Large-size resin ultra-thin cutting blade and preparation method thereof

By using the angle structure between the cutting layer and the reinforcing mesh and the untwisted bundled reinforcing mesh in the large-diameter resin cutting piece, combined with the hardening treatment, the problem that the thickness of the large-diameter resin cutting piece is difficult to reach an ultra-thin state is solved, and the The product's flatness and efficient cutting performance reduce material usage and scrap rates.

CN114346920BActive Publication Date: 2024-10-11NINGBO DAHUA GRINDING WHEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111488983.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-08
Publication Date
2024-10-11
Estimated Expiration
2041-12-08

AI Technical Summary

Technical Problem

It is difficult to achieve ultra-thin thickness of large-diameter resin cutting sheets, resulting in uneven products, which seriously limits its use and development.

Method used

A cutting sheet composed of upper and lower cutting layers and a reinforced mesh sheet in the middle is used. The cutting layer and the reinforced mesh sheet are at an angle of 0.25-0.75°. The thickness gradually changes from the center to the edge. An untwisted bundled resin reinforced mesh sheet is used, and Through controlled hardening and cooling treatments, a disc structure with a thick center and thin edges is formed.

Benefits of technology

It effectively reduces the stress of the cutting blade itself, avoids warping and deformation of the grinding wheel, saves materials, improves the sharpness and durability of the cutting blade, and reduces scrap problems caused by warping.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114346920B_ABST
    Figure CN114346920B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of abrasive material, and specifically relates to a large-sized resin ultra-thin cutting blade. The large-sized resin ultra-thin cutting blade of the present invention adopts an untwisted mesh to greatly reduce the stress generated by the cutting blade itself; the present invention changes the flat structure of the cutting blade, adopts a gradual decrease in thickness from the center to the edge to resist the stress generated inside the grinding wheel, and adopts reasonable hardening treatment and cooling to maintain the normal working performance of the cutting blade, while greatly reducing the problem of scrapping the cutting blade caused by warping and unevenness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of abrasive tool materials, and in particular relates to a large-size resin ultra-thin cutting blade and a preparation method thereof. Background Art

[0002] As the country advocates energy conservation and emission reduction, reducing the loss of cutting workpieces and the reduction of cutting blade materials, the development trend of resin cutting blades towards ultra-thin is becoming more and more urgent. The thickness of small-diameter (less than 200mm in diameter) resin cutting blades is less than 1.2mm, but the thickness of large-diameter (200-405mm in diameter) resin cutting blades can only be about 3mm. If the thickness is less than 3mm, it is easy to cause the product to be warped and scrapped, which seriously restricts the use and development of large-diameter resin ultra-thin cutting blades. Therefore, it is urgent to provide a large-size resin ultra-thin cutting blade that can maintain normal working performance. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention provides a large-size resin ultra-thin cutting blade with excellent cutting performance and a flat product without warping.

[0004] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a large-size resin ultra-thin cutting blade, which consists of two upper and lower cutting layers and a reinforcing mesh in the middle. The upper and lower cutting layers have the same thickness. The diameter of the cutting blade is 200-405mm, the thickness of the outer diameter edge is 1-2mm, the thickness of the inner diameter hole of the cutting blade is 2-3mm, and the thickness gradually decreases from the center to the outer edge.

[0005] In the above-mentioned large-size resin ultra-thin cutting blade, the gradual decrease is specifically that the outer surface of the cutting layer and the reinforcing mesh form an angle of 0.25-0.75°. The upper and lower surfaces of the cutting blade of the present invention are changed from the traditional parallel to the outer surface of the cutting layer and the reinforcing mesh form an angle of 0.25-0.75°, and the cutting blade is changed from a traditional parallel disc to a disc with a thick center and thin edges. The thickness of the center of this shape ensures the strength of the cutting blade. The center part is close to the center of the circle and the lever arm is small. Because the moment = force × lever arm, the shrinkage force (stress) generated by the hardening of the material remains unchanged, and the stress moment of the center part is very small. The stress generated by the thin edge due to the decrease in material becomes smaller. Because the lever arm remains unchanged, the stress moment of the outer circle part will become smaller. The strength of the center part can withstand this part of the deformation, so that this shape ensures The grinding wheel does not warp or deform, and at the same time, it largely meets the requirements of reducing the loss of the cut workpiece and the reduction of the material used for the cutting blade. Because during the cutting operation, the workpiece first contacts the outer circumference of the grinding wheel, and the thin outer diameter of the grinding wheel meets the requirement of reducing the loss of the cut workpiece. At the same time, since the thickness of the outer circumference is the smallest and gradually thickens toward the center, it can be seen from the area formula of the circle that the larger the radius, the larger the area. Therefore, although the outer circumference seems to be not much thinner, a large amount of material is saved. The present invention not only saves 15-30% of the material by gradually reducing the thickness from the center to the edge, but also reduces the resistance and improves the sharpness of the cutting blade.

[0006] In the above-mentioned large-size resin ultra-thin cutting blade, a reinforcing hole ring is provided in the center of the cutting blade.

[0007] In the above-mentioned large-size resin ultra-thin cutting blade, the cutting layer includes the following raw materials in percentage by mass: cryolite 10-12%, phenolic resin liquid 5-8%, phenolic resin powder 10-15%, plated brown corundum 15-25%, plated white corundum 25-35%, plated white corundum 15-25%.

[0008] Preferably, the cutting layer comprises the following raw materials in percentage by mass: 11% cryolite, 6% phenolic resin liquid, 13% phenolic resin powder, 20% plated brown corundum, 30% plated white corundum, and 20% plated white corundum.

[0009] Preferably, the particle size of the plated brown corundum is F36.

[0010] Preferably, the particle size of the plated white corundum is F40.

[0011] Preferably, the particle size of the plated white corundum is F46.

[0012] In the above-mentioned large-size resin ultra-thin cutting blade, the reinforced mesh is a twist-free binding resin reinforced mesh. Conventional mesh blanks are twisted for the convenience of weaving. After being twisted, they are made into resin reinforced meshes through a gluing process, and there is residual stress. When used in a resin grinding wheel and hardened through a grinding wheel process, a large stress will be generated, causing the grinding wheel to deform. The present invention avoids the influence of this part of stress by adopting a twist-free binding type.

[0013] The present invention also provides a method for preparing a large-size resin ultra-thin cutting blade, the preparation method comprising the following steps:

[0014] S1. Weigh and mix the cutting layer raw materials for later use;

[0015] S2, putting the mixed cutting layer raw materials into the mold, and flattening them with a scraper to obtain the bottom cutting layer;

[0016] S3, placing a layer of untwisted binding reinforcement mesh on the cutting layer, using a heating device to soften the mesh, and then pressing the mesh;

[0017] S4, putting the cutting layer raw material onto the mesh of S3, and flattening it with a scraper to obtain the top cutting layer;

[0018] S5. After the hole ring is placed, it is pressed into shape, then hardened, and finally cooled to obtain the finished cutting piece.

[0019] Preferably, in step S2, the mold is divided into two surfaces, one surface is concave at the center, and the other surface is horizontal; wherein the angle between the concave surface and the horizontal plane is 0.25-0.75°.

[0020] Preferably, the temperature of the heating device in step S3 is 30-50°C.

[0021] In the above-mentioned large-size resin ultra-thin cutting blade, the specific hardening treatment in step S5 is: first keep warm at 45-55°C for 20-30h, heat up to 95-105°C after 3-5h, keep warm for 1-3h; then keep warm at 110-115°C for 2-4h; then keep warm at 115-125°C for 1-1.5h; then keep warm at 125-135°C for 1-1.5h; then keep warm at 135-145°C for 1-1.5h; finally keep warm at 155-180°C for 3-5h. In order to release the water and ammonia generated by the resin during the hardening process before the cutting blade is completely hardened, and avoid the occurrence of bubbles, the present invention needs to strictly control the hardening temperature.

[0022] In the above-mentioned large-size resin ultra-thin cutting blade, the cooling rate in step S5 is 5-10°C / h. The present invention needs to control the cooling rate to 5-10°C / h, because too fast a cooling rate will cause the cutting blade to deform and the grinding wheel to crack due to temperature difference stress.

[0023] Compared with the prior art, the present invention has the following beneficial effects: the large-size resin ultra-thin cutting blade of the present invention adopts an untwisted mesh to greatly reduce the stress generated by the cutting blade itself; the present invention changes the flat structure of the cutting blade and adopts a gradual decrease in thickness from the center to the edge to resist the stress generated inside the grinding wheel, and adopts reasonable hardening treatment and cooling to maintain the normal working performance of the cutting blade, while greatly reducing the problem of cutting blade scrapping caused by warping and unevenness. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a cross-sectional view of the cutting sheet prepared in Example 1, 1: reinforcing mesh, 2: cutting layer, 3: hole ring. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is further described below through specific embodiments, but the present invention is not limited to these embodiments.

[0026] Example 1

[0027] S1. Weigh and mix the cutting layer raw materials according to the following mass percentages for later use;

[0028] Cryolite 11%, phenolic resin liquid 6%, phenolic resin powder 13%, plated brown corundum 20%, plated white corundum 30%, plated white corundum 20%.

[0029] S2. Put the mixed cutting layer raw materials into the mold and flatten them with a shovel to obtain the bottom cutting layer; the mold is divided into two sides, one side is concave at the center of the circle, and the other side is horizontal; the angle between the concave side and the horizontal plane is 0.5°.

[0030] S3, placing a layer of untwisted binding reinforcement mesh on the cutting layer, using a heating device to soften the mesh, and then pressing the mesh;

[0031] S4, put the cutting layer raw material on the mesh of S3, flatten it with a scraper to get the top cutting layer, put in the hole ring and press it into shape.

[0032] S5. Then carry out hardening treatment: first keep warm at 50℃ for 25h, then heat to 100℃ after 4h, keep warm for 2h; heat to 115℃ after 1h, keep warm for 3h; then keep warm at 120℃ for 1h; then keep warm at 130℃ for 1h; then keep warm at 140℃ for 1.5h; finally keep warm at 165℃ for 4h.

[0033] S6. Finally, the temperature is lowered to room temperature at 8°C / h to obtain a finished cut piece, with the upper and lower surfaces of the cut piece forming an angle of 1.0°.

[0034] Embodiment 2:

[0035] S1. Weigh and mix the cutting layer raw materials according to the following mass percentages for later use;

[0036] Cryolite 11%, phenolic resin liquid 6%, phenolic resin powder 13%, plated brown corundum 20%, plated white corundum 30%, plated white corundum 20%.

[0037] S2. Put the mixed cutting layer raw materials into the mold and flatten them with a shovel to obtain the bottom cutting layer; the mold is divided into two sides, one side is concave at the center of the circle, and the other side is horizontal; the angle between the concave side and the horizontal plane is 0.25°.

[0038] S3, placing a layer of untwisted binding reinforcement mesh on the cutting layer, using a heating device to soften the mesh, and then pressing the mesh;

[0039] S4, put the cutting layer raw material on the mesh of S3, flatten it with a scraper to get the top cutting layer, put in the hole ring and press it into shape.

[0040] S5. Then carry out hardening treatment: first keep warm at 45℃ for 20h, raise the temperature to 95℃ after 3h, keep warm for 1h; then keep warm at 110℃ for 2h; then keep warm at 115℃ for 1h; then keep warm at 125℃ for 1h; then keep warm at 135℃ for 1h; finally keep warm at 155℃ for 3h.

[0041] S6. Finally, the temperature is lowered to room temperature at 5°C / h to obtain a finished cut piece. The upper and lower surfaces of the cut piece form an angle of 0.5° with the horizontal line.

[0042] Embodiment 3:

[0043] S1. Weigh and mix the cutting layer raw materials according to the following mass percentages for later use;

[0044] Cryolite 11%, phenolic resin liquid 6%, phenolic resin powder 13%, plated brown corundum 20%, plated white corundum 30%, plated white corundum 20%.

[0045] S2. Put the mixed cutting layer raw materials into the mold and flatten them with a shovel to obtain the bottom cutting layer; the mold is divided into two sides, one side is concave at the center of the circle, and the other side is horizontal; the angle between the concave side and the horizontal plane is 0.75°.

[0046] S3, placing a layer of untwisted binding reinforcement mesh on the cutting layer, using a heating device to soften the mesh, and then pressing the mesh;

[0047] S4, put the cutting layer raw material on the mesh of S3, flatten it with a scraper to get the top cutting layer, put in the hole ring and press it into shape.

[0048] S5. Then carry out hardening treatment: first keep warm at 55°C for 30 hours, raise the temperature to 105°C after 5 hours, and keep warm for 3 hours; then keep warm at 115°C for 4 hours; then keep warm at 125°C for 1.5 hours; then keep warm at 135°C for 1.5 hours; then keep warm at 145°C for 1.5 hours; finally keep warm at 180°C for 5 hours.

[0049] S6. Finally, the temperature is lowered to room temperature at 10°C / h to obtain a finished cut piece. The upper and lower surfaces of the cut piece form an angle of 1.5° with the horizontal line.

[0050] Embodiment 4:

[0051] The only difference from Example 1 is that the hardening treatment in step S5 is: first keep warm at 45°C for 2 hours, heat to 105°C after 1 hour, and keep warm for 0.5 hours; heat to 125°C after 0.5 hours, and then keep warm at 125°C for 0.5 hours; then keep warm at 125-135°C for 1-1.5 hours; then keep warm at 135-145°C for 1-1.5 hours; finally keep warm at 155-180°C for 3-5 hours.

[0052] Embodiment 5:

[0053] The only difference from Example 1 is that step S6 is to cool down to room temperature at a rate of 50° C. / h.

[0054] Embodiment 6:

[0055] The only difference from Example 1 is that the included angle between the inner concave surface of the mold and the horizontal plane is 0.02° to obtain the cutting blade.

[0056] Embodiment 7:

[0057] The only difference from Example 1 is that the middle mesh is a twisted resin reinforced mesh.

[0058] Comparative Example 1:

[0059] The only difference from Example 1 is that the thickness of the cutting piece remains constant at 2 mm from the center to the edge.

[0060] Comparative Example 2:

[0061] The only difference from Example 1 is that the thickness of the cutting blade remains constant at 3 mm from the center to the edge.

[0062] To ensure the accuracy of the data, the same specifications of cutting discs were uniformly made: outer diameter 355mm, thickness at the inner diameter hole 2mm, and hole ring diameter 25.4mm; the outer diameter of the cutting disc of comparative example 2 was 355mm, thickness at the inner diameter hole 3mm, and hole ring diameter 25.4mm. All used were Hitachi brand, 3000W power, and 3800r / min two-phase cutting machines. The steel cut was 25mm diameter solid round steel (45#), and each grinding wheel cut a maximum of 10 times.

[0063] Table 1: Performance test results of cutting blades prepared in Examples 1-6 and Comparative Examples 1-3

[0064] Example Appearance Cutting ratio Cutting efficiency Example 1 normal 1.1 16 seconds Example 2 normal 1.05 15 seconds Example 3 normal 0.9 14 seconds Example 4 Foaming Cannot be used Cannot be used Example 5 Warping, unevenness and deformation Cannot be used Cannot be used Example 6 Warping, unevenness and deformation Cannot be used Cannot be used Example 7 Warping, unevenness and deformation Cannot be used Cannot be used Comparative Example 1 Warping, unevenness and deformation Cannot be used Cannot be used Comparative Example 2 normal 0.6 21 seconds

[0065] Cutting ratio: the ratio of workpiece area loss to grinding wheel area loss. The higher the ratio, the more durable it is.

[0066] Cutting efficiency: The average time taken to cut a workpiece once, the shorter the better.

[0067] Figure 1 This is a cross-sectional view of the cutting blade prepared in Example 1, 1: reinforcing mesh, 2: cutting layer, 3: hole ring. The upper and lower surfaces of the cutting blade are changed from being parallel to each other in the traditional way, so that the outer surface of the cutting layer and the reinforcing mesh form an angle of 0.5°, and the cutting blade is changed from a traditional parallel disc to a disc with a thick center and a thin edge. This shape ensures that the grinding wheel does not warp and deform, and at the same time largely meets the requirements of reducing the loss of the cutting workpiece and reducing the material used for the cutting blade.

[0068] It can be seen from the above results that the present invention uses an untwisted mesh to greatly reduce the stress generated by the cutting blade itself; the present invention changes the flat structure of the grinding wheel and adopts a gradual decrease in thickness from the center to the edge to resist the stress generated inside the grinding wheel, thereby greatly reducing the scrapping caused by warping and unevenness of the product.

[0069] The parts of the technical scope of the present invention that are not exhausted by the midpoint value of the embodiment and the new technical solutions formed by the equivalent replacement of single or multiple technical features in the technical solutions of the embodiments are also within the scope of protection claimed by the present invention, and unless otherwise specified, there is no unique and irreplaceable combination between all the parameters involved in the solutions of the present invention.

[0070] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

[0071] Although the present invention has been described in detail and some specific embodiments have been cited, it is obvious to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention.

Claims

1. A large-size resin ultra-thin cutting blade, It is characterized in that The cutting blade consists of two cutting layers and a reinforcing mesh in the middle. The thickness of the two cutting layers is the same. The diameter of the cutting blade is 200-405mm, the thickness of the outer edge is 1-2mm, and the thickness of the inner hole of the cutting blade is 2-3mm. The thickness decreases gradually from the center to the outer edge. The gradual decrease is specifically that the outer surface of the cutting layer and the reinforcing mesh form an angle of 0.5°; A reinforcing ring is provided in the center of the cutting disc, and the diameter of the ring is 16-32mm; The cutting layer includes the following raw materials in percentage by mass: 11% cryolite, 6% phenolic resin liquid, 13% phenolic resin powder, 20% plated brown corundum, 30% first plated white corundum, and 20% second plated white corundum; The reinforcement mesh is a twist-free binding reinforcement mesh; The method for preparing the large-size resin ultra-thin cutting blade comprises the following steps: S1. Weigh and mix the cutting layer raw materials for later use; S2, putting the mixed cutting layer raw materials into the mold, and flattening them with a scraper to obtain the bottom cutting layer; S3, placing a layer of untwisted binding reinforcement mesh on the cutting layer, using a heating device to soften the mesh, and then pressing the mesh; S4, putting the cutting layer raw material onto the mesh of S3, and flattening it with a scraper to obtain the top cutting layer; S5. After the hole ring is placed, it is pressed into shape, and then hardened. Finally, the temperature is cooled to room temperature at 8°C / h to obtain a finished cutting piece. The upper and lower surfaces of the cutting piece are at an angle of 1.0°. The hardening treatment is specifically as follows: first keep warm at 50°C for 25 hours, then heat to 100°C after 4 hours, and keep warm for 2 hours; heat to 115°C after 1 hour, and keep warm for 3 hours; then keep warm at 120°C for 1 hour; then keep warm at 130°C for 1 hour; then keep warm at 140°C for 1.5 hours; finally keep warm at 165°C for 4 hours.