Polarizing film laminate with adhesive layer, and optical display panel using the polarizing film laminate with adhesive layer

By adjusting the iodine concentration and water content of the polarizing film and controlling the acid content in the adhesive layer, the problems of polyolefin formation, decolorization, and heating reddening of polarizing film laminates under high temperature and high humidity environments were solved, improving adhesion durability and reprocessability, making it suitable for polarizing film laminates in powered vehicles.

CN114341682BActive Publication Date: 2024-10-18NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202080061044.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-20
Publication Date
2024-10-18
Estimated Expiration
2040-08-20

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively address the polyolefination, decolorization, and heating reddening issues of polarization film laminates in high-temperature or high-humidity environments, especially when used in powered vehicles, where the performance of the polarization film deteriorates significantly.

Method used

By adjusting the iodine concentration of the polarizing film and the moisture content of the polarizing film laminate, and controlling the acid content in the adhesive layer, the composition of the adhesive polymer is optimized to ensure the durability and reprocessability of the adhesive layer.

Benefits of technology

It achieves a comprehensive solution to the problems of polyolefination, decolorization, and heating reddening of polarization film laminates under high temperature and high humidity conditions, improves adhesion durability and reprocessability, and ensures the reliability of polarization films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114341682B_ABST
    Figure CN114341682B_ABST
Patent Text Reader

Abstract

The present invention provides a polarizing film laminate that can comprehensively solve the problems of polyeneization, discoloration and red discoloration on heating. The above-mentioned polarizing film laminate is a polarizing film laminate with an adhesive layer, which has a polarizing film containing a polyvinyl alcohol resin and an adhesive layer provided on at least one side of the polarizing film directly or through an optically transparent polarizing film protective film, wherein the adhesive layer contains an adhesive polymer, and the adhesive polymer is copolymerized with an acid component, and the amount of the acid component in all monomer components constituting the adhesive polymer is less than 5% by weight, wherein, in an x-y orthogonal coordinate system formed by taking the iodine concentration of the polarizing film as the x-axis and the moisture content of the polarizing film laminate as the y-axis, the iodine concentration and moisture content of the polarizing film laminate are included in the following area, and the area is connected by an iodine concentration of 7.0wt.% and a moisture content of 0.7g / m 2 The first coordinate point and iodine concentration 2.2wt.% and moisture content 3.2g / m 2 The first line segment of the second coordinate point, connecting the second coordinate point and the iodine concentration of 2.2wt.% and the moisture content of 4.0g / m 2 The second line segment of the third coordinate point, connecting the third coordinate point and the iodine concentration of 3.0wt.% and the water content of 4.0g / m 2 The third line segment of the fourth coordinate point, connecting the fourth coordinate point and the iodine concentration of 10.0wt.% and the water content of 0.7g / m 2 It is surrounded by a fourth line segment of the fifth coordinate point and a fifth line segment connecting the first coordinate point and the fifth coordinate point.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing film laminate with an adhesive layer, and an optical display panel using the polarizing film laminate with an adhesive layer. Background Art

[0002] In recent years, optical display panels such as liquid crystal panels and organic EL panels have been used in electronic devices such as smartphones and personal computers, and electrical products such as IoT home appliances. In addition, various possibilities have been found for their use in powered vehicles such as automobiles, trains, and airplanes. For example, it is conceivable to mount optical display panels on the windshield, dashboard, exterior, and other various parts of the vehicle body to provide various information to the driver and to transmit various information to the outside.

[0003] However, unlike smart phones, in most cases, power vehicles are used in harsh outdoor environments. The performance of optical display panels, especially polarizing film stacks (polarizers) used for optical display panels, and polarizing films (polarizers) used for polarizing film stacks may deteriorate due to usage environments such as high temperature or high humidity. In the worst case, they may even become unusable.

[0004] Patent Document 1 discloses an example of a polarizer having improved durability in a high temperature or high humidity environment, a polarizing plate using the polarizer, and a liquid crystal display device using the polarizing plate. As durability, red leakage (depolarization of long wavelength light) under crossed Nicols that occurs when placed under high temperature conditions is considered a problem, and in order to solve this problem, a scheme is proposed in which zinc is contained and the relationship between the zinc content and the iodine content is adjusted to a given range.

[0005] Similarly, Patent Document 2 relates to a polarizing plate for an in-vehicle image display device having improved durability in a high temperature or high humidity environment, wherein attention is paid to the moisture content of the polarizing plate and the saturated water absorption of the protective film. In-vehicle polarizing plates are required to have high temperature durability, but in a high temperature environment, the transmittance of the polarizing plate may be significantly reduced due to polyeneization. In order to solve this problem, Patent Document 2 proposes a solution of using a transparent protective film having a saturated water absorption within a given range as a transparent protective film bonded to a polarizer and reducing the moisture content of the polarizing plate.

[0006] Patent Document 3 also relates to a polarizing plate with improved durability under high temperature or high humidity, and focuses on the moisture content of the polarizing plate and the moisture permeability of the protective film. In a high temperature environment, the interior of the polarizing plate reaches a high temperature and high humidity state, resulting in a large change in transmittance, polarization degree, image hue, etc., and a decrease in reliability as a polarizing plate. Therefore, the patent document proposes a solution of attaching a protective film with low moisture permeability while reducing the moisture content of the polarizer as much as possible.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2003-29042

[0010] Patent Document 2: Japanese Patent Application Publication No. 2014-102353

[0011] Patent Document 3: Japanese Patent Application Publication No. 2002-90546 Summary of the invention

[0012] Problems to be solved by the invention

[0013] Regarding optical display panels, especially polarizing film laminates used in optical display panels and polarizing films used in polarizing film laminates, "polyeneization", "discoloration" and "heat reddening" are known as problems that may occur in high temperature or high humidity environments.

[0014] Generally speaking, "polyeneization" refers to the phenomenon that the monomer transmittance of a polarizing film stack decreases due to being placed in a high temperature or high humidity environment. In addition, "discoloration" and "heat reddening" are also caused by being placed in a high temperature or high humidity environment. When the polarizing film stack is configured in an orthogonal Nicol manner and the orthogonal transmittances at wavelengths of 410nm and 700nm are measured, the orthogonal transmittance increases. Among them, "discoloration" is particularly known as the phenomenon of increased transmittance on the long wavelength side of about 700nm and the short wavelength side of about 410nm, and discoloration occurring under black display. On the other hand, "heat reddening" is particularly known as the phenomenon of increased transmittance on the long wavelength side of about 700nm and discoloration of the polarizing film to red.

[0015] Patent Document 1 focuses on the problem of "decolorization", Patent Document 2 focuses on the problem of "polyeneization", and Patent Document 3 focuses on the problem of "reddening upon heating". It can be considered that the solutions proposed in each document are at least effective in solving the respective problems. However, the inventions described in each patent document may not be sufficient to solve these problems comprehensively.

[0016] "Polyeneization", "bleaching" and "heat reddening" are all related to each other through iodine and moisture, and further through temperature and humidity that affect moisture. Based on such facts, the applicant of the present application has repeatedly conducted in-depth research and obtained the following insights: these problems can be solved comprehensively by adjusting the iodine concentration of the polarizing film and the moisture content of the polarizing film laminate.

[0017] An object of the present invention is to comprehensively solve the above three problems by adjusting the iodine concentration of the polarizing film and the water content of the polarizing film laminate.

[0018] When laminating a polarizing film to a liquid crystal cell, etc., an adhesive is usually used. In addition, since the polarizing film can be instantly fixed to the liquid crystal cell, etc., and there is no need to perform a drying process for affixing the polarizing film to the liquid crystal cell, etc., the adhesive is often provided in advance on one side of the polarizing film in the form of an adhesive layer. That is, in laminating a polarizer, a polarizer with an adhesive layer is usually used.

[0019] The properties required of the adhesive layer include: adhesion that does not decrease over time and high durability; when the polarizing film is bonded to the liquid crystal unit, even if the bonding position is wrong or foreign matter is embedded in the bonding surface, the polarizing film can be peeled off from the surface of the liquid crystal panel and bonded again (reworkability), etc.

[0020] When the optical display panel is used in a powered vehicle, the adhesive used to attach the polarizing film constituting the optical display panel to the liquid crystal cell, etc., also requires high temperature durability. In such applications, as the adhesive composition constituting the adhesive, an adhesive composition containing an acid component such as acrylic acid in the monomer component of the adhesive polymer can be appropriately used.

[0021] The inventors of the present invention have found that a new problem has arisen in that the acid component copolymerized in the adhesive polymer deteriorates the polyene. In the above-mentioned prior art, although research related to the polyene of the polarizing film has been conducted, research on the durability and reworkability of the adhesive layer has not been conducted, and there is no disclosure on this issue.

[0022] An object of the present invention is to provide a polarizing plate with an adhesive layer, wherein an adhesive layer is provided on a polarizing film directly or via an optically transparent polarizing film protective film, and the polarizing plate has excellent reliability of optical characteristics, adhesion durability, and reworkability.

[0023] Solutions to the problem

[0024] The inventors of the present invention focused on the effect of the acid component in the monomer components of the adhesive polymer contained in the adhesive layer on the performance of the polarizing film, and thus completed the present invention. In the prior art, there has been no research on the adhesive polymer contained in the adhesive layer from the perspective of the correlation between the proportion of the acid component in the monomer components and the performance of the polarizing film laminate with the adhesive layer, such as the reliability of optical properties, adhesion durability, and reworkability. The inventors of the present invention have discovered the amount of the acid component in the total monomer components of the adhesive polymer required to obtain a polarizing film laminate with an adhesive layer having excellent properties.

[0025] Although not bound by any theory, it is believed that if a substance containing an acid component such as acrylic acid is used in the monomer component of the binder polymer, although the high-temperature durability is improved due to the hydrogen bonding of the COOH group of the acid component, the acid component acts as a catalyst for the dehydration condensation of the polyvinyl alcohol (PVA)-type resin film constituting the polarizing film, thereby promoting polyeneization.

[0026] In order to solve the above-mentioned problems, a polarizing film laminate according to one embodiment of the present invention is a polarizing film laminate with an adhesive layer, comprising a polarizing film containing a polyvinyl alcohol-based resin and an adhesive layer provided on at least one side of the polarizing film directly or via an optically transparent polarizing film protective film.

[0027] The adhesive layer comprises an adhesive polymer, the adhesive polymer is copolymerized with an acid component, and the amount of the acid component in all monomer components constituting the adhesive polymer is 5% by weight or less,

[0028] The iodine concentration (wt.%) of the polarizing film is taken as the x-axis, the moisture content (g / m 2 ) as the y-axis, has an iodine concentration and a water content within the following region, which is formed by connecting an iodine concentration of 7.0 wt.% and a water content of 0.7 g / m 2 The first coordinate point and iodine concentration 2.2wt.% and moisture content 3.2g / m 2 The first line segment of the second coordinate point of the iodine concentration of 2.2wt.% and the water content of 4.0g / m 2 The second line segment of the third coordinate point, connecting the third coordinate point and the iodine concentration of 3.0wt.% and the water content of 4.0g / m 2 The third line segment of the fourth coordinate point, connecting the fourth coordinate point and the iodine concentration of 10.0wt.% and the water content of 0.7g / m 2 The fourth line segment of the fifth coordinate point and the fifth line segment connecting the first coordinate point and the fifth coordinate point are surrounded by the fourth line segment.

[0029] According to the polarizing film laminate with an adhesive layer of this embodiment, the problems of "polyeneization", "discoloration", "blushing due to heating", "adhesion durability" and "reworkability" can be solved comprehensively.

[0030] In the polarizing film laminate of the above embodiment, the polydispersity coefficient (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the binder polymer may be 3.0 or less. This also applies to (another) other embodiment of the present invention.

[0031] In the polarizing film laminate of the above embodiment, the polarizing film may have a thickness of 4 to 20 μm.

[0032] In addition, a polarizing film laminate according to another embodiment of the present invention is a polarizing film laminate with an adhesive layer, comprising a polarizing film containing a polyvinyl alcohol-based resin and an adhesive layer provided on at least one side of the polarizing film directly or via an optically transparent polarizing film protective film.

[0033] The adhesive layer comprises an adhesive polymer, the adhesive polymer is copolymerized with an acid component, and the amount of the acid component in all monomer components constituting the adhesive polymer is 5% by weight or less,

[0034] The iodine concentration (wt.%) of the polarizing film is taken as the x-axis, the moisture content (g / m 2 ) as the y-axis, has an iodine concentration and a water content within the following region, which is formed by connecting an iodine concentration of 4.5 wt.% and a water content of 2.0 g / m 2 The sixth coordinate point and iodine concentration 2.2wt.% and moisture content 3.2g / m 2 The sixth line segment of the second coordinate point of the iodine concentration of 2.2wt.% and the water content of 4.0g / m 2 The second line segment of the third coordinate point, connecting the third coordinate point and the iodine concentration of 3.0wt.% and the water content of 4.0g / m 2 The third line segment of the fourth coordinate point, connecting the fourth coordinate point and the iodine concentration of 4.5wt.% and the water content of 3.3g / m 2 It is surrounded by a seventh line segment of the seventh coordinate point and an eighth line segment connecting the sixth coordinate point and the seventh coordinate point.

[0035] In the polarizing film laminate of the above embodiment, the sixth coordinate point may have an iodine concentration of 4.0 wt.% and a water content of 2.3 g / m 2 The seventh coordinate point has an iodine concentration of 4.0 wt.% and a water content of 3.5 g / m 2 The coordinate point of .

[0036] In the polarizing film laminate of the above embodiment, the film thickness of the polarizing film may be 11 to 20 μm.

[0037] A polarizing film laminate according to another embodiment of the present invention is a polarizing film laminate with an adhesive layer, comprising a polarizing film containing a polyvinyl alcohol-based resin and an adhesive layer provided on at least one side of the polarizing film directly or via an optically transparent polarizing film protective film.

[0038] The adhesive layer comprises an adhesive polymer, the adhesive polymer is copolymerized with an acid component, and the amount of the acid component in all monomer components constituting the adhesive polymer is 5% by weight or less,

[0039] The iodine concentration (wt.%) of the polarizing film is taken as the x-axis, the moisture content (g / m 2 ) as the y-axis, has an iodine concentration and a water content within the following region, which is formed by connecting an iodine concentration of 7.0 wt.% and a water content of 0.7 g / m 2 The first coordinate point and iodine concentration 3.0wt.% and water content 2.6g / m 2 The eleventh line segment of the eighth coordinate point, connecting the eighth coordinate point and the iodine concentration of 6.0wt.% and the water content of 2.6g / m 2 The tenth line segment of the ninth coordinate point connects the ninth coordinate point and the iodine concentration of 10.0wt.% and the water content of 0.7g / m 2 The fifth coordinate point is surrounded by a twelfth line segment and a fifth line segment connecting the first coordinate point and the fifth coordinate point.

[0040] According to the polarizing film laminate with an adhesive layer of this embodiment, the problems of "polyeneization", "discoloration", "blushing due to heating", "adhesion durability" and "reworkability" can be solved comprehensively.

[0041] In the polarizing film laminate of the above embodiment, the eighth coordinate point may be 4.5 wt.% iodine concentration and 2.0 g / m 2 The sixth coordinate point, the ninth coordinate point is iodine concentration 7.2wt.% and water content 2.0g / m 2 The tenth coordinate point.

[0042] In the polarizing film laminate of the above embodiment, the polarizing film may have a thickness of 4 to 11 μm.

[0043] Moreover, in the polarizing film laminated body of the said embodiment, it is preferable that the said polarizing film contains zinc.

[0044] Furthermore, in the polarizing film stack of the above-mentioned embodiment, for a sample comprising a polarizing film stack and glass plates laminated on both sides of the polarizing film stack via an adhesive, the monomer transmittance after heating at 95°C / 500 hours is the same as or greater than the monomer transmittance before heating.

[0045] Thereby, the problem of polyeneization can be effectively solved.

[0046] Preferably, in the polarizing film stack of the above-mentioned embodiment, for a sample comprising a polarizing film stack and glass plates laminated on both sides of the polarizing film stack via an adhesive, the change in the orthogonal transmittance at a wavelength of 410 nm caused by a heat treatment at 95°C / 500 hours is less than 1%, and the change in the orthogonal transmittance at a wavelength of 700 nm is less than 5%.

[0047] Thereby, the problem of discoloration can be effectively solved.

[0048] Preferably, in the polarizing film stack of the above-mentioned embodiment, for a sample comprising a polarizing film stack and glass plates laminated on both sides of the polarizing film stack via an adhesive, the change in orthogonal transmittance at a wavelength of 410 nm caused by a heat treatment at 95°C / 500 hours is greater than 1%, and the change in orthogonal transmittance at a wavelength of 700 nm is less than 5%.

[0049] Thereby, the problem of reddening due to heating can be effectively solved.

[0050] In the polarizing film laminate of the above embodiment, an antireflection layer may be provided on the visible side of the polarizing film via a substrate, and the moisture permeability of the antireflection film including the substrate and the antireflection layer is 15 g / m 2 ·More than 24h.

[0051] Furthermore, in the polarizing film laminate of the above embodiment, it is preferred that:

[0052] A liquid crystal cell having a liquid crystal layer including liquid crystal molecules oriented in one direction in a plane in a state where no electric field is applied;

[0053] a first polarizing film disposed on one side of the liquid crystal unit; and

[0054] A second polarizing film is disposed on the other side of the liquid crystal unit in a manner such that its absorption axis is orthogonal to the absorption axis of the first polarizing film.

[0055] Between the first polarizing film and the liquid crystal unit, a first phase difference layer and a second phase difference layer are sequentially arranged from one side of the first polarizing film. When the refractive index of the first phase difference layer in the slow axis x direction within the plane is set to nx1, the refractive index in the fast axis direction is set to ny1, and the refractive index in the thickness z direction is set to nz1, the first phase difference layer satisfies the relationship of nx1>ny1>nz1. When the refractive index of the second phase difference layer in the slow axis x direction within the plane is set to nx2, the refractive index in the fast axis direction is set to ny2, and the refractive index in the thickness z direction is set to nz2, the second phase difference layer satisfies the relationship of nz2>nx2≥ny2.

[0056] Furthermore, in the polarizing film laminate of the above embodiment, it is preferred that:

[0057] A liquid crystal cell having a liquid crystal layer including liquid crystal molecules oriented in one direction in a plane in a state where no electric field is applied;

[0058] a first polarizing film disposed on one side of the liquid crystal unit; and

[0059] A second polarizing film is disposed on the other side of the liquid crystal unit in a manner such that its absorption axis is orthogonal to the absorption axis of the first polarizing film.

[0060] Between the first polarizing film and the liquid crystal unit, a first phase difference layer and a second phase difference layer are sequentially arranged from one side of the first polarizing film. When the refractive index of the first phase difference layer in the slow axis x direction within the plane is set to nx1, the refractive index in the fast axis direction is set to ny1, and the refractive index in the thickness z direction is set to nz1, the first phase difference layer satisfies the relationship of nz1>nx1=ny1. When the refractive index of the second phase difference layer in the slow axis x direction within the plane is set to nx2, the refractive index in the fast axis direction is set to ny2, and the refractive index in the thickness z direction is set to nz2, the second phase difference layer satisfies the relationship of nx2>ny2=nz2.

[0061] Furthermore, it is preferred that the polarizing film laminate of the above embodiment comprises:

[0062] A liquid crystal cell comprising a liquid crystal layer including liquid crystal molecules oriented in one direction within a plane in a state where no electric field is applied; and

[0063] A polarizing film is disposed on one side of the liquid crystal unit.

[0064] A phase difference layer is arranged between the above-mentioned polarizing film and the above-mentioned liquid crystal unit. When the refractive index in the slow axis x direction within the plane of the phase difference layer is set to nx, the refractive index in the fast axis direction is set to ny, and the refractive index in the thickness z direction is set to nz, the phase difference layer satisfies the relationship nx>nz>ny.

[0065] Furthermore, in order to solve the above-mentioned problem, an optical display panel of one embodiment of the present invention comprises: an optical display unit, a polarizing film stack described in any one of the above items joined to one side of the above-mentioned optical display unit directly or via other optical films, and an optically transparent cover plate arranged on the opposite side of the above-mentioned optical display unit along the above-mentioned polarizing film stack, the above-mentioned optical display unit, the above-mentioned polarizing film stack and the above-mentioned transparent cover plate are bonded together by a transparent adhesive layer filled therebetween with no gaps.

[0066] In the optical display panel of the above embodiment, the transparent cover plate may have a function of a capacitive touch sensor.

[0067] In the optical display panel of the above embodiment, an ITO layer serving as a constituent element of a capacitive touch sensor may be provided between the transparent cover plate and the polarizing film laminate.

[0068] Effects of the Invention

[0069] According to the present invention, the problems of "polyeneization", "discoloration", "blushing due to heating", "adhesion durability" and "reworkability" can be solved comprehensively. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1 is a schematic diagram showing the layer structure of an optical display panel.

[0071] Figure 2 This is a diagram for explaining an example of a method for producing a polarizing film.

[0072] Figure 3 This is a diagram showing a calibration curve for calculating the iodine concentration of a polarizing film.

[0073] Figure 4 It is a diagram showing a structure used for reliability test.

[0074] Figure 5 This is a graph in which the results of Examples and Comparative Examples are plotted.

[0075] Explanation of symbols

[0076] 1 Optical display panel

[0077] 10 Optical display unit

[0078] 11. Transparent adhesive

[0079] 12 Polarizing film laminate

[0080] 13 Transparent adhesive

[0081] 14 Transparent cover

[0082] 120 polarizing film

[0083] 121 Polarizing film protective film

[0084] 122 Polarizing film protective film DETAILED DESCRIPTION

[0085] Hereinafter, a preferred embodiment of the present invention will be described with reference to the accompanying drawings. For the convenience of description, only the preferred embodiment is shown, but the present invention is of course not limited to this.

[0086] The present invention is directed to an optical display panel, in particular an optical display panel mounted on the body of a car, a train, an airplane, or other powered vehicle, and a polarizing film laminate for use with the optical display panel. Here, "mounted on the body" does not necessarily refer only to the case where the optical display panel or polarizing film laminate is fixed to the body, but also includes the case where, for example, the optical display panel or polarizing film laminate used in a smart phone or the like is freely mounted or brought into a powered vehicle. In other words, "mounted on the body" includes all situations where the optical display panel or polarizing film laminate is used together with a powered vehicle and may be exposed to a high temperature or high humidity environment.

[0087] 1. Optical display panel

[0088] Figure 1 An example of the layer structure of the optical display panel 1 is shown in a schematic diagram. The optical display panel 1 includes at least: an optical display unit 10, a polarizing film laminate 12 laminated on one side 10a (visible side) of the optical display unit 10, and an optically transparent cover plate 14 arranged on the opposite side of the optical display unit 10, i.e., the visible side, along the polarizing film laminate 12. On the other side 10b of the optical display unit 10, another polarizing film laminate 17 is arranged via a transparent adhesive 16. The optical display unit 10, the polarizing film laminate 12, and the cover plate 14 are bonded together by layers of transparent adhesive 11 and 13 filled therebetween in a state without gaps. It should be noted that in this specification, unless otherwise specified, the term "bonding" includes adhesion (pressure-sensitive bonding). The optical display unit 10 and the polarizing film laminate 12 may be directly bonded together by the transparent adhesive 11, but may also be bonded together via other optical films (not shown) such as a retardation film and a viewing angle compensation film as required.

[0089] 1-1. Optical display unit

[0090] Examples of the optical display unit 10 include a liquid crystal unit and an organic EL unit.

[0091] As the organic EL unit, an organic EL unit in which a transparent electrode, an organic light-emitting layer and a metal electrode are sequentially stacked on a transparent substrate to form a light-emitting body (organic electroluminescent light-emitting body) can be suitably used. The organic light-emitting layer is a laminate of various organic thin films, and can adopt various layer structures, including, for example: a laminate of a hole injection layer made of a triphenylamine derivative and a light-emitting layer made of a fluorescent organic solid such as anthracene, a laminate of these light-emitting layers and an electron injection layer made of a perylene derivative, or a laminate of a hole injection layer, a light-emitting layer and an electron injection layer.

[0092] As the liquid crystal cell, any of a reflective liquid crystal cell utilizing external light, a transmissive liquid crystal cell utilizing light from a light source such as the backlight 18, and a semi-transmissive and semi-reflective liquid crystal cell utilizing both light from the outside and light from the light source can be used. In the case where the liquid crystal cell is a liquid crystal cell utilizing light from a light source, such as Figure 1 As shown, a polarizing film laminate 17 may also be arranged on the side opposite to the visible side of the optical display unit (liquid crystal unit) 10, and a light source 18 such as a backlight may be arranged. The polarizing film laminate 17 on the light source side and the liquid crystal unit 10 are bonded together via a layer of a suitable transparent adhesive 17. As a driving mode of the liquid crystal unit, any type of mode such as VA mode, IPS mode, TN mode, STN mode, bend orientation (π type) may be adopted.

[0093] 1-2. Cover

[0094] As examples of the cover plate 14, a transparent plate (window layer), a touch panel, etc. can be cited. As a transparent plate, a transparent plate with suitable mechanical strength and thickness can be used. As such a transparent plate, a transparent resin plate such as an acrylic resin or a polycarbonate resin, or a glass plate, etc. can be used. For example, a low-reflection film (not shown) can be used to apply a low-reflection treatment to the surface of the cover plate 14. As a touch panel, various touch panels such as a resistive film method, an electrostatic capacitance method, an optical method, an ultrasonic method, etc., a glass plate with a touch sensor function, a transparent resin plate, etc. can be used.

[0095] When a capacitive touch panel is used as the cover plate 14, a front transparent plate made of glass or a transparent resin plate is preferably provided on the side closer to the visible side than the touch panel. In this case, the transparent adhesive 13 joining the cover plate 14 and the polarizing film laminate 12 is provided with an ITO layer (not shown) which is a component of the capacitive touch sensor.

[0096] [Adhesive composition]

[0097] The adhesive composition that can be used in the transparent adhesive 11 and the like will be described.

[0098] <Binder polymer>

[0099] The adhesive polymer contained in the adhesive composition is not particularly limited as long as it is a polymer with adhesive properties that is generally used as a base polymer of an adhesive. For the reason of easily achieving a balance in adhesive properties, a polymer with a Tg of 0° C. or less (usually -100° C. or more) is preferred. Among these adhesive polymers, polyester polymers, (meth) acrylic polymers, etc. can be appropriately used.

[0100] The binder polymer used in the present invention is copolymerized with an acid component.

[0101] As the polyester polymer, a saturated polyester or copolyester formed of a polyol and a polycarboxylic acid is generally used.

[0102] Examples of the polyol include diols such as ethylene glycol, propylene glycol, hexamethylene glycol, neopentyl glycol, 1,2-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, decamethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-bis(4-hydroxyphenyl)propane, and bis(4-hydroxyphenyl)sulfone.

[0103] Examples of the polycarboxylic acid include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 2,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, diphenyl carboxylic acid, diphenoxyethane dicarboxylic acid, diphenyl sulfone carboxylic acid, and anthracene dicarboxylic acid; alicyclic dicarboxylic acids such as 1,3-cyclopentane dicarboxylic acid, 1,3-cyclohexane dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid; and aliphatic dicarboxylic acids such as malonic acid, dimethylmalonic acid, succinic acid, 3,3-diethylsuccinic acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, azelaic acid, dimer acid, sebacic acid, suberic acid, and dodecanedicarboxylic acid. As the polycarboxylic acid, two or more polycarboxylic acids, for example, an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid are often used in combination.

[0104] In the present invention, by making the binder polymer contain such an acid component, the durability of the adhesive is improved, and the occurrence of foaming, peeling, etc. can be prevented for a long time. Based on the amount of all monomer components constituting the binder polymer, the upper limit of the acid component amount is less than 5 weight %, preferably less than 3 weight %, and more preferably less than 2 weight %. If the acid component amount exceeds the upper limit, there is a tendency that the polyene of the polarizing film has an adverse effect and the reworkability of the adhesive layer is also reduced. Based on the amount of all monomer components constituting the binder polymer, the lower limit of the acid component amount is preferably more than 0.01 weight %, more preferably more than 0.2 weight %, and more preferably more than 0.5 weight %. If the amount of the acid component is small, there is a tendency that the durability of the adhesive layer is reduced.

[0105] As the polyol and polycarboxylic acid used for the polyester polymer, various polyols and polycarboxylic acids can be used without particular limitation. As the polyol, a polymer polyol such as polycarbonate diol can be used. In addition, the polyester polymer can be obtained by reacting the above-mentioned diol component with a polyol having a valence of 3 or more and / or a polycarboxylic acid having a valence of 3 or more. The weight average molecular weight of the polyester polymer is usually 11,000 or more.

[0106] The (meth)acrylic polymer generally contains an alkyl (meth)acrylate as a main component as a monomer unit. In addition, the (meth)acrylate refers to an acrylate and / or a methacrylate.

[0107] As the (meth)acrylic acid alkyl ester constituting the main skeleton of the (meth)acrylic acid polymer, there can be exemplified a linear or branched (meth)acrylic acid alkyl ester having an alkyl group with 1 to 18 carbon atoms. For example, as the above-mentioned alkyl group, there can be exemplified a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a pentyl group, a hexyl group, a cyclohexyl group, a heptyl group, a 2-ethylhexyl group, an isooctyl group, a nonyl group, a decyl group, an isodecyl group, a dodecyl group, an isotetradecyl group, an undecyl group, a tridecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, etc. These (meth)acrylic acid alkyl esters can be used alone or in combination. The average carbon number of these alkyl groups is preferably 3 to 9.

[0108] In addition, alkyl (meth)acrylates containing aromatic rings such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate can be used. The alkyl (meth)acrylate containing aromatic rings can be used by mixing the polymer obtained by polymerizing the alkyl (meth)acrylates with the above-mentioned (meth)acrylic polymers. However, from the viewpoint of transparency, the alkyl (meth)acrylate containing aromatic rings is preferably used by copolymerizing with the above-mentioned alkyl (meth)acrylates.

[0109] In order to improve adhesiveness and heat resistance, one or more comonomers having a polymerizable functional group containing an unsaturated double bond such as a (meth)acryloyl group or a vinyl group may be introduced into the (meth)acrylic polymer by copolymerization. Specific examples of such copolymerizable monomers include: hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and 4-hydroxymethylcyclohexyl methacrylate; carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride; caprolactone adducts of acrylic acid; sulfonic acid group-containing monomers such as styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; phosphoric acid group-containing monomers such as 2-hydroxyethylacryloyl phosphate, and the like.

[0110] Among the comonomers as described above, as the acid component in the present invention, there can be cited comonomers having polymerizable functional groups having unsaturated double bonds such as (meth)acryloyl or vinyl groups. Specific examples of comonomers used as acid components include: carboxyl group-containing monomers such as acrylic acid, (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, etc.; acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride; caprolactone adducts of acrylic acid; sulfonic acid group-containing monomers such as styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, (meth)acrylic acid sulfonic acid propyl ester, (meth)acryloyloxynaphthalenesulfonic acid, etc.; phosphoric acid group-containing monomers such as 2-hydroxyethylacryloyl phosphate, etc.

[0111] When an acid component is present, from the viewpoint of adverse effects of the acid, a relatively weak acid such as a carboxyl group-containing monomer is preferred, followed by a phosphoric acid group-containing monomer, a sulfonic acid group-containing monomer, and the like.

[0112] Examples of the monomer used for the purpose of modification include (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-butyl (meth)acrylamide, N-methylol (meth)acrylamide, N-methylolpropane (meth)acrylamide and other (N-substituted)amide monomers; (meth)acrylic acid alkylaminoalkyl ester monomers such as (meth)aminoethyl acrylate, N,N-dimethylaminoethyl (meth)acrylate, and tert-butylaminoethyl (meth)acrylate; (meth)acrylic acid alkoxyalkyl ester monomers such as (meth)methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; N-(meth)acryloyloxy Succinimide monomers such as methylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, N-(meth)acryloyl-8-oxyoctamethylene succinimide, and N-acryloyl morpholine; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-dodecylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-dodecylitaconimide.

[0113] In addition, as the modifying monomer, vinyl acetate, vinyl propionate, N-vinyl pyrrolidone, methyl vinyl pyrrolidone, vinyl pyridine, vinyl piperidone, vinyl pyrimidine, vinyl piperazine, vinyl pyrazine, vinyl pyrrole, vinyl imidazole, vinyl Vinyl monomers such as oxazole, vinyl morpholine, N-vinyl carboxylic acid amides, styrene, α-methylstyrene, and N-vinyl caprolactam; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy-containing acrylic monomers such as glycidyl (meth)acrylate; polyethylene glycol (meth)acrylate, polypropylene (meth)acrylate, methoxyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, etc.; acrylate monomers such as tetrahydrofurfuryl (meth)acrylate, fluorine-containing (meth)acrylate, silicone (meth)acrylate, 2-methoxyethyl acrylate, etc. In addition, isoprene, butadiene, isobutylene, vinyl ether, etc. can be cited.

[0114] In addition, as copolymerizable monomers other than the above, silane monomers containing silicon atoms can be cited. As silane monomers, for example, 3-acryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 4-vinylbutyltrimethoxysilane, 4-vinylbutyltriethoxysilane, 8-vinyloctyltrimethoxysilane, 8-vinyloctyltriethoxysilane, 10-methacryloxydecyltrimethoxysilane, 10-acryloxydecyltrimethoxysilane, 10-methacryloxydecyltriethoxysilane, 10-acryloxydecyltriethoxysilane, etc. can be cited.

[0115] In addition, as the comonomer, a polyfunctional monomer having two or more unsaturated double bonds such as (meth)acrylic acid or vinyl groups, such as esters of (meth)acrylic acid and polyols such as tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, caprolactone-modified dipentaerythritol hexa(meth)acrylate, and polyester (meth)acrylates, epoxy (meth)acrylates, urethane (meth)acrylates, and the like in which two or more unsaturated double bonds such as (meth)acryloyl groups or vinyl groups are added to the skeleton of polyester, epoxy, urethane, and the like as the same functional groups as the monomer components can be used.

[0116] Among these comonomers, from the viewpoint of adhesion and durability, hydroxyl-containing monomers and carboxyl-containing monomers are preferably used. Hydroxyl-containing monomers and carboxyl-containing monomers can be used in combination. When the adhesive composition contains a crosslinking agent, these comonomers become reaction points with the crosslinking agent. Since hydroxyl-containing monomers, carboxyl-containing monomers, etc. are sufficiently reactive with intermolecular crosslinking agents, they are preferably used to improve the cohesiveness and heat resistance of the obtained adhesive layer. From the viewpoint of reworkability, hydroxyl-containing monomers are preferably used. In addition, from the viewpoint of both durability and reworkability, carboxyl-containing monomers are preferably used.

[0117] The hydroxyl group-containing monomer may be used in an amount of about 0.01 to 30% by weight, preferably about 0.03 to 20% by weight, and more preferably about 0.05 to 10% by weight, based on the total monomer components constituting the binder polymer.

[0118] In addition to the above, a comonomer other than the acid component may be used in an amount of about 0 to 30% by weight, preferably about 0.1 to 20%, more preferably about 0.1 to 10%, of all monomer components constituting the binder polymer.

[0119] The weight average molecular weight (Mw) of the adhesive polymer used in the present invention is preferably 900,000 to 3,000,000. Considering durability, especially heat resistance, the weight average molecular weight is more preferably 1,200,000 to 2,500,000. If the weight average molecular weight is less than 900,000, the low molecular weight polymer component increases, the crosslinking density of the gel (adhesive layer) increases, and with this, the adhesive layer becomes hard, and the stress relaxation property is impaired, so it is not preferred. In addition, if the weight average molecular weight is greater than 3,000,000, the viscosity increases, and gelation occurs during the polymerization of the polymer, so it is not preferred.

[0120] The polydispersity coefficient (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the adhesive polymer used in the present invention is preferably 3.0 or less, more preferably 1.05 to 2.5, and further preferably 1.05 to 2.0. When the polydispersity coefficient (Mw / Mn) exceeds 3.0, the low molecular weight polymer becomes more, and in order to increase the gel fraction of the adhesive layer, a large amount of crosslinking agent must be used, whereby the remaining crosslinking agent reacts with the already gelled polymer, and the crosslinking density of the gel (adhesive layer) becomes higher, and with this, the adhesive layer becomes harder, and the stress relaxation property is impaired, which is not preferred. In addition, it is believed that when there are many low molecular weight polymers and more uncrosslinked polymers and oligomers (sol part), the adhesive layer is destroyed due to the segregation of uncrosslinked polymers near the interface of the adhesive layer in contact with the adherend under heating / humidification conditions, etc., which becomes the cause of the adhesive layer peeling. It should be noted that the weight average molecular weight and the polydispersity coefficient (Mw / Mn) are determined by GPC (gel permeation chromatography) and the values ​​calculated by polystyrene conversion.

[0121] The binder polymer used in the present invention can be produced by appropriately selecting a known production method such as solution polymerization, bulk polymerization, emulsion polymerization, various radical polymerizations, etc. The obtained binder polymer may be any copolymer such as a random copolymer, a block copolymer, or a graft copolymer.

[0122] It should be noted that, in solution polymerization, as a polymerization solvent, ethyl acetate, toluene, etc. are used. As a specific solution polymerization example, the reaction is carried out under a stream of an inert gas such as nitrogen, with a polymerization initiator added, usually at a temperature of about 50 to 70° C. for about 10 minutes to 30 hours. In particular, by shortening the polymerization time to about 30 minutes to 3 hours, the generation of low molecular weight oligomers generated in the late stage of polymerization can be suppressed, and the polydispersity coefficient (Mw / Mn) is adjusted to a preferred range of 3.0 or less.

[0123] The polymerization initiator, chain transfer agent, emulsifier, etc. used in the free radical polymerization are not particularly limited and can be appropriately selected for use. It should be noted that the weight average molecular weight of the binder polymer can be controlled according to the amount of the polymerization initiator and chain transfer agent and the reaction conditions, and the appropriate amount can be adjusted according to the type of the above substances.

[0124] Examples of the polymerization initiator include azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis(2-methylpropionamidine) disulfate, 2,2'-azobis(N.N'-dimethyleneisobutylamidine), and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate (manufactured by Wako Pure Chemical Industries, Ltd., VA-057); persulfates such as potassium persulfate and ammonium persulfate; di(2-ethylhexyl) peroxydicarbonate; and di(4-hydroxyethyl) peroxydicarbonate. The invention also includes peroxide initiators such as tert-butyl cyclohexyl) ester, di-tert-butyl peroxydicarbonate, tert-butyl peroxyneodecanoate, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, di(4-methylbenzoyl) peroxide, dibenzoyl peroxide, tert-butyl peroxyisobutyrate, 1,1-di-tert-hexylperoxycyclohexane, tert-butyl hydroperoxide, hydrogen peroxide, and the like; and redox initiators in which a peroxide and a reducing agent are combined, but are not limited thereto.

[0125] The above-mentioned polymerization initiators may be used alone or in combination of two or more. The total content thereof is preferably about 0.005 to 1 part by weight, more preferably about 0.02 to 0.5 part by weight, based on 100 parts by weight of the monomer.

[0126] For example, in order to produce the (meth)acrylic polymer having the weight average molecular weight using 2,2'-azobisisobutyronitrile as a polymerization initiator, the amount of the polymerization initiator used is preferably about 0.06 to 0.2 parts by weight, more preferably about 0.08 to 0.175 parts by weight, based on 100 parts by weight of the total amount of the monomer components.

[0127] Examples of the chain transfer agent include dodecyl mercaptan, glycidyl mercaptan, thioglycolic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethylhexyl thioglycolate, 2,3-dimercapto-1-propanol, etc. The chain transfer agent may be used alone or in combination of two or more, and the total content thereof is preferably about 0.1 parts by weight or less relative to 100 parts by weight of the total amount of the monomer components.

[0128] In addition, examples of the emulsifier used when performing emulsion polymerization include anionic emulsifiers such as sodium dodecyl sulfate, ammonium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyoxyethylene alkyl ether ammonium sulfate, and polyoxyethylene alkylphenyl ether sodium sulfate, and nonionic emulsifiers such as polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene fatty acid ester, and polyoxyethylene-polyoxypropylene block polymer. These emulsifiers may be used alone or in combination of two or more.

[0129] In addition, as a reactive emulsifier, an emulsifier introduced with a free radical polymerizable functional group such as an propylene group or an allyl ether group specifically includes, for example: AQUALON HS-10, HS-20, KH-10, BC-05, BC-10, BC-20 (all of which are manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), ADEKA REASOAP SE10N (manufactured by Asahi Electric Chemical Co., Ltd.), etc. Reactive emulsifiers are preferred because they enter the polymer chain after polymerization, thereby improving water resistance. The amount of the emulsifier used is preferably 0.3 to 5 parts by weight relative to 100 parts by weight of the total amount of the monomer components, and more preferably 0.5 to 1 part by weight from the perspective of polymerization stability and mechanical stability.

[0130] The binder polymer used in the present invention generally uses a binder polymer with a weight average molecular weight in the range of 300,000 to 4,000,000. Considering durability, especially heat resistance, it is preferred to use a binder polymer with a weight average molecular weight of 500,000 to 3,000,000. More preferably, it is 650,000 to 2,000,000. When the weight average molecular weight is less than 300,000, it is not preferred from the aspect of heat resistance. In addition, when the weight average molecular weight is greater than 4,000,000, it is not preferred from the aspect of reduced adhesion and adhesive force. It should be noted that the weight average molecular weight refers to the value measured by GPC (gel permeation chromatography) and calculated by polystyrene conversion.

[0131] <Other components in the adhesive composition>

[0132] In addition, the adhesive composition used in the present invention may contain a crosslinking agent. As the crosslinking agent, an organic crosslinking agent or a multifunctional metal chelate can be used. As the organic crosslinking agent, there can be listed: isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, imine crosslinking agents, etc. The multifunctional metal chelate is a chelate obtained by covalently bonding or coordinate bonding a polyvalent metal to an organic compound. As the polyvalent metal atom, there can be listed Al, Cr, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Sr, Ba, Mo, La, Sn, Ti. As the atom in the organic compound that is covalently bonded or coordinately bonded, there can be listed oxygen atoms, etc., and as the organic compound, there can be listed alkyl esters, alcohol compounds, carboxylic acid compounds, ether compounds, ketone compounds, etc.

[0133] As the crosslinking agent, an isocyanate crosslinking agent and / or a peroxide crosslinking agent are preferred. As the compound of the isocyanate crosslinking agent, for example, isocyanate monomers such as toluene diisocyanate, chlorophenylene diisocyanate, tetramethylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, and isocyanate compounds obtained by adding these isocyanate monomers to trimethylolpropane, etc., isocyanurate compounds, biuret compounds, and polyether polyols, polyester polyols, acrylic polyols, polybutadiene polyols, polyisoprene polyols, etc. are urethane prepolymer-type isocyanates that have undergone addition reactions. Particularly preferred are polyisocyanate compounds, such as one selected from hexamethylene diisocyanate, hydrogenated xylylene diisocyanate, and isophorone diisocyanate, or polyisocyanate compounds derived therefrom. Here, the polyisocyanate compound selected from one of hexamethylene diisocyanate, hydrogenated xylylene diisocyanate and isophorone diisocyanate or derived therefrom includes hexamethylene diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, polyol-modified hexamethylene diisocyanate, polyol-modified hydrogenated xylylene diisocyanate, trimer-type hydrogenated xylylene diisocyanate, and polyol-modified isophorone diisocyanate, etc. For the exemplified polyisocyanate compounds, in particular, the acid or base contained in the polymer is used as a catalyst, and the reaction with the hydroxyl group proceeds rapidly, so it is particularly helpful to accelerate the crosslinking speed, and thus it is preferred.

[0134] As the peroxide-type crosslinking agent, any peroxide that generates free radical active species by heating or light irradiation and crosslinks the base polymer of the adhesive composition can be suitably used, but in consideration of operability and stability, it is preferred to use a peroxide with a 1-minute half-life temperature of 80°C to 160°C, and more preferably a peroxide with a 1-minute half-life temperature of 90°C to 140°C.

[0135] Examples of peroxides that can be used as crosslinking agents include di(2-ethylhexyl) peroxydicarbonate (1-minute half-life temperature: 90.6°C), di(4-tert-butylcyclohexyl) peroxydicarbonate (1-minute half-life temperature: 92.1°C), di-sec-butyl peroxydicarbonate (1-minute half-life temperature: 92.4°C), tert-butyl peroxyneodecanoate (1-minute half-life temperature: 103.5°C), tert-hexyl peroxypivalate (1-minute half-life temperature: 109.1°C), tert-butyl peroxypivalate (1-minute half-life temperature: 110.3°C), di-tert-butyl peroxydicarbonate (1-minute half-life temperature: 112.1°C), di-tert-butyl peroxydicarbonate (1-minute half-life temperature: 113.7°C), di-tert-butyl peroxyneodecanoate (1-minute half-life temperature: 114.6°C), di-tert-butyl peroxydicarbonate (1-minute half-life temperature: 115.9°C), di-tert-butyl peroxydicarbonate (1-minute half-life temperature: 116.3°C), di-tert-butyl peroxydicarbonate (1-minute half-life temperature: 117.7°C), di-tert-butyl peroxydicarbonate (1-minute half-life temperature: 118.9°C), di-tert-butyl peroxydicarbonate (1-minute half-life temperature: 119. Lauroyl (1 minute half-life temperature: 116.4℃), dioctanoyl peroxide (1 minute half-life temperature: 117.4℃), 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate (1 minute half-life temperature: 124.3℃), di(4-methylbenzoyl) peroxide (1 minute half-life temperature: 128.2℃), dibenzoyl peroxide (1 minute half-life temperature: 130.0℃), tert-butyl peroxyisobutyrate (1 minute half-life temperature: 136.1℃), 1,1-di(tert-hexylperoxide)cyclohexane (1 minute half-life temperature: 149.2℃). Among them, since the cross-linking reaction efficiency is particularly excellent, di(4-tert-butylcyclohexyl) peroxydicarbonate (1 minute half-life temperature: 92.1°C), dilauroyl peroxide (1 minute half-life temperature: 116.4°C), dibenzoyl peroxide (1 minute half-life temperature: 130.0°C), etc. can be cited.

[0136] It should be noted that the half-life of peroxide is an index representing the decomposition rate of peroxide, refers to the time until the residual amount of peroxide becomes half. About obtaining the decomposition temperature of half-life at any time, the half-life time under any temperature, in the manufacturer's catalogue etc., record to some extent, for example, be recorded in " Organic Peroxide Catalogue the 9th Edition (May, 2003) " etc. of Japan Oil and Fats Co., Ltd.

[0137] The amount of the crosslinking agent used is preferably 0.01 to 20 parts by weight, more preferably 0.03 to 10 parts by weight, relative to 100 parts by weight of the binder polymer. It should be noted that if the crosslinking agent is less than 0.01 parts by weight, there is a tendency for the cohesive force of the binder to be insufficient, and there is a concern that foaming will occur during heating. On the other hand, if it is more than 20 parts by weight, the moisture resistance is insufficient and peeling is likely to occur during reliability tests, etc.

[0138] The isocyanate crosslinking agent may be used alone or in combination of two or more. The total content is preferably 0.01 to 2 parts by weight of the polyisocyanate compound crosslinking agent, more preferably 0.02 to 2 parts by weight, and further preferably 0.05 to 1.5 parts by weight, relative to 100 parts by weight of the binder polymer. The amount may be appropriately contained in consideration of cohesive strength, prevention of peeling in a durability test, etc.

[0139] The peroxide may be used alone or in combination of two or more. The total content is 0.01 to 2 parts by weight, preferably 0.04 to 1.5 parts by weight, and more preferably 0.05 to 1 part by weight, relative to 100 parts by weight of the binder polymer. The peroxide may be appropriately selected within this range to adjust processability, reworkability, crosslinking stability, peelability, etc.

[0140] The amount of decomposed peroxide remaining after the reaction treatment can be measured by, for example, HPLC (high performance liquid chromatography).

[0141] More specifically, for example, about 0.2 g of the adhesive composition after the reaction treatment can be taken out each time, immersed in 10 ml of ethyl acetate, shaken at 120 rpm for 3 hours at 25° C. by a shaker, and then left to stand at room temperature for 3 days. Next, 10 ml of acetonitrile is added, shaken at 120 rpm for 30 minutes at 25° C., and about 10 μl of the extract obtained by filtering through a membrane filter (0.45 μm) is injected into HPLC for analysis as the amount of peroxide after the reaction treatment.

[0142] As an additive, it is particularly preferred to add a silane coupling agent. Examples of the silane coupling agent include: silicon compounds having an epoxy structure such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino-containing silicon compounds such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)3-aminopropylmethyldimethoxysilane; 3-chloropropyltrimethoxysilane; (meth)acryl-containing silane coupling agents such as acetoacetyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, and 3-methacryloxypropyltriethoxysilane; and isocyanate-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane. In particular, 3-glycidoxypropyltrimethoxysilane and acetoacetyl trimethoxysilane are preferably used because they can effectively inhibit. Silane coupling agents can impart durability, especially the effect of inhibiting peeling in a humidified environment. The amount of silane coupling agent used is 1 part by weight or less, and further 0.01 to 1 part by weight, preferably 0.02 to 0.6 part by weight relative to 100 parts by weight of the binder polymer. If the amount of silane coupling agent used increases, the adhesion to the liquid crystal unit increases excessively, and sometimes there is a situation where it affects the reworkability, etc.

[0143] In addition, the adhesive composition used in the present invention may contain other known additives, for example, powders such as colorants and pigments, dyes, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, softeners, antioxidants, anti-aging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, inorganic or organic fillers, metal powders, granular materials, foils, etc. may be appropriately added to the adhesive composition according to the intended use. In addition, within a controllable range, a redox type in which a reducing agent is added may also be used.

[0144] When forming the adhesive layer from the adhesive composition, it is preferred to adjust the total amount of crosslinking agents added while fully considering the effects of the crosslinking treatment temperature and the crosslinking treatment time.

[0145] The crosslinking treatment temperature and the crosslinking treatment time can be adjusted according to the crosslinking agent used. The crosslinking treatment temperature is preferably 170° C. or lower.

[0146] The crosslinking treatment may be performed at the same temperature as the drying step of the adhesive layer, or may be performed in a separate crosslinking treatment step after the drying step.

[0147] The crosslinking treatment time can be set in consideration of productivity and operability, but is usually about 0.2 to 20 minutes, preferably about 0.5 to 10 minutes.

[0148] [Adhesive layer]

[0149] The adhesive layer will be described.

[0150] The pressure-sensitive adhesive layer-attached polarizing film laminate of the present invention includes a pressure-sensitive adhesive layer provided on at least one surface of a polarizing film directly or via an optically transparent polarizing film protective film.

[0151] As a method for forming an adhesive layer, for example, the adhesive composition is applied to a separator that has been subjected to a peeling treatment, and after drying and removing the polymerization solvent to form an adhesive layer, the adhesive layer is transferred to an optical film; or the adhesive composition is applied to an optical film, and the polymerization solvent is dried and removed to form an adhesive layer on the optical film. It should be noted that when applying the adhesive, one or more solvents other than the polymerization solvent may be appropriately added.

[0152] As the separator subjected to the release treatment, a silicone release liner can be preferably used. In the process of applying the above-mentioned adhesive composition on such a liner and drying it to form an adhesive layer, as a method for drying the adhesive, an appropriate method can be appropriately adopted according to the purpose. Preferably, a method of heating and drying the above-mentioned coated film is adopted. The heating and drying temperature is preferably 40°C to 200°C, more preferably 50°C to 180°C, and particularly preferably 70°C to 170°C. By making the heating temperature within the above-mentioned range, an adhesive layer with excellent adhesive properties can be obtained.

[0153] The drying time can be appropriately adopted as appropriate, and the drying time is preferably 5 seconds to 20 minutes, more preferably 5 seconds to 10 minutes, and particularly preferably 10 seconds to 5 minutes.

[0154] In addition, an adhesion-promoting layer may be formed on the surface of the polarizing film, or the adhesive layer may be formed after various adhesion-promoting treatments such as corona treatment and plasma treatment. In addition, the surface of the adhesive layer may be subjected to adhesion-promoting treatment.

[0155] When the anchor layer or the adhesive layer formed when the adhesive layer is provided on the surface of the polarizing film is used, it is desirable to use a system that does not contain an acid.

[0156] As a specific method for forming a thickening layer, there is the following method: a solution containing a carbamate polymer (manufactured by Nagase ChemteX: Denatron B510-C, etc.) is adjusted with a water / isopropyl alcohol (volume ratio of 65:35) mixed solution to a solid content of 0.2% by weight, the adjusted solution is applied to a polarizer using a Meyer rod #5, and dried at 50°C for 30 seconds to form a 25nm thick thick thickening coating layer.

[0157] Various methods can be used to form the adhesive layer, and specific examples include roll coating, lick roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, rod coating, blade coating, air knife coating, curtain coating, die lip coating, extrusion coating using a die coater, and the like.

[0158] The thickness of the pressure-sensitive adhesive layer is not particularly limited, and is, for example, about 1 to 500 μm, preferably 1 to 250 μm, more preferably 1 to 100 μm, and even more preferably 1 to 35 μm.

[0159] By reducing the thickness of the pressure-sensitive adhesive layer, the total amount of acid in the pressure-sensitive adhesive relative to the polarizing film can be reduced, and the influence of polyeneization on the pressure-sensitive adhesive layer-attached polarizing film laminate can be reduced.

[0160] In addition, generally, if the thickness of the adhesive layer is reduced, the adhesive strength is reduced, and there is a tendency for the adhesive durability to be reduced, such as warping and peeling, due to the shrinkage stress of the polarizer caused by the shrinkage of the polarizing film under high temperature and high humidity, so it is not preferred to reduce the thickness of the adhesive layer. However, by thinning the polarizing film, the shrinkage stress of the polarizer can be reduced, and as a result, even if the thickness of the adhesive layer is thinned, the adhesive durability can be maintained or improved.

[0161] When the pressure-sensitive adhesive layer is exposed, the pressure-sensitive adhesive layer may be protected by a release-treated sheet (separator) until it is actually used.

[0162] As the constituent material of the separator, for example, plastic films such as polyethylene, polypropylene, polyethylene terephthalate, and polyester films, porous materials such as paper, cloth, and non-woven fabrics, nets, foam sheets, metal foils, and suitable thin sheets such as laminates thereof are listed, but plastic films are preferably used from the perspective of excellent surface smoothness.

[0163] The plastic film is not particularly limited as long as it is a film that can protect the above-mentioned adhesive layer, and examples thereof include polyethylene films, polypropylene films, polybutylene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polybutylene terephthalate films, polyurethane films, and ethylene-vinyl acetate copolymer films.

[0164] The thickness of the above-mentioned separator is usually 5 to 200 μm, preferably about 5 to 100 μm. The above-mentioned separator can also be subjected to demoulding and antifouling treatments using silicone, fluorine, long-chain alkyl or fatty acid amide release agents, silica powder, etc. as needed, or antistatic treatments such as coating, mixing, and vapor deposition can be applied to the above-mentioned separator. In particular, the peelability of the separator relative to the above-mentioned adhesive layer can be further improved by appropriately subjecting the surface of the above-mentioned separator to peeling treatments such as silicone treatment, long-chain alkyl treatment, and fluorine treatment.

[0165] The release-treated sheet used in producing the pressure-sensitive adhesive layer-attached polarizing film laminate may be used as a separator of the pressure-sensitive adhesive layer-attached polarizing film laminate as it is, thereby simplifying the process.

[0166] 2. Polarizing film laminate

[0167] The polarizing film laminate 12 includes at least a polarizing film 120 and a polarizing film protective film 121 bonded to at least one side of the polarizing film 120, for example, the visible side. As in the present embodiment, polarizing film protective films 121 and 122 may be bonded to both sides of the polarizing film 120, i.e., the visible side and the side opposite to the visible side of the polarizing film 120, respectively, via an appropriate adhesive (not shown). Although not particularly shown, other optical films may be provided between the polarizing film 120 and the polarizing film protective films 121 and 122.

[0168] In order to comprehensively solve the problems that occur in high temperature or high humidity environments, especially the problems of "polyeneization", "discoloration" and "heat reddening", the present invention particularly focuses on the iodine concentration (wt.%) of the polarizing film 120 and the moisture content (g / m 2 ). These values ​​can be adjusted, for example, during the manufacture of a polarizing film or a polarizing film laminate.

[0169] 2-1.Polarizing film

[0170] Polarizing film 120 is made of a polyvinyl alcohol (PVA) resin film containing iodine. As a material suitable for PVA-type films of polarizing film, PVA or its derivatives can be used. As derivatives of PVA, in addition to polyvinyl formal, polyvinyl acetal, etc., derivatives modified by olefins such as ethylene and propylene, unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, or their alkyl esters, acrylamide, etc. can also be listed. PVA generally uses PVA with a degree of polymerization of about 1000 to 10000 and a saponification degree of about 80 to 100 mol%. PVA-type films made of these materials tend to contain moisture easily.

[0171] The PVA film may also contain additives such as plasticizers. Examples of the plasticizer include polyols and condensates thereof, such as glycerol, diglycerol, triglycerol, ethylene glycol, propylene glycol, and polyethylene glycol. The amount of the plasticizer is not particularly limited, but is preferably 20% by weight or less in the PVA film.

[0172] 2-1-1. Manufacturing of polarizing film

[0173] When manufacturing a polarizing film having a thickness of 6 μm or more, for example, a dyeing treatment of dyeing the PVA film with iodine and a stretching treatment of stretching the PVA film in at least one direction are performed. Generally, a series of treatments including swelling, dyeing, cross-linking, stretching, washing and drying can be performed on the PVA film.

[0174] The swelling treatment can be performed, for example, by immersing the PVA film in a swelling bath (water bath). By this treatment, the PVA film can be swollen while cleaning the dirt and anti-blocking agent on the surface of the PVA film, thereby preventing uneven dyeing and the like. Glycerin, potassium iodide, etc. can also be appropriately added to the swelling bath. The temperature of the swelling bath is, for example, about 20 to 60° C., and the immersion time in the swelling bath is, for example, about 0.1 to 10 minutes.

[0175] The dyeing treatment can be performed, for example, by immersing the PVA film in an iodine solution. The iodine solution is usually an iodine aqueous solution, which contains potassium iodide as iodine and a dissolving aid. The iodine concentration is, for example, about 0.01 to 1% by weight, preferably 0.02 to 0.5% by weight. The potassium iodide concentration is, for example, about 0.01 to 10% by weight, preferably 0.02 to 8% by weight.

[0176] During the dyeing treatment, the temperature of the iodine solution is, for example, about 20 to 50° C., preferably 25 to 40° C. The immersion time is, for example, about 10 to 300 seconds, preferably 20 to 240 seconds. During the iodine dyeing treatment, the concentration of the iodine solution, the immersion temperature of the PVA film in the iodine solution, the immersion time, and other conditions are adjusted so that the iodine content and potassium content in the PVA film are within the above ranges.

[0177] The cross-linking treatment can be carried out, for example, by immersing the PVA film after iodine dyeing in a treatment bath containing a cross-linking agent. As a cross-linking agent, any appropriate cross-linking agent can be used. As specific examples of cross-linking agents, boric compounds such as boric acid and borax, glyoxal, glutaraldehyde, etc. can be cited. These cross-linking agents can be used alone or in combination. As a solvent for the solution of the cross-linking bath, water is usually used, but an organic solvent compatible with water can also be appropriately added. Relative to 100 parts by weight of the solvent, the cross-linking agent is used in a ratio of, for example, 1 to 10 parts by weight. Preferably, the solution of the cross-linking bath further contains an auxiliary agent such as iodide. The concentration of the auxiliary agent is preferably 0.05 to 15% by weight, and more preferably 0.5 to 8% by weight. The temperature of the cross-linking bath is, for example, about 20 to 70°C, and preferably 40 to 60°C. The immersion time in the cross-linking bath is, for example, about 1 second to 15 minutes, and preferably 5 seconds to 10 minutes.

[0178] Stretching treatment is a treatment in which the PVA film is stretched in at least one direction. Generally speaking, the PVA film is uniaxially stretched in the conveying direction (length direction). There is no particular limitation on the stretching method, and any method of wet stretching method and dry stretching method can be adopted. In the case of wet stretching method, the PVA film is stretched to a given ratio in a treatment bath. As a solution of the stretching bath, a solution obtained by adding compounds necessary for various treatments to solvents such as water or organic solvents (such as ethanol) can be appropriately used. As a dry stretching method, for example, an inter-roll stretching method, a heated roller stretching method, a compression stretching method, etc. can be cited. In the manufacture of polarizing film, stretching treatment can be carried out in any stage. Specifically, it can be carried out simultaneously with swelling, dyeing, and cross-linking, or it can be carried out at any time before and after the above-mentioned treatments. In addition, stretching can also be carried out in multiple stages. The cumulative stretching ratio of the PVA film is, for example, more than 5 times, preferably about 5 to 7 times.

[0179] The PVA-based film (stretched film) subjected to the above-mentioned respective treatments is subjected to water washing treatment and drying treatment according to a conventional method.

[0180] The water washing treatment can be carried out, for example, by immersing the PVA film in a water washing bath. The water washing bath can be pure water or an aqueous solution of an iodide (e.g., potassium iodide, sodium iodide, etc.). The concentration of the iodide aqueous solution is preferably 0.1 to 10% by weight. An auxiliary agent such as zinc sulfate or zinc chloride can also be added to the iodide aqueous solution.

[0181] The water washing temperature is, for example, 5 to 50° C., preferably 10 to 45° C., and more preferably 15 to 40° C. The immersion time is, for example, about 10 to 300 seconds, preferably 20 to 240 seconds. The water washing treatment may be performed only once, or may be performed multiple times as needed. When multiple water washing treatments are performed, the type and concentration of the additives contained in the water washing bath used for each treatment may be appropriately adjusted.

[0182] The drying treatment of the PVA-based film can be performed by any appropriate method (for example, natural drying, air drying, and heat drying).

[0183] 2-1-2. Manufacturing of polarizing film

[0184] Polarizing films with a film thickness of less than 6 μm can be manufactured, for example, by the manufacturing method disclosed in Japanese Patent Gazette No. 4751481. The manufacturing method includes: a laminate preparation process in which a PVA-type resin layer is formed on a thermoplastic substrate; a stretching process in which the PVA-type resin layer and the thermoplastic resin substrate are stretched integrally; a dyeing process in which a dichroic substance is adsorbed on the PVA resin layer, and the like. Insolubilization treatment and cross-linking treatment, drying treatment, cleaning treatment, and the like of the PVA-type resin layer can also be adopted as needed. The stretching treatment can be implemented before or after the dyeing treatment. In addition, any stretching method of stretching in a gas atmosphere and stretching in an aqueous solution such as a boric acid aqueous solution can be adopted. In addition, the stretching can be a one-stage stretching or a multi-stage stretching of more than two stages.

[0185] Reference Figure 2 Here, an example of a method for producing a polarizing film is described. Here, a PVA-based resin layer formed on a resin substrate is stretched integrally with the resin substrate to produce a polarizing film.

[0186] [Laminate production process (A)]

[0187] First, a non-crystalline ester thermoplastic resin substrate with a glass transition temperature of 75°C and a thickness of 200 μm, for example, isophthalic acid copolymerized polyethylene terephthalate (hereinafter referred to as "non-crystalline PET") 6 with 6 mol% of isophthalic acid, and a 4-5 wt% PVA aqueous solution obtained by dissolving PVA powder with a polymerization degree of 1000 or more and a saponification degree of 99% or more in water are prepared. Next, in a laminate production device 20 having a coating mechanism 21, a drying mechanism 22, and a surface modification treatment device 23, the PVA aqueous solution is coated on the non-crystalline PET substrate 6, and dried at a temperature of 50-60°C, and a PVA layer 2 with a glass transition temperature of 80°C and a thickness of 7 μm is formed on the PET substrate 6. In this way, a laminate 7 including a 7 μm thick PVA layer can be produced. At this time, by corona-treating the surface of the amorphous PET substrate 6 using the surface modification treatment device 23, the adhesion between the amorphous PET substrate 6 and the PVA layer 2 formed thereon can be improved.

[0188] Next, the laminate 7 including the PVA layer was subjected to the following treatment including two-step stretching treatment of auxiliary stretching in an air atmosphere and stretching in a boric acid aqueous solution, thereby finally producing a polarizing film having a thickness of 3 μm.

[0189] [Assisted stretching treatment in gas atmosphere (B)]

[0190] In the first stage of the in-air auxiliary stretching treatment (B), the laminate 7 including the 7 μm thick PVA layer 2 is stretched integrally with the PET substrate 6 to generate a "stretched laminate 8" including the 5 μm thick PVA layer 2. Specifically, in the in-air auxiliary stretching treatment device 30 equipped with a stretching mechanism 31 in the oven 33, the laminate 7 including the 7 μm thick PVA layer 2 is placed in the stretching mechanism 31 of the oven 33 set to a stretching temperature environment of 130°C, and the free-end uniaxial stretching is performed in such a way that the stretching ratio reaches 1.8 times to generate the stretched laminate 8. In this stage, the roll 8' of the stretched laminate 8 can be manufactured by the winding device 32 also provided in the oven 30.

[0191] [Dyeing treatment (C)]

[0192] Next, by dyeing treatment (C), a colored laminate 9 is produced in which iodine, which is a dichroic substance, is adsorbed on a 5 μm thick PVA layer 2 in which PVA molecules are oriented. Specifically, in a dyeing device 40 having a dye bath 42 of a dyeing liquid 41, a stretched laminate 8 is continuously unloaded from a continuous unloading device 43 equipped with a roll 8' provided in the dyeing device 40, and is immersed in a dyeing liquid 41 containing iodine and potassium iodide at a liquid temperature of 30° C. for an arbitrary period of time, and the monomer transmittance of the PVA layer constituting the polarizing film finally produced is made to be 40 to 44%, thereby producing a colored laminate 9 in which iodine is adsorbed on the oriented PVA layer 2 of the stretched laminate 8.

[0193] In this treatment, in order to prevent the dyeing liquid 41 from dissolving the PVA layer 2 contained in the stretched laminate 8, water is used as a solvent and the iodine concentration is set to 0.30 wt%. In addition, the concentration of potassium iodide in the dyeing liquid 41 for dissolving iodine in water is set to 2.1 wt%. The ratio of the concentration of iodine to potassium iodide is 1 to 7. More specifically, the stretched laminate 8 is immersed in the dyeing liquid 41 with an iodine concentration of 0.30 wt% and a potassium iodide concentration of 2.1 wt% for 60 seconds, thereby generating a colored laminate 9 in which iodine is adsorbed on the PVA layer 2 with a thickness of 5 μm after the PVA molecules are oriented.

[0194] [Stretching treatment in a boric acid aqueous solution (D)]

[0195] The colored laminate 9 including the iodine-oriented PVA layer 2 is further stretched by the second stage of the boric acid aqueous solution stretching treatment, thereby generating an optical film laminate 60 including a 3 μm thick PVA layer constituting a polarizing film and oriented with iodine. Specifically, in the boric acid aqueous solution stretching treatment device 50 having a boric acid bath 52 of the boric acid aqueous solution 51 and a stretching mechanism 53, the colored laminate 9 continuously discharged from the dyeing device 40 is immersed in the boric acid aqueous solution 51 containing boric acid and potassium iodide and set to a stretching temperature environment of 65°C. Next, the free-end uniaxial stretching is performed in the stretching mechanism 53 provided in the boric acid aqueous solution treatment device 50 so as to achieve a stretching ratio of 3.3 times, thereby generating an optical film laminate 60 including a 3 μm thick PVA layer.

[0196] [Cleaning treatment (G)]

[0197] Next, the optical film laminate 60 including the polarizing film is preferably directly sent to the cleaning process (G). The purpose of the cleaning process (G) is to wash away the unnecessary residues attached to the surface of the polarizing film by the cleaning liquid 81 of the cleaning device 80. However, the cleaning process (G) can also be omitted, and the optical film laminate 60 including the polarizing film taken out can be directly sent to the drying process (H).

[0198] [Drying treatment (H)]

[0199] The cleaned optical film laminate 60 is sent to a drying process (H) and dried there. Next, the dried optical film laminate 60 is rolled up into a continuous web of optical film laminate 60 by a winding device 91 provided together with the drying device 90, thereby generating a roll of the optical film laminate 60 including the polarizing film. As the drying process (H), any appropriate method may be adopted, such as natural drying, air drying, and heating drying. For example, in the drying device 90 of the oven, hot air at 60°C is used for drying for 240 seconds.

[0200] 2-1-3. Others

[0201] The polarizing film preferably contains zinc. By making the polarizing film contain zinc, there is a tendency to suppress the decrease in transmittance and hue degradation of the polarizing film laminate after the heating test. When the polarizing film contains zinc, the content of zinc in the polarizing film is preferably 0.002 to 2% by weight, and more preferably 0.01 to 1% by weight.

[0202] Preferably, the polarizing film further contains sulfate ions. By making the polarizing film contain sulfate ions, there is a tendency to suppress the decrease in the transmittance of the polarizing film laminate after the heating test. In the case where the polarizing film contains sulfate ions, the content of sulfate ions in the polarizing film is preferably 0.02 to 0.45 weight%, more preferably 0.05 to 0.35 weight%, and further preferably 0.1 to 0.25 weight%. It should be noted that the content of sulfate ions in the polarizing film can be calculated based on the sulfur atom content.

[0203] In order to include zinc in the polarizing film, it is preferred to perform zinc impregnation treatment in the production process of the polarizing film. In addition, in order to include sulfate ions in the polarizing film, it is preferred to perform sulfate ion treatment in the production process of the polarizing film.

[0204] The zinc impregnation treatment can be carried out, for example, by immersing the PVA film in a zinc salt solution. As the zinc salt, an inorganic chlorine compound in an aqueous solution of zinc halides such as zinc chloride and zinc iodide, zinc sulfate, zinc acetate, etc. is preferred. In addition, various zinc complexes can also be used in the zinc impregnation treatment. In addition, when the zinc salt solution uses an aqueous solution containing potassium ions and iodide ions using potassium iodide, etc., it is easy to impregnate the zinc ions, so it is preferred. The potassium iodide concentration in the zinc salt solution is preferably set to about 0.5 to 10% by weight, and more preferably set to 1 to 8% by weight.

[0205] Sulfate ion treatment can be performed, for example, by immersing the PVA film in an aqueous solution containing a metal sulfate. As the metal sulfate, the following metal sulfate is preferred: it is easy to separate into sulfate ions and metal ions in the treatment solution, and it is easy to introduce the metal sulfate into the PVA film in the form of ions. For example, as the type of metal forming the metal sulfate, alkali metals such as sodium and potassium; alkaline earth metals such as magnesium and calcium; and transition metals such as cobalt, nickel, zinc, chromium, aluminum, copper, manganese, and iron can be listed.

[0206] In the manufacture of polarizing film, the above-mentioned zinc impregnation treatment and sulfate ion treatment can be carried out at any stage. That is, the zinc impregnation treatment and sulfate ion treatment can be carried out before the dyeing treatment or after the dyeing treatment. The zinc impregnation treatment and sulfate ion treatment can also be carried out simultaneously. Preferably, zinc sulfate is used as the above-mentioned zinc salt and the above-mentioned metal sulfate salt, and the PVA-type film is immersed in a treatment bath containing zinc sulfate, so that the zinc impregnation treatment and the sulfate ion treatment are carried out simultaneously. In addition, the above-mentioned zinc salt and the above-mentioned metal sulfate salt can also be coexisted in the dyeing solution in advance, and the zinc impregnation treatment and / or sulfate ion treatment can be carried out simultaneously with the dyeing treatment. The zinc impregnation treatment and the sulfate ion treatment can also be carried out simultaneously with the stretching.

[0207] 2-2. Polarizing film protective film

[0208] As materials constituting the polarizing film protective films 121 and 122, for example, thermoplastic resins having excellent transparency, mechanical strength, and thermal stability can be cited. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene resins), polyarylate resins, polystyrene resins, PVA resins, and mixtures thereof.

[0209] The polarizing film protective film may also function as a phase difference film.

[0210] The thickness of the polarizing film protective film can be appropriately adjusted for the purpose of adjusting the moisture content of the polarizing film laminate, and is preferably about 1 to 500 μm, more preferably 2 to 300 μm, and even more preferably 5 to 200 μm in view of strength, workability such as handling, and thinness.

[0211] The polarizing film protective film may contain one or more optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, mold release agents, anti-coloring agents, flame retardants, nucleating agents, antistatic agents, pigments, colorants, etc.

[0212] 2-3. Other optical films

[0213] The polarizing film and the polarizing film protective film may also be directly bonded, but may also be laminated with other optical films. For other optical films, there is no particular limitation, and for example, phase difference films, viewing angle compensation films, etc. may be used. The phase difference film as other optical films may be a film having a function as a protective film.

[0214] As described above, the polarizing film protective film may also have the function of a phase difference film, but in this case, the phase difference film as other optical films may be omitted. On the other hand, in the case where the polarizing film protective film also has the function of a phase difference film, a phase difference film may also be provided as other optical films. In this case, it substantially includes two or more layers of phase difference films.

[0215] 2-4. Adhesive

[0216] The polarizing film 120 and the polarizing film protective films 121 and 122 may be bonded together, or other optical films such as a retardation film and these films may be bonded together using, for example, a radical polymerization curable adhesive, a cationic polymerization curable adhesive, or a water-based adhesive.

[0217] (Free radical polymerization curing adhesive)

[0218] The above-mentioned free radical polymerization curable adhesive contains a free radical polymerizable compound as a curable compound. The free radical polymerizable compound can be a compound that is cured by active energy rays or a compound that is cured by heat. Examples of active energy rays include electron beams, ultraviolet rays, and visible light.

[0219] As the above-mentioned free radical polymerizable compound, for example, a compound having a free radical polymerizable functional group having a carbon-carbon double bond such as a (meth)acryloyl group and a vinyl group can be cited. As the free radical polymerizable compound, a polyfunctional free radical polymerizable compound is preferably used. The free radical polymerizable compound can be used alone or in combination of two or more. In addition, a polyfunctional free radical polymerizable compound and a monofunctional free radical polymerizable compound can also be used in combination.

[0220] As the above-mentioned polymerizable compound, preferably use the compound with high logP value (octanol / water partition coefficient), as the free radical polymerizable compound, preferably use the compound with high logP value.Herein, logP value is the index of the lipophilicity of the characterization substance, and represents the logarithm value of the partition coefficient of octanol / water.High logP value means lipophilicity, that is, means low water absorption.The logP value can be measured (flask penetration method recorded in JIS-Z-7260), and can also be calculated by calculation based on the structure of each compound as the constituent component (curable component, etc.) of the curing adhesive (ChemDraw Ultra manufactured by Cambridge Soft).

[0221] The logP value of the radical polymerizable compound is preferably 2 or more, more preferably 3 or more, and particularly preferably 4 or more. Within such a range, deterioration of the polarizer due to moisture can be prevented, and a polarizing film having excellent durability under high temperature and high humidity can be obtained.

[0222] Examples of the polyfunctional radical polymerizable compound include tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol diacrylate, 2-ethyl-2-butylpropylene glycol di(meth)acrylate, bisphenol A di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, bisphenol A propylene oxide adduct di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, cyclic trimethylolpropane formal(meth)acrylate, dimethacrylate, and bisphenol A diglycidyl ether di(meth)acrylate. Esterification products of (meth)acrylates and polyols such as alkanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and EO-modified diglycerol tetra(meth)acrylate; 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene; epoxy (meth)acrylate; urethane (meth)acrylate; polyester (meth)acrylate, etc.

[0223] Among the above-mentioned multifunctional free radical polymerizable compounds, those with high logP values ​​are preferred. Examples of such compounds include alicyclic (meth)acrylates such as tricyclodecane dimethanol di(meth)acrylate (logP=3.05) and isobornyl (meth)acrylate (logP=3.27); long-chain aliphatic (meth)acrylates such as 1,9-nonanediol di(meth)acrylate (logP=3.68) and 1,10-decanediol diacrylate (logP=4.10); polybranched (meth)acrylates such as hydroxypivalic acid neopentyl glycol (meth)acrylate adduct (logP=3.35) and 2-ethyl-2-butylpropylene glycol di(meth)acrylate (logP=3.92); (Meth)acrylates containing aromatic rings, such as bisphenol A di(meth)acrylate (logP=5.46), bisphenol A ethylene oxide 4 mole addition product di(meth)acrylate (logP=5.15), bisphenol A propylene oxide 2 mole addition product di(meth)acrylate (logP=6.10), bisphenol A propylene oxide 4 mole addition product di(meth)acrylate (logP=6.43), 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene (logP=7.48), and p-phenylphenol (meth)acrylate (logP=3.98).

[0224] When a multifunctional free radical polymerizable compound and a monofunctional free radical polymerizable compound are used in combination, the content ratio of the multifunctional free radical polymerizable compound is preferably 20 to 97% by weight, more preferably 50 to 95% by weight, further preferably 75 to 92% by weight, and particularly preferably 80 to 92% by weight relative to the total amount of the free radical polymerizable compound. If it is within such a range, a polarizing film having excellent durability under high temperature and high humidity can be obtained.

[0225] Examples of the monofunctional radical polymerizable compound include (meth)acrylamide derivatives having a (meth)acrylamide group. When a (meth)acrylamide derivative is used, a pressure-sensitive adhesive layer having excellent adhesiveness can be formed with high productivity. Specific examples of (meth)acrylamide derivatives include N-alkyl (meth)acrylamide derivatives such as N-methyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-butyl (meth)acrylamide, and N-hexyl (meth)acrylamide; N-hydroxyalkyl (meth)acrylamide derivatives such as N-hydroxymethyl (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, and N-hydroxymethyl-N-propane (meth)acrylamide; N-aminoalkyl (meth)acrylamide derivatives such as aminomethyl (meth)acrylamide and aminoethyl (meth)acrylamide; N-alkoxy (meth)acrylamide derivatives such as N-methoxymethylacrylamide and N-ethoxymethylacrylamide; N-mercaptoalkyl (meth)acrylamide derivatives such as mercaptomethyl (meth)acrylamide and mercaptoethyl (meth)acrylamide, and the like. In addition, as heterocyclic (meth)acrylamide derivatives in which the nitrogen atom of the (meth)acrylamide group forms a heterocyclic ring, for example, N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylpyrrolidine, etc. can be used. Among these, N-hydroxyalkyl (meth)acrylamide derivatives are preferred, and N-hydroxyethyl (meth)acrylamide is more preferred.

[0226] In addition, as the above-mentioned monofunctional free radical polymerizable compound, a (meth)acrylic acid derivative having a (meth)acryloyloxy group can be used; a carboxyl group-containing monomer such as (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, etc.; a lactam vinyl monomer such as N-vinylpyrrolidone, N-vinyl-ε-caprolactam, methylvinylpyrrolidone, etc.; vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyl Vinyl monomers having a nitrogen-containing heterocyclic ring such as oxazole and vinyl morpholine, etc.

[0227] When a multifunctional free radical polymerizable compound and a monofunctional free radical polymerizable compound are used in combination, the monofunctional free radical polymerizable compound is preferably contained in an amount of 3 to 80% by weight, more preferably 5 to 50% by weight, further preferably 8 to 25% by weight, and particularly preferably 8 to 20% by weight relative to the total amount of the free radical polymerizable compound. If it is within such a range, a polarizing film having excellent durability under high temperature and high humidity can be obtained.

[0228] The above-mentioned free radical polymerization curing adhesive may further contain other additives. In the case where the free radical polymerization curing adhesive contains a curable compound cured by active energy rays, the adhesive may further contain, for example, a photopolymerization initiator, a photoacid generator, a silane coupling agent, etc. In addition, in the case where the free radical polymerization curing adhesive contains a curable compound cured by heat, the adhesive may further contain a thermal polymerization initiator, a silane coupling agent, etc. In addition, as other additives, for example, an inhibitor, a polymerization initiation aid, a leveling agent, a wettability improver, a surfactant, a plasticizer, an ultraviolet absorber, an inorganic filler, a pigment, a dye, etc. can be cited.

[0229] (Cationic polymerization curing adhesive)

[0230] The above-mentioned cationic polymerization curing adhesive contains a cationic polymerizable compound as a curable compound. As the cationic polymerizable compound, for example, a compound having an epoxy group and / or an oxetane group can be cited. The compound having an epoxy group is preferably a compound having at least two epoxy groups in the molecule. As the compound having an epoxy group, for example, a compound having at least two epoxy groups and at least one aromatic ring (aromatic epoxy compounds), a compound having at least two epoxy groups in the molecule and at least one of which is formed between two adjacent carbon atoms constituting an alicyclic ring (alicyclic epoxy compounds), etc. can be cited.

[0231] Preferably, the above-mentioned cationic polymerization curing adhesive contains a photocationic polymerization initiator. The photocationic polymerization initiator generates cationic species or Lewis acid by irradiation with active energy rays such as visible light, ultraviolet rays, X-rays, electron beams, etc., thereby initiating the polymerization reaction of epoxy groups and oxetane groups. In addition, the cationic polymerization curing adhesive may further contain the above-mentioned additives.

[0232] (Water-based adhesive)

[0233] As the aqueous adhesive, for example, aqueous solutions (for example, having a solid content concentration of 0.5 to 60% by weight) of aqueous adhesives such as isocyanate adhesives, PVA adhesives, gelatin adhesives, vinyl latex adhesives, and aqueous polyester adhesives can be preferably used.

[0234] The adhesive may be applied to any one of the polarizing film 120, the polarizing film protective films 121, 122, and other optical films, or to any two of them. Generally, it is preferred to immerse the polarizing film in an aqueous adhesive solution and then laminate it with the polarizing film protective films 121, 122 by a roll laminator or the like. The thickness of the adhesive layer is not particularly limited, and is, for example, about 30 nm to 1000 nm in thickness after drying.

[0235] After laminating the polarizing film, the polarizing film protective film, and other optical films with an adhesive, the laminate is subjected to a drying process. In the drying process of the laminate, in addition to the purpose of drying and solidifying the adhesive, it is also carried out for the purpose of reducing the moisture content of the polarizing film laminate to improve the initial optical properties. As a drying method, heating drying is generally used. As drying conditions, the range of 50 to 95°C is preferred, and the range of 60 to 85°C is more preferred.

[0236] The drying conditions of the laminate are not particularly limited, but in consideration of treatment efficiency and practicality, the drying temperature is preferably 50° C. or higher, and in view of making the optical properties of the polarizing film laminate uniform, it is preferably 95° C. or lower. The drying temperature may be increased stepwise within the above temperature range.

[0237] The drying of the laminate can be carried out continuously with the bonding process of the polarizing film, the polarizing film protective film, and other optical films. In addition, after the laminate of the polarizing film, the polarizing film protective film, and other optical films is temporarily wound into a roll state, it can be dried as another treatment.

[0238] Generally speaking, in order to reduce the moisture content of the polarizing film laminate, high temperature / long time drying conditions are necessary. From the perspective of reducing the moisture content of the polarizing film laminate, high temperature / long time drying is preferred, but on the other hand, it sometimes causes a reduction in the optical properties of the polarizing film laminate. By using a polarizing film protective film with a small saturated water absorption and a polarizing film protective film with a high moisture permeability, the moisture content of the polarizing film laminate can be adjusted to the above-mentioned desired range even without using strict drying conditions.

[0239] 2-5. Adhesive

[0240] The adhesive described in the above-mentioned "1-3. Transparent adhesive" can be used in the same manner.

[0241] 3. Reliability evaluation project

[0242] Multiple phenomena that may occur in polarizing film laminates, namely, polyeneization, discoloration, heat blushing, adhesion durability, and reworkability were evaluated. The mechanism of each phenomenon is not yet clear, but it can be roughly estimated as follows.

[0243] <Polyene>

[0244] In a high temperature and high humidity environment, the single transmittance of the polarizing film laminate decreases. It is speculated that this decrease is due to the polyeneization of PVA. Polyene refers to -(CH=CH) n -, which can be formed in the polarizing film by heating. Polyene will cause the transmittance of the polarizing film to be significantly reduced. In addition, in a high temperature and high humidity environment, the PVA-polyiodine complex is destroyed and I - and I2.

[0245] The polyene formation of PVA is considered to be initiated by a dehydration reaction promoted by iodine (I2) generated in a high temperature and high humidity environment and heating as shown in the following chemical formula 1.

[0246] (Chemical formula 1)

[0247]

[0248] It is believed that the PVA-polyiodine complex present in the polarizing film is destroyed by heating, and the I2 generated thereby forms a charge transfer complex (HO···I2) with the OH group in the PVA, and then polyene is formed via the OI group. It is believed that when the adhesive layer contains a large amount of acid components, the protons generated by the acid components act as a catalyst for the dehydration reaction of PVA, thereby further promoting polyene.

[0249] <Decolorization>

[0250] In the iodine-dyed and stretched PVA film (polarizing film), iodine is present in the form of I3 - and I5 - The polyiodide ions of PVA form a complex (PVA polyiodide complex) with the oriented PVA. At this time, PVA forms crosslinking points through a crosslinking agent such as boric acid, thereby maintaining the orientation.

[0251] However, if the polarizing film is placed under high temperature and high humidity, the hydrolysis of the boric acid crosslinking will be induced, resulting in a decrease in the orientation of PVA and the disintegration of the PVA polyiodine complex. As a result, the visible light absorption based on the PVA polyiodine complex decreases, and the transmittance on the long wavelength side of about 700nm and the short wavelength side of about 410nm increases. In this way, discoloration in black display will occur in the polarizing film placed under high temperature and high humidity.

[0252] <Heating and turning red>

[0253] In the iodine-dyed and stretched PVA film (polarizing film), iodine is present in the form of I3 - and I5 - The polyiodide ion forms a complex with PVA (PVA polyiodine complex). - It has a broad absorption peak around 470nm, I5 - It has a broad absorption peak around 600nm. That is, PVA-I3 - The complex is responsible for the absorption on the short wavelength side (blue side), PVA-I5 - The complex is responsible for absorption on the long wavelength side (red side).

[0254] However, the PVA-I5 -The complex has weak resistance to heating. If the polarizing film is placed at high temperature, PVA and I5 - The complex formation of I5 - break down.

[0255] Therefore, in the polarizing film placed at high temperature, PVA-I5 responsible for absorption on the long wavelength side - As the amount of complexes decreases, the transmittance on the long wavelength side of about 700 nm increases, and the color of the polarizing film changes to red.

[0256] Example

[0257] 4. Examples and Comparative Examples

[0258] Hereinafter, although an Example and a comparative example are demonstrated together, it is needless to say that this invention is not limited to the description in these Examples.

[0259] As examples and comparative examples, the “thickness of polarizing film (μm)”, and / or the “iodine concentration of polarizing film (wt.%)”, and / or the “water content of polarizing film laminate (g / m 2 )” samples of various polarizing film stacks with different

[0260] <Film thickness of polarizing film>

[0261] The film thickness (μm) of the polarizing film is measured using a spectroscopic film thickness meter MCPD-1000 (manufactured by Otsuka Electronics Co., Ltd.). The thickness of the polarizing film protective film is also measured using the spectroscopic film thickness meter. The polarizing film contained in the sample can be taken out by immersing the sample in a solvent and dissolving the polarizing film protective film. As the solvent, respectively, for example, when the polarizing film protective film is a cellulose triacetate resin, dichloromethane is used, when the polarizing film protective film is a cycloolefin resin, cyclohexane is used, and when the polarizing film protective film is an acrylic resin, methyl ethyl ketone is used. It should be noted that when the resin of the polarizing film protective film provided on one side of the polarizing film is different from the resin of the polarizing film protective film provided on the other side, the above-mentioned solvent is used to dissolve each resin in turn.

[0262] <Iodine concentration of polarizing film>

[0263] When producing a polarizing film, the iodine concentration (wt. %) of the polarizing film can be changed by adjusting, for example, the concentration of the iodine aqueous solution in which the PVA-based film or the PVA layer is immersed and the immersion time.

[0264] The iodine concentration of the polarizing film is measured by the following method: The polarizing film contained in the sample can be taken out by immersing the sample in a solvent and dissolving the polarizing film protective film in the same manner as when measuring the film thickness of the polarizing film.

[0265] (Fluorescence X-ray measurement)

[0266] When measuring the iodine concentration of the polarizing film, first, the iodine concentration was quantitatively determined using a calibration curve method of fluorescent X-ray analysis. A fluorescent X-ray analyzer ZSX-PRIMUS IV (manufactured by Rigaku Corporation) was used as an apparatus.

[0267] The value directly obtained by the fluorescent X-ray analyzer is not the concentration of each element, but the fluorescent X-ray intensity (kcps) of the wavelength inherent to each element. Therefore, in order to determine the iodine concentration contained in the polarizing film, it is necessary to use a calibration curve to convert the fluorescent X-ray intensity into a concentration. The iodine concentration of the polarizing film in this specification refers to the iodine concentration (wt%) based on the weight of the polarizing film.

[0268] (Preparation of calibration curve)

[0269] The calibration curve was prepared according to the following steps.

[0270] 1. A known amount of potassium iodide was dissolved in a PVA aqueous solution to prepare 7 types of PVA aqueous solutions containing iodine at known concentrations. The PVA aqueous solution was applied to polyethylene terephthalate, dried, and then peeled off to prepare samples 1 to 7 of PVA films containing iodine at known concentrations.

[0271] The iodine concentration (wt %) of the PVA film was calculated according to the following mathematical formula 1.

[0272] [Mathematical formula 1]

[0273] Iodine concentration (wt%) = {potassium iodide amount (g) / (potassium iodide amount (g) + PVA amount (g))} × (127 / 166)

[0274] (Molecular weight of iodine: 127Molecular weight of potassium: 39)

[0275] 2. For the produced PVA film, the fluorescence X-ray intensity (kcps) corresponding to iodine was measured using a fluorescence X-ray analyzer ZSX-PRIMUS IV (manufactured by Rigaku Corporation). The fluorescence X-ray intensity (kcps) was set as the peak value of the fluorescence X-ray spectrum. In addition, the film thickness of the produced PVA film was measured using a spectroscopic film thickness meter MCPD-1000 (manufactured by Otsuka Electronics Co., Ltd.).

[0276] 3. The fluorescence X-ray intensity was divided by the thickness (μm) of the PVA film to obtain the fluorescence X-ray intensity per unit thickness of the film (kcps / μm). Table 1 shows the iodine concentration and the fluorescence X-ray intensity per unit thickness of each sample.

[0277] [Table 1]

[0278]

[0279] 4. Based on the results shown in Table 1, a calibration curve was prepared with the fluorescence X-ray intensity per unit thickness of the PVA film (kcps / μm) as the horizontal axis and the iodine concentration (wt%) contained in the PVA film as the vertical axis. The prepared calibration curve is shown in Figure 3 The mathematical formula for calculating the iodine concentration from the fluorescent X-ray intensity per unit thickness of the PVA film using the calibration curve is determined as shown in Mathematical Formula 2. It should be noted that, Figure 3 R 2 is the correlation coefficient.

[0280] [Mathematical formula 2]

[0281] (iodine concentration) (wt%) = 14.474 × (fluorescent X-ray intensity per unit thickness of PVA film) (kcps / μm)

[0282] (Calculation of iodine concentration)

[0283] The fluorescent X-ray intensity per unit thickness (kcps / μm) was calculated by dividing the fluorescent X-ray intensity obtained by measuring the sample by the thickness. The fluorescent X-ray intensity per unit thickness of each sample was substituted into Formula 2 to calculate the iodine concentration.

[0284] <Water content of polarizing film laminate>

[0285] Moisture content of polarizing film laminate (g / m 2 ) can be mainly determined by adjusting the film thickness of the polarizing film, the material and thickness of the polarizing film protective film bonded to the polarizing film, etc. In addition, it can also be adjusted by cross-linking treatment (boric acid content, etc.) during the manufacture of the polarizing film.

[0286] The moisture content of the polarizing film laminate is measured by the following method.

[0287] First, the polarizing film laminated bodies obtained in Examples and Comparative Examples were cut into a square of 0.1 m×0.1 m.

[0288] Put the cut samples into a thermostat and humidity chamber and place them in an environment with a temperature of 23°C and a relative humidity of 55% for 48 hours. Then, take out the samples in a clean room with the same environment as that in the thermostat, i.e., a temperature of 23°C and a relative humidity of 55%, and measure the weight within 5 minutes after taking them out. The sample weight at this time is set as the initial weight W1 (g). It should be noted that as long as it is within about 15 minutes after taking it out, even if the temperature in the clean room fluctuates by about 2°C to 3°C, and even if the relative humidity in the clean room fluctuates by about ±10%, it will not have a substantial impact on the initial weight.

[0289] Next, the sample is put into a dryer and dried at 120°C for 2 hours. Then, the dried sample is taken out in the clean room set at a temperature of 23°C and a relative humidity of about 55%, and the weight is measured within 10 minutes after taking it out. The sample weight at this time is set as the dried weight W2 (g). Different from the above, it is set to within 10 minutes instead of within 5 minutes, taking into account the cooling time. It should be noted that, as mentioned above, as long as it is within about 15 minutes after taking it out, it will not have a substantial impact on the dried weight.

[0290] The equilibrium moisture content M (g / m2) of the polarizing film laminate is calculated from the initial weight W1 and the weight W2 of the sample obtained in this way by the following formula: 2 ).

[0291] (Formula) M = (W1-W2) / (0.1×0.1)

[0292] The “water content of the polarizing film laminate” referred to in the present invention refers to the equilibrium water content calculated by the above-mentioned method.

[0293] (Preparation of Adhesive Layer A)

[0294] First, 80.9 parts of butyl acrylate, 18 parts of benzyl acrylate, 1 part of acrylic acid, and 0.1 part of 4-hydroxybutyl acrylate were added to a 4-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube, and a condenser to obtain a monomer mixture. Furthermore, 0.1 part of 2,2'-azobisisobutyronitrile as a polymerization initiator was added together with 100 parts of ethyl acetate to 100 parts of the monomer mixture (solid content). While the mixture was slowly stirred, nitrogen gas was generally introduced into the flask for nitrogen substitution. The liquid temperature in the flask was maintained at about 55°C, and a polymerization reaction was performed for 8 hours, thereby preparing a solution of an acrylic polymer with a weight average molecular weight (Mw) of 1.85 million and Mw / Mn=3.8.

[0295] Next, 0.45 parts of an isocyanate crosslinking agent (Coronate L manufactured by Tosoh Corporation, trimethylolpropane toluene diisocyanate), 0.1 parts of benzoyl peroxide (NYPER BMT manufactured by NOF Corporation) and 0.2 parts of γ-glycidoxypropylmethoxysilane (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) were further added to 100 parts of the solid content of the acrylic polymer solution to prepare a solution of an acrylic adhesive composition.

[0296] Next, the obtained solution was applied to one side of a separator (MRF38 manufactured by Mitsubishi Chemical Polyester Film Co., Ltd.). The separator was a polyethylene terephthalate film treated with a silicone release agent. The obtained coating film was dried at 155° C. for 1 minute, thereby forming an adhesive layer A on the surface of the separator. The thickness of the adhesive layer was 20 μm.

[0297] (Preparation of Adhesive Layer B)

[0298] First, in a 4-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube and a condenser, 99 parts by weight of butyl acrylate (hereinafter the same), 1.0 part of 4-hydroxybutyl acrylate, and 0.3 part of 2,2'-azobisisobutyronitrile were added together with 100 parts of ethyl acetate. While the mixture was slowly stirred, nitrogen gas was introduced into the flask for nitrogen substitution. The liquid temperature in the flask was maintained at about 55°C, and a polymerization reaction was performed for 4 hours, thereby preparing a solution of an acrylic polymer with a weight average molecular weight (Mw) of 1.65 million and Mw / Mn=3.7.

[0299] Next, 0.3 parts of dibenzoyl peroxide (NYPER BMT manufactured by NOF Corporation), 0.1 parts of trimethylolpropane xylene diisocyanate (Takenate D110N manufactured by Mitsui Takeda Chemicals, Inc.), and 0.2 parts of a silane coupling agent (A-100 manufactured by Midoriken Chemical Co., Ltd., acetoacetyl group-containing silane coupling agent) were added per 100 parts of the solid content of the acrylic polymer solution to prepare an adhesive composition.

[0300] Next, the obtained solution was applied to one side of a separator (MRF38 manufactured by Mitsubishi Chemical Polyester Film Co., Ltd.). The separator was a polyethylene terephthalate film treated with a silicone release agent. The obtained coating film was dried at 155° C. for 1 minute, thereby forming an adhesive layer B on the surface of the separator. The thickness of the adhesive layer was 20 μm.

[0301] (Preparation of Adhesive Layer C)

[0302] In the preparation of the pressure-sensitive adhesive layer A, a pressure-sensitive adhesive layer C was prepared in the same manner except that the polymerization time of the acrylic polymer was set to 2 hours. The weight average molecular weight (Mw) of the acrylic polymer was 1.9 million, and Mw / Mn=2.5.

[0303] (Preparation of Adhesive Layer D)

[0304] In the preparation of the adhesive layer A, the adhesive layer D was prepared in the same manner except that the composition of the acrylic polymer was 80.9 parts of butyl acrylate, 18 parts of benzyl acrylate, 4.8 parts of acrylic acid, and 0.1 parts of 4-hydroxybutyl acrylate. The weight average molecular weight (Mw) of the acrylic polymer was 2.1 million, and Mw / Mn=4.0.

[0305] (Preparation of Adhesive Layer E)

[0306] First, in a 4-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube and a condenser, 71.9 parts of butyl acrylate, 18 parts of benzyl acrylate, 10 parts of acrylic acid, and 0.1 parts of 4-hydroxybutyl acrylate were added to obtain a monomer mixture. Furthermore, 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator were added together with 70 parts of ethyl acetate and 30 parts of toluene to 100 parts of the monomer mixture (solid content). While slowly stirring the mixture, nitrogen gas was introduced into the flask for nitrogen substitution. The liquid temperature in the flask was maintained at about 55°C, and a polymerization reaction was carried out for 8 hours, thereby preparing a solution of an acrylic polymer with a weight average molecular weight (Mw) of 800,000 and Mw / Mn=3.6.

[0307] Next, 1 part of an isocyanate crosslinking agent (Coronate L manufactured by Tosoh Corporation, trimethylolpropane toluene diisocyanate), 0.1 part of benzoyl peroxide (NYPER BMT manufactured by NOF Corporation) and 0.2 part of γ-glycidoxypropylmethoxysilane (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) were further added to 100 parts of the solid content of the acrylic polymer solution to prepare a solution of an acrylic adhesive composition.

[0308] Next, the obtained solution was applied to one side of a separator (MRF38 manufactured by Mitsubishi Chemical Polyester Film Co., Ltd.). The separator was a polyethylene terephthalate film treated with a silicone release agent. The obtained coating film was dried at 155° C. for 1 minute, thereby forming an adhesive layer E on the surface of the separator. The thickness of the adhesive layer was 20 μm.

[0309] [Example 1]

[0310] (Production of polarizing film)

[0311] As the resin substrate, a long amorphous isophthalic acid copolymer polyethylene terephthalate film (isophthalic acid group modification degree 5 mol%, thickness: 100 μm) (modification degree = isophthalic acid unit / (ethylene terephthalate unit + isophthalic acid unit)) was used. One side of the resin substrate was subjected to corona treatment (treatment conditions: 55 W·min / m 2), and an aqueous solution containing PVA (polymerization degree 4200, saponification degree 99.2 mol%) and 13 parts by weight of potassium iodide relative to PVA was applied to the corona treated surface at room temperature. The PVA was prepared by mixing 90 parts by weight of PVA (polymerization degree 4200, saponification degree 99.2 mol%) and 10 parts by weight of acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER Z410"), and then dried at 60°C to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate.

[0312] The obtained laminate was subjected to free-end uniaxial stretching to 2.4 times in the longitudinal direction (length direction) between rolls having different peripheral speeds in an oven at 130° C. (auxiliary stretching in a gas atmosphere).

[0313] Next, the laminate was immersed in an insolubilization bath (boric acid aqueous solution prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).

[0314] Next, the film was immersed in a dyeing bath (an iodine aqueous solution prepared by mixing iodine and potassium iodide at a weight ratio of 1:7 per 100 parts by weight of water) at a liquid temperature of 30° C. for 60 seconds while adjusting the concentration so as to give a predetermined transmittance (dyeing treatment).

[0315] Next, the mixture was immersed in a crosslinking bath (boric acid aqueous solution prepared by blending 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment).

[0316] Then, while the laminate was immersed in a boric acid aqueous solution (boric acid concentration: 3.0 wt%) at a liquid temperature of 70°C, it was uniaxially stretched (stretched in aqueous solution) in the longitudinal direction (length direction) between rollers with different peripheral speeds so that the total stretching ratio became 5.5 times.

[0317] Then, the laminated body was immersed in a cleaning bath (an aqueous solution containing 4 parts by weight of potassium iodide per 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment).

[0318] Thereafter, the sample was dried in an oven maintained at 90° C. (drying treatment) and brought into contact with a SUS metal roll maintained at a surface temperature of 75° C. for 2 seconds or more (hot roll drying treatment).

[0319] In this way, a polarizing film having a thickness of 5.4 μm was obtained on the resin substrate.

[0320] (Production of Polarizing Film Laminate)

[0321] A cycloolefin film (ZT12, 18 μm, manufactured by Japan Zeon Co., Ltd.) as a polarizing film protective film is bonded to the side of the obtained polarizing film opposite to the resin substrate using an ultraviolet curing adhesive. Specifically, the curing adhesive described below is applied in a manner such that the total thickness reaches 1.0 μm, and a roller machine is used for bonding. Then, UV light is irradiated from the cycloolefin film side to cure the adhesive. Next, the resin substrate is peeled off to obtain a polarizing film laminate comprising a cycloolefin polarizing film protective film and a polarizing film.

[0322] The details of the curable adhesive are as follows. An adhesive was prepared by mixing 40 parts by weight of N-hydroxyethyl acrylamide (HEAA), 60 parts by weight of acryloyl morpholine (ACMO) and 3 parts by weight of a photoinitiator "IRGACURE 819" (manufactured by BASF). The adhesive was applied on a polarizing film so that the thickness of the cured adhesive layer reached 1.0 μm, and ultraviolet rays were irradiated as active energy rays to cure the adhesive. For ultraviolet irradiation, a metal halide lamp enclosed in gallium was used, an irradiation device: Light HAMMER10 manufactured by Fusion UV Systems, Inc., valve: V valve, peak illuminance: 1600 mW / cm 2 , cumulative exposure 1000 / mJ / cm 2 (wavelength 380 to 440 nm), and the illuminance of ultraviolet rays was measured using the Sola-Check system manufactured by Solatell.

[0323] (Removal of polarizing film)

[0324] The polarizing film was taken out from the polarizing film laminate using cyclohexane as a solvent, and the iodine concentration of the polarizing film was measured.

[0325] (Production of Polarizing Film Laminated Body with Adhesive Layer)

[0326] The pressure-sensitive adhesive layer A was transferred to one side of the polarizing film of the polarizing film laminate, thereby producing a pressure-sensitive adhesive layer-attached polarizing film laminate of Example 1.

[0327] [Example 2]

[0328] When the polarizing film of Example 1 was prepared, the concentration of the iodine aqueous solution and the immersion time were adjusted to change the iodine concentration during the dyeing process, and the thickness of the polarizing film protective film was adjusted to change the moisture content of the polarizing film laminate.

[0329] [Example 3]

[0330] When the polarizing film of Example 1 was prepared, the concentration of the iodine aqueous solution and the immersion time were adjusted during the dyeing process to change the iodine concentration, and the thickness of the polarizing film protective film was adjusted to change the moisture content of the polarizing film laminate. In addition, when the polarizing film laminate of Example 1 was prepared, a cycloolefin film (ZF12, 13 μm, manufactured by Japan Zeon Co., Ltd.) was bonded as the polarizing film protective film. The other conditions were the same as those of Example 1.

[0331] [Example 4]

[0332] When the polarizing film laminate of Example 1 was prepared, a triacetyl cellulose film (TJ40UL manufactured by Fuji Film Co., Ltd., thickness 40 μm) was bonded as a polarizing film protective film. In addition, when the polarizing film of Example 1 was prepared, the concentration of the iodine aqueous solution and the immersion time were adjusted during the dyeing process to change the iodine concentration. The other conditions were the same as those of Example 1.

[0333] [Example 5]

[0334] When the polarizing film laminate of Example 1 was prepared, a transparent protective film (Nitto Denko Corporation) with a thickness of 40 μm formed of a modified acrylic polymer having a lactone ring structure was bonded as a polarizing film protective film. In addition, when the polarizing film of Example 1 was prepared, the concentration of the iodine aqueous solution and the immersion time were adjusted during the dyeing process to change the iodine concentration. The other conditions were the same as those of Example 1.

[0335] [Example 6]

[0336] (Production of polarizing film)

[0337] A PVA film with an average degree of polymerization of 2700 and a thickness of 30 μm was stretched and transported while being dyed between rollers with different peripheral speed ratios. First, the PVA film was immersed in a 30°C water bath for 1 minute to swell the film, and then stretched 1.2 times in the transport direction. Then, it was immersed in an aqueous solution (liquid temperature 30°C) of potassium iodide (0.03 wt%) and iodine (0.3 wt%) for 1 minute, thereby being stretched to 3 times in the transport direction while being dyed (based on the unstretched film). Next, the stretched film was immersed in an aqueous solution (bath) of boric acid (4 wt%), potassium iodide (5 wt%) and zinc sulfate (3.5 wt%) for 30 seconds, while being stretched to 6 times in the transport direction (based on the unstretched film). After stretching, it was dried in an oven at 40°C for 3 minutes to obtain a 12.0 μm polarizing film.

[0338] (Production of Polarizing Film Laminate)

[0339] As an adhesive, an aqueous solution containing a polyvinyl alcohol resin containing an acetoacetyl group (average degree of polymerization 1200, saponification degree 98.5 mol%, acetoacetylation degree 5 mol%) and methylol melamine in a weight ratio of 3:1 was used. Using the adhesive, a 20 μm thick transparent protective film (Nitto Denko Corporation) formed of a modified acrylic polymer having a lactone ring structure was bonded to one side of the polarizing film using a roll laminator at a temperature of 30°C, and a 27 μm thick transparent protective film having a 2 μm thick hard coating layer (HC) formed on a 25 μm thick cellulose triacetate film (manufactured by Konica Minolta, trade name "KC2UA") was bonded to the other side, and then continued to heat at 70°C in an oven for 5 minutes to dry it, thereby obtaining a polarizing film laminate having transparent protective films bonded to both sides of the polarizing film.

[0340] The hard coat layer is formed by the following method. First, a hard coat layer forming material is prepared. The material is made as follows: a UV-curable resin monomer or oligomer with urethane acrylate as the main component is dissolved in butyl acetate, and in the obtained resin solution (DIC Corporation, trade name "UNIDIC 17-806". Solid content concentration 80% by weight), 5 parts by weight of a photopolymerization initiator (BASF Corporation, product name "IRGACURE906") and 0.01 parts by weight of a leveling agent (DIC Corporation, product name "GRANDIC PC4100") are added to the above-mentioned compounding solution in a ratio of 45:55 so that the solid content concentration in the above-mentioned solution reaches 36% by weight, thereby making a hard coat layer forming material. The hard coating forming material prepared in this way was applied to the transparent protective film so that the thickness of the hard coating after curing was 2 μm to form a coating film. Next, the film was dried at 90° C. for 1 minute and then irradiated with a high pressure mercury lamp at a cumulative light intensity of 300 mJ / cm 2 The coating film was cured by ultraviolet rays.

[0341] (Removal of polarizing film)

[0342] The polarizing film was taken out from the polarizing film laminate using dichloromethane and methyl ethyl ketone as a solvent, and the iodine concentration of the polarizing film was measured.

[0343] (Production of Polarizing Film Laminated Body with Adhesive Layer)

[0344] The pressure-sensitive adhesive layer A was transferred to one side of the acrylic transparent protective film of the polarizing film laminate, thereby producing a pressure-sensitive adhesive layer-attached polarizing film laminate of Example 6.

[0345] [Example 7]

[0346] When the polarizing film of Example 6 was prepared, the concentration of the iodine aqueous solution and the immersion time were adjusted during the dyeing process to change the iodine concentration. In addition, when the polarizing film laminate of Example 6 was prepared, as a polarizing film protective film, a transparent protective film with a thickness of 30 μm formed of a modified acrylic polymer having a lactone ring structure (Nitto Denko Corporation) was bonded to one side of the obtained polarizing film, and a transparent protective film with a thickness of 49 μm formed on a cellulose triacetate film with a thickness of 40 μm (manufactured by Konica Minolta, trade name "KC4UY") with a thickness of 9 μm HC was bonded to the other side. The other conditions were the same as those of Example 6.

[0347] [Example 8]

[0348] In Example 7, a polarizing film laminate with an adhesive layer was produced in the same manner except that the adhesive layer C was transferred to one side of the acrylic transparent protective film of the polarizing film laminate.

[0349] [Example 9]

[0350] When the polarizing film of Example 6 was prepared, a PVA film with a thickness of 45 μm was stretched and transported during the stretching process to obtain a polarizing film with a thickness of 18.0 μm. In addition, during the dyeing process, the concentration of the iodine aqueous solution and the immersion time were adjusted to change the iodine concentration. In addition, when the polarizing film laminate of Example 6 was prepared, as a polarizing film protective film, a transparent protective film with a thickness of 30 μm formed of a modified acrylic polymer having a lactone ring structure (Nitto Denko Corporation) was bonded to one side of the obtained polarizing film, and a triacetyl cellulose film (TJ40UL, manufactured by Fuji Film Co., Ltd., thickness 40 μm) was bonded to the other side. The other conditions were the same as those of Example 6.

[0351] [Example 10] to [Example 13]

[0352] When the polarizing film of Example 9 was prepared, the concentration of the iodine aqueous solution and the immersion time were adjusted to change the iodine concentration during the dyeing process, and the thickness of the polarizing film protective film was adjusted to change the moisture content of the polarizing film laminate.

[0353] [Example 14]

[0354] In Example 9, a pressure-sensitive adhesive layer-attached polarizing film laminate was produced in the same manner except that the pressure-sensitive adhesive layer C was transferred to one side of the acrylic transparent protective film of the polarizing film laminate.

[0355] [Example 15]

[0356] In Example 9, a polarizing film laminate with an adhesive layer was produced in the same manner except that the adhesive layer D was transferred to one side of the acrylic transparent protective film of the polarizing film laminate.

[0357] [Comparative Example 1] to [Comparative Example 2]

[0358] When the polarizing film of Example 1 was produced, the concentration of the iodine aqueous solution and the immersion time were adjusted to change the iodine concentration during the dyeing process, and the thickness of the polarizing film protective film was adjusted to change the moisture content of the polarizing film laminate.

[0359] Furthermore, the pressure-sensitive adhesive layer B was transferred to one side of the polarizing film of the polarizing film laminate, thereby producing pressure-sensitive adhesive layer-attached polarizing film laminates of Comparative Examples 1 and 2. Other conditions were the same as those of Example 1.

[0360] [Comparative Example 3] to [Comparative Example 4]

[0361] When the polarizing film of Example 6 was produced, the concentration of the iodine aqueous solution and the immersion time were adjusted to change the iodine concentration during the dyeing process, and the thickness of the polarizing film protective film was adjusted to change the moisture content of the polarizing film laminate.

[0362] Furthermore, the pressure-sensitive adhesive layer B was transferred to one side of the acrylic transparent protective film of the polarizing film laminate, thereby producing pressure-sensitive adhesive layer-attached polarizing film laminates of Comparative Examples 3 and 4. Other conditions were the same as those of Example 6.

[0363] [Comparative Example 5]

[0364] When the polarizing film of Example 7 was produced, the concentration of the iodine aqueous solution and the immersion time were adjusted to change the iodine concentration during the dyeing process, and the thickness of the polarizing film protective film was adjusted to change the moisture content of the polarizing film laminate.

[0365] Furthermore, the pressure-sensitive adhesive layer B was transferred to one side of the acrylic transparent protective film of the polarizing film laminate, thereby producing a pressure-sensitive adhesive layer-attached polarizing film laminate of Comparative Example 5. The other conditions were the same as those of Example 7.

[0366] [Comparative Example 6]

[0367] When the polarizing film of Example 9 was produced, the concentration of the iodine aqueous solution and the immersion time were adjusted to change the iodine concentration during the dyeing process, and the thickness of the polarizing film protective film was adjusted to change the moisture content of the polarizing film laminate.

[0368] Furthermore, the pressure-sensitive adhesive layer B was transferred to one side of the acrylic transparent protective film of the polarizing film laminate, thereby producing a pressure-sensitive adhesive layer-attached polarizing film laminate of Comparative Example 6. Other conditions were the same as those of Example 9.

[0369] [Comparative Example 7]

[0370] (Production of polarizing film)

[0371] When the polarizing film of Example 9 was prepared, a PVA film with a thickness of 60 μm was stretched and transported in the stretching process to obtain a polarizing film with a thickness of 22.0 μm. In addition, in the dyeing process, the concentration of the iodine aqueous solution and the immersion time were adjusted to change the iodine concentration, and the thickness of the polarizing film protective film was adjusted to change the moisture content of the polarizing film laminate. The other conditions were the same as those of Example 9.

[0372] (Production of Polarizing Film Laminate)

[0373] As a polarizing film protective film, a transparent protective film with a thickness of 30 μm formed of a modified acrylic polymer having a lactone ring structure (Nitto Denko Corporation) was bonded to one side of the obtained polarizing film, and a transparent protective film with a thickness of 49 μm formed on a cellulose triacetate film with a thickness of 40 μm (manufactured by Konica Minolta, trade name "KC4UY") with a thickness of 9 μm was bonded to the other side. The other treatments were the same as in Example 9.

[0374] (Removal of polarizing film)

[0375] The conditions for taking out are the same as those in Example 9.

[0376] (Production of Polarizing Film Laminated Body with Adhesive Layer)

[0377] The pressure-sensitive adhesive layer B was transferred to one side of the acrylic transparent protective film of the polarizing film laminate, thereby producing a pressure-sensitive adhesive layer-attached polarizing film laminate of Comparative Example 7.

[0378] [Comparative Example 8]

[0379] When the polarizing film of Comparative Example 7 was prepared, the concentration of the iodine aqueous solution and the immersion time were adjusted during the dyeing process to change the iodine concentration, and the thickness of the polarizing film protective film was adjusted to change the moisture content of the polarizing film laminate. In addition, as the polarizing film protective film, a transparent protective film with a thickness of 20 μm formed of a modified acrylic polymer having a lactone ring structure (Nitto Denko Corporation) was bonded to one side of the polarizing film. The other conditions were the same as those of Comparative Example 7.

[0380] [Comparative Example 9]

[0381] When preparing the polarizing film of Example 9, a PVA film with a thickness of 75 μm was stretched and conveyed during the stretching process to obtain a polarizing film with a thickness of 28 μm. In addition, during the dyeing process, the concentration of the iodine aqueous solution and the immersion time were adjusted to change the iodine concentration, and the thickness of the polarizing film protective film was adjusted to change the moisture content of the polarizing film laminate.

[0382] Furthermore, the pressure-sensitive adhesive layer B was transferred to one side of the acrylic transparent protective film of the polarizing film laminate, thereby producing a pressure-sensitive adhesive layer-attached polarizing film laminate of Comparative Example 9. Other conditions were the same as those of Example 9.

[0383] [Comparative Example 10]

[0384] A polarizing film laminate with an adhesive layer of Comparative Example 10 was produced in the same manner as in Comparative Example 9, except that the adhesive layer D was transferred to one side of the acrylic transparent protective film of the polarizing film laminate.

[0385] [Comparative Example 11]

[0386] A polarizing film laminate with an adhesive layer of Comparative Example 11 was prepared in the same manner as in Comparative Example 6, except that the adhesive layer E was transferred to one side of the acrylic transparent protective film of the polarizing film laminate.

[0387] 4-1. Reliability test

[0388] Using the polarizing film laminate 12 obtained in the examples and comparative examples, Figure 4 As shown, glass plates (slide glass manufactured by Matsunami Glass, product number: S2000423, specifications: water-edge-grinded 65×165 mm, thickness 1.3 mm) were laminated on both surfaces of a polarizing film laminate 12 via adhesives 11 and 13, respectively, and this was used as a sample.

[0389] As the adhesive, CS9868US (manufactured by Nitto Denko Corporation) having a thickness of 200 μm was used on the side of the polarizing film laminate where the adhesive layers A to D were not provided.

[0390] After the sample was left at 95°C for 250 hours (95°C / 250H), discoloration and reddening due to heating were evaluated. After the sample was left at 95°C for 500 hours (95°C / 500H), polyeneization was evaluated.

[0391] 4-2. Evaluation criteria

[0392] The evaluation criteria for polyene formation, red change upon heating, and discoloration are shown below.

[0393] <Polyene>

[0394] The single-body transmittance of the sample was measured before and after the 95° C. / 500 H heating test, and the change in single-body transmittance ΔTs was calculated according to the following formula.

[0395] (Formula) ΔTs=Ts 500 -Ts0

[0396] Where Ts0 is the single transmittance of the sample before heating, Ts 500It is the single body transmittance after heating at 95℃ / 500H.

[0397] When the change ΔTs is a negative value, it is evaluated as "polyeneization (reduction in monomer transmittance)" of the sample. In other words, when the monomer transmittance after heating at 95°C / 500 hours is the same as the monomer transmittance before heating, or is greater than the monomer transmittance before heating, it is evaluated that there is no problem of polyeneization.

[0398] The single-piece transmittance of the sample was measured using a spectrophotometer (product name "DOT-3" manufactured by Murakami Color Research Laboratory Co., Ltd.) The single-piece transmittance can be determined based on JIS Z 8701.

[0399] <Discoloration / Reddening by heating>

[0400] Before and after the 95°C / 250H heating test, the samples were arranged in an orthogonal Nicol manner, and the orthogonal transmittance (%) at wavelengths of 410nm and 700nm was measured by the above-mentioned spectrophotometer, and the changes ΔHs were calculated. 410 and ΔHs 700 .

[0401] The case where both of the following two conditions were satisfied was evaluated as "discoloration" of the sample.

[0402] ·Change ΔHs 410 More than 1%

[0403] ·Change ΔHs 700 More than 5%

[0404] In other words, when the change in the cross transmittance at a wavelength of 410 nm due to the heat treatment at 95° C. / 500 hours was less than 1%, and the change in the cross transmittance at a wavelength of 700 nm was less than 5%, it was evaluated that there was no problem of discoloration.

[0405] In addition, the case where the following conditions were satisfied was evaluated as the "heating reddening" of the sample.

[0406] ·Change ΔHs 410 Less than 1%

[0407] ·Change ΔHs 700 More than 5%

[0408] In other words, when the change in cross transmittance at a wavelength of 410 nm due to the heat treatment at 95° C. / 500 hours is 1% or more and the change in cross transmittance at a wavelength of 700 nm is less than 5%, it is evaluated that there is no problem of heat reddening.

[0409] <Adhesion durability>

[0410] The polarizing film laminate with adhesive layer was cut into 420 mm in length and 320 mm in width, and attached to both sides of a 0.7 mm thick alkali-free glass plate using a laminator. Then, the sample was subjected to autoclave treatment at 50°C and 5 atm for 15 minutes to completely adhere to the alkali-free glass plate. The sample subjected to the above treatment was treated at 95°C for 500 hours (heating test), and the state of foaming, peeling, and warping was evaluated by naked eye observation according to the following criteria.

[0411] “◎”: No changes in appearance such as foaming, peeling, and warping

[0412] "○": There is slight peeling or foaming at the end, but there is no problem in practical use

[0413] "△": There is peeling or foaming at the end, but there is no problem in practical use unless it is for special purposes

[0414] "×": There is significant peeling or foaming at the end, which is problematic in practical use

[0415] <Heavy workability>

[0416] The polarizing film laminate with adhesive layer obtained in the examples and comparative examples was cut into 200 mm in length and 100 mm in width as a sample. The sample was bonded to 0.7 mm thick alkali-free glass (trade name: EG-XG, manufactured by Corning) using a laminator. Next, an autoclave treatment was performed at 50°C and 0.5 MPa for 15 minutes to completely adhere the sample. The sample was peeled off from the alkali-free glass by hand, and the reworkability was evaluated according to the following criteria. For the evaluation of reworkability, 3 sheets were made in the above-mentioned order and repeated 3 times.

[0417] ◎: All three films had no residual adhesive and no film breakage, and could be peeled off well.

[0418] ○: The films of three sheets were partially broken, but could be peeled off by peeling again.

[0419] △: The film was broken in all three sheets, but could be peeled off by peeling again.

[0420] ×: All three films had adhesive residue or the film broke no matter how many times it was peeled off.

[0421] The evaluation results in each of the Examples and Comparative Examples are shown in Table 2 below.

[0422]

[0423] 5. Summary of evaluation results

[0424] Figure 5 The results of the examples and comparative examples (except comparative example 11) are plotted in an xy orthogonal coordinate system. The x-axis (horizontal axis) represents the iodine concentration (wt.%) of the polarizing film, and the y-axis (vertical axis) represents the moisture content (g / m 2 ).

[0425] (1) According to the results of the mapping and technical common sense, it can be generally considered that when the iodine concentration is small and the water content is too small, the problem of heating red discoloration under high temperature conditions is likely to occur, and on the other hand, when the iodine concentration is large and the water content is too large, the problems of polyene and decolorization are likely to occur. In addition, it can be considered that when the iodine concentration is small and the water content is too large, the problem of decolorization under high temperature and high humidity conditions is likely to occur. In this case, as the iodine concentration increases, the problem of polyene is likely to occur. In particular, a transition region between decolorization and polyene is also observed (Comparative Examples 13 and 15).

[0426] On the other hand, it can be seen that when the iodine concentration and the water content fall within a given range, all the problems of heating red change, polyeneization and decolorization can be solved comprehensively. For example, the results of the examples are all located on the upper side of the dividing line "α", i.e., y = (1043-125x) / 240, and on the lower side of the dividing line "β", i.e., y = (379-33x) / 70, and the dividing line "α" is the periphery of the plot representing the results of Example 3 with the minimum water content, i.e., iodine concentration of 7.0 wt.% and water content of 0.7 g / m 2 The coordinate point (hereinafter referred to as the first coordinate point) and the surrounding area of ​​the plot representing the result of Example 9 with the minimum iodine concentration, that is, the iodine concentration is 2.2wt.% and the moisture content is 3.2g / m 2 The line of the coordinate point (hereinafter referred to as the second coordinate point) of the embodiment 8 having the maximum water content is drawn around the iodine concentration of 3.0wt.% and the water content of 4.0g / m 2 The coordinate point (hereinafter referred to as the fourth coordinate point) and the surrounding area of ​​the plot representing the result of Example 2 having the maximum iodine concentration, that is, the iodine concentration is 10.0wt.% and the moisture content is 0.7g / m 2 The coordinate point (hereinafter referred to as the fifth coordinate point) of the polarizing film can be obtained as a line representing the conditions necessary for comprehensively solving all problems of reddening, polyeneization and bleaching. It should be noted that these dividing lines "α" and "β" have nothing to do with the thickness of the polarizing film. In other words, they are applicable to all polarizing films with a film thickness of about 4 to 20 μm.

[0427] In Comparative Example 6 using Binder B (the amount of the acid component in the total monomer components constituting the binder polymer: 0 wt%), although reddening upon heating was observed, polyene formation did not occur. However, polyene formation was observed in Comparative Example 11 in which the binder was changed to Binder E (the amount of the acid component in the total monomer components constituting the binder polymer: 10 wt%). It is presumed that the use of an acid component in the monomer components of the binder polymer in an amount exceeding a given amount promotes polyene formation.

[0428] (2) In addition, according to the results of the mapping and technical common sense, in particular, for all polarizing films having a film thickness of about 4 to 20 μm, when the iodine concentration and the water content of the polarizing film laminate are contained in the following area, all problems of "polyeneization", "bleaching" and "heat reddening" can be solved comprehensively. The area is the area surrounded by a to e, and more specifically, the area surrounded by the iodine concentration of 7.0 wt.% and the water content of 0.7 g / m 2 The first coordinate point ("a" in the figure) and the iodine concentration are 2.2wt.% and the moisture content is 3.2g / m 2 The first line segment of the second coordinate point ("b" in the figure), connecting the second coordinate point "b" and the iodine concentration of 2.2wt.% and the moisture content of 4.0g / m 2 The second line segment of the third coordinate point ("c" in the figure), connecting the third coordinate point "c" and the iodine concentration of 3.0wt.% and the water content of 4.0g / m 2 The third line segment of the fourth coordinate point ("d" in the figure), connecting the fourth coordinate point "d" and the iodine concentration of 10.0wt.% and the water content of 0.7g / m 2 The area surrounded by the fourth line segment of the fifth coordinate point ("e" in the figure) and the fifth line segment connecting the first coordinate point "a" and the fifth coordinate point "e".

[0429] (3) Similarly, it can be seen that, especially for polarizing films having a film thickness of about 11 to 20 μm, all problems of "polyeneization", "bleaching" and "heat reddening" can be solved comprehensively when the iodine concentration and the moisture content of the polarizing film laminate are contained in the following area: the area surrounded by f, b, c, d, and g, more specifically, the area surrounded by the iodine concentration of 4.5 wt.% and the moisture content of 2.0 g / m 2 The sixth line segment connecting the sixth coordinate point ("f" in the figure) and the second coordinate point "b", the second line segment connecting the second coordinate point "b" and the third coordinate point "c", the third line segment connecting the third coordinate point "c" and the fourth coordinate point "d", the third line segment connecting the fourth coordinate point "d" and the iodine concentration of 4.5wt.% and the moisture content of 3.3g / m 2The area surrounded by the seventh line segment connecting the seventh coordinate point ("g" in the figure) and the eighth line segment connecting the sixth coordinate point "f" and the seventh coordinate point "g".

[0430] It can be considered that, in particular, at the sixth coordinate point "f", the iodine concentration is 4.0 wt.% and the water content is 2.3 g / m 2 The coordinate point "f-1" and the seventh coordinate point "g" have an iodine concentration of 4.0 wt.% and a water content of 3.5 g / m 2 In the case of the coordinate point "g-1", the ideal result can be obtained.

[0431] In addition, it can be inferred that, for a polarizing film having a film thickness of about 11 to 20 μm, better results can be obtained in all aspects of "polyeneization", "bleaching" and "heat reddening" when the iodine concentration and the water content of the polarizing film laminate are contained in the following region: the region surrounded by f, b, c, d, g and divided by the line segment connecting h and i, more specifically, the region surrounded by the iodine concentration of 3.3 wt.% and the water content of 2.6 g / m 2 The ninth line segment connecting the eighth coordinate point ("h" in the figure) and the second coordinate point "b", the second line segment connecting the second coordinate point "b" and the third coordinate point "c", the third line segment connecting the third coordinate point "c" and the fourth coordinate point "d", the seventh line segment connecting the fourth coordinate point "d" and the seventh coordinate point "g", the eighth line segment connecting the sixth coordinate point "f" and the seventh coordinate point "g", and the eighth line segment connecting the eighth coordinate point "h" and the iodine concentration of 6.0wt.% and the moisture content of 2.6g / m 2 The area enclosed by the tenth line segment of the ninth coordinate point ("i" in the figure).

[0432] (4) It can be further known that, in particular, with respect to a polarizing film having a film thickness of about 4 to 11 μm, preferably a film thickness of 4 to 7 μm, and more preferably a film thickness of 4.5 to 6 μm, when the iodine concentration and the moisture content of the polarizing film stack are contained in the following area, all problems of "polyeneization", "bleaching", and "heat reddening" can be solved comprehensively. The area is an area surrounded by a, h, i, and e. More specifically, it is an area surrounded by the eleventh line segment connecting the first coordinate point "a" and the eighth coordinate point "h", the tenth line segment connecting the eighth coordinate point "h" and the ninth coordinate point "i", the twelfth line segment connecting the ninth coordinate point "i" and the fifth coordinate point "e", and the fifth line segment connecting the first coordinate point "a" and the fifth coordinate point "e".

[0433] It can be considered that, in particular, the eighth coordinate point "h" is the sixth coordinate point "f" and the ninth coordinate point "i" is the iodine concentration of 7.2 wt.% and the water content of 2.0 g / m 2In the case of the tenth coordinate point ("j" in the figure), the ideal result can be obtained.

[0434] It can also be inferred that, for a polarizing film having a film thickness of about 4 to 11 μm, preferably a film thickness of 4 to 7 μm, and more preferably a film thickness of 4.5 to 6 μm, better results can be obtained in all aspects of "polyeneization", "bleaching" and "heat reddening" when the iodine concentration and the water content of the polarizing film laminate are contained in the following region: the region is the region surrounded by a, k, i, and e, and more specifically, the region connecting the first coordinate point "a" and the iodine concentration of 6.0 wt.% and the water content of 1.2 g / m 2 The area surrounded by the thirteenth line segment connecting the eleventh coordinate point ("k" in the figure), the fourteenth line segment connecting the eleventh coordinate point "k" and the ninth coordinate point "i", the twelfth line segment connecting the ninth coordinate point "i" and the fifth coordinate point "e", and the fifth line segment connecting the first coordinate point "a" and the fifth coordinate point "e".

[0435] It can be considered that, in particular, at the eleventh coordinate point "k", the iodine concentration is 6.5 wt.% and the water content is 1.0 g / m 2 The coordinate point (k-1) and the ninth coordinate point "i" have an iodine concentration of 6.5wt.% and a water content of 2.3g / m 2 In the case of the coordinate point (i-1), a more ideal result can be obtained.

Claims

1. A polarizing film laminate, comprising a polarizing film containing a polyvinyl alcohol-based resin, and an adhesive layer provided on at least one side of the polarizing film directly or via an optically transparent polarizing film protective film, The adhesive layer comprises an adhesive polymer, the adhesive polymer is copolymerized with an acid component, and the amount of the acid component in all monomer components constituting the adhesive polymer is 5% by weight or less, in, The iodine concentration (wt.%) of the polarizing film is taken as the x-axis, the moisture content (g / m 2 ) as the y-axis, has an iodine concentration and a water content contained in the following area, the area is surrounded by a first line segment connecting the first coordinate point and the second coordinate point, a second line segment connecting the second coordinate point and the third coordinate point, a third line segment connecting the third coordinate point and the fourth coordinate point, a fourth line segment connecting the fourth coordinate point and the fifth coordinate point, and a fifth line segment connecting the first coordinate point and the fifth coordinate point, The first coordinate point is an iodine concentration of 7.0 wt.% and a water content of 0.7 g / m 2 The coordinate point of The second coordinate point is an iodine concentration of 2.2 wt.% and a water content of 3.2 g / m 2 The coordinate point of The third coordinate point is an iodine concentration of 2.2 wt.% and a moisture content of 4.0 g / m 2 The coordinate point of The fourth coordinate point is an iodine concentration of 3.0 wt.% and a water content of 4.0 g / m 2 The coordinate point of The fifth coordinate point is an iodine concentration of 10.0 wt.% and a water content of 0.7 g / m 2 The coordinate point of .

2. The polarizing film laminate according to claim 1, wherein: The polydispersity coefficient (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the binder polymer is 3.0 or less.

3. The polarizing film laminate according to claim 1 or 2, wherein: The polarizing film has a thickness of 4 to 20 μm.

4. A polarizing film laminate, comprising a polarizing film containing a polyvinyl alcohol-based resin, and an adhesive layer provided on at least one side of the polarizing film directly or via an optically transparent polarizing film protective film, The adhesive layer comprises an adhesive polymer, the adhesive polymer is copolymerized with an acid component, and the amount of the acid component in all monomer components constituting the adhesive polymer is 5% by weight or less, in, The iodine concentration (wt.%) of the polarizing film is taken as the x-axis, the moisture content (g / m 2 ) as the y-axis in an xy orthogonal coordinate system, having an iodine concentration and a water content within the following region, The area is surrounded by a sixth line segment connecting the sixth coordinate point and the second coordinate point, a second line segment connecting the second coordinate point and the third coordinate point, a third line segment connecting the third coordinate point and the fourth coordinate point, a seventh line segment connecting the fourth coordinate point and the seventh coordinate point, and an eighth line segment connecting the sixth coordinate point and the seventh coordinate point. The sixth coordinate point is an iodine concentration of 4.5 wt.% and a moisture content of 2.0 g / m 2 The coordinate point of The second coordinate point is an iodine concentration of 2.2 wt.% and a water content of 3.2 g / m 2 The coordinate point of The third coordinate point is an iodine concentration of 2.2 wt.% and a moisture content of 4.0 g / m 2 The coordinate point of The fourth coordinate point is an iodine concentration of 3.0 wt.% and a water content of 4.0 g / m 2 The coordinate point of The seventh coordinate point is iodine concentration 4.5wt.% and water content 3.3g / m 2 The coordinate point of .

5. The polarizing film laminate according to claim 4, wherein: The sixth coordinate point is an iodine concentration of 4.0 wt.% and a water content of 2.3 g / m 2 The coordinate point of The seventh coordinate point is iodine concentration 4.0wt.% and water content 3.5g / m 2 The coordinate point of .

6. The polarizing film laminate according to claim 4 or 5, wherein: The polarizing film has a thickness of 11 to 20 μm.

7. A polarizing film laminate, comprising a polarizing film containing a polyvinyl alcohol-based resin, and an adhesive layer provided on at least one side of the polarizing film directly or via an optically transparent polarizing film protective film, The adhesive layer comprises an adhesive polymer, the adhesive polymer is copolymerized with an acid component, and the amount of the acid component in all monomer components constituting the adhesive polymer is 5% by weight or less, in, The iodine concentration (wt.%) of the polarizing film is taken as the x-axis, the moisture content (g / m 2 ) as the y-axis, has an iodine concentration and a water content contained in the following area, the area is surrounded by the eleventh line segment connecting the first coordinate point and the eighth coordinate point, the tenth line segment connecting the eighth coordinate point and the ninth coordinate point, the twelfth line segment connecting the ninth coordinate point and the fifth coordinate point, and the fifth line segment connecting the first coordinate point and the fifth coordinate point, The first coordinate point is an iodine concentration of 7.0 wt.% and a water content of 0.7 g / m 2 The coordinate point of The eighth coordinate point has an iodine concentration of 3.3 wt.% and a water content of 2.6 g / m 2 The coordinate point of The ninth coordinate point has an iodine concentration of 6.0 wt.% and a water content of 2.6 g / m 2 The coordinate point of The fifth coordinate point is an iodine concentration of 10.0 wt.% and a water content of 0.7 g / m 2 The coordinate point of .

8. The polarizing film laminate according to claim 7, wherein: The eighth coordinate point is iodine concentration 4.5wt.% and water content 2.0g / m 2 The sixth coordinate point of The ninth coordinate point is an iodine concentration of 7.2 wt.% and a water content of 2.0 g / m 2 The tenth coordinate point.

9. The polarizing film laminate according to claim 7 or 8, wherein: The polarizing film has a thickness of 4 to 11 μm.

10. The polarizing film laminate according to any one of claims 1 to 9, wherein The polarizing film contains zinc.

11. The polarizing film laminate according to any one of claims 1 to 10, wherein For a sample composed of the polarizing film laminate and glass plates laminated on both sides of the polarizing film laminate via an adhesive, the single body transmittance after heating at 95° C. / 500 hours is the same as or greater than the single body transmittance before heating.

12. The polarizing film laminate according to any one of claims 1 to 11, wherein For a sample comprising the polarizing film stack and glass plates laminated on both sides of the polarizing film stack via an adhesive, the change in orthogonal transmittance at a wavelength of 410 nm caused by a heat treatment at 95°C / 500 hours is less than 1%, and the change in orthogonal transmittance at a wavelength of 700 nm is less than 5%.

13. The polarizing film laminate according to any one of claims 1 to 11, wherein For a sample comprising the polarizing film stack and glass plates laminated on both sides of the polarizing film stack via an adhesive, the change in orthogonal transmittance at a wavelength of 410 nm caused by a heat treatment at 95°C / 500 hours is greater than 1%, and the change in orthogonal transmittance at a wavelength of 700 nm is less than 5%.

14. An optical display panel comprising: Optical display unit; The polarizing film laminate according to any one of claims 1 to 13, which is bonded to one surface of the optical display unit directly or via another optical film; and an optically transparent cover plate disposed along the polarizing film laminate on the opposite side of the optical display unit, The optical display unit, the polarizing film stack, and the transparent cover are bonded together by a transparent adhesive layer filled therebetween without any gaps.

15. The optical display panel according to claim 14, wherein: The transparent cover has a function of a capacitive touch sensor.

16. The optical display panel according to claim 15, wherein: An ITO layer serving as a component of a capacitive touch sensor is provided between the transparent cover plate and the polarizing film laminate.

Citation Information

Patent Citations

  • Polarizing plate and method for manufacturing the same

    JP2002090546A

  • Polarizer, polarizing plate and liquid crystal display device

    JP2003029042A

  • Optical adhesive layer, manufacturing method of optical adhesive layer, optical film with adhesive layer, and image display device

    CN109790422A

  • Polarizing plate with adhesive and image display device

    CN110133784A

  • Polarizing plate and image display device, and manufacturing method of those

    JP2014102353A