Electro-optical crystal film, preparation method and electronic component

By performing two ion implantations and heat treatment in the film matrix, an electro-optical crystal film is formed, which solves the problem of damage to the lithium niobate film layer caused by the etching method, improves the accuracy of the optical waveguide structure and the etching efficiency of the film material, and ensures performance of electronic devices.

CN114355635BActive Publication Date: 2024-10-29JINAN JINGZHENG ELECTRONICS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210049833.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-17
Publication Date
2024-10-29
Estimated Expiration
2042-01-17

AI Technical Summary

Technical Problem

In the prior art, when etching methods are used to prepare optical waveguide structures, damage is caused to the lithium niobate thin film layer, affecting the performance of electronic devices.

Method used

Using two ion implantation methods, the first implantation layer and the second implantation layer are formed in the film matrix, and they are separated through heat treatment to form an electro-optical crystal film to avoid damage during the etching process, and the implantation depth is controlled by ion implantation energy. Improve the accuracy of optical waveguide structures.

Benefits of technology

It successfully avoids damage to the thin film layer caused by the etching method, improves the accuracy of the optical waveguide structure and the etching efficiency of the thin film material, and ensures the performance of the electronic device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114355635B_ABST
    Figure CN114355635B_ABST
Patent Text Reader

Abstract

The present application provides an electro-optical crystal film, a preparation method and an electronic component, wherein a first mask is prepared on a film substrate; a first ion is injected into the film substrate to form a first injection layer in the film substrate; the first mask is removed; a second mask is prepared on the film substrate, the pattern of the second mask is opposite to the pattern of the first mask; a second ion is injected into the film substrate to form a second injection layer in the film substrate, the pattern of the second injection layer is the same as the first mask; the second mask is removed; the film substrate is bonded to a supporting substrate to obtain a bonded body; the bonded body is heat-treated to separate the film substrate at the first injection layer and the second injection layer to obtain an electro-optical crystal film. After two ion injections and stripping off the residual layer, an electro-optical crystal film with an optical waveguide structure can be obtained, which can avoid the damage to the film layer caused by the etching method for preparing the optical waveguide structure, and can also avoid the problem of low etching efficiency of the film material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of semiconductor technology, and in particular relates to an electro-optical crystal film, a preparation method and an electronic component. Background Art

[0002] Electro-optical crystal materials such as lithium niobate or lithium tantalate are widely used in nonlinear optics, ferroelectrics, piezoelectrics, electro-optics and other fields due to their advantages such as high Curie temperature, strong spontaneous polarization, high electromechanical coupling coefficient, and excellent electro-optical effect. They are particularly gaining more and more attention and application in the fields of thin-film bulk acoustic wave devices, filters, and optical modulators. If electro-optical crystal materials such as lithium niobate or lithium tantalate are used to prepare optical modulators, the lithium niobate film needs to be further prepared into the required optical waveguide structure, and then the high refractive index difference between the lithium niobate film and silicon dioxide is used to confine the light in the lithium niobate film layer.

[0003] At present, the method of preparing lithium niobate film into the required optical waveguide structure mainly includes the following steps: first, preparing a substrate layer, an isolation layer and a lithium niobate film layer stacked in sequence, and then etching the lithium niobate film into the required optical waveguide structure using an etching method, wherein commonly used lithium niobate etching methods include wet etching, dry etching, FIB (focused ion beam) etching and other methods.

[0004] However, since lithium niobate and lithium tantalate have very stable physical and chemical properties, etching on the thin film layer is very difficult and may cause certain damage to the thin film layer, thereby affecting the performance of the applied electronic devices. Summary of the invention

[0005] In order to solve the problem in the prior art that the etching method is used to prepare the optical waveguide structure, which will cause certain damage to the thin film layer, thereby affecting the performance of the applied electronic devices, the present application provides an electro-optical crystal film, a preparation method and an electronic component.

[0006] In a first aspect, the present application provides a method for preparing an electro-optical crystal thin film, comprising:

[0007] preparing a supporting substrate and a film substrate;

[0008] Prepare a first mask on the first surface of the thin film substrate, wherein the first mask has a pattern that is the same as or opposite to that of the target optical waveguide structure;

[0009] Implanting first ions into a region on the first surface of the thin film substrate that is not covered by the first mask to form a first implantation layer in the thin film substrate, wherein a pattern of the first implantation layer is opposite to that of the first mask;

[0010] removing the first mask;

[0011] Preparing a second mask on the first surface or the second surface of the thin film substrate, wherein a pattern of the second mask is opposite to that of the first mask;

[0012] Implanting second ions into an area on the surface of the thin film substrate on which the second mask is prepared and not covered by the second mask, to form a second injection layer in the thin film substrate, wherein the pattern of the second injection layer is the same as that of the first mask, wherein the distance difference between the first injection layer and the second injection layer is the same as the height of the target optical waveguide structure;

[0013] removing the second mask;

[0014] Bonding the film substrate to the support substrate to obtain a bonded body;

[0015] The bonded body is heat treated to separate the thin film substrate at the first injection layer and the second injection layer to obtain an electro-optical crystal thin film, wherein the electro-optical crystal thin film includes a supporting substrate, a thin film layer formed on the supporting substrate, and the target optical waveguide structure integrally formed on the thin film layer.

[0016] In one implementation, if the distance difference between the second injection layer and the first surface of the thin film substrate is greater than or equal to the distance difference between the second injection layer and the second surface of the thin film substrate, the second injection layer is formed by preparing a second mask on the second surface of the thin film substrate and injecting second ions into the area on the second surface of the thin film substrate that is not covered by the second mask.

[0017] In one implementation, if the distance difference between the second injection layer and the first surface of the thin film substrate is less than or equal to the distance difference between the second injection layer and the second surface of the thin film substrate, the second injection layer is formed by preparing a second mask on the first surface of the thin film substrate and injecting second ions into the area on the first surface of the thin film substrate that is not covered by the second mask.

[0018] In an implementable manner, if the distance between the first injection layer and the first surface of the thin film substrate is equal to the thickness of the thin film layer, the bonding body is obtained by bonding the first surface of the thin film substrate to the supporting substrate.

[0019] In an implementable manner, if the distance between the second injection layer and the second surface of the thin film substrate is equal to the thickness of the thin film layer, the bonding body is obtained by bonding the second surface of the thin film substrate to the supporting substrate.

[0020] In an implementable manner, the distance difference between the first injection layer and the second injection layer is 50-1000 nm.

[0021] In one achievable manner, the first ion and the second ion are the same as or different from each other.

[0022] In one implementation, the first ions are helium ions, hydrogen ions, nitrogen ions, oxygen ions, or argon ions, and the second ions are helium ions, hydrogen ions, nitrogen ions, oxygen ions, or argon ions.

[0023] In a second aspect, the present application provides an electro-optical crystal film, which is prepared using any method for preparing an electro-optical crystal film described in the first aspect.

[0024] In a third aspect, the present application provides an electronic component, wherein the electronic component includes the electro-optical crystal thin film described in the second aspect.

[0025] In summary, the present application provides an electro-optical crystal film, a preparation method and an electronic component. Through two ion implantations with different implantation depths, an electro-optical crystal film with an optical waveguide structure can be obtained after stripping off the residual layer. This can avoid damage to the film layer caused by the etching method in preparing the optical waveguide structure, and can also avoid the problem of low etching efficiency of the film material. In addition, the present application can also control the ion implantation depth by the ion implantation energy, thereby improving the accuracy of the prepared optical waveguide structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 A schematic diagram of the structure of an electro-optical crystal film provided in an embodiment of the present application;

[0028] Figure 2 A flow chart of a method for preparing an electro-optical crystal thin film provided in an embodiment of the present application;

[0029] Figure 3 A schematic diagram of a structure with a second mask provided in an embodiment of the present application;

[0030] Figure 4 A schematic diagram of another structure with a second mask provided in an embodiment of the present application;

[0031] Figure 5A schematic diagram of the positional relationship between a first injection layer and a second injection layer provided in an embodiment of the present application;

[0032] Figure 6 A schematic diagram of the positional relationship between another first injection layer and a second injection layer provided in an embodiment of the present application.

[0033] Description of Reference Numerals

[0034] 10-film substrate, 20-support substrate, 30-first mask, 40-second mask, 50-bonding body;

[0035] 110 - first injection layer, 120 - second injection layer, 130 - thin film layer, 140 - optical waveguide structure, 150 - residual material layer. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.

[0037] To facilitate understanding of a method for preparing an electro-optical crystal film provided in an embodiment of the present application, the structure of the electro-optical crystal film is first introduced.

[0038] like Figure 1 As shown, the electro-optical crystal film prepared by the present application comprises a supporting substrate 20 , a thin film layer 130 formed on the supporting substrate 20 , and an optical waveguide structure 140 integrally formed on the thin film layer 130 .

[0039] It should be noted that if Figure 1 As shown, the present application refers to the structure protruding from the thin film layer 130 as an optical waveguide structure 140 , wherein the optical waveguide structure 140 is arranged in an array on the surface of the thin film layer 130 .

[0040] In the prior art, the method of obtaining the thin film layer 130 and the optical waveguide structure 140 by etching the thin film substrate 10 (the thin film substrate 10 refers to a basic material with a certain thickness for obtaining the thin film layer 130 and the optical waveguide structure 140) will cause certain damage to the thin film layer 130, thereby affecting the performance of the applied electronic device. In order to solve this technical problem, the present application provides a method for preparing an electro-optical crystal thin film.

[0041] The method for preparing the electro-optical crystal film provided in the present application prepares the desired thin film layer 130 and optical waveguide structure 140 in the thin film substrate 10 by means of two ion implantations. This preparation method does not require etching of the thin film substrate 10 and will not cause damage to the thin film layer.

[0042] A method for preparing an electro-optical crystal thin film provided in an embodiment of the present application is described in detail below in conjunction with the accompanying drawings.

[0043] like Figure 2 As shown, the present application provides a method for preparing an electro-optical crystal thin film, comprising the following steps:

[0044] Step 100 : preparing a film substrate 10 and a supporting substrate 20 .

[0045] The embodiment of the present application does not limit the material of the thin film substrate 10, as long as it can form a three-layer structure of a thin film layer, a separation layer and a residual layer by an ion implantation method, and then can prepare the thin film layer by bonding, heating and separation. For example, the thin film substrate 10 can be a crystalline material such as lithium niobate, lithium tantalate, potassium titanyl phosphate (also called KTP), rubidium titanyl phosphate (also called RTP), etc.

[0046] The support substrate 20 may be a single-layer substrate or a composite substrate, that is, the support substrate 20 includes at least one substrate layer. The material of each substrate layer may be the same or different, and this application does not limit this. For example, the substrate layer material may be silicon, lithium niobate, SOI, molten SOI, sapphire, lithium tantalate, etc., and this application does not limit this. The substrate layer material may be the same or different from the material of the film substrate 10.

[0047] Step 200 : preparing a first mask 30 on a first surface of a thin film substrate 10 . The pattern of the first mask 30 is the same as or opposite to that of a target optical waveguide structure.

[0048] First, it should be noted that the target optical waveguide structure in the embodiment of the present application refers to the optical waveguide structure in the electro-optical crystal film prepared by the target, for example Figure 1 The optical waveguide structure 140 is shown in FIG.

[0049] It should also be noted that the first mask 30 and the target optical waveguide structure have the same pattern, which can be understood as: the projection of the target optical waveguide structure on the first surface of the thin film substrate 10 is the same as the pattern covered by the first mask 30 on the first surface; the first mask 30 and the target optical waveguide structure have opposite patterns, which can be understood as: the projection of the target optical waveguide structure on the first surface of the thin film substrate 10 and the pattern covered by the first mask 30 on the first surface can just form a complete first surface.

[0050] Among them, the first surface of the film substrate 10 can be the top surface or the bottom surface of the film substrate, which is not limited in the present application. For the convenience of description, the first surface of the film substrate 10 is referred to as the A surface of the film substrate 10 below.

[0051] Step 300 , first ions are implanted into the area on the A surface of the thin film substrate 10 that is not covered by the first mask 30 to form a first implantation layer 110 in the thin film substrate 10 . The pattern of the first implantation layer 110 is opposite to that of the first mask 30 .

[0052] like Figure 2 As shown, first ions are injected into the thin film substrate 10 in the exposed area of ​​the A surface of the thin film substrate 10, and the injected first ions form a first injection layer 110 in the thin film substrate 10. Wherein, due to the shielding of the first mask 30, the area in the layer where the first injection layer 110 is located corresponding to the first mask 30 is not injected with the first ions, and therefore, the pattern of the formed first injection layer 110 is opposite to that of the first mask 30.

[0053] It should be noted that the first ions in the present application are ions that can generate gas through heat treatment, for example, they can be helium ions, hydrogen ions, nitrogen ions, oxygen ions or argon ions.

[0054] The present application can control the position of the first implantation layer 110 in the film substrate 10 by adjusting the implantation dose and energy of the first ions.

[0055] It should also be noted that when the first ions are injected, the ion beam is injected vertically into the film substrate 10 , so that a regular first injection layer 110 can be formed in the film substrate 10 and aligned with the area not covered by the first mask 30 .

[0056] Step 400 : removing the first mask 30 .

[0057] The embodiment of the present application does not limit the method for removing the first mask 30. For example, if the material of the first mask 30 is photoresist, the first mask 30 can be dissolved by an acetone solution; for another example, if the material of the first mask 30 is silicon oxide, silicon nitride, aluminum oxide, silicon carbide or aluminum nitride, the first mask 30 can be removed by dry etching or wet etching.

[0058] Step 500 : preparing a second mask 40 on the first surface (surface A) or the second surface (surface B) of the film substrate 10 , wherein the pattern of the second mask 40 is opposite to the pattern of the first mask 30 .

[0059] Step 600, injecting second ions into the area on the surface of the thin film substrate 10 prepared with the second mask 40 and not covered by the second mask 40, so as to form a second injection layer 120 in the thin film substrate 10, wherein the pattern of the second injection layer 120 is the same as that of the first mask 30, wherein the distance difference between the first injection layer 110 and the second injection layer 120 is the same as the height of the target optical waveguide structure.

[0060] First, the second surface of the film substrate 10 is a surface opposite to the first surface. For the sake of distinction, the second surface of the film substrate 10 is referred to as the B surface of the film substrate 10 hereinafter.

[0061] Secondly, the second ion is also an ion that can generate a gas through heat treatment, for example, it can be a helium ion, a hydrogen ion, a nitrogen ion, an oxygen ion or an argon ion. Among them, the second ion can be selected from the same or different ions as the first ion. The present application can control the position of the second injection layer 120 in the film substrate 10 by adjusting the injection dose and energy of the second ion.

[0062] In step 500, the second mask 40 can be prepared on the A surface of the film substrate 10, or on the B surface of the film substrate 10, which is not limited in the present application. In order to form the second injection layer 120 in the film substrate 10 more efficiently, it can be determined whether to prepare the second mask 40 on the A surface or the B surface of the film substrate 10 according to the position of the second injection layer 120 to be formed in the film substrate 10.

[0063] like Figure 3 As shown, if the position of the second injection layer 120 formed in the thin film substrate 10 in step 600 satisfies: the distance difference d1 between the second injection layer 120 and the A surface of the thin film substrate is greater than or equal to the distance difference d2 between the second injection layer 120 and the B surface of the thin film substrate, then in step 500, a second mask 40 can be prepared on the B surface of the thin film substrate 10, and then, second ions are injected from the area of ​​the B surface of the thin film substrate 10 that is not covered by the second mask 40 to form the second injection layer 120 in the thin film substrate 10.

[0064] like Figure 4 As shown, if the position at which the second injection layer 120 is formed in the thin film substrate 10 in step 600 satisfies: the distance difference d1 between the second injection layer 120 and the A surface of the thin film substrate is less than or equal to the distance difference d2 between the second injection layer 120 and the B surface of the thin film substrate, then in step 500, a second mask 40 can be prepared on the A surface of the thin film substrate 10, and then, second ions are injected into the area of ​​the A surface of the thin film substrate 10 that is not covered by the second mask 40 to form the second injection layer 120 in the thin film substrate 10.

[0065] It should be noted that, due to the obstruction of the second mask 40, the area in the layer where the second injection layer 120 is located that corresponds to the second mask 40 is not injected with the second ions. Therefore, the pattern of the formed second injection layer 120 is opposite to that of the second mask 40. Since the pattern of the second mask 40 is opposite to that of the first mask 30, the first ions and the second ions are alternately injected into the thin film substrate 10, thereby forming the first injection layer 110 and the second injection layer 120 without overlapping areas in the thin film substrate 10, that is, the second injection layer 120 finally formed in the thin film substrate has the opposite pattern to that of the first injection layer 110.

[0066] It should be understood that the first injection layer 110 and the second injection layer 120 of the present application are not on the same layer, that is, there is a certain distance difference between the first injection layer 110 and the second injection layer 120. The distance difference between the first injection layer 110 and the second injection layer 120 is the same as the height of the target optical waveguide structure, so that in step 900, the structure identical to the target optical waveguide structure can be peeled off from the film substrate 10 by heat treatment.

[0067] It should also be noted that when the second ions are injected, the ion beam is injected vertically into the film substrate 10 , so that a regular second injection layer 120 aligned with the area not covered by the second mask 40 can be formed in the film substrate 10 .

[0068] Step 700 : removing the second mask 40 .

[0069] The embodiment of the present application does not limit the method for removing the second mask 40. For example, if the material of the second mask 40 is photoresist, the second mask 40 can be dissolved by an acetone solution; for another example, if the material of the second mask 40 is silicon oxide, silicon nitride, aluminum oxide, silicon carbide or aluminum nitride, the second mask 40 can be removed by dry etching or wet etching.

[0070] Step 800 , bonding the film substrate 10 to the support substrate 20 to obtain a bonded body 50 .

[0071] In one implementation, Figure 5 As shown, if the distance D1 between the first injection layer 110 and the A surface of the film substrate 10 is equal to the thickness of the film layer 130 in the target electro-optical crystal film, the bonding body 50 is obtained by bonding the A surface of the film substrate 10 to the supporting substrate 20 .

[0072] In another implementation, Figure 6 As shown, if the distance D2 between the second injection layer 120 and the B surface of the film substrate 10 is equal to the thickness of the film layer 130 in the target electro-optical crystal film, the bonding body 50 is bonded to the support substrate 20 through the B surface of the film substrate 10 .

[0073] In the embodiment of the present application, the bonding body 50 refers to a bonding body formed after the processed film substrate 10 is bonded to the supporting substrate 20 , wherein the processed film substrate 10 is not peeled off from the supporting substrate 20 .

[0074] The present application does not particularly limit the method for bonding the treated film substrate 10 to the supporting substrate 20. Any method for bonding the treated film substrate to the supporting substrate 20 in the prior art can be adopted. For example, the bonding surface (surface A or surface B) of the treated film substrate 10 is surface activated, and the bonding surface of the supporting substrate 20 is also surface activated, and then the two activated surfaces are bonded to obtain a bonded body 50.

[0075] The present application does not make any special limitation on the method for surface activation of the bonding surface of the treated film substrate 10, and any method in the prior art can be used to surface activate the bonding surface of the treated film substrate 10, such as plasma activation and chemical solution activation. Similarly, the present application does not make any special limitation on the method for surface activation of the bonding surface of the supporting substrate 20, and any method in the prior art that can be used for surface activation of the bonding surface of the supporting substrate 20 can be used, such as plasma activation.

[0076] Step 900, heat-treating the bonding body 50 to separate the film substrate 10 at the first injection layer 110 and the second injection layer 120 to obtain an electro-optical crystal film, wherein the electro-optical crystal film includes a supporting substrate 20, a thin film layer 130 formed on the supporting substrate 20, and an optical waveguide structure 140 integrally formed on the thin film layer 130.

[0077] The present application performs a heat treatment on the bonding body 50, and the heat treatment temperature can be 100°C to 600°C. During the heat treatment, bubbles are formed in the first injection layer 110 and the second injection layer 120. For example, H ions form hydrogen, and He ions form helium. As the heat treatment progresses, the bubbles in the first injection layer 110 are connected together, and the bubbles in the second injection layer 120 are connected together; finally, the area on the layer where the first injection layer 110 is located and the area on the layer where the second injection layer 120 is located and the area on the layer where the second injection layer 120 is located and the second ion is injected is cracked. In this way, after the heat treatment, the first injection layer 110 and the second injection layer 120 can separate the thin film substrate 10 into two parts, such as Figure 2 As shown, a portion remains on the supporting substrate 20 , which portion includes a thin film layer 130 and an optical waveguide structure 140 , wherein the thin film layer 130 and the optical waveguide structure 140 are an integrally formed structure; the other portion is peeled off from the supporting substrate 20 , which may be referred to as a residual layer 150 .

[0078] It should be noted that, when the distance difference between the first injection layer 110 and the second injection layer 120 is 50-1000 nm, the residual layer 150 can be well peeled off from the support substrate 20. For example, the residual layer 150 and the film layer 130 can be pulled in opposite directions by a mechanical separation device, so as to peel off the residual layer 150 from the support substrate 20; for another example, the residual layer 150 can be peeled off from the support substrate 20 manually.

[0079] In summary, the method for preparing the electro-optical crystal film provided in the embodiment of the present application can obtain an electro-optical crystal film with an optical waveguide structure after stripping off the residual layer through two ion implantations with different implantation depths. This can avoid damage to the film layer caused by the etching method in preparing the optical waveguide structure, and can also avoid the problem of low etching efficiency of the film material. In addition, the present application can also control the ion implantation depth by means of ion implantation energy, thereby improving the accuracy of the prepared optical waveguide structure.

[0080] The embodiment of the present application also provides an electronic component, which includes an electro-optical crystal film prepared by the preparation method provided in the embodiment of the present application. For example, the electro-optical crystal film in the above embodiment is applied to electronic devices such as thin film bulk acoustic wave devices, filters, and modulators. Specifically, the sizes of the supporting substrate 20, the thin film layer 130, and the optical waveguide structure 140 in the electro-optical crystal film can be prepared according to the needs of the electronic device.

[0081] The thickness of the thin film layer 130 refers to the thickness of the thin film that completely covers the support substrate 20 in the electro-optical crystal thin film. Figure 1 The mark h1 shown in the figure; the height of the optical waveguide structure 140 refers to the height of the optical waveguide structure in a direction perpendicular to the bonding surface of the thin film layer 130 and the supporting substrate 20, such as Figure 1 The tag h2 is shown in FIG.

[0082] Several examples of preparing electro-optical crystal thin films using the preparation method provided in the embodiments of the present application are listed below.

[0083] Example 1

[0084] (1) A Si wafer having a size of 4 inches, a thickness of 0.5 mm and a smooth surface was prepared.

[0085] (2) The Si wafer obtained above was cleaned and an isolation layer was deposited. The deposition material was SiO2 and the deposition thickness was 100 nm.

[0086] (3) A lithium niobate wafer with a size of 4 inches, a thickness of 0.5 mm and a smooth surface is prepared and cleaned, and a first mask with the same pattern as the target waveguide structure array is prepared on the lithium niobate wafer. Argon ions are implanted into the lithium niobate wafer by an ion implantation method. The implantation energy of the argon ions is 120 KeV and the dose is 4E 16 ions / cm 2 A first injection layer is formed in the area of ​​the lithium niobate wafer that is not covered by the first mask.

[0087] (4) Remove the first mask.

[0088] (5) A second mask having a pattern opposite to that of the target waveguide structure array is prepared on the lithium niobate wafer, and helium ions are implanted into the lithium niobate wafer by ion implantation. The implantation energy of the helium ions is 250 KeV and the dose is 4E 16 ions / cm 2 , forming a second injection layer in the area of ​​the lithium niobate wafer not covered by the second mask; removing the second mask;

[0089] At this time, a residual layer, a first injection layer, a second injection layer and a thin film layer with an optical waveguide structure are formed in the lithium niobate wafer injection piece.

[0090] (6) The thin film layer with an optical waveguide structure of the lithium niobate wafer injection piece is bonded to the silicon dioxide layer on the Si wafer by a plasma bonding method to form a bonded body; the bonded body is then placed in a heating device for heat preservation at a high temperature until the residual layer is separated from the bonded body to form a lithium niobate electro-optical crystal thin film with an optical waveguide structure.

[0091] The insulation process is carried out in a vacuum environment or in a protective atmosphere formed by at least one of nitrogen and inert gases, with a insulation temperature of 400°C and a insulation time of 3 hours. This step can increase the bonding force by more than 10 MPa and can restore the damage to the thin film layer caused by ion implantation, so that the obtained lithium niobate thin film layer with an optical waveguide structure has properties close to those of a lithium niobate wafer.

[0092] In the lithium niobate electro-optical crystal thin film prepared in Example 1, the thickness h1 of the thin film layer is 87 nm, and the height h2 of the optical waveguide structure on the thin film layer is 743 nm.

[0093] Example 2

[0094] (1) A lithium niobate wafer having a size of 4 inches, a thickness of 0.5 mm and a smooth surface is prepared.

[0095] (2) The lithium niobate wafer obtained above is cleaned and an isolation layer is deposited. The deposition material is SiO2 and the deposition thickness is 100 nm.

[0096] (3) A lithium niobate wafer with a size of 4 inches, a thickness of 0.5 mm and a smooth surface is prepared and cleaned, and a first mask with the same pattern as the target waveguide structure array is prepared on the lithium niobate wafer. Oxygen ions are implanted into the lithium niobate wafer by ion implantation. The implantation energy of the oxygen ions is 150 KeV and the dose is 2E 16 ions / cm 2 A first injection layer is formed in the area of ​​the lithium niobate wafer that is not covered by the first mask.

[0097] (4) removing the first mask;

[0098] (5) A second mask having a pattern opposite to that of the target waveguide structure array is prepared on the lithium niobate wafer, and hydrogen ions are implanted into the lithium niobate wafer by ion implantation. The hydrogen ion implantation energy is 180 KeV and the dose is 2E 16 ions / cm 2 , forming a second injection layer in the area of ​​the lithium niobate wafer not covered by the second mask; removing the second mask;

[0099] At this time, a residual layer, a first injection layer, a second injection layer and a thin film layer with an optical waveguide structure are formed in the lithium niobate wafer injection piece.

[0100] (6) The waveguide structure thin film layer of the lithium niobate wafer injection piece is bonded to the silicon dioxide layer on the lithium niobate wafer by a plasma bonding method to form a bonded body, and then the bonded body is placed in a heating device for heat preservation at a high temperature until the residual layer is separated from the bonded body to form a lithium niobate electro-optical crystal film with an optical waveguide structure.

[0101] The insulation process is carried out in a vacuum environment or in a protective atmosphere formed by at least one of nitrogen and inert gases, with an insulation temperature of 100°C and an insulation time of 48 hours. This step can increase the bonding force by more than 10 MPa and can restore the damage to the thin film layer caused by ion implantation, so that the obtained lithium niobate thin film layer with an optical waveguide structure has properties close to those of a lithium niobate wafer.

[0102] In the lithium niobate electro-optical crystal thin film prepared in Example 2, the thickness h1 of the thin film layer is 239 nm, and the height h2 of the optical waveguide structure on the thin film layer is 811 nm.

[0103] Example 3

[0104] (1) A Si wafer having a size of 6 inches, a thickness of 0.5 mm and a smooth surface was prepared.

[0105] (2) The Si wafer obtained above was cleaned and an isolation layer was deposited. The deposition material was SiO2 and the deposition thickness was 100 nm.

[0106] (3) A lithium tantalate wafer with a size of 6 inches, a thickness of 0.5 mm and a smooth surface is prepared and cleaned, and a first mask with the same pattern as the target waveguide structure array is prepared on the lithium tantalate wafer. Nitrogen ions are implanted into the lithium tantalate wafer by ion implantation. The implantation energy of the nitrogen ions is 110 KeV and the dose is 4E 16 ions / cm 2 A first injection layer is formed in the area covered by the first mask on the surface of the lithium tantalate wafer.

[0107] (4) Remove the first mask.

[0108] (5) A second mask with a pattern opposite to the target waveguide structure array is prepared on the lithium tantalate wafer, and helium ions (He+) are implanted into the lithium tantalate wafer using an ion implantation method. The implantation energy of the helium ions is 275 KeV and the dose is 4E 16 ions / cm 2 , forming a second injection layer in the area of ​​the lithium tantalate wafer not covered by the second mask; removing the second mask;

[0109] At this time, a residual layer, a first injection layer, a second injection layer and a thin film layer with an optical waveguide structure are formed in the lithium tantalate wafer injection piece.

[0110] (6) The waveguide structure thin film layer of the lithium tantalate wafer injection piece is bonded to the silicon dioxide layer on the Si wafer by a plasma bonding method to form a bonded body, and then the bonded body is placed in a heating device for heat preservation at a high temperature until the residual layer is separated from the bonded body to form a lithium tantalate electro-optical crystal film with an optical waveguide structure.

[0111] Among them, the insulation process is carried out in a vacuum environment or in a protective atmosphere formed by at least one of nitrogen and inert gases, with a insulation temperature of 400°C and a insulation time of 3 hours. This step can increase the bonding force by more than 10MPa and can restore the damage to the thin film layer caused by ion implantation, so that the obtained lithium tantalate thin film layer with an optical waveguide structure has properties close to those of the lithium tantalate wafer.

[0112] In the lithium tantalate electro-optical crystal thin film prepared in Example 3, the thickness h1 of the thin film layer is 163 nm, and the height h2 of the optical waveguide structure on the thin film layer is 656 nm.

[0113] Example 4

[0114] (1) Prepare a 6-inch SOI wafer with a thickness of 0.5 mm and a smooth surface.

[0115] (2) The SOI wafer obtained above is cleaned and an isolation layer is deposited. The deposition material is silicon oxide with a deposition thickness of 100 nm.

[0116] (3) A 6-inch, 0.5 mm thick, smooth KTP wafer is prepared and cleaned, a first mask having the same pattern as the target waveguide structure array is prepared on the KTP wafer, and helium ions are implanted into the KTP wafer using an ion implantation method. The helium ion implantation energy is 120 KeV and the dose is 4E 16 ions / cm 2 , a first implantation layer is formed in the area of ​​the KTP wafer not covered by the first mask.

[0117] (4) Remove the first mask.

[0118] (5) A second mask with a pattern opposite to the target waveguide structure array is prepared on the KTP wafer. Helium ions are implanted into the KTP wafer using an ion implantation method. The implantation energy of the helium ions is 275 KeV and the dose is 4E 16 ions / cm 2 , forming a second implantation layer in the area of ​​the KTP wafer not covered by the second mask; removing the second mask;

[0119] At this time, a residual substance layer, a first injection layer, a second injection layer and a thin film layer with an optical waveguide structure are formed in the KTP wafer injection film.

[0120] (6) The waveguide structure thin film layer of the KTP wafer implant is bonded to the silicon oxide layer on the SOI wafer by plasma bonding to form a bonded body, and then the bonded body is placed in a heating device for heat preservation at high temperature until the residual layer is separated from the bonded body to form a KTP electro-optical crystal film with an optical waveguide structure.

[0121] The insulation process is carried out in a vacuum environment or in a protective atmosphere formed by at least one of nitrogen and inert gases. The insulation temperature is 600°C and the insulation time is 1 minute. This step can increase the bonding force by more than 10MPa and can restore the damage to the thin film layer caused by ion implantation, so that the obtained KTP thin film layer with an optical waveguide structure has properties close to those of the KTP wafer.

[0122] In the KTP electro-optical crystal thin film prepared in Example 4, the thickness h1 of the thin film layer is 662 nm, and the height h2 of the optical waveguide structure on the thin film layer is 478 nm.

[0123] Example 5:

[0124] (1) An SOI substrate having a size of 6 inches, a thickness of 0.5 mm and a smooth surface is prepared.

[0125] (2) The SOI substrate obtained above was cleaned and an isolation layer was deposited. The deposited material was silicon oxide with a deposition thickness of 100 nm.

[0126] (3) A lithium niobate wafer with a size of 6 inches, a thickness of 0.5 mm and a smooth surface is prepared and cleaned, and a first mask with the same pattern as the target waveguide structure array is prepared on the lithium niobate wafer. Helium ions are implanted into the lithium niobate wafer by ion implantation. The helium ion implantation energy is 180 KeV and the dose is 4E 16 ions / cm 2 A first injection layer is formed in the area of ​​the lithium niobate wafer that is not covered by the first mask.

[0127] (4) Remove the first mask.

[0128] (5) A second mask having a pattern opposite to that of the target waveguide structure array is prepared on the lithium niobate wafer, and helium ions are implanted into the lithium niobate wafer by ion implantation. The implantation energy of the helium ions is 250 KeV and the dose is 4E 16 ions / cm 2 , forming a second injection layer in the area covered by the second mask on the surface of the lithium niobate wafer; removing the second mask;

[0129] At this time, a residual layer, a first injection layer, a second injection layer and a thin film layer with an optical waveguide structure are formed in the lithium niobate wafer injection film.

[0130] (6) The waveguide structure thin film layer of the lithium niobate wafer implantation sheet is bonded to the silicon oxide layer on the SOI substrate by a plasma bonding method to form a bonded body, and then the bonded body is placed in a heating device for heat preservation at a high temperature until the residual layer is separated from the bonded body to form a lithium niobate electro-optical crystal thin film with an optical waveguide structure.

[0131] The insulation process is carried out in a vacuum environment or in a protective atmosphere formed by at least one of nitrogen and inert gases, with a insulation temperature of 500°C and a insulation time of 1 hour. This step can increase the bonding force by more than 10 MPa and can restore the damage to the thin film layer caused by ion implantation, so that the obtained lithium niobate thin film layer with an optical waveguide structure has properties close to those of a lithium niobate wafer.

[0132] In the lithium niobate electro-optical crystal thin film prepared in Example 5, the thickness h1 of the thin film layer is 663 nm, and the height h2 of the optical waveguide structure on the thin film layer is 167 nm.

[0133] The same or similar parts between the various embodiments in this specification can refer to each other, especially the embodiment part corresponding to the electro-optical crystal film can refer to the preparation method part of the electro-optical crystal film.

[0134] The present application is described in detail above in conjunction with specific implementation methods and exemplary examples, but these descriptions cannot be understood as limiting the present application. Those skilled in the art understand that, without departing from the spirit and scope of the present application, a variety of equivalent replacements, modifications or improvements can be made to the technical solution of the present application and its implementation methods, all of which fall within the scope of the present application. The scope of protection of the present application shall be subject to the attached claims.

Claims

1. A method for preparing an electro-optical crystal thin film, characterized in that: include: preparing a supporting substrate and a film substrate; Prepare a first mask on the first surface of the thin film substrate, wherein the first mask has a pattern that is the same as or opposite to that of the target optical waveguide structure; Implanting first ions into a region on the first surface of the thin film substrate that is not covered by the first mask to form a first implantation layer in the thin film substrate, wherein a pattern of the first implantation layer is opposite to that of the first mask; removing the first mask; Preparing a second mask on the first surface or the second surface of the thin film substrate, wherein a pattern of the second mask is opposite to that of the first mask; Implanting second ions into an area on the surface of the thin film substrate on which the second mask is prepared and not covered by the second mask, to form a second injection layer in the thin film substrate, wherein the pattern of the second injection layer is the same as that of the first mask, wherein the distance difference between the first injection layer and the second injection layer is the same as the height of the target optical waveguide structure; removing the second mask; Bonding the film substrate to the support substrate to obtain a bonded body; The bonded body is heat treated to separate the thin film substrate at the first injection layer and the second injection layer to obtain an electro-optical crystal thin film, wherein the electro-optical crystal thin film includes a supporting substrate, a thin film layer formed on the supporting substrate, and the target optical waveguide structure integrally formed on the thin film layer.

2. The preparation method according to claim 1, characterized in that: If the distance difference between the second injection layer and the first surface of the thin film substrate is greater than or equal to the distance difference between the second injection layer and the second surface of the thin film substrate, the second injection layer is formed by preparing a second mask on the second surface of the thin film substrate and injecting second ions into the area on the second surface of the thin film substrate that is not covered by the second mask.

3. The preparation method according to claim 1, characterized in that: If the distance difference between the second injection layer and the first surface of the thin film substrate is less than or equal to the distance difference between the second injection layer and the second surface of the thin film substrate, the second injection layer is formed by preparing a second mask on the first surface of the thin film substrate and injecting second ions into the area on the first surface of the thin film substrate not covered by the second mask.

4. The preparation method according to claim 1, characterized in that: If the distance between the first injection layer and the first surface of the thin film substrate is equal to the thickness of the thin film layer, the bonding body is obtained by bonding the first surface of the thin film substrate to the supporting substrate.

5. The preparation method according to claim 1, characterized in that: If the distance between the second injection layer and the second surface of the thin film substrate is equal to the thickness of the thin film layer, the bonding body is obtained by bonding the second surface of the thin film substrate to the supporting substrate.

6. The preparation method according to claim 1, characterized in that: The distance difference between the first injection layer and the second injection layer is 50-1000 nm.

7. The preparation method according to claim 1, characterized in that: The first ion is the same as or different from the second ion.

8. The preparation method according to claim 7, characterized in that: The first ions are helium ions, hydrogen ions, nitrogen ions, oxygen ions or argon ions, and the second ions are helium ions, hydrogen ions, nitrogen ions, oxygen ions or argon ions.

9. An electro-optical crystal film, characterized in that: The electro-optical crystal film is prepared by the method for preparing the electro-optical crystal film as described in any one of claims 1 to 8.

10. An electronic component, characterized in that: The electronic component comprises the electro-optical crystal thin film as claimed in claim 9.

Citation Information

Patent Citations

  • Electro-optical crystal film, preparation method and electronic component

    CN112764244A

  • Method of forming top gate type Thin Film Transistor

    KR1020010110917A

  • Blank mask and photo mask fabricated using it

    KR1020110016727A

  • Mask blank, transfer mask, method for producing mask blank, method for producing transfer mask, and method for manufacturing semiconductor device