Break-resistant glass-based products

The formation of glass-based products with specific stress distribution through ion exchange treatment solves the problem that existing glass-based products are fragile when they fall, achieves a balance between thinness and strength, and improves fracture resistance and compression resistance Capability, suitable for covering glass for electronic devices.

CN114401931BActive Publication Date: 2024-11-01CORNING INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080064425.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-13
Filing Date
2020-09-11
Publication Date
2024-11-01
Estimated Expiration
2040-09-11

AI Technical Summary

Technical Problem

Existing glass-based products are fragile when dropped, making it difficult to find a balance between thinness and strength, especially when used as a cover glass in electronic devices, it is prone to damage due to hard surface collisions.

Method used

The glass-based product with a specific stress distribution is formed by ion exchange treatment, including a compressive stress layer and a region of negative curvature, thereby improving the fracture resistance of the glass-based product. The stress distribution characteristics of the glass-based article include peak tension greater than or equal to 70 MPa and points with a second derivative less than or equal to -4000 MPa/mm2, located in the 0.025 t to 0.25 t region, enhancing its anti-compression and anti-sharp contact capabilities.

Benefits of technology

It significantly improves the crack resistance of glass-based products, so that they can remain intact after multiple drops. It is suitable for thin electronic devices to cover glass, enhancing its resistance to hard surface collisions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114401931B_ABST
    Figure CN114401931B_ABST
Patent Text Reader

Abstract

Glass-based articles comprising a stress profile that provides improved fracture resistance. The stress profile contains regions of high peak tension and high negative curvature. The glass-based articles herein provide high fracture resistance after multiple drops.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority to U.S. Provisional Application Serial No. 62 / 900,157, filed on September 13, 2019, the contents of which are hereby based upon and incorporated herein by reference in their entirety.

[0003] background Technical Field

[0004] The present disclosure generally relates to stress distribution for fracture resistance stress distribution in glass-based articles. More specifically, the present disclosure relates to stress distribution for glass-based articles that may contain lithium and may be used in electronic devices. Background Art

[0005] The mobile nature of portable devices such as smartphones, tablets, portable media players, personal computers, and cameras makes these devices particularly susceptible to damage from accidental drops onto hard surfaces such as the ground. Such devices often include cover glass that can be damaged after impact with a hard surface. In many of these devices, the cover glass acts as a display cover and may include touch functionality such that the use of the device is adversely affected when the cover glass is damaged.

[0006] There are two main failure modes of cover glass when the associated portable device is dropped on a hard surface. One of the modes is flexure failure, which is caused by bending of the glass when the device is subjected to dynamic loads generated by collision with a hard surface. The other mode is sharp contact failure, which is caused by damage to the glass surface. The collision of glass with rough hard surfaces such as asphalt, granite, etc. can produce sharp indentations in the glass surface. These indentations become failure sites in the glass surface from which cracks can develop and propagate.

[0007] Glass manufacturers and handheld device manufacturers are constantly striving to improve the resistance of handheld devices to failure. It is also desirable for portable devices to be as thin as possible. Therefore, in addition to strength, it is also desirable for glass used as cover glass in portable devices to be as thin as possible. Therefore, in addition to increasing the strength of the cover glass, it is also desirable for the glass to have certain mechanical properties to allow the glass to be formed by methods for making thin glass products (e.g., thin glass sheets).

[0008]

[0006] Therefore, there is a need for a glass-based article that can be strengthened (eg, by ion exchange) and that has mechanical properties that allow it to be formed as a thin article. Summary of the invention

[0009] Aspects of the present disclosure relate to glass-based articles and their manufacture and use. The glass-based articles herein exhibit high fracture resistance. Specifically, the glass-based articles herein provide high fracture resistance after multiple drops.

[0010] According to aspect (1), a glass-based article is provided. The glass-based article comprises: a glass-based substrate, the glass-based substrate comprising a first surface and a second surface opposite to each other, the first surface and the second surface defining a substrate thickness (t); and a stress distribution. The stress distribution comprises: a peak tension (PT) greater than or equal to 70 MPa; and a second derivative value less than or equal to -4000 MPa / mm 2 A point, wherein the point is located in the region from greater than or equal to 0.025t to less than or equal to 0.25t.

[0011] According to aspect (2), there is provided a glass-based article of the aforementioned aspect, wherein the stress distribution comprises a second-order derivative value of 0 MPa / mm 2 A curvature transition point (curvature transition point), wherein the curvature transition point is located in a region greater than or equal to 0.025t to less than or equal to 0.25t.

[0012] According to aspect (3), there is provided a glass-based article according to any one of the preceding aspects, wherein the stress distribution comprises a second-order derivative value of 0 MPa / mm 2 A curvature transition point, wherein the curvature transition point is located in a region from greater than or equal to 0.7·DOC to less than or equal to 0.25t.

[0013] According to aspect (4), there is provided a glass-based article according to any one of the preceding aspects, wherein the stress distribution comprises a second-order derivative value less than or equal to -5000 MPa / mm 2 A point, wherein the point is located in the region from greater than or equal to 0.025t to less than or equal to 0.25t.

[0014] According to aspect (5), there is provided a glass-based article of any of the preceding aspects, wherein the stress distribution comprises a second-order derivative value less than or equal to -2550 / t 2 MPa / mm 2 A point, where t is in mm, and where the point is located in the region from greater than or equal to 0.025 t to less than or equal to 0.25 t.

[0015] According to aspect (6), a glass-based article of any of the preceding aspects is provided, wherein the glass-based article comprises a compression region extending from the first surface to a depth of compression (DOC), wherein the stress distribution comprises a local maximum in the absolute value of the slope within 0.1·DOC of the DOC.

[0016] According to aspect (7), there is provided the glass-based article of aspect (6), wherein the local maximum value of the absolute value of the slope is greater than or equal to 0.5 MPa / μm.

[0017] According to aspect (8), there is provided a glass-based article according to any one of the preceding aspects, wherein the PT is greater than or equal to 80 MPa.

[0018] According to aspect (9), there is provided a glass-based article according to any one of the preceding aspects, wherein the PT is less than or equal to 200 MPa.

[0019] According to aspect (10), there is provided a glass-based article according to any one of the preceding aspects, wherein PT is greater than or equal to MPa, where the unit of t is mm.

[0020] According to aspect (11), there is provided a glass-based article according to any one of the preceding aspects, wherein PT is less than or equal to MPa, where the unit of t is mm.

[0021] According to aspect (12), there is provided a glass-based article of any of the preceding aspects, wherein the glass-based substrate having the same composition and structure as the center of the glass-based article has a K greater than or equal to 0.85 MPa√m IC .

[0022] According to aspect (13), there is provided a glass-based article of any of the preceding aspects, wherein the glass-based substrate having the same composition and structure as the center of the glass-based article has a K of less than or equal to 2 MPa√m IC .

[0023] According to aspect (14), there is provided a glass-based article according to any one of the preceding aspects, comprising a knee compressive stress (CS k ).

[0024] According to aspect (15), there is provided a glass-based article according to any one of the preceding aspects, comprising greater than or equal to MPa knee compression stress (CS k ), where t is in mm.

[0025] According to aspect (16), there is provided a glass-based article of any of the preceding aspects, comprising a compression region extending from the first surface to a depth of compression (DOC), and the DOC is greater than or equal to 0.15t.

[0026] According to aspect (17), there is provided a glass-based article of any of the preceding aspects, comprising a compressed region extending from the first surface to a depth of compression (DOC), and the DOC is greater than or equal to 130 μm.

[0027] According to aspect (18), there is provided a glass-based article of any of the preceding aspects, comprising a compressive stress greater than or equal to 330 MPa.

[0028] According to aspect (19), there is provided a glass-based article according to any of the preceding aspects, comprising a spike region extending from the first surface to a depth of spike layer (DOL sp ), and DOL sp Greater than or equal to 3μm.

[0029] According to aspect (20), there is provided a glass-based article of any of the preceding aspects, comprising a peak region extending from the first surface to a depth of peak layer (DOL sp ), and DOL sp Less than or equal to 15μm.

[0030] According to aspect (21), a glass-based article of any of the preceding aspects is provided, wherein the stress distribution comprises: a first compression region, a second compression region, and a tension region, the first compression region extending from the first surface to a first compression depth DOC1, the second compression region extending from the second surface to a second compression depth DOC2, and the tension region extending from DOC1 to DOC2, wherein the tension region has a tensile stress factor K greater than or equal to 1.41 MPa·√m T .

[0031] According to aspect (22), there is provided a glass-based article of any of the preceding aspects, wherein the glass-based article is non-brittle.

[0032] According to aspect (23), there is provided a glass-based article according to any one of the preceding aspects, comprising Li2O.

[0033] According to aspect (24), there is provided a glass-based article of any one of the preceding aspects, wherein the Li2O concentration at the center of the glass-based article is greater than or equal to 8 mol%.

[0034] According to aspect (25), there is provided a glass-based article of any one of the preceding aspects, wherein a maximum K2O concentration in the glass-based article is 7.5 mol% or less greater than a K2O concentration at a center of the glass-based article.

[0035] According to aspect (26), there is provided a glass-based article of any of the preceding aspects, comprising a peak region extending from the first surface to a depth of peak layer (DOL sp ), wherein in the peak region, the integral of the K2O concentration relative to the value of the K2O concentration at the center of the glass-based article is less than or equal to 29 mol%·μm.

[0036] According to aspect (27), there is provided a glass-based article of any of the preceding aspects, comprising a peak region extending from the first surface to a peak layer depth (DOL sp ), wherein in the peak region, the integral of the K2O concentration relative to the integral of the increase in the K2O concentration at the center of the glass-based article is greater than or equal to 4 mol%·μm.

[0037] According to aspect (28), a glass-based article of any of the preceding aspects is provided, wherein the center of the glass-based article has a Li2O / Na2O molar ratio greater than or equal to 3.3.

[0038] According to aspect (29), a glass-based article of any of the preceding aspects is provided, wherein the center of the glass-based article has a Li2O / Na2O molar ratio of less than or equal to 100.

[0039] According to aspect (30), there is provided a glass-based article of any one of the preceding aspects, wherein t is greater than or equal to 0.2 mm to less than or equal to 2.0 mm.

[0040] According to aspect (31), there is provided a glass-based article of any one of the preceding aspects, wherein t is greater than or equal to 0.3 mm and less than or equal to 1.0 mm.

[0041] According to aspect (32), a glass-based article according to any of the preceding aspects is provided, comprising a compressive region extending from a first surface to a depth of compression (DOC), and wherein the compressive stress at a depth of 0.6·DOC from the first surface is greater than or equal to 45 MPa.

[0042] According to aspect (33), a glass-based article according to any of the preceding aspects is provided, comprising a compression region extending from the first surface to a depth of compression (DOC), and wherein the compressive stress at a depth of 0.65·DOC from the first surface is greater than or equal to 40 MPa.

[0043] According to aspect (34), a glass-based article according to any of the preceding aspects is provided, comprising a compression region extending from a first surface to a depth of compression (DOC), and having a compressive stress greater than or equal to 37 MPa at a depth of 0.7·DOC from the first surface.

[0044] According to aspect (35), a glass-based article of any of the preceding aspects is provided, comprising a compression region extending from a first surface to a depth of compression (DOC), and wherein the compressive stress at a depth of 0.75·DOC from the first surface is greater than or equal to 32 MPa.

[0045] According to aspect (36), a glass-based article of any of the preceding aspects is provided, comprising a compression region extending from the first surface to a depth of compression (DOC), and wherein the compressive stress at a depth of 0.8·DOC from the first surface is greater than or equal to 26 MPa.

[0046] According to aspect (37), a glass-based article according to any of the preceding aspects is provided, comprising a compression region extending from a first surface to a depth of compression (DOC), and having a compressive stress of greater than or equal to 18 MPa at a depth of 0.85·DOC from the first surface.

[0047] According to aspect (38), a glass-based article of any of the preceding aspects is provided, comprising a compression region extending from a first surface to a depth of compression (DOC), and wherein the compressive stress at a depth of 0.9·DOC from the first surface is greater than or equal to 11 MPa.

[0048] According to aspect (39), a glass-based product of any of the preceding aspects is provided, comprising a Na2O concentration distribution in a region greater than or equal to 0.025t to less than or equal to 0.25t, and wherein the Na2O concentration distribution presents a positive curvature or no curvature in the region greater than or equal to 0.025t to less than or equal to 0.25t.

[0049] According to aspect (40), a glass-based article of any of the preceding aspects is provided, wherein the center of the glass-based article comprises: 50 mol% to 69 mol% SiO2; 12.5 mol% to 25 mol% Al2O3; 0 mol% to 8 mol% B2O3; greater than 0 mol% to 4 mol% CaO; greater than 0 mol% to 17.5 mol% MgO; 0.5 mol% to 8 mol% Na2O; 0 mol% to 2.5 mol% La2O3; and greater than 8 mol% to 18 mol% Li2O; wherein: (Li2O+Na2O+MgO) / Al2O3 is from 0.9 to less than 1.3; and Al2O3+MgO+Li2O+ZrO2+La2O3+Y2O3 is from greater than 23 mol% to less than 50 mol%.

[0050] According to aspect (41), a consumer electronic product is provided. The consumer electronic product comprises: a housing, the housing comprising a front surface, a rear surface and a side surface; an electrical component, the electrical component at least partially disposed in the housing, the electrical component comprising at least a controller, a memory and a display, the display being disposed at or adjacent to the front surface of the housing; and a cover plate, the cover plate being disposed above the display; wherein at least a portion of at least one of the housing and the cover plate comprises the glass-based product of one of the aforementioned aspects.

[0051] According to aspect (42), a method is provided. The method includes: exposing a glass-based substrate to an ion exchange treatment to form a glass-based article having a stress profile, the glass-based substrate comprising a first surface and a second surface opposite to each other, the first surface and the second surface defining a substrate thickness (t), the stress profile comprising: a peak tension (PT) greater than or equal to 70 MPa; and a second derivative value less than or equal to -4000 MPa / mm 2 A point, wherein the point is located in the region from greater than or equal to 0.025t to less than or equal to 0.25t.

[0052] According to aspect (43), the method of aspect (42) is provided, wherein the ion exchange treatment is a single ion exchange treatment.

[0053] According to aspect (44), a method as described in any one of aspects (42) to (43) is provided, wherein the glass-based substrate comprises: 50 mol% to 69 mol% SiO2; 12.5 mol% to 25 mol% Al2O3; 0 mol% to 8 mol% B2O3; greater than 0 mol% to 4 mol% CaO; greater than 0 mol% to 17.5 mol% MgO; 0.5 mol% to 8 mol% Na2O; 0 mol% to 2.5 mol% La2O3; and greater than 8 mol% to 18 mol% Li2O; wherein: (Li2O+Na2O+MgO) / Al2O3 is from 0.9 to less than 1.3; and Al2O3+MgO+Li2O+ZrO2+La2O3+Y2O3 is from greater than 23 mol% to less than 50 mol%.

[0054] According to aspect (45), the method of any one of aspects (42) to (44) is provided, wherein the glass-based substrate comprises: SiO2; Al2O3; and Li2O, wherein the glass is characterized by: a K greater than or equal to 0.85 MPa√m 1C value.

[0055] Additional features and advantages are set forth in the following detailed description, some of which will be apparent to those skilled in the art from the description or may be learned by practicing the embodiments described herein, including the following detailed description, claims, and accompanying drawings.

[0056] It should be understood that both the foregoing general description and the following detailed description describe various embodiments and are intended to provide an overall review or framework for understanding the nature and characteristics of the claimed subject matter. The included drawings provide a further understanding of the various embodiments, and the drawings are incorporated into and constitute a part of this specification. The drawings illustrate the various embodiments described herein and, together with the description, are used to explain the principles and operations of the claimed subject matter. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 schematically depicts a cross-section of glass having a compressive stress layer on a surface thereof according to embodiments disclosed and described herein;

[0058] Figure 2 is a schematic diagram of stress distribution including knee stress;

[0059] Figure 3 For determining the fracture toughness K IC Schematic diagram of the sample and its cross section;

[0060] Figure 4A is a plan view of an exemplary electronic device including any of the glass articles disclosed herein;

[0061] Figure 4B for Figure 4A A perspective view of an exemplary electronic device;

[0062] Figure 5 is a representative picture of the non-fragile sample after the fragility test;

[0063] Figure 6 It is a representative picture of the fragility sample after fragility test;

[0064] Figure 7 is a diagram of stress distribution according to an embodiment;

[0065] Figure 8 For polynomial fitting Figure 7 A diagram of a portion of the stress distribution;

[0066] Fig. 9 for Figure 8 A graph of the second derivative of the polynomial fit;

[0067] Fig.10 is a diagram of stress distribution according to one embodiment;

[0068] Fig.11 For polynomial fitting Fig.10 A diagram of a portion of the stress distribution;

[0069] Fig.12 for Fig.11 A graph of the second derivative of the polynomial fit;

[0070] Fig.13 is a diagram of stress distribution according to an embodiment;

[0071] Fig.14 For polynomial fitting Fig.13 A diagram of a portion of the stress distribution;

[0072] Fig.15 for Fig.14 A graph of the second derivative of the polynomial fit;

[0073] Fig.16 is a diagram of stress distribution according to one embodiment;

[0074] Fig.17 For polynomial fitting Fig.16 A diagram of a portion of the stress distribution;

[0075] Fig.18 for Fig.17 A graph of the second derivative of the polynomial fit;

[0076] Fig.19 is a diagram of stress distribution according to one embodiment;

[0077] Fig. 20 For polynomial fitting Fig.19 A diagram of a portion of the stress distribution;

[0078] Fig.21 for Fig. 20 Graph of the second derivative of the polynomial fit. DETAILED DESCRIPTION

[0079] Before describing several exemplary embodiments, it should be understood that the present disclosure is not limited to the details of construction or process steps set forth in the following disclosure. The disclosure provided herein is capable of other embodiments and can be implemented or carried out in various ways.

[0080] The "one embodiment", "certain embodiments", "various embodiments", "one or more embodiments" or "an embodiment" mentioned in the specification means that the specific features, structures or properties described in conjunction with the embodiment are included in at least one embodiment of the present disclosure. Therefore, the phrases "in one or more embodiments", "in certain embodiments", "in various embodiments", "in one embodiment" or "in an embodiment" appearing in various places in the specification do not necessarily refer to the same embodiment, or to only one embodiment. In addition, specific features, structures, materials or characteristics may be combined in one or more embodiments in any suitable manner.

[0081] Definition and measurement techniques

[0082] The terms "glass-based article" and "glass-based substrate" are used to include any object made entirely or partially of glass, including glass-ceramics (comprising an amorphous phase and a crystalline phase). Generally speaking, a glass-based substrate is subjected to an ion exchange treatment to form a glass-based article. Laminated glass-based articles include laminates of glass and non-glass materials, laminates of glass and crystalline materials. The glass-based substrate according to one or more embodiments may be selected from soda-lime silicate glass, alkali aluminosilicate glass, alkali-containing borosilicate glass, alkali-containing aluminoborosilicate glass, and alkali-containing glass-ceramics.

[0083] "Base composition" is the chemical composition of the substrate prior to any ion exchange (IOX) treatment. That is, the base composition is not doped with any ions from the IOX. In other words, prior to being subjected to ion exchange treatment, the glass-based substrate has a base composition. The center of the glass-based article that has been subjected to the IOX treatment is least affected by the IOX treatment and may not be affected by the IOX treatment. To this end, when the IOX treatment conditions are such that the ions supplied to the IOX do not diffuse into the center of the substrate, the composition at the center of the glass-based article can be the same as the base composition. In one or more embodiments, the center composition at the center of the glass article includes the base composition. In addition, a glass-based substrate having the same composition and structure as the center of a glass-based article can have properties equivalent to the substrate used to form the glass-based article.

[0084] It should be noted that the terms "substantially" and "approximately" may be used herein to represent the degree of inherent uncertainty that may be caused by any quantitative comparison, value, measurement or other method of representation. These terms are also used herein to represent that the value of a quantity may vary from the stated reference value, but will not result in a change in the basic function of the subject matter discussed. Thus, for example, a glass-based article that is "substantially free of MgO" means that MgO is not actively added or formulated into the glass-based article, but it may be present in very small amounts as a contaminant. As used herein, the term "approximately" means that the amount, size, formula, parameter and other quantities and characteristics are not precise and do not need to be precise, but may be approximate and / or larger or smaller as required, such as reflecting tolerances, conversion factors, rounding, measurement errors, etc., as well as other factors known to those skilled in the art. When the term "about" is used to describe a value or an endpoint of a range, the disclosure should be understood to include the specific value or endpoint mentioned. Regardless of whether the value or endpoint of a range in the specification is listed using "about", the value or endpoint of the range is intended to include two embodiments: one modified by "about" and the other not modified by "about". It will be further understood that the endpoints of each of the ranges are significant both in conjunction with the other endpoint, and independently of the other endpoint.

[0085] Unless otherwise stated, all compositions described herein are expressed as mole percent (mol %) based on oxides.

[0086] A "stress profile" is stress as a function of thickness across a glass-based article. A compressive stress region extends from a first surface of the article to a depth of compression (DOC), wherein the article is under compressive stress. A central tension region extends from the DOC to include a region of the article under tensile stress. In other words, a first compressive stress region may extend from the first surface to a first depth of compression (DOC1), a tension region extends from DOC1 to a second depth of compression (DOC2), and a second compressive region extends from DOC2 to the second surface. In embodiments where the stress profile is symmetrical, the distance from each surface to the respective DOC is equal.

[0087] As used herein, depth of compression (DOC) refers to the depth at which stress within a glass-based article changes from compressive stress to tensile stress. At the DOC, the stress changes from a positive stress (compressive stress) to a negative stress (tensile stress), thereby exhibiting a zero stress value. According to common practice in the field of mechanics, compression is represented by negative (<0) stress and tension is represented by positive (>0) stress. However, in this specification, a positive stress value is a compressive stress (CS), which is represented by a positive value or an absolute value, that is, as described herein, CS=|CS|. In addition, a negative stress value is a tensile stress. However, when used with the term "tensile", stress or central tension (CT) can be expressed as a positive value, that is, CT=|CT|. Central tension (CT) refers to the tensile stress in the central region or central tension region of a glass-based article. Maximum central tension (maximum CT or CT 最大 ) occurs in the central tension zone, nominally at 0.5·t, where t is the article thickness, allowing for some deviation from the exact center where the maximum tensile stress is located. Peak tension (PT) refers to the maximum tension measured, which may or may not be at the center of the article.

[0088] The "knee" of a stress profile is the depth in the article where the slope of the stress profile transitions from steep to flat. The steep portion of the stress profile extending from the surface into the glass-based article is referred to as a "spike." The knee may refer to a transition region within a depth range where the slope varies. The knee compressive stress (CS k ) is defined as the deeper part of the CS distribution extrapolated to the spike depth (DOL sp ) at the compressive stress value. DOL sp Reported by surface stress gauge measurements by known methods. Figure 2 A schematic diagram of the stress distribution including the knee stress is provided.

[0089] A non-zero concentration of metal oxide relative to the metal oxide that varies from a first surface to a depth of layer or at least along a majority of the thickness (t) of the article indicates that stress has been induced in the article due to ion exchange. A change in metal oxide concentration may be referred to herein as a metal oxide concentration gradient. A metal oxide that is not zero and varies from a first surface to a depth of layer or along a portion of the thickness may be described as inducing stress in the glass-based article. The concentration gradient or change of the metal oxide is produced by chemically strengthening the glass-based substrate, wherein a plurality of first metal ions in the glass-based substrate are exchanged with a plurality of second metal ions.

[0090] Unless otherwise stated, CT and CS are expressed herein in megapascals (MPa), thickness is expressed in millimeters, and DOC and DOL are expressed in micrometers (micrometers or μm).

[0091] The compressive stress (including peak CS, CS 最大 ). Surface stress measurements rely on accurate measurement of the stress-optical coefficient (SOC), which is related to the birefringence of the glass. SOC is measured according to Protocol C (Glass Disk Method) as described in ASTM Standard C770-16, entitled "Standard Test Method for Measurement of Glass Stress-Optical Coefficient", which is incorporated herein by reference in its entirety.

[0092] The maximum central tension (CT) and peak tension (PT) and stress retention values ​​are measured using a scattered light polariscope (SCALP) technique known in the art. The refracted near field (RNF) method or SCALP can be used to measure stress distribution and depth of compression (DOC). When the RNF method is used to measure the stress distribution, the maximum CT value provided by the SCALP is used in the RNF method. Specifically, the stress distribution measured by the RNF is force balanced and calibrated to the maximum CT value provided by the SCALP measurement. The RNF method is described in U.S. Patent No. 8,854,623 entitled "Systems and methods for measuring a profile characteristic of a glass sample", which is incorporated herein by reference in its entirety. Specifically, the RNF method includes placing a glass article near a reference block, generating a polarization switching beam that switches between orthogonal polarizations at a frequency of 1 Hz to 50 Hz, measuring the amount of power in the polarization switching beam, and generating a polarization switching reference signal, wherein the amount of power measured in each orthogonal polarization is within 50% of each other. The method further includes the steps of transmitting a polarization-switched beam through the glass sample and a reference block to different depths in the glass sample, and then relaying the transmitted polarization-switched beam to a signal photodetector using a relay optical system, and the signal photodetector generates a polarization-switched detector signal. The method further includes the steps of dividing the detector signal by a reference signal to form a normalized detector signal, and determining a distribution characteristic of the glass sample from the normalized detector signal.

[0093] As used herein, the fracture toughness (K) was measured by the double cantilever beam (DCB) method. IC ). K is measured on a glass-based substrate prior to ion exchange to form a glass-based article. IC The geometry of the DCB specimen is shown in Figure 3 , where the parameters are the crack length a, the applied load P, the cross-sectional dimensions w and 2h, and the thickness b of the crack guiding groove. The samples were cut into rectangles with a width 2h = 1.25 cm and a thickness ranging from w = 0.3 mm to 1 mm, while the total length of the sample (not a critical dimension) varied between 5 cm and 10 cm. Holes were drilled at both ends using a diamond drill to provide a means of attaching the sample to a sample holder and load. A wafer dicing saw with a diamond blade was used to cut the crack "guiding groove" along the length of the sample on two flat faces, leaving approximately half the total plate thickness ( Figure 1The "web" of material with dimension b) in (a) and having a height of 180 μm, corresponding to the blade thickness. The high-precision dimensional tolerances of the dicing saw minimize variations between samples. The dicing saw is also used to cut an initial crack of a=15 mm. As a result of this final operation, a very thin wedge of material is produced near the crack tip (due to the blade curvature), allowing cracks in the sample to initiate more easily. The sample is mounted in a metal sample holder using a steel wire in the bottom hole of the sample. The sample is also supported at the other end to keep the sample horizontal under load conditions. A spring hook in series with the load cell (FUTEK, LSB200) is then gradually extended using a rope and a high-precision slide to gradually apply the load. The crack is monitored using a microscope with a resolution of 5 μm and attached to a digital camera and a computer. The applied stress intensity K P Use the following equation (III) to calculate:

[0094]

[0095] For each sample, a crack is first initiated at the tip of the web, and then the initial crack is carefully grown subcritically until the ratio of the size a / h is greater than 1.5, and the stress intensity is accurately calculated according to equation (III). At this point, the crack length a is measured and recorded using a mobile display mirror with a resolution of 5 μm. A drop of toluene is then dropped into the crack groove and wicks along the entire length of the groove under the action of capillary forces, which prevents the crack from moving before the fracture toughness is reached. The load is then increased until sample fracture occurs, and the critical stress intensity is calculated based on the failure load and sample size, where, due to the measurement method, K P Equivalent to K IC .

[0096] As used herein, a glass-based article is considered non-fragile when the glass-based article exhibits at least one of the following in the test area as a result of a fragility test: (1) four or fewer fragments with a maximum dimension of at least 1 mm, and / or (2) the number of forks is less than or equal to 1.5 forks / crack branches. Fragments, forks, and crack branches are calculated based on any 5 cm×5 cm square centered on the impact point. Therefore, for any 5 cm×5 cm square centered on the impact point, if the glass meets one or both of the tests (1) and (2), the glass is considered non-fragile, wherein the impact point is the place where the break is generated according to the following procedure. In the fragility test, an impact probe is brought into contact with the glass, wherein the depth to which the impact probe extends into the glass increases with successive repeated contacts. The gradually increasing depth of the impact probe allows the flaw generated by the impact probe to reach the tension zone while preventing the application of excessive external forces, which would prevent accurate determination of the fragility characteristics of the glass. The glass-based article is placed on a rigid surface, such as the MVN precision vertical stage available from Newport Corporation. The impact probe is a stylus with a tungsten carbide tip (available from Fisher Scientific Industries under the trademark and manufacturer identification number #13-378, with a 60 degree cone spherical tip), has a 40 g weight, and is connected to a fixture on a gear drive mechanism that moves the stylus up and down. In one embodiment, the depth of the impact probe in the glass can increase by about 5 μm for each repeated contact, where the impact probe does not contact the glass between each repeated contact. The test area is any 5 cm x 5 cm square centered on the impact point. Figure 5 The non-fragile test results are shown. Figure 5 As shown, the test area is a square centered at the impact point 135, wherein the side length a of the square is 5 cm. Figure 5 The non-fragile sample shown includes three fragments 142 as well as two crack branches 140 and one fork 150. Thus, Figure 5 The non-fragile sample shown contains less than 4 pieces of fragments with a maximum dimension of at least 1 mm, and the number of forks is less than or equal to the number of crack branches (0.5 forks / crack branch). As used herein, crack branches originate from the impact point, and if any portion of the fragment extends into the test area, the fragment is considered to be within the test area. Although coatings, adhesive layers, etc. can be used in conjunction with the strengthened glass-based articles described herein, these external constraints are not used to determine the fragility or fragility characteristics of the glass-based articles. In some embodiments, a film that does not affect the fracture properties of the glass-based article can be applied to the glass-based article before the fragility test to prevent fragments from being ejected from the glass-based article, thereby improving the safety of the personnel performing the test.

[0097] Figure 6 A frangible sample is shown. The frangible sample comprises 6 fragments 142 having a largest dimension of at least 1 mm. Figure 6 The sample shown includes 2 crack branches 140 and 4 forks 150, which produces more forks than crack branches (2 forks / crack branch). Figure 6 The samples shown did not exhibit four or fewer fragments or less than or equal to 1.5 forks / crack branches. Figure 5 and 5 Two crack branches 140 are included originating from the impact point 135, but it should be understood that there may be more than two crack branches originating from the impact point, such as three or more crack branches.

[0098] In the fragility test described herein, an impact is delivered to the surface of the glass article with a force that is just sufficient to release the internal stored energy present in the strengthened glass article. That is, the point impact force is sufficient to generate at least one new crack in the surface of the strengthened glass sheet and cause the crack to extend through the compressive stress CS region (i.e., through the compression depth) and into the central tension region.

[0099] Overview of properties of glass-based products

[0100] The glass-based articles herein have stress profiles designed to increase the probability of surviving multiple drops onto hard surfaces. When combined with these favorable stress profiles, high fracture toughness provides new, higher levels of fracture resistance. The stress profiles may include regions of negative curvature in the compressive stress layer, identified by having a negative second derivative, and may be characterized by a high degree of negative curvature, which contributes to the ability of the glass-based articles to survive multiple drops. Without wishing to be bound by any particular theory, regions of negative curvature may increase the amount of compressive stress in the glass-based article at greater depths, such as depths approaching the DOC.

[0101] The glass-based substrate used to form the glass-based articles having stress profiles described herein can be formed of any suitable material, such as alkali aluminosilicate glass. Alkali aluminosilicate glass has good ion exchangeability, and chemical strengthening processes have been used to achieve high strength and high toughness properties in alkali aluminosilicate glass. Sodium aluminosilicate glass is a highly ion-exchangeable glass with high glass formability and quality. Lithium aluminosilicate glass is a highly ion-exchangeable glass with high glass quality. Al2O3 substitution into the silicate glass network can increase the cross-diffusivity of monovalent cations during the ion exchange process. Glass with high strength, high toughness and high pressure mark crack resistance can be achieved by chemical strengthening in a molten salt bath (e.g., KNO3 and / or NaNO3). The shape of the stress profile achieved by chemical strengthening can affect the drop performance, strength, toughness and other properties of the glass-based article.

[0102] Lithium aluminosilicate glasses are particularly ideal for forming chemically strengthened glass-based articles because they provide good physical properties, chemical durability, and ion exchangeability. Through different ion exchange processes, greater peak tension (PT), depth of compression (DOC), and compressive stress (CS) can be achieved. The stress profiles described herein provide improved fracture resistance and can be preferably applied to lithium-containing glass-based articles.

[0103] In the embodiments of the glass compositions described herein, unless otherwise indicated, the concentrations of the constituent components (e.g., SiO2, Al2O3, Li2O, etc.) are specified as mole percent (mol%) of the oxide. It should be understood that any of the various recited ranges for one component may be independently combined with any of the various recited ranges for any other component.

[0104] The stress profiles disclosed herein exhibit increased fracture resistance, which can be characterized by improved performance in drop tests. Figure 1 , the glass has a first region under compressive stress (e.g., Figure 1 The first region extends from the surface of the glass to the depth of compression (DOC), and the second region (e.g., Figure 1 The second region extends from the DOC into the center or interior region of the glass.

[0105] The compressive stress (CS) has a maximum or peak value that usually occurs at the glass surface (but this is not necessarily the case, as the peak may occur at some depth from the glass surface), and the CS varies with the distance d from the surface as a function. Figure 1, the first compressive stress layer 120 extends from the first surface 110 to a depth d1, while the second compressive stress layer 122 extends from the second surface 112 to a depth d2. Together, these segments define the compression or CS of the glass 100.

[0106] The tension stored in the central area (130) of the glass is used to balance the tension between the two main surfaces ( Figure 1 110, 112) compressive stress.

[0107] In a glass-based article, there is an alkali metal oxide having a non-zero concentration, the non-zero concentration being a variation between one or both of the first and second surfaces and the depth of layer (DOL) relative to the metal oxide. A stress profile is generated due to the non-zero concentration of one or more metal oxides that varies from the first surface. The non-zero concentration may vary along a portion of the thickness of the article. In some embodiments, the concentration of the alkali metal oxide is non-zero and varies along a thickness range of about 0·t to about 0.3·t. In some embodiments, the concentration of the alkali metal oxide is non-zero and varies along a thickness range of about 0·t to about 0.35·t, about 0·t to about 0.4·t, about 0·t to about 0.45·t, about 0·t to about 0.48·t, or about 0·t to about 0.50·t. The variation in concentration may be continuous along the above thickness range. The variation in concentration may include a change in the metal oxide concentration of about 0.2 mol% or more along a thickness segment of about 100 microns. The change in metal oxide concentration along a thickness segment of about 100 microns can be about 0.3 mol% or more, about 0.4 mol% or more, or about 0.5 mol% or more. This change can be measured by methods known in the art (including microprobes).

[0108] In some embodiments, the change in concentration can be continuous along a thickness segment in the range of about 10 microns to about 30 microns. In some embodiments, the concentration of the alkali metal oxide decreases from the first surface to a value between the first surface and the second surface and increases from this value to the second surface.

[0109] The concentration of alkali metal oxides may include more than one metal oxide (e.g., a combination of Na2O and KO). In some embodiments, when two metal oxides are used and the ion radii are different from each other, at a shallow depth, the concentration of ions with a larger radius is greater than the concentration of ions with a smaller radius, and at a deeper depth, the concentration of ions with a smaller radius is greater than the concentration of ions with a larger radius.

[0110] In one or more embodiments, the alkali metal oxide concentration gradient extends through a majority of the thickness t of the article. In some embodiments, the concentration of the metal oxide along the entire thickness of the first and / or second portion may be about 0.5 mol% or more (e.g., about 1 mol% or more) and is maximum at the first surface and / or the second surface 0·t, and decreases substantially constantly to a value between the first surface and the second surface. At this value, the concentration of the metal oxide along the entire thickness t is minimum; however, the concentration at this point is also not zero. In other words, the non-zero concentration of the particular metal oxide extends along a majority of the thickness t (as described herein) or the entire thickness t. The total concentration of the particular metal oxide in the glass-based article may be in the range of about 1 mol% to about 20 mol%.

[0111] The concentration of alkali metal oxides can be determined by the baseline amount of metal oxides in the glass-based substrate that is ion exchanged to form the glass-based article. The baseline amount of metal oxides can be defined as the concentration of metal oxides at the center of the glass-based article. The metal oxide ions added to the glass-based article as a result of the ion exchange process can be characterized with reference to the baseline amount. For example, the amount of added metal oxide ions at the surface can be determined by subtracting the baseline amount from the amount measured at the surface.

[0112] In one or more embodiments, the glass-based article comprises a stress profile, wherein the stress profile comprises a region of negative curvature. The region of negative curvature is located between the peak and the compression depth. The curvature of the stress profile is given by a second derivative.

[0113] In an embodiment, the stress distribution includes a minimum value of the second derivative value located in the region greater than or equal to 0.025t to 0.25t, which is less than or equal to -4000MPa / mm 2 , for example less than or equal to -5000MPa / mm 2 , less than or equal to -6000MPa / mm 2 , less than or equal to -7000MPa / mm 2 , less than or equal to -8000MPa / mm 2 In an embodiment, the stress distribution includes a minimum value of the second-order derivative value located in a region greater than or equal to 0.025t to 0.25t, which is less than or equal to MPa / mm 2 , where t is the thickness of the glass-based article in millimeters, the minimum value of the second-order derivative value may be, for example, less than or equal to MPa / mm 2 , less than or equal to MPa / mm 2 , less than or equal to MPa / mm 2In an embodiment, the minimum value of the second-order derivative in the region of 0.025t to 0.25t is greater than or equal to -50000 MPa / mm 2 , for example greater than or equal to -40000MPa / mm 2 , greater than or equal to -30000MPa / mm 2 , greater than or equal to -20000MPa / mm 2 , greater than or equal to -10000MPa / mm 2 In an embodiment, the minimum value of the second-order derivative in the region of 0.025t to 0.25t is greater than or equal to MPa / mm 2 , such as greater than or equal to MPa / mm 2 , greater than or equal to MPa / mm 2 or greater. The minimum value of the second derivative in the region greater than or equal to 0.025t to 0.25t may fall within the range formed between any of the above values. A low second derivative value in the region of 0.025t to 0.25t corresponds to a higher amount of stress in this region compared to a distribution with a higher second derivative value. A low second derivative value indicates that the region has a high degree of negative curvature. This negative curvature allows for more "area under the curve" and thus produces greater compressive stresses compared to a stress distribution with no curvature or with positive curvature.

[0114] The second derivative values ​​described herein are determined from a polynomial fit of the measured stress distribution. The polynomial fit is applied to the stress distribution from 1.3·DOL sp The region of the stress distribution extending to 0.3t (where t is the thickness of the glass-based article). The polynomial fit was selected so that the fit had an R greater than 0.99. 2 A fit quality value, such as greater than or equal to 0.9995, greater than or equal to 0.9997, or greater than or equal to 0.9999. A third-order polynomial is preferred for the fit. 2 In the case of fitting mass values, a fourth-order polynomial can be used to achieve the required R 2 Then, by calculating 1.3·DOL sp The second derivative of the polynomial fit in the region from 0.3t to 0.5t is used to determine the second derivative of the stress distribution in this region. For stress distribution excluding the peak region, DOL sp is equal to 0, and a polynomial fit can be performed in the region of 0 to 0.3t.

[0115] In an embodiment, the stress profile includes a curvature transition point, which is defined as a point without curvature in a region deeper than the peak and less than the compression depth. The curvature transition point may indicate a transition from negative curvature to positive curvature, while the transition point itself has no curvature. The curvature transition point has a curvature of 0 MPa / mm 2 The second derivative of .

[0116] In an embodiment, the curvature transition point is located in a region greater than or equal to 0.025t to less than or equal to 0.25t, for example, greater than or equal to 0.05t to less than or equal to 0.25t, greater than or equal to 0.10t to less than or equal to 0.24t, or greater than or equal to 0.15t to less than or equal to 0.23t. The curvature transition point may be located in a region greater than or equal to 0.7·DOC to less than or equal to 0.25t, for example, greater than or equal to 0.75·DOC to less than or equal to DOC, greater than or equal to 0.8·DOC to less than or equal to DOC, greater than or equal to 0.85·DOC to less than or equal to DOC. The curvature transition point may be located in a range formed between any of the foregoing values. The high depth of the curvature transition point produces a stress profile with negative curvature at a greater depth of the glass-based article, which allows for greater compressive stress in the deep portion of the stress profile close to the DOC. Higher compressive stresses in the deep portion of the stress profile may improve fracture resistance, as evidenced by improved performance in drop tests.

[0117] In one or more embodiments, the glass-based article comprises a peak tension (PT) of 70 MPa or greater, such as 75 MPa or greater, 80 MPa or greater, 85 MPa or greater, 90 MPa or greater, 95 MPa or greater, 100 MPa or greater, 105 MPa or greater, 110 MPa or greater, 115 MPa or greater, or greater. In an embodiment, the glass-based article has a PT of 200 MPa or less, such as 190 MPa or less, 180 MPa or less, 170 MPa or less, 160 MPa or less, 150 MPa or less, 140 MPa or less, 130 MPa or less, 120 MPa or less, 110 MPa or less, or less. In an embodiment, the glass-based article may have a PT of 100 MPa or less. MPa (where t is the thickness of the glass-based article in millimeters), if greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa or greater. In an embodiment, the PT of the glass-based article may be less than or equal to MPa (where t is the thickness of the glass-based article in millimeters), if less than or equal to MPa, less than or equal to MPa, less than or equal to MPa, less than or equal to MPa, less than or equal to MPa, less than or equal to MPa, less than or equal to MPa or less. PT may fall within a range formed between any of the aforementioned values. PT is related to the amount of compressive stress introduced into the glass-based article by the ion exchange process. Therefore, a higher PT value may indicate that a greater compressive stress has been applied to the glass-based article, which may allow for greater fracture resistance. If the PT value is too high, the glass-based article may become brittle, which is not ideal for many applications.

[0118] In one or more embodiments, the glass-based substrate used to form the glass-based article has a fracture toughness (K IC ), for example, greater than or equal to 0.86 MPa√m, greater than or equal to 0.87 MPa√m, greater than or equal to 0.88 MPa√m, greater than or equal to 0.89 MPa√m, greater than or equal to 0.90 MPa√m, greater than or equal to 0.91 MPa√m, greater than or equal to 0.92 MPa√m, 0.93 MPa√m, or greater. In an embodiment, the glass-based substrate used to form the glass-based article has a fracture toughness (K less than or equal to 2 MPa√m). IC ), for example, less than or equal to 1.5 MPa√m, less than or equal to 1.4 MPa√m, less than or equal to 1.3 MPa√m, less than or equal to 1.36 MPa√m or less. K IC The K of the glass-based substrate used to form the glass-based article may fall within the range formed between any of the above values. IC The K of the glass-based substrate having the same composition and structure as the center of the glass-based article may be equal to or similar to that of the glass-based substrate having the same composition and structure as the center of the glass-based article. IC . High K glass substrate IC The glass-based article has an increased resistance to fracture, such as when dropped. Again, without wishing to be bound by any particular theory, the high K IC Glass-based articles may be allowed to have stress profiles with higher peak tensions without becoming brittle.

[0119] In one or more embodiments, the glass-based article comprises a peak compressive stress (CS) greater than or equal to 330 MPa. 最大), for example, greater than or equal to 400 MPa, greater than or equal to 500 MPa, greater than or equal to 600 MPa or greater. In an embodiment, CS 最大 Less than or equal to 1 GPa, for example, less than or equal to 900 MPa, less than or equal to 800 MPa, less than or equal to 700 MPa, less than or equal to 650 MPa or less. CS 最大 The range may be defined between any of the aforementioned values. The peak compressive stress may be located at or near the surface of the glass-based article.

[0120] In one or more embodiments, the glass-based article comprises a knee compressive stress (CS) greater than or equal to 80 MPa. k ), for example, 85 MPa or more, 90 MPa or more, 95 MPa or more, 100 MPa or more, 105 MPa or more, 110 MPa or more, 115 MPa or more, 120 MPa or more, 130 MPa or more, 140 MPa or more, or more. In an embodiment, CS k Greater than or equal to MPa (where t is the thickness of the glass-based article in millimeters), for example greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa, greater than or equal to MPa or greater. In an embodiment, CS k Less than or equal to 200 MPa, such as less than or equal to 190 MPa, less than or equal to 180 MPa, less than or equal to 170 MPa, less than or equal to 160 MPa, less than or equal to 150 MPa or less. In an embodiment, CS k Less than or equal to MPa (where t is the thickness of the glass-based article in millimeters) or less. CS k The range may be within any range defined between the above values. k The high level of protection of the glass-based article prevents the glass-based article from breaking due to a mechanism that introduces sharp damage combined with bending of the glass-based article while or after the sharp damage is introduced, such as by being dropped on a rough surface.

[0121] The stress profiles described herein may be characterized by a high level of compressive stress at a depth close to the depth of compression. In an embodiment, the compressive stress of the glass-based article at a depth of 0.6·DOC from the first surface is greater than or equal to 45 MPa, such as greater than or equal to 50 MPa, greater than or equal to 55 MPa, or greater than or equal to 59 MPa. In an embodiment, the compressive stress of the glass-based article at a depth of 0.65·DOC from the first surface is greater than or equal to 40 MPa, such as greater than or equal to 45 MPa, greater than or equal to 50 MPa, or greater than or equal to 55 MPa. In an embodiment, the compressive stress of the glass-based article at a depth of 0.7·DOC from the first surface is greater than or equal to 37 MPa, such as greater than or equal to 41 MPa or greater than or equal to 45 MPa. In an embodiment, the compressive stress of the glass-based article at a depth of 0.75·DOC from the first surface is greater than or equal to 32 MPa, such as greater than or equal to 35 MPa or greater than or equal to 38 MPa. In an embodiment, the compressive stress of the glass-based article at a depth of 0.8·DOC from the first surface is greater than or equal to 26 MPa, such as greater than or equal to 29 MPa or greater than or equal to 32 MPa. In an embodiment, the compressive stress of the glass-based article at a depth of 0.85·DOC from the first surface is greater than or equal to 18 MPa, such as greater than or equal to 20 MPa or greater than or equal to 23 MPa. In an embodiment, the compressive stress of the glass-based article at a depth of 0.9·DOC from the first surface is greater than or equal to 11 MPa, such as greater than or equal to 13 MPa or greater than or equal to 15 MPa. High compressive stress in the deep portion of the stress profile can improve fracture resistance, as demonstrated by improved performance in a drop test.

[0122] In one or more embodiments, the glass-based article comprises a depth of compression (DOC) greater than or equal to 0.15t (where t is the thickness of the glass-based article), such as greater than or equal to 0.16t, greater than or equal to 0.17t, greater than or equal to 0.18t, greater than or equal to 0.19t, greater than or equal to 0.20t, greater than or equal to 0.21t, greater than or equal to 0.22t, greater than or equal to 0.23t, or greater. In an embodiment, the DOC is greater than or equal to 130 μm, such as greater than or equal to 140 μm, greater than or equal to 150 μm, greater than or equal to 160 μm, greater than or equal to 170 μm, greater than or equal to 180 μm, or greater. In an embodiment, the DOC is less than or equal to 0.30t, where t is the thickness of the glass-based article, such as less than or equal to 0.29t, less than or equal to 0.28t, less than or equal to 0.27t, less than or equal to 0.26t, less than or equal to 0.25t, less than or equal to 0.24t, or less. In an embodiment, the DOC is less than or equal to 300 MPa, such as less than or equal to 250 MPa, less than or equal to 200 MPa, or less. The DOC may fall within a range formed between any of the above values.

[0123] In one or more embodiments, the glass-based article comprises a peak layer depth (DOL) greater than or equal to 0.003t (where t is the thickness of the glass-based article). sp ), for example, greater than or equal to 0.004t, greater than or equal to 0.005t, greater than or equal to 0.006t, greater than or equal to 0.007t, greater than or equal to 0.008t, greater than or equal to 0.009t, greater than or equal to 0.01t or greater. In an embodiment, DOL sp In an embodiment, DOL is greater than or equal to 3 μm, for example, greater than or equal to 3.5 μm, greater than or equal to 4 μm, greater than or equal to 4.5 μm, greater than or equal to 5 μm, greater than or equal to 5.5 μm or greater. sp Less than or equal to 15 μm, for example, less than or equal to 14 μm, less than or equal to 13 μm, less than or equal to 12 μm, less than or equal to 11 μm or less. DOL sp The range may be within any of the above values.

[0124] The stress distribution described herein may have a local maximum in the absolute value of the slope near the DOC. In an embodiment, the stress distribution has a local maximum in the absolute value of the slope within 0.1 DOC of the DOC, such as within 0.09 DOC of the DOC, within 0.08 DOC of the DOC, within 0.07 DOC of the DOC, within 0.06 DOC of the DOC, within 0.05 DOC of the DOC, within 0.04 DOC of the DOC, within 0.03 of the DOC, within 0.02 DOC of the DOC, within 0.01 DOC of the DOC, or at the DOC. The slope of the stress distribution can be calculated based on the polynomial fit described above, and the slope is given by the derivative of the fitting polynomial. The local maximum in the absolute value of the slope of the stress distribution near the DOC indicates that the compressive stress at the depth close to the DOC is higher. As shown in the improved drop performance, the compressive stress increased at a large depth can provide improved fracture resistance. In some embodiments, a local maximum in the absolute value of the slope of the stress distribution may be located at a curvature transition point.

[0125] The glass-based article may have any suitable thickness. In one or more embodiments, the glass-based article has a thickness (t) of greater than or equal to 0.2 mm to less than or equal to 2.0 mm, such as greater than or equal to 0.3 mm to less than or equal to 1.0 mm, greater than or equal to 0.4 mm to less than or equal to 0.9 mm, greater than or equal to 0.5 mm to less than or equal to 0.8 mm, greater than or equal to 0.6 mm to less than or equal to 0.7 mm. In an embodiment, the glass-based article may have a thickness (t) of about 0.75 mm. The thickness (t) may fall within a range formed between any of the above values. The thickness of the glass-based article may be determined by the thickness of the glass-based substrate used to produce the glass-based article. In an embodiment, the thickness of the glass-based article may be less than the thickness of the glass-based substrate used to form the glass-based article due to IOX post-processing such as surface polishing or etching.

[0126] In one or more embodiments, the center of the glass-based article comprises a Li2O / Na2O molar ratio of greater than or equal to 3.3, such as greater than or equal to 4, greater than or equal to 5, greater than or equal to 6, or greater. In an embodiment, the center of the glass-based article comprises a Li2O / Na2O molar ratio of less than or equal to 100, such as less than or equal to 60 or more. The Li2O / Na2O molar ratio at the center of the glass-based article may fall within a range formed between any of the above values. The Li2O / Na2O molar ratio at the center of the glass-based article may be equal to the Li2O / Na2O molar ratio of the glass-based substrate used to form the glass-based article.

[0127] The glass-based article may include Li2O. In one or more embodiments, the center of the glass-based article comprises a molar concentration of Li2O greater than or equal to 8 mol%, such as greater than or equal to 8.5 mol%, greater than or equal to 9 mol%, greater than or equal to 9.5 mol%, greater than or equal to 10 mol%, greater than or equal to 10.5 mol%, greater than or equal to 11 mol%, greater than or equal to 11.5 mol%, or more.

[0128] In embodiments, the glass-based articles described herein are non-brittle. Without wishing to be bound by any particular theory, the non-brittle nature of the glass-based substrate may be due, at least in part, to the shape of the stress profile and the high fracture toughness of the glass-based substrate used to form the glass-based article, particularly in light of the high peak tension of the stress profile. The shape of the stress profile is characterized, at least in part, by the region of negative curvature described above. For example, previously known glass-based articles having peak tension values ​​within the range of the stress profiles described herein are brittle.

[0129] In an embodiment, the stress profile of the glass-based article may have a tensile stress factor (K T ), for example, greater than or equal to 1.45 MPa·√m, greater than or equal to 1.49 MPa·√m, greater than or equal to 1.50 MPa·√m or greater. T As used herein, the tensile stress factor (K) is given by the following equation: T ):

[0130]

[0131] where σ is the stress represented by an in-plane component (assuming that the in-plane components are equal), and z is the position in the thickness direction. K T The stress value under integration should be in MPa, and the thickness position scale z should be in m. The calculation for K can be generated similarly to the description of the second-order derivative above. T Polynomial fit of the stress profile in the tension region of 0.001 Å with a value of 0.001 Å. The high tensile stress factor of the stress profile described herein represents the amount of stress imparted to the glass-based article by the ion exchange treatment and may be affected by the shape of the stress profile in the tension region.

[0132] The glass-based articles described herein may also be characterized by an amount of potassium added to the glass-based substrate during the ion exchange process. The glass-based article may have a maximum increase in K2O concentration of 7.5 mol% or less, such as 7.0 mol% or less, 6.5 mol% or less, 6.0 mol% or less, 5.5 mol% or less, or less, relative to the K2O concentration at the center of the glass-based article. The glass-based article may have a maximum increase in K2O concentration of 1.5 mol% or more, such as 2.0 mol% or more, 3.0 mol% or more, 4.0 mol% or more, 4.5 mol% or more, or more, relative to the K2O concentration at the center of the glass-based article. The maximum increase in K2O concentration relative to the K2O concentration at the center of the glass-based article may fall within a range formed between any of the above values. In addition to the fracture resistance provided by the high compressive stress in the spike, the K2O concentration in the spike can increase the ability of the glass-based article to resist lateral crack formation during scratching.

[0133] In embodiments, the glass-based article may have an average K2O concentration within the first 1 μm from the surface that is 6.7 mol% or less greater than the K2O concentration at the center of the glass-based article, such as 6.2 mol% or less, 5.7 mol% or less, 5.3 mol% or less, 4.9 mol% or less, or less. In embodiments, the glass-based article may have an average K2O concentration within the first 1 μm from the surface that is 1.0 mol% or more greater than the K2O concentration at the center of the glass-based article, such as 2.0 mol% or more, 3.0 mol% or more, or more. The value by which the average K2O concentration within the first 1 μm from the surface is greater than the K2O concentration at the center of the glass-based article may fall within a range formed between any of the aforementioned values.

[0134] In embodiments, the glass-based article may have an average K2O concentration within the first 1.5 μm from the surface that is 6.3 mol% or less greater than the K2O concentration at the center of the glass-based article, such as 5.8 mol% or less, 5.3 mol% or less, 4.9 mol% or less, 4.6 mol% or less, or less. In embodiments, the glass-based article may have an average K2O concentration within the first 1.5 μm from the surface that is 1.0 mol% or more greater than the K2O concentration at the center of the glass-based article, such as 2.0 mol% or more, 3.0 mol% or more, or more. The value by which the average K2O concentration within the first 1.5 μm from the surface is greater than the K2O concentration at the center of the glass-based article may fall within a range formed between any of the aforementioned values.

[0135] In embodiments, the glass-based article may have an average K2O concentration within the first 2 μm from the surface that is 5.9 mol% or less greater than the K2O concentration at the center of the glass-based article, such as 5.4 mol% or less, 4.9 mol% or less, 4.5 mol% or less, 4.1 mol% or less, or less. In embodiments, the glass-based article may have an average K2O concentration within the first 2 μm from the surface that is 1.0 mol% or more greater than the K2O concentration at the center of the glass-based article, such as 2.0 mol% or more, 3.0 mol% or more, or more. The value by which the average K2O concentration within the first 2 μm from the surface is greater than the K2O concentration at the center of the glass-based article may fall within a range formed between any of the aforementioned values.

[0136] The K2O concentration in the peak region may be characterized in that the integral of the K2O concentration in the peak region is greater than the K2O concentration at the center of the glass-based article. In an embodiment, in the peak region, the integral of the increase in the K2O concentration relative to the K2O concentration at the center of the glass-based article is less than or equal to 29 mol%·μm, for example, less than or equal to 25 mol%·μm, less than or equal to 20 mol%·μm, less than or equal to 16 mol%·μm, less than or equal to 12 mol%·μm, or less. In an embodiment, in the peak region, the integral of the increase in the K2O concentration relative to the K2O concentration at the center of the glass-based article is greater than or equal to 4 mol%·μm, for example, greater than or equal to 6 mol%·μm, greater than or equal to 8 mol%·μm, or greater. The integral of the increase in the K2O concentration in the peak region relative to the K2O concentration at the center of the glass-based article may fall within a range formed between any of the above values.

[0137] The glass-based articles described herein may be characterized by a Na2O concentration profile. In an embodiment, a region of the glass-based article from 0.025t or more to 0.25t or less has a Na2O concentration profile that has a positive curvature or no curvature. In other words, in an embodiment, a region of the glass-based article from 0.025t or more to 0.25t or less has a Na2O concentration profile that has no negative curvature.

[0138] Glass articles having stress profiles as described herein provide an overall advantage of improved fracture resistance when multiple failure modes are considered simultaneously, namely, excessive stresses caused by being dropped on a smooth hard surface (e.g., by using a glass article having a high CS and a deep DOL). spThe stress profiles described herein can also be generated at faster 10X times when using lithium-containing glass-based substrates.

[0139] Glass-based articles may be characterized by any or all of the properties and features described herein. For example, stress profiles of the type described herein may be characterized by any combination of the properties described herein.

[0140] Glass-based substrate

[0141] Examples of glass that can be used as a substrate may include alkali aluminosilicate glass compositions or alkali-containing aluminoborosilicate glass compositions, but other glass compositions are also contemplated. Specific examples of glass-based substrates that can be used include, but are not limited to, alkali aluminosilicate glass, alkali-containing borosilicate glass, alkali aluminoborosilicate glass, alkali-containing lithium aluminosilicate glass, or alkali-containing phosphate glass. Glass-based substrates have a base composition that is characterized as being ion-exchangeable. As used herein, "ion exchangeable" means that a substrate comprising a composition is capable of exchanging cations located at or near the substrate surface with cations of the same value that are larger or smaller in size. In one or more embodiments, the glass-based substrate may include a lithium-containing aluminosilicate.

[0142] In embodiments, the glass-based substrate may be formed from any composition capable of forming a stress profile. In some embodiments, the glass-based substrate may be formed from a glass composition described in U.S. Patent Application No. 16 / 370,002, filed on March 29, 2019, entitled “Glasses Having High Fracture Toughness,” the entire contents of which are incorporated herein by reference.

[0143] In an embodiment, a glass-based substrate may be formed from a composition comprising: 50 mol% to 69 mol% SiO2; 12.5 mol% to 25 mol% Al2O3; 0 mol% to 8 mol% B2O3; greater than 0 mol% to 4 mol% CaO; greater than 0 mol% to 17.5 mol% MgO; 0.5 mol% to 8 mol% Na2O; 0 mol% to 2.5 mol% La2O3; and greater than 8 mol% to 18 mol% Li2O; wherein: (Li2O+Na2O+MgO) / Al2O3 is from 0.9 to less than 1.3; and Al2O3+MgO+Li2O+ZrO2+La2O3+Y2O3 is from greater than 23 mol% to less than 50 mol%.

[0144] In an embodiment, a glass-based substrate may be formed from a composition comprising: SiO2; Al2O3; and Li2O, wherein the glass is characterized by: a K greater than or equal to 0.85 MPa√m 1C value.

[0145] The stress profile having the desirable properties described herein can potentially be obtained in a lithium-free Na-containing glass by performing a two-step ion exchange in a bath containing different ratios of Na and K. However, in this case, the ion exchange time is long (on the order of several days) and the fracture toughness of the glass composition is low. Therefore, it is preferred to use a lithium-containing glass-based substrate for producing a glass-based article having a desired stress profile.

[0146] The glass-based substrate may include Li2O. In one or more embodiments, the glass-based substrate includes Li2O at a molar concentration of greater than or equal to 8 mol%, such as greater than or equal to 8.5 mol%, greater than or equal to 9 mol%, greater than or equal to 9.5 mol%, greater than or equal to 10 mol%, greater than or equal to 10.5 mol%, greater than or equal to 11 mol%, greater than or equal to 11.5 mol%, or greater. Including Li2O in the glass-based substrate may increase the fracture toughness of the glass-based substrate and may reduce the time required to generate a desired stress profile via ion exchange.

[0147] The glass-based substrate may be characterized by the manner in which the glass-based substrate is formed. For example, the glass-based substrate may be characterized as being float formable (i.e., formed by a float process), down-draw formable, and specifically, fusion formable or slot drawable (i.e., formed by a down-draw process such as a fusion draw process or a slot draw process).

[0148] Ion Exchange (IOX) Treatment

[0149] The chemical strengthening of the glass-based substrate having the base composition is performed by placing the ion-exchangeable glass-based substrate in a solution containing cations (e.g., K +、Na + 、Ag + The cations diffuse into the glass, while the smaller alkali ions (e.g., Na + , Li + ) diffuse into the molten bath. Replacing smaller cations with larger cations creates compressive stresses near the top surface of the glass-based article. Tensile stresses are created in the interior of the glass-based article that balance the near-surface compressive stresses.

[0150] Regarding the ion exchange process, it can be an independent thermal diffusion process or an electrodiffusion process. Non-limiting examples of ion exchange processes in which a glass-based substrate is immersed in multiple ion exchange baths and a cleaning and / or annealing step is performed between immersions are described in U.S. Patent No. 8,561,429, entitled "Glass with Compressive Surface for Consumer Applications" by Douglas C. Allan et al., published on October 22, 2013, which claims priority to U.S. Provisional Patent Application No. 61 / 079,995 filed on July 11, 2008, for strengthening glass by immersing it in salt baths of different concentrations in multiple consecutive ion exchange treatments; and Christopher M. Lee et al., entitled "Dual Stage Ion Exchange for Chemical Strengthening of No. 8,312,739, filed on July 29, 2008, wherein the glass is strengthened by ion exchange by immersing the glass in a first bath diluted with effluent ions and then in a second bath having a lower concentration of effluent ions than the first bath. The contents of U.S. Pat. Nos. 8,561,429 and 8,312,739 are incorporated herein by reference in their entirety.

[0151] The bath used to ion exchange the glass-based substrate to form the glass-based articles disclosed herein may include a mixture of salts. For example, the ion exchange bath may include a mixture of sodium nitrate and potassium nitrate without lithium nitrate. In other embodiments, the ion exchange bath may include a mixture of sodium nitrate, potassium nitrate, and lithium nitrate. The bath may also include silicic acid, for example in an amount of about 0.5% by weight of the total amount of nitrates.

[0152] The ion exchange process is preferably performed in a single step. For example, a single ion exchange bath may be used to produce the glass-based article. In embodiments, a multi-step ion exchange process may be utilized to form the glass-based article, such as an ion exchange process having two or more bath processes.

[0153] After the ion exchange process is performed, it is understood that the composition of the surface of the glass-based article is different from the composition of the formed glass-based substrate. This is due to the presence of one type of alkali metal ion (such as Li + Or Na + ) are respectively replaced by larger alkali metal ions (such as, for example, Na + or K + However, in embodiments, the composition at or near the center of the depth of the glass-based article will still be the same as the composition of the formed glass-based substrate.

[0154] Final product

[0155] The glass-based articles disclosed herein can be incorporated into another article, for example, an article having a display (or display article) (e.g., consumer electronic devices, including smartphones, tablets, computers, navigation systems, etc.); architectural articles; transportation articles (e.g., cars, trains, aircraft, ships, etc.); appliance articles or any article requiring a certain degree of transparency, scratch resistance, abrasion resistance, or a combination of the above properties. Figure 4A and 4A Exemplary articles comprising any of the glass articles disclosed herein are shown. Specifically, Figure 4A and 4B A consumer electronic device 200 is shown, which includes a housing 202 having a front surface 204, a rear surface 206, and side surfaces 208; electrical components (not shown) at least partially or completely located within the housing and including at least a controller, a memory, and a display 210, the display being located at or adjacent to the front surface of the housing; and a cover substrate 212 at or above the front surface of the housing such that the cover substrate 212 is above the display. In some embodiments, the cover substrate 212 can include any glass article disclosed herein.

[0156] Example

[0157] The embodiments are further described by the following examples. It should be understood that these examples do not limit the above embodiments.

[0158] A glass substrate having the following composition was formed: 58.35 mol% SiO2, 17.81 mol% Al2O3, 6.07 mol% B2O3, 1.73 mol% Na2O, 0.20 mol% K2O, 10.74 mol% Li2O, 4.43 mol% MgO, 0.57 mol% CaO, and 0.08 mol% SnO2.

[0159] Example 1

[0160] A glass-based substrate having a thickness of 0.8 mm was ion exchanged in a bath containing 7 wt % NaNO3 and 93 wt % KNO3 and substantially no LiNO3 for a period of 12 hours to form the glass-based article of Example 1. The bath was maintained at a temperature of 450°C and silicate was added to the bath at a level of 0.5% of the total weight of nitrates. The stress distribution of Example 1 is shown in Figure 7 The stress profile of Example 1 is substantially symmetrical. Example 1 has a DOC of 189.5 μm (0.237 t). The stress profile is non-brittle.

[0161] Figure 8 The measured deep portion of the stress distribution of Example 1 is shown, along with a third-order polynomial fit (dashed line). The measured stress distribution was smoothed using the LOESS smoothing algorithm before the polynomial fit was performed. The polynomial fit was performed in the depth region of 19 μm to 300 μm to avoid oscillations at the base of the peaks in the measured stress distribution. The oscillations are an artifact of the RNF stress distribution extraction method, not a feature of the stress distribution.

[0162] Fig. 9 for Figure 8 A graph of the second derivative of a polynomial fit to . Fig. 9 As shown, the value of the second derivative is zero, indicating the curvature transition point at 189.5 μm (0.237 t) or approximately the depth of compression. Fig. 9 The minimum value of the second-order derivative is -9080MPa / mm 2 , and occurs at the calculated minimum depth.

[0163] Example 2

[0164] A glass-based substrate having a thickness of 0.81 mm was ion exchanged in a bath containing 2 wt% LiNO3, 12 wt% NaNO3, and 86 wt% KNO3 for a period of 8.4 hours to form the glass-based article of Example 2. The bath was maintained at a temperature of 450°C, and silicate was added to the bath at a level of 0.5% of the total weight of nitrates. The stress distribution of Example 2 is shown in Fig.10The stress distribution of Example 2 is substantially symmetrical. Example 2 has a DOC of 174 μm (0.215 t), a CS of 603 MPa, and a 最大 , 5.41μm DOL sp , CS of 141.2MPa k , PT of 101.9 MPa at the center of the glass-based article. The depth integral of the compressive stress region in each compressive stress region is 15.896 MPa·mm, and the depth integral of the compressive stress in the first 10 μm is 2.686 MPa·mm. The stress distribution is not brittle.

[0165] Fig.11 The measured stress distribution of Example 2 is shown in the deep part, and the third-order polynomial fit. Before the polynomial fit, the measured stress distribution is smoothed using the LOESS smoothing algorithm. The polynomial fit is performed in the depth region of 20 μm to 220 μm.

[0166] Fig.12 for Fig.11 A graph of the second derivative of a polynomial fit to . Fig.12 As shown, the value of the second derivative is zero, indicating a curvature transition point at 149.2 μm (0.857·DOC; 0.184t). Fig.12 The minimum value of the second-order derivative is -12670MPa / mm 2 , and occurs at the calculated minimum depth.

[0167] Example 3

[0168] A glass-based substrate having a thickness of 0.761 mm was ion exchanged in a bath containing 1.2 wt % LiNO3, 10 wt % NaNO3, and 88.8 wt % KNO3 for a period of 8.4 hours to form the glass-based article of Example 3. The bath was maintained at a temperature of 447°C, and silicate was added to the bath at a level of 0.5% of the total weight of nitrates. The stress distribution of Example 3 is shown in Fig.13 The stress distribution of Example 3 is substantially symmetrical. Example 3 has a DOC of 164 μm (0.2155 t), a CS of 646 MPa, and a 最大 , 5.41μm DOL sp , CS of 156MPa k , PT of 108 MPa at the center of the glass-based article. The depth integral of the compressive stress region in each compressive stress region is 15.753 MPa·mm (20.7 t), and the depth integral of the compressive stress in the first 10 μm is 2.9 MPa·mm (3.8 t). The stress distribution is not brittle.

[0169] Fig.14 The measured stress distribution of Example 3 is shown in the deep part, and the third-order polynomial fit (dashed line). Before the polynomial fit, the measured stress distribution was smoothed using the LOESS smoothing algorithm. The polynomial fit was performed in the depth region of 7 μm to 250 μm.

[0170] Fig.15 for Fig.14 A graph of the second derivative of a polynomial fit to . Fig.15 As shown, the value of the second derivative is zero, indicating a curvature transition point at 139.3 μm (0.85·DOC; 0.183t). Fig.15 The minimum value of the second-order derivative is -15651MPa / mm 2 , and occurs at the calculated minimum depth.

[0171] Example 4

[0172] A glass-based substrate having a thickness of 0.658 mm was ion exchanged in a bath containing 1.2 wt % LiNO3, 10 wt % NaNO3 and 88.8 wt % KNO3 for a period of 7 hours to form the glass-based article of Example 4. The bath was maintained at a temperature of 447°C and silicate was added to the bath at a level of 0.5% of the total weight of nitrates. The stress distribution of Example 4 is shown in Fig.16 The stress distribution of Example 4 is substantially symmetrical. Example 4 has a DOC of 149 μm (0.226 t), a CS of 640 MPa, and a 最大 , 4.96μm DOL sp , CS of 152MPa k , PT of 121 MPa at the center of the glass-based article. The depth integral of the compressive stress region in each compressive stress region is 14.5 MPa·mm (22.04 t), and the depth integral of the compressive stress in the first 10 μm is 2.54 MPa·mm (3.86 t). The stress distribution is not brittle.

[0173] Fig.17 The measured stress distribution of Example 4 is shown in the deep part, and the third-order polynomial fit (dashed line). Before the polynomial fit, the measured stress distribution is smoothed using the LOESS smoothing algorithm. The polynomial fit is performed in the depth region of 5 μm to 198 μm (0.3t).

[0174] Fig.18 for Fig.17 A graph of the second derivative of a polynomial fit to . Fig.18 As shown, the value of the second derivative is zero, indicating the curvature transition point at 127 μm (0.853·DOC; 0.193t). Fig.18 The minimum value of the second-order derivative is -17026MPa / mm 2 , and appears at a depth of 16.5μm. Fig.16 The maximum absolute value of the negative slope of the deep portion of the stress distribution is 1.381 MPa / μm at a depth of 127 μm. The slope of the stress distribution at the DOC is -1.34 MPa / μm.

[0175] Example 5

[0176] A glass-based substrate having a thickness of 0.538 mm was ion exchanged in a bath containing 1.2 wt % LiNO3, 10 wt % NaNO3, and 88.8 wt % KNO3 for a period of 7 hours to form the glass-based article of Example 5. The bath was maintained at a temperature of 447°C, and silicate was added to the bath at a level of 0.5% of the total weight of nitrates. The stress distribution of Example 5 is shown in Fig.19 The stress distribution of Example 5 is substantially symmetrical. Example 5 has a DOC of 123 μm (0.226 t), a CS of 621 MPa, and a 最大 , 4.8μm DOL sp , CS in the range of 120MPa to 130MPa k , PT of 134.9 MPa at the center of the glass-based article. The depth integral of the compressive stress region in each compressive stress region is 9.78 MPa·mm (18.2 t), and the depth integral of the compressive stress in the first 10 μm is 2.3 MPa·mm (4.3 t). The stress distribution is not brittle.

[0177] Fig. 20 The measured stress distribution of Example 5 is shown in the deep part, and the third-order polynomial fit (dashed line). Before the polynomial fit, the measured stress distribution is smoothed using the LOESS smoothing algorithm. The polynomial fit is performed in the depth region of 5.5 μm to 161 μm (0.3t).

[0178] Fig.21 for Fig. 20 A graph of the second derivative of a polynomial fit to . Fig.21 As shown, the value of the second derivative is zero, indicating the curvature transition point at 145 μm (1.19·DOC; 0.27t). Fig.18 The minimum value of the second-order derivative is -16500MPa / mm 2 , and appears at a depth of 13.5μm. Fig.19 The maximum absolute value of the negative slope of the deep portion of the stress distribution is 1.45 MPa / μm at a depth of 145 μm. The slope of the stress distribution at the DOC is -1.42 MPa / μm.

[0179] Example 6

[0180] A glass-based substrate having a thickness of 0.658 mm was ion exchanged in a bath containing 1.4 wt% LiNO3, 10 wt% NaNO3, and 88.6 wt% KNO3 for a period of 7.33 hours to form the glass-based article of Example 6. The bath was maintained at a temperature of 447°C, and silicate was added to the bath at a level of 0.5% of the total weight of nitrates. The stress profile of Example 6 was substantially symmetrical. Example 6 had a DOC of 140 μm, a CS of 630 MPa, and a TEM of 1.40 μm. 最大 , 4.7μm DOL sp , CS in the range of 141MPa k , PT of 123 MPa at the center of the glass-based article. The depth integral of the compressive stress region in each compressive stress region is 12.3 MPa·mm (19.6 t). The stress distribution is not brittle. A third-order polynomial fit is performed in the depth region from 5.5 μm to 0.3 t, and R 2 The value is 0.9996. The value of the second-order derivative is zero, indicating that the curvature transition point is at 135μm (0.96t). The minimum value of the second-order derivative in the region from 0.025t to 0.25t is -13900MPa / mm 2 The maximum absolute value of the negative slope of the deep portion of the stress distribution is 1.306 MPa / μm at a depth of 135 μm. The slope of the stress distribution at the DOC is -1.304 MPa / μm.

[0181] Comparative Example

[0182] Preparation of Comparative Glass-Based Articles The compositions of the glass-based substrates used to form the comparative glass-based substrates are given in Table 1. The thickness of all glass-based substrates used to form the comparative examples was 0.8 mm.

[0183] Table 1

[0184]

[0185]

[0186] Table 2 below provides the ion exchange treatments used for the comparative examples.

[0187] Table 2

[0188]

[0189] Table 3 below provides the measured properties of the comparative examples. Comparative Example 1 is the only comparative example that exhibits a negative curvature region. The minimum value of the second-order derivative of Comparative Example 1 in the region from greater than or equal to 0.025t to less than or equal to 0.25t is greater than -3000 MPa / mm 2 , and the curvature inflection point is about 0.58·DOC.

[0190] Table 3

[0191]

[0192] Unless otherwise stated, all composition components, relationships and ratios described in this specification are provided in mole %. Regardless of whether explicitly stated before or after the disclosed range, all ranges disclosed in this specification include any and all ranges and sub-ranges encompassed by the broadly disclosed range.

[0193] It is obvious to those skilled in the art that various modifications and changes can be made to the embodiments described herein without departing from the spirit and scope of the subject matter of the patent right. Therefore, this specification is intended to cover the modifications and changes of the various embodiments described herein, as long as these modifications and changes are within the scope of the attached claims and their equivalents.

Claims

1. A glass-based product comprising: a glass-based substrate comprising opposing first and second surfaces defining a substrate thickness (t); and Stress distribution, the stress distribution comprising: A peak tension (PT) greater than or equal to 70 MPa; and The second-order derivative value is less than or equal to -5000MPa / mm 2 A point, wherein the point is located in the region of greater than or equal to 0.025t to less than or equal to 0.25t.

2. The glass-based article of claim 1, wherein the stress distribution comprises a second-order derivative value of 0 MPa / mm 2 A curvature transition point, wherein the curvature transition point is located in a region greater than or equal to 0.025t to less than or equal to 0.25t.

3. The glass-based article of claim 1 or 2, wherein the stress distribution comprises a second-order derivative value of 0 MPa / mm 2 A curvature transition point, wherein the curvature transition point is located in a region from greater than or equal to 0.7·DOC to less than or equal to 0.25t.

4. The glass-based article of claim 1 or 2, wherein the stress distribution comprises a second-order derivative value less than or equal to -2550 / t 2 MPa / mm 2 A point, where t is in mm, and where the point is located in the region from greater than or equal to 0.025 t to less than or equal to 0.25 t.

5. The glass-based article of claim 1 or 2, comprising a compression region extending from the first surface to a depth of compression (DOC), wherein the stress profile comprises a local maximum in the absolute value of the slope within 0.1·DOC of the DOC. 6 . The glass-based article according to claim 5 , wherein a local maximum value of the absolute value of the slope is greater than or equal to 0.5 MPa / μm.

7. The glass-based article of claim 1 or 2, wherein the PT is greater than or equal to 80 MPa.

8. The glass-based article of claim 1 or 2, wherein the PT is less than or equal to 200 MPa.

9. The glass-based article of claim 1 or 2, wherein the PT is greater than or equal to MPa, where the unit of t is mm.

10. The glass-based article of claim 1 or 2, wherein the PT is less than or equal to MPa, where the unit of t is mm.

11. The glass-based article of claim 1 or 2, wherein the glass-based substrate having the same composition and structure as the center of the glass-based article has a K greater than or equal to 0.85 MPa√m. IC .

12. The glass-based article of claim 1 or 2, wherein the glass-based substrate having the same composition and structure as the center of the glass-based article has a K of less than or equal to 2 MPa√m. IC .

13. The glass-based article of claim 1 or 2, comprising a knee compressive stress (CS) greater than or equal to 80 MPa. k ).

14. The glass-based article according to claim 1 or 2, comprising greater than or equal to MPa knee compression stress (CS k ), where t is in mm.

15. The glass-based article of claim 1 or 2, comprising a compression region extending from the first surface to a depth of compression (DOC), and the DOC is greater than or equal to 0.15t.

16. The glass-based article of claim 1 or 2, comprising a compressed region extending from the first surface to a depth of compression (DOC), and the DOC is greater than or equal to 130 μm.

17. The glass-based article of claim 1 or 2, comprising a compressive stress greater than or equal to 330 MPa.

18. The glass-based article of claim 1 or 2, comprising a peak region extending from the first surface to a depth of layer (DOL) of the peak region. sp ), and the DOL sp is greater than or equal to 3 μm.

19. The glass-based article of claim 1 or 2, comprising a peak region extending from the first surface to a depth of layer (DOL) of the peak region. sp ), and the DOL sp Less than or equal to 15 μm.

20. The glass-based article of claim 1 or 2, wherein the stress profile comprises: a first compression region, a second compression region, and a tension region, the first compression region extending from the first surface to a first compression depth DOC1, the second compression region extending from the second surface to a second compression depth DOC2, and the tension region extending from DOC1 to DOC2, The tension region has a tensile stress factor K greater than or equal to 1.41 MPa·√m T .

21. The glass-based article of claim 1 or 2, wherein the glass-based article is non-breakable.

22. The glass-based article of claim 1 or 2, comprising Li2O.

23. The glass-based article of claim 1 or 2, wherein the Li2O concentration at the center of the glass-based article is greater than or equal to 8 mol%.

24. The glass-based article of claim 1 or 2, wherein the maximum K2O concentration in the glass-based article is 7.5 mol% or less greater than the K2O concentration at the center of the glass-based article.

25. The glass-based article of claim 1 or 2, comprising a peak region extending from the first surface to a depth of layer (DOL) of the peak region. sp ), wherein in the peak region, the integral of the increase in K2O concentration relative to the K2O concentration at the center of the glass-based article is less than or equal to 29 mol%·μm.

26. The glass-based article of claim 1 or 2, comprising a peak region extending from the first surface to a depth of layer (DOL) of the peak region. sp ), wherein in the peak region, the integral of the increase in K2O concentration relative to the K2O concentration at the center of the glass-based article is greater than or equal to 4 mol%·μm.

27. The glass-based article of claim 1 or 2, wherein the center of the glass-based article has a Li2O / Na2O molar ratio greater than or equal to 3.

3.

28. The glass-based article of claim 1 or 2, wherein the center of the glass-based article has a Li2O / Na2O molar ratio of less than or equal to 100.

29. The glass-based article of claim 1 or 2, wherein t is greater than or equal to 0.2 mm and less than or equal to 2.0 mm.

30. The glass-based article of claim 1 or 2, wherein t is greater than or equal to 0.3 mm to less than or equal to 1.0 mm.

31. The glass-based article of claim 1 or 2, comprising a compressive region extending from the first surface to a depth of compression (DOC), and a compressive stress at a depth of 0.6·DOC from the first surface is greater than or equal to 45 MPa.

32. The glass-based article of claim 1 or 2, comprising a compressive region extending from the first surface to a depth of compression (DOC), and having a compressive stress greater than or equal to 40 MPa at a depth of 0.65·DOC from the first surface.

33. The glass-based article of claim 1 or 2, comprising a compressive region extending from the first surface to a depth of compression (DOC), and a compressive stress at a depth of 0.7·DOC from the first surface is greater than or equal to 37 MPa.

34. The glass-based article of claim 1 or 2, comprising a compressive region extending from the first surface to a depth of compression (DOC), and a compressive stress at a depth of 0.75·DOC from the first surface is greater than or equal to 32 MPa.

35. The glass-based article of claim 1 or 2, comprising a compressive region extending from the first surface to a depth of compression (DOC), and a compressive stress at a depth of 0.8·DOC from the first surface is greater than or equal to 26 MPa.

36. The glass-based article of claim 1 or 2, comprising a compressive region extending from the first surface to a depth of compression (DOC), and a compressive stress at a depth of 0.85·DOC from the first surface is greater than or equal to 18 MPa.

37. The glass-based article of claim 1 or 2, comprising a compressive region extending from the first surface to a depth of compression (DOC), and a compressive stress at a depth of 0.9·DOC from the first surface is greater than or equal to 11 MPa.

38. The glass-based article of claim 1 or 2, comprising a Na2O concentration distribution in a region from greater than or equal to 0.025t to less than or equal to 0.25t, wherein the Na2O concentration distribution exhibits a positive curvature or no curvature in a region from greater than or equal to 0.025t to less than or equal to 0.25t.

39. The glass-based article of claim 1 or 2, wherein the center of the glass-based article comprises: 50 mol % to 69 mol % SiO2; 12.5 mol% to 25 mol% Al2O3; 0 mol % to 8 mol % B2O3; greater than 0 mol % to 4 mol % CaO; greater than 0 mol % to 17.5 mol % MgO; 0.5 mol% to 8 mol% Na2O; 0 mol % to 2.5 mol % La2O3; and greater than 8 mol% to 18 mol% Li2O; in: (Li2O+Na2O+MgO) / Al2O3 is from 0.9 to less than 1.3; and Al2O3+MgO+Li2O+ZrO2+La2O3+Y2O3 is from greater than 23 mol% to less than 50 mol%.

40. The glass-based article of claim 1 or 2, wherein the point has a second-order derivative value of -6000 MPa / mm 2 To -50000MPa / mm 2 .

41. The glass-based article of claim 40, wherein the point has a second-order derivative value of -7000 MPa / mm 2 To -40000MPa / mm 2 .

42. The glass-based article of claim 41, wherein the point has a second derivative value of -8000 MPa / mm 2 To -30000MPa / mm 2 .

43. A consumer electronic product comprising: A housing, the housing comprising a front surface, a rear surface and side surfaces; an electrical component, the electrical component being at least partially disposed within the housing, the electrical component comprising at least a controller, a memory, and a display, the display being disposed at or adjacent to a front surface of the housing; and A cover plate, which is arranged above the display; At least a portion of at least one of the housing and the cover plate comprises the glass-based article as claimed in claim 1 or 2.

44. A method comprising: A glass-based substrate is ion exchange treated to form a glass-based article, the glass-based substrate comprising a first surface and a second surface opposite each other, the first surface and the second surface defining a substrate thickness (t), the glass-based article having a stress profile, the stress profile comprising: A peak tension (PT) greater than or equal to 70 MPa; and The second-order derivative value is less than or equal to -5000MPa / mm 2 A point, wherein the point is located in the region of greater than or equal to 0.025t to less than or equal to 0.25t.

45. The method of claim 44, wherein the ion exchange treatment is a single ion exchange treatment.

46. ​​The method of any one of claims 44 or 45, wherein the glass-based substrate comprises: 50 mol % to 69 mol % SiO2; 12.5 mol% to 25 mol% Al2O3; 0 mol % to 8 mol % B2O3; greater than 0 mol % to 4 mol % CaO; greater than 0 mol % to 17.5 mol % MgO; 0.5 mol% to 8 mol% Na2O; 0 mol % to 2.5 mol % La2O3; and greater than 8 mol% to 18 mol% Li2O; in: (Li2O+Na2O+MgO) / Al2O3 is from 0.9 to less than 1.3; and Al2O3+MgO+Li2O+ZrO2+La2O3+Y2O3 is from greater than 23 mol% to less than 50 mol%.

47. The method of any one of claims 44 to 45, wherein the glass-based substrate comprises: SiO2; Al2O3; and Li2O, The glass is characterized in that: K is greater than or equal to 0.85 MPa√m 1C value.

48. The method of claim 44 or 45, wherein the point has a second derivative value of -6000 MPa / mm 2 To -50000MPa / mm 2 .

49. The method of claim 48, wherein the point has a second derivative value of -7000 MPa / mm 2 To -40000MPa / mm 2 .

50. The method of claim 49, wherein the point has a second derivative value of -8000 MPa / mm 2 To -30000MPa / mm 2 .