltage is 40 kV, the light tube current is 95 mA, the spectroscopic crystal is LiF, the peak position measurement time is 60 s, the low PHA value is 25, and the high PHA value is 75.

[0076] Performance Testing

[0077] 1. Detection of samples containing silicon: Prepare standard plates according to the methods in Examples 1-5, and detect the passivation film weight of the samples to be tested by the methods in Examples 1-5, wherein the silicon element in the passivator accounts for 25% of the solid content as an example. Each embodiment uses 8 groups of samples to be tested, and the 8 groups of samples to be tested are numbered respectively. The silicon content in the standard plate is recorded as the standard value, and the silicon content in the sample to be tested is recorded as the standard curve test value. The standard value and the relative deviation of the test group are recorded in Table 1.

[0078] Table 1 Comparison results of the test group and the standard value in the sample to be tested using the standard curve method

[0079]

[0080] From the data in Table 1, it can be seen that the standard curve is drawn using the standard sample containing silicon element, and the content of silicon element in the sample to be tested is measured. The measured data has a relative deviation within 3%, an average deviation of 1.05%, and an average relative deviation of 1.08%. The measurement results are accurate and the error is small, especially the silicon content in the chromium-free passivation agent is 24.82-61.22mg / m 2 The passivation film between them.

[0081] In Example 2, Example 3 and Example 4, the light tube voltage, light tube current and peak position measurement time for detecting silicon-containing samples were respectively reduced. From the comparison of the data in Table 1, it can be seen that the relative deviation of the silicon content in the samples to be tested in Example 2, Example 3 and Example 4 is large, and the accuracy of the measurement results is reduced. In Example 5, the peak position measurement time is increased, but the impact on the measurement results is small, which is not much different from Example 1.

[0082] 2. Detection of samples containing zirconium: Prepare standard plates according to the methods in Examples 6-10, and detect the passivation film weight of the samples to be tested by the methods in Examples 6-10, wherein zirconium in the passivator accounts for 14% of the solid content as an example. Each embodiment uses 8 groups of samples to be tested, and the 8 groups of samples to be tested are numbered respectively. The zirconium content in the standard plate is recorded as the standard value, and the zirconium content in the sample to be tested is recorded as the standard curve test value. The standard value, test group and relative deviation are recorded in Table 2.

[0083] Table 2 Comparison results of the test group and the standard value in the sample to be tested using the standard curve method

[0084]

[0085]

[0086] From the data in Table 2, it can be seen that the curve drawn by the standard sample containing zirconium element is used to test the sample containing zirconium element. The test results show that the maximum relative deviation is only 3.8%, and the average relative deviation is 1.96%. The test error is small and the accuracy is high, especially for the chromium-free passivation film with a film weight of 81.5-142.2mg / m 2 The test results are more accurate.

[0087] In Example 7, Example 8 and Example 9, the light tube voltage, light tube current and peak measurement time for detecting zirconium-containing samples are respectively reduced. Table 2 shows that the zirconium contents detected in Examples 7-9 have large deviations from the standard value, and the accuracy of the detection results decreases. In Example 10, the peak measurement time is increased. Compared with the measurement results of Example 6, the relative deviation of the test results in Example 10 is close to that of Example 6.

[0088] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for testing the weight of chromium-free passivation film of color-coated sheet, characterized in that: The following steps are involved: S1. Preparation of standard samples: (1) Select a galvanized sheet with a flat and uniform surface, cut it into the same size and grind off the burrs as the substrate; (2) The chromium-free passivator containing characteristic elements was mixed with water in a weight ratio of 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, and 1:40, and the chromium-free passivator was coated on the degreased substrate using 3#RDS stainless steel wire rod and 6#RDS stainless steel wire rod, respectively, at a PMT of 60°C, to obtain passivated plates of different thicknesses; (3) The passivated plate is made into a disc with a diameter of 30-50 mm or a square with a side length of 30-35 mm, and the spectral line intensity corresponding to the characteristic elements in the samples of different thicknesses is detected by an X-ray fluorescence analyzer; (4) Detect the content of characteristic elements in samples of different thicknesses; (5) Select samples with increasing characteristic element contents as standard samples; S2. Plotting a standard curve: plotting a standard curve with the content of the characteristic element in the standard sample as the abscissa and the intensity of the spectral line corresponding to the content of the characteristic element in the standard sample measured in step (3) as the ordinate; S3. Selection of samples to be tested and detection of spectral line intensity: Select a chromium-free passivation agent coated sample containing characteristic elements, make a disc-shaped sample with a diameter of 30-50 mm or a square with a side length of 30-35 mm, and use an X-ray fluorescence analyzer to detect the spectral line intensity of the characteristic elements in the sample to be tested; S4. Detection of characteristic element content in the sample to be tested: quantitatively analyze the characteristic element content in the sample to be tested according to the standard curve and the spectral line intensity of the characteristic element in the sample to be tested, and obtain the characteristic element content per unit area in the passivation film; S5. Calculation of the film weight of the passivation film of the sample to be tested: Determine the film weight of the passivation film according to the content of characteristic elements per unit area in the passivation film; In step S1 and step S3, the characteristic element is silicon; The spectral line intensity test conditions of the silicon-containing sample and standard sample are as follows: the analytical spectrum is Ka, the detector is FPC, the light tube voltage is 40kV, the light tube current is 70mA, the spectroscopic crystal is PET, the peak position measurement time is 20s, and the PHA is 25-75.

2. The method for testing the weight of the chromium-free passivation film of the color-coated plate according to claim 1, characterized in that: In step S2, the standard curve equation of the silicon-containing standard sample is X1=1.7Y1-2.16, R 2 =0.999, where Y1 is the spectral line intensity of silicon in the standard sample, in kcps; X1 is the spectral line intensity of silicon in the standard sample corresponding to the silicon content, in mg / m 2 .

3. The method for testing the weight of the chromium-free passivation film of the color-coated plate according to claim 1, characterized in that: The method for determining the film weight of the passivation film of the sample to be tested in step S5 is: dividing the content of the characteristic element per unit area in the passivation film of the sample to be tested by the weight percentage of the characteristic element in the solid part of the passivator to calculate the film weight of the passivation film containing the characteristic element.

4. The method for testing the weight of the chromium-free passivation film of the color-coated plate according to claim 1, characterized in that: In the step S1, the content of characteristic elements in the sample is measured by an inductively coupled plasma optical emission spectrometer.

5. The method for testing the weight of the chromium-free passivation film of the color-coated plate according to claim 1, characterized in that: The degreasing method of the substrate in step S1 is: immerse the substrate in a degreasing agent with a mass percentage of 2-4% and a temperature of 45-60° C., wipe it repeatedly with gauze for 3-5 minutes, take it out, rinse it with tap water for 2-3 minutes, rinse it with pure water for 1-2 minutes, and dry it.