Secondary battery and electronic device

By installing coatings with different porosities on the separator of the secondary battery, the liquid storage capacity of the electrolyte is improved, and the problem of high demand for electrolyte is solved by the negative electrode sheet of silicon material, which improves circulation performance and safety.

CN119069772AActive Publication Date: 2024-12-03NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
CN202411389197.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

The negative electrode sheets containing silicon materials in existing secondary batteries have a high demand for electrolyte during circulation, resulting in insufficient liquid storage capacity and affecting circulation performance. Too much free electrolyte will increase slippage and safety risks.

Method used

By installing coatings with different porosities on the separator of the secondary battery, the porosity of the separator facing the negative electrode side is greater, so as to improve the liquid storage capacity of the electrolyte, and supply the electrolyte in time when the negative electrode sheet is required to reduce Risk of interface deterioration caused by insufficient electrolyte.

Benefits of technology

The circulating performance of the secondary battery is improved, and the risk of lithium excretion and circulation diving caused by insufficient electrolyte is reduced, while taking into account both drop performance and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069772A_ABST
    Figure CN119069772A_ABST
Patent Text Reader

Abstract

The invention provides a secondary battery and an electronic device, the secondary battery comprises an electrode assembly, the electrode assembly comprises a pole piece and a first diaphragm, the pole piece comprises a positive pole piece and a negative pole piece, the negative pole piece comprises a negative pole material layer, the negative pole material layer comprises a silicon element, based on the mass of the negative pole material layer, the mass percentage content of the silicon element is W, and W is greater than or equal to 3%. The first diaphragm comprises a base film, a first coating and a second coating, the base film comprises a first surface and a second surface along the thickness direction of the first diaphragm, the first surface faces the negative pole piece, the second surface faces the positive pole piece, the first coating is arranged on the first surface, and the second coating is arranged on the second surface. The porosity of the first coating is P1, the porosity of the second coating is P2, and P1 is larger than P2. Through the arrangement, the risk of negative electrode interface deterioration caused by insufficient electrolyte is reduced, and the cycle performance of the secondary battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to a secondary battery and an electronic device. Background Art

[0002] Secondary batteries, such as lithium-ion batteries, have the characteristics of large specific energy, high operating voltage, low self-discharge rate, small size and light weight, and are widely used in the field of consumer electronics.

[0003] As the demand for secondary battery energy density increases, silicon, as a material with a high gram capacity of 4200mAh / g, relatively low cost and environmentally friendly, is increasingly used in secondary battery systems. Due to the ultra-high gram capacity of current silicon materials, the negative electrode material layer containing silicon-based materials, especially when the proportion of silicon elements in the negative electrode material layer is high, has a low coating weight during coating, which is only about a quarter of that of traditional graphite materials, and the thickness is less than half of that of traditional graphite pole pieces. At this time, the electrolyte storage capacity of the negative electrode pole piece is relatively poor, and since the demand for electrolyte of silicon-based materials during the secondary battery cycle is higher than that of conventional graphite, higher requirements are placed on the liquid storage capacity of the negative electrode pole piece containing silicon materials. Summary of the invention

[0004] The purpose of the present application is to provide a secondary battery and an electronic device to improve the liquid storage capacity of the separator facing the negative electrode side, improve lithium plating at the negative electrode interface, and improve the cycle performance of the secondary battery.

[0005] It should be noted that in the invention content of the present application, a lithium-ion battery is used as an example of a secondary battery to explain the present application, but the secondary battery of the present application is not limited to a lithium-ion battery.

[0006] In the prior art, the problem of liquid storage of negative electrode plates containing silicon materials is mainly solved by retaining more electrolyte inside the secondary battery shell to increase the liquid storage capacity of the negative electrode plates. However, the excess electrolyte inside the shell will be stored in a free state and cannot be supplied and transmitted to the silicon-based material of the negative electrode plates in time. At this time, the excess free electrolyte will increase the sliding properties between the layers inside the electrode assembly, affecting the drop performance of the secondary battery. At the same time, when there is too much excess electrolyte, the secondary battery will swell and the shell may bulge, deform or crack. Based on this, the present application provides a secondary battery that can supply electrolyte in time when the negative electrode plate containing silicon elements needs electrolyte, thereby reducing the negative electrode interface ion conduction bridge breakage caused by insufficient electrolyte in the late cycle, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation or even cycle diving, thereby improving the cycle performance of the secondary battery. The specific technical scheme is as follows:

[0007] The first aspect of the present application provides a secondary battery, the secondary battery includes an electrode assembly, the electrode assembly includes a pole piece and a first diaphragm, the pole piece includes a positive pole piece and a negative pole piece, the negative pole piece includes a negative electrode material layer, the negative electrode material layer includes silicon element, based on the mass of the negative electrode material layer, the mass percentage of silicon element is W, W ≥ 3%. The first diaphragm includes a base film, a first coating and a second coating, along the thickness direction of the first diaphragm, the base film includes a first surface and a second surface, the first surface faces the negative pole piece, the second surface faces the positive pole piece, the first coating is arranged on the first surface, and the second coating is arranged on the second surface. The porosity of the first coating is P1, the porosity of the second coating is P2, P1>P2. In a secondary battery containing silicon, coatings with different porosities are applied to the positive and negative electrodes of the diaphragm in the secondary battery, so that the porosity of the coating facing the negative electrode side of the diaphragm is larger. At this time, the coating with larger porosity has more particle gaps, and the diaphragm facing the negative electrode side can absorb more electrolyte, thereby improving the liquid storage capacity of the diaphragm facing the negative electrode side, and being able to supply electrolyte in time when the negative electrode plate containing silicon needs electrolyte, thereby reducing the negative electrode interface ion conduction bridge breakage caused by insufficient electrolyte in the late cycle, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation and even cycle water diving, thereby improving the cycle performance of the secondary battery.

[0008] In some embodiments of the present application, 3%≤W≤80%. By adjusting the value of W within the above range, the risk of negative electrode interface deterioration caused by insufficient electrolyte is more significantly reduced, further improving the cycle performance of the secondary battery.

[0009] In some embodiments of the present application, the first coating layer includes a first ceramic layer, and the second coating layer includes a second ceramic layer. Through the above arrangement, the risk of deterioration of the negative electrode interface due to insufficient electrolyte is reduced, and the cycle performance of the secondary battery is improved. In some embodiments of the present application, 1<P1 / P2≤5, 30%≤P1≤70%. By regulating the values ​​of P1 / P2 and P1 within the above range, while taking into account the mechanical strength of the first diaphragm, the risk of deterioration of the negative electrode interface due to insufficient electrolyte is reduced, and the cycle performance of the secondary battery is improved.

[0010] In some embodiments of the present application, 0.6P1 / P2<0.04W×100+0.98≤1.5P1 / P2. By adjusting the value of 0.04W×100+0.98 within the above range, the risk of deterioration of the negative electrode interface due to insufficient electrolyte is reduced while taking into account the energy density of the secondary battery, thereby improving the cycle performance of the secondary battery.

[0011] In some embodiments of the present application, 3%≤W≤10%, 1<P1 / P2≤1.5, 30%≤P1≤40%. When 3%≤W≤10%, by adjusting the values ​​of P1 / P2 and P1 within the above range, the content of silicon element and the porosity between different coatings are synergistically acted, while taking into account the energy density of the secondary battery, the risk of deterioration of the negative electrode interface due to insufficient electrolyte is reduced, and the cycle performance of the secondary battery is improved.

[0012] In some embodiments of the present application, 10%<W≤30%, 1.5<P1 / P2≤2.5, 40%<P1≤55%. When 10%<W≤30%, by adjusting the values ​​of P1 / P2 and P1 within the above range, the risk of deterioration of the negative electrode interface due to insufficient electrolyte is reduced while taking into account the energy density of the secondary battery, thereby improving the cycle performance of the secondary battery.

[0013] In some embodiments of the present application, 30%<W≤80%, 2.5<P1 / P2≤5, 55%<P1≤70%. When 30%<W≤80%, by adjusting the values ​​of P1 / P2 and P1 within the above range, the risk of deterioration of the negative electrode interface due to insufficient electrolyte is reduced while taking into account the energy density of the secondary battery, thereby improving the cycle performance of the secondary battery.

[0014] In some embodiments of the present application, the first ceramic layer includes first ceramic particles, the second ceramic layer includes second ceramic particles, and the first ceramic particles and the second ceramic particles are each independently selected from at least one of aluminum oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide or boehmite. The average particle size of the first ceramic particles is D1μm, 0.5≤D1≤3; the average particle size of the second ceramic particles is D2μm, 0.25≤D2≤0.45. By selecting the above-mentioned types of first ceramic particles and second ceramic particles, and regulating the average particle size of the first ceramic particles and the second ceramic particles within the above-mentioned range, it is beneficial to adjust the porosity of the first coating and the porosity of the second coating, reduce the risk of deterioration of the negative electrode interface due to insufficient electrolyte, and improve the cycle performance of the secondary battery.

[0015] In some embodiments of the present application, the first coating also includes a first bonding layer, the first bonding layer and the first ceramic layer are sequentially stacked on the first surface, and the first ceramic layer is located between the first bonding layer and the base film. The second coating also includes a second bonding layer, the second bonding layer and the second ceramic layer are sequentially stacked on the second surface, and the second ceramic layer is located between the second bonding layer and the base film. The first bonding layer includes a first binder, and the second bonding layer includes a second binder. The first binder and the second binder are each independently selected from at least one of styrene-butadiene latex, styrene-acrylic latex, polymethyl methacrylate, polybutyl methacrylate, polyethyl acrylate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate, polyurethane, polyvinylidene fluoride or vinylidene fluoride and hexafluoropropylene copolymer. By providing the first bonding layer and the second bonding layer, and selecting the first bonding layer and the second bonding layer of the above types, while taking into account the cycle performance, it has better electrode interface bonding, thereby improving the safety performance of the secondary battery.

[0016] In some embodiments of the present application, the thickness of the first adhesive layer is 0.5 μm to 3 μm. By adjusting the thickness T1 of the first adhesive layer within the above range, the safety performance and cycle performance of the secondary battery are further improved.

[0017] In some embodiments of the present application, the first binder includes at least one of styrene-butadiene latex, styrene-acrylic latex, polymethyl methacrylate, polybutyl methacrylate, polyethyl acrylate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate or polyurethane, and the second binder includes at least one of polyvinylidene fluoride or vinylidene fluoride and hexafluoropropylene copolymer. By selecting the above-mentioned first binder and second binder, the bonding force of the second bonding layer is stronger than that of the first bonding layer, and the ion conductivity of the first bonding layer has better electrode interface bonding than the second bonding layer, and further optimizes the ion conduction between the interfaces. While taking into account the safety performance of the secondary battery, the risk of deterioration of the negative electrode interface due to insufficient electrolyte is reduced, and the cycle performance of the secondary battery is improved.

[0018] In some embodiments of the present application, the electrode assembly is a laminated structure. In some embodiments of the present application, the electrode assembly also includes a second diaphragm, the pole piece includes two outer pole pieces and a plurality of inner pole pieces, the two outer pole pieces are respectively located on the outermost sides of the electrode assembly, the first diaphragm is at least arranged between the outer pole piece and the inner pole piece adjacent to the outer pole piece, and the second diaphragm is arranged between two adjacent inner pole pieces. In some embodiments of the present application, the number of layers of the first diaphragm is m, the total number of layers of the first diaphragm and the second diaphragm is n, and 1 / 5≤m / n≤1. Through the above-mentioned arrangement, while reducing the risk of deterioration of the negative electrode interface due to insufficient electrolyte and improving the cycle performance of the secondary battery, it also takes into account the operational difficulty and processing cost in the actual production process, and further improves the energy density of the secondary battery.

[0019] In some embodiments of the present application, the first separator is in a Z-shaped folded structure in the electrode assembly, and the Z-shaped first separator separates the adjacent positive electrode sheet from the negative electrode sheet. Through the above arrangement, the stability of the electrode assembly stacking structure is further improved, and while improving the cycle performance of the secondary battery, the safety performance of the secondary battery is further improved.

[0020] The second aspect of the present application provides an electronic device, which includes the secondary battery in any of the above embodiments. The secondary battery of the present application has good cycle performance, so the electronic device of the present application has a long service life.

[0021] Beneficial effects of the embodiments of the present application:

[0022] The present application provides a secondary battery and an electronic device. By using coatings with different porosities on both sides of the diaphragm facing the positive and negative electrodes in the secondary battery, the diaphragm has a coating with a larger porosity on the negative electrode side, which is beneficial for the diaphragm to absorb more electrolyte on the negative electrode side, thereby improving the liquid storage capacity of the diaphragm on the negative electrode side. When the negative electrode plate containing silicon elements needs electrolyte, it can be supplied in time, thereby reducing the negative electrode interface ion conduction bridge breakage in the late cycle due to insufficient electrolyte, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, thereby leading to the risk of lithium precipitation and even cycle water drop, thereby improving the cycle performance of the secondary battery.

[0023] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.

[0025] Figure 1 It is a schematic diagram of a partial cross-sectional structure of an electrode assembly in one embodiment of the present application after it is unfolded along its thickness direction;

[0026] Figure 2 This is a schematic diagram of a partial cross-sectional structure of an electrode assembly in another embodiment of the present application after it is unfolded along its thickness direction;

[0027] Figure 3 This is a schematic diagram of a cross-sectional structure of a secondary battery in another embodiment of the present application observed along its length direction;

[0028] Figure 4 This is a schematic diagram of the cross-sectional structure of a secondary battery in another embodiment of the present application observed along its length direction.

[0029] Figure numerals: secondary battery 001; electrode assembly 01; shell 02; pole piece 10; first separator 20; base film 201; first coating 202; second coating 203; first ceramic layer 2021; first bonding layer 2022; second ceramic layer 2031; second bonding layer 2032; positive electrode pole piece 11; positive electrode current collector 111; positive electrode material layer 112; negative electrode pole piece 12; negative electrode current collector 121; negative electrode material layer 122; second separator 21; outer pole piece 101; inner pole piece 102. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.

[0031] It should be noted that in the specific implementation of the present application, lithium-ion batteries are used as an example of secondary batteries to explain the present application, but the secondary batteries of the present application are not limited to lithium-ion batteries. The specific technical solutions are as follows:

[0032] The first aspect of the present application provides a secondary battery, the secondary battery includes an electrode assembly, the electrode assembly includes a pole piece and a first diaphragm, the pole piece includes a positive pole piece and a negative pole piece, the negative pole piece includes a negative electrode material layer, the negative electrode material layer includes silicon element, based on the mass of the negative electrode material layer, the mass percentage of silicon element is W, W ≥ 3%. The first diaphragm includes a base film, a first coating and a second coating, along the thickness direction of the first diaphragm, the base film includes a first surface and a second surface, the first surface faces the negative pole piece, the second surface faces the positive pole piece, the first coating is arranged on the first surface, and the second coating is arranged on the second surface. The porosity of the first coating is P1, the porosity of the second coating is P2, P1>P2.

[0033] In this application, the electrode assembly is defined as having its own length direction as the X direction, its own width direction as the Y direction, and its own thickness direction as the Z direction in the unfolded state. It is understood that the thickness direction of the negative electrode sheet, the positive electrode sheet, and the separator in the unfolded state is the same as that of the electrode assembly. For example, Figure 1As shown, the electrode assembly 01 includes a pole piece 10 and a first separator 20, the pole piece 10 includes a positive pole piece 11 and a negative pole piece 12, and the negative pole piece 12 includes a negative electrode material layer 122. The first separator 20 includes a base film 201, a first coating 202, and a second coating 203. Along the thickness direction Z direction of the first separator 20, the base film 201 includes a first surface (not shown in the figure) and a second surface (not shown in the figure), the first surface faces the negative pole piece 12, and the second surface faces the positive pole piece 11. The first coating 202 is arranged on the first surface, and the second coating 203 is arranged on the second surface.

[0034] The inventors have found that in the prior art, the coating of the diaphragm is generally symmetrically designed. In this case, the porosity of the two coatings on the two surfaces of the diaphragm is equal, or, only the surface of the diaphragm facing the positive electrode side has a coating. In this case, the liquid storage capacity of the diaphragm facing the negative electrode side is poor. When the negative electrode plate contains silicon, the demand for electrolyte during the secondary battery cycle is higher than that of conventional graphite. In the late stage of the cycle, insufficient electrolyte may cause the negative electrode interface ion conduction bridge to break in the late stage of the cycle, and the silicon particles may expand during the cycle, causing the SEI film to be destroyed and the electrolyte cannot be replenished in time, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation and even cycle water diving, affecting the cycle life of the secondary battery and reducing the cycle performance of the secondary battery. In addition, when a high-porosity coating is applied on both surfaces of the diaphragm in the electrode assembly, the diaphragm stores too much electrolyte, and the excess electrolyte inside the shell will be stored in a free state, and cannot be supplied and transmitted to the silicon-based material of the negative electrode plate in time. At this time, the excess free electrolyte will increase the sliding properties between the layers inside the electrode assembly, affecting the drop performance and safety performance of the secondary battery. At the same time, when there is too much excess electrolyte, the secondary battery will swell and the shell may bulge, deform or crack. In the secondary battery containing silicon, the present application uses coatings with different porosities on both sides of the diaphragm facing the positive and negative electrodes in the secondary battery, so that the porosity of the coating facing the negative electrode side of the diaphragm is larger. At this time, the coating with a larger porosity has more particle gaps, and the diaphragm facing the negative electrode side can absorb more electrolyte, thereby improving the liquid storage capacity of the diaphragm facing the negative electrode side, and can supply electrolyte in time when the negative electrode plate containing silicon elements needs electrolyte, thereby reducing the negative electrode interface ion conduction bridge breakage caused by insufficient electrolyte in the late cycle, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation and even cycle diving. While taking into account the drop performance and safety performance, the cycle performance of the secondary battery is improved.

[0035] In some embodiments of the present application, 3% ≤ W ≤ 80%. For example, the value of W can be 3%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, 72%, 75%, 78%, 80% or a range consisting of any two of the values. By regulating the value of W within the above range, while taking into account the structural stability of the negative electrode sheet during the charge and discharge process, it is beneficial to improve the energy density of the secondary battery. At the same time, the first diaphragm in the secondary battery of the present application can absorb more electrolyte facing the negative electrode side, which improves the liquid storage capacity of the diaphragm facing the negative electrode side, and can be supplied in time when the negative electrode sheet containing silicon elements requires electrolyte. As the mass percentage of silicon element increases, the demand for electrolyte by the negative electrode plate increases accordingly. Therefore, the effect of reducing the risk of lithium plating and even cycle water drop caused by insufficient electrolyte at the negative electrode interface in the late cycle, as well as the risk of electrolyte failure due to the destruction of SEI film by cyclic expansion of silicon particles, and the inability to replenish electrolyte in time, further improves the cycle performance of secondary batteries.

[0036] In some embodiments of the present application, the first coating layer includes a first ceramic layer, and the second coating layer includes a second ceramic layer. Figure 1 As shown, the first coating 202 includes a first ceramic layer 2021, and the second coating 203 includes a second ceramic layer 2031. Through the above arrangement, in a secondary battery containing silicon, the diaphragm in the secondary battery is coated with coatings of different porosities on both sides facing the positive and negative electrodes, so that the porosity of the coating on the diaphragm facing the negative electrode side is larger. At this time, the coating with a larger porosity has more particle gaps, and the diaphragm facing the negative electrode side can absorb more electrolyte, thereby improving the liquid storage capacity of the diaphragm facing the negative electrode side, and can supply electrolyte in time when the negative electrode plate containing silicon elements needs electrolyte, thereby reducing the negative electrode interface ion conduction bridge breakage caused by insufficient electrolyte in the late cycle, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, thereby leading to the risk of lithium precipitation or even cycle jump, while taking into account the drop performance and safety performance, the cycle performance of the secondary battery is improved.

[0037] In some embodiments of the present application, 1<P1 / P2≤5, 30%≤P1≤70%. For example, the value of P1 / P2 can be 1.1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8, 3, 3.2, 3.5, 3.8, 4, 4.2, 4.5, 4.8, 5 or a range consisting of any two of them; the value of P1 can be 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70% or a range consisting of any two of them. By regulating the values ​​of P1 / P2 and P1 within the above range, while taking into account the mechanical strength of the first diaphragm, the porosity of the first coating on the negative electrode side of the first diaphragm is larger, and the first diaphragm can absorb more electrolyte on the negative electrode side, thereby improving the liquid storage capacity of the diaphragm facing the negative electrode side, and can supply electrolyte in time when the negative electrode plate containing silicon elements requires electrolyte, thereby reducing the negative electrode interface ion conduction bridge breakage in the late cycle due to insufficient electrolyte, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation and even cycle diving, thereby improving the cycle performance of the secondary battery.

[0038] In one embodiment of the present application, 6%≤P2<70%. For example, the value of P2 can be 6%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 69% or a range consisting of any two of the values. By regulating the value of P2 within the above range, while improving the liquid storage capacity of the first diaphragm facing the negative electrode side, the liquid storage capacity of the first diaphragm facing the positive electrode side is taken into account, so that electrolyte can be supplied in time when the positive and negative electrode plates need electrolyte, thereby reducing the ion conduction bridge breakage at the electrode plate interface in the late cycle due to insufficient electrolyte, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation and even cycle diving, thereby improving the cycle performance of the secondary battery.

[0039] In some embodiments of the present application, 0.6P1 / P2≤0.04W×100+0.98≤1.5P1 / P2. For example, the value of 0.04W×100+0.98 / (P1 / P2) can be 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, or a range consisting of any two of the values. When the silicon content in the negative electrode material layer is high, the demand for electrolyte during the cycle is correspondingly higher. By adjusting the value of 0.04W×100+0.98 within the above range, the negative electrode sheets with different silicon content are matched with two coatings with different porosity ratios, so that the silicon content and the porosity between different coatings work synergistically. While taking into account the mechanical strength of the first diaphragm, the first diaphragm facing the negative electrode side can absorb more electrolyte, which improves the liquid storage capacity of the diaphragm facing the negative electrode side, and can supply electrolyte in time when the negative electrode sheet containing silicon needs electrolyte. While taking into account the energy density of the secondary battery, it reduces the negative electrode interface ion conduction bridge breakage caused by insufficient electrolyte in the late cycle, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation or even cycle jump, thereby improving the cycle performance of the secondary battery.

[0040] In some embodiments of the present application, 3%≤W≤10%, 1<P1 / P2≤1.5, 30%≤P1≤40%. For example, when 3%≤W≤10%, the value of P1 / P2 can be 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5 or a range consisting of any two of them; the value of P1 can be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40% or a range consisting of any two of them. When 3%≤W≤10%, by adjusting the values ​​of P1 / P2 and P1 within the above range, the silicon content in the negative electrode material layer is low, and the negative electrode sheet has relatively good liquid retention capacity. With smaller P1 / P2 and P1, the silicon content and the porosity between different coatings work synergistically. While taking into account the mechanical strength of the first diaphragm, the first diaphragm can absorb more electrolyte facing the negative electrode side, which improves the liquid storage capacity of the diaphragm facing the negative electrode side, and can supply electrolyte in time when the negative electrode sheet containing silicon elements needs electrolyte. While taking into account the energy density of the secondary battery, it reduces the negative electrode interface ion conduction bridge breakage caused by insufficient electrolyte in the late cycle, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation or even cycle jump, thereby improving the cycle performance of the secondary battery.

[0041] In some embodiments of the present application, 10%<W≤30%, 1.5<P1 / P2≤2.5, 40%<P1≤55%. For example, when 10%<W≤30%, the value of P1 / P2 can be 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5 or a range consisting of any two of them; the value of P1 can be 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55% or a range consisting of any two of them. When 10%<W≤30%, by adjusting the values ​​of P1 / P2 and P1 within the above range, the silicon content in the negative electrode material layer is relatively high, and the demand for electrolyte during the cycle is correspondingly high. The ratio of the porosity of different coatings increases accordingly, and the porosity of the first coating also increases accordingly, so that the silicon content and the porosity between different coatings work synergistically, and the first diaphragm facing the negative electrode side can absorb more electrolyte, further improving the storage capacity of the diaphragm facing the negative electrode side, and can supply electrolyte in time when the negative electrode plate containing silicon elements needs electrolyte. While taking into account the energy density of the secondary battery, it reduces the negative electrode interface ion conduction bridge breakage caused by insufficient electrolyte in the late cycle, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation or even cycle jump, thereby improving the cycle performance of the secondary battery.

[0042] In some embodiments of the present application, 30%<W≤80%, 2.5<P1 / P2≤5, 55%<P1≤70%. For example, when 30%<W≤80%, the value of P1 / P2 can be 2.6, 2.7, 2.8, 2.9, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5 or a range consisting of any two of the values; the value of P1 can be 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70% or a range consisting of any two of the values. When 30%<W≤80%, by adjusting the values ​​of P1 / P2 and P1 within the above range, the silicon content in the negative electrode material layer is high, and the larger porosity ratio of different coatings and the larger porosity of the first coating make the silicon content and the porosity between different coatings work together, which can better meet the demand for electrolyte during the cycle. The first diaphragm facing the negative electrode side can absorb more electrolyte, further improving the storage capacity of the diaphragm facing the negative electrode side, and can supply electrolyte in time when the negative electrode plate containing silicon elements needs electrolyte. While taking into account the energy density of the secondary battery, it reduces the negative electrode interface ion conduction bridge breakage caused by insufficient electrolyte in the late cycle, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation and even cycle jump, thereby improving the cycle performance of the secondary battery.

[0043] In some embodiments of the present application, the first ceramic layer includes first ceramic particles, the second ceramic layer includes second ceramic particles, and the first ceramic particles and the second ceramic particles are each independently selected from at least one of aluminum oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide or boehmite. The average particle size of the first ceramic particles is D1 μm, 0.5≤D1≤3, for example, the value of D1 can be 0.5, 0.8, 1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8, 3 or a range consisting of any two of the values; the average particle size of the second ceramic particles is D2 μm, 0.25≤D2≤0.45, for example, the value of D2 can be 0.25, 0.28, 0.3, 0.32, 0.35, 0.38, 0.4, 0.42, 0.45 or a range consisting of any two of the values. By selecting the above-mentioned types of first ceramic particles and second ceramic particles, and regulating the average particle size of the first ceramic particles and the second ceramic particles within the above-mentioned range, it is beneficial to adjust the porosity of the first coating and the porosity of the second coating, so that the porosity of the first coating is greater than that of the second coating, and the porosity of the first coating on the negative electrode side of the first diaphragm is larger. The first diaphragm can absorb more electrolyte on the negative electrode side, thereby improving the liquid storage capacity of the diaphragm facing the negative electrode side. When the negative electrode plate containing silicon elements requires electrolyte, it can be supplied in time, thereby reducing the negative electrode interface ion conduction bridge breakage in the late cycle due to insufficient electrolyte, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation and even cycle diving, thereby improving the cycle performance of the secondary battery.

[0044] The present application does not particularly limit the method for regulating the average particle size of the ceramic particles, as long as the purpose of the present application can be achieved. For example, the average particle size of the ceramic particles can be regulated by grading and grinding the particles of the ceramic particles. Exemplarily, when other conditions remain unchanged, the average particle size of the ceramic particles decreases when the grinding time is extended; and the average particle size of the ceramic particles increases when the grinding time is shortened.

[0045] In some embodiments of the present application, the first coating further includes a first bonding layer, the first bonding layer and the first coating are sequentially stacked on the first surface, and the first ceramic layer is located between the first bonding layer and the base film. The second coating further includes a second bonding layer, the second bonding layer and the second ceramic layer are sequentially stacked on the second surface, and the second ceramic layer is located between the second bonding layer and the base film. For example, Figure 2As shown, the first coating 202 further includes a first bonding layer 2022, the first bonding layer 2022 and the first ceramic layer 2021 are sequentially stacked on the surface of the base film 201 facing the negative electrode plate 12, and the first ceramic layer 2021 is located between the first bonding layer 2022 and the base film 201; the second coating 203 further includes a second bonding layer 2032, the second bonding layer 2032 and the second ceramic layer 2031 are sequentially stacked on the surface of the base film 201 facing the positive electrode plate 11, and the second ceramic layer 2031 is located between the second bonding layer 2032 and the base film 201. The first bonding layer includes a first binder, and the second bonding layer includes a second binder, and the first binder and the second binder are each independently selected from at least one of styrene-butadiene latex, styrene-acrylic latex, polymethyl methacrylate, polybutyl methacrylate, polyethyl acrylate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate, polyurethane, polyvinylidene fluoride, or vinylidene fluoride and hexafluoropropylene copolymer. By providing the first adhesive layer and the second adhesive layer, and selecting the first adhesive and the second adhesive of the above type, it is beneficial to improve the bonding force between the first diaphragm and the positive electrode sheet, and between the first diaphragm and the negative electrode sheet, strengthen the interface between the first diaphragm and the positive electrode sheet, and between the first diaphragm and the negative electrode sheet, which is beneficial to the transmission of lithium ions, and at the same time reduces the possibility of the first ceramic layer and the second ceramic layer falling off. When the first diaphragm is applied to the secondary battery, while taking into account the cycle performance, it has better electrode interface bonding, and improves the safety performance of the secondary battery.

[0046] In some embodiments of the present application, the thickness T1 of the first bonding layer is 0.5 μm to 3 μm. For example, the thickness of the first bonding layer can be 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2 μm, 2.2 μm, 2.5 μm, 2.8 μm, 3 μm or a range consisting of any two of these values. By regulating the thickness T1 of the first bonding layer within the above range, while the first coating has a higher porosity, the first diaphragm and the negative electrode plate have a higher bonding force, which strengthens the interface between the first diaphragm and the negative electrode plate, is beneficial to the transmission of lithium ions during the cycle, and reduces the possibility of the first ceramic layer falling off from the base film, thereby further improving the safety performance and cycle performance of the secondary battery.

[0047] In one embodiment of the present application, the thickness T2 of the second bonding layer is 0.25 μm to 5 μm. For example, the thickness T2 of the second bonding layer can be 0.25 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1.0 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2.0 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm or a range consisting of any two of the values. By regulating the thickness T2 of the second bonding layer within the above range, while making the porosity of the first coating greater than the porosity of the second coating, the first diaphragm and the positive electrode sheet have a higher bonding force, strengthening the interface between the first diaphragm and the positive electrode sheet, which is beneficial to the transmission of lithium ions during the cycle, while reducing the possibility of the second ceramic layer falling off from the base film, thereby further improving the safety performance and cycle performance of the secondary battery.

[0048] In the present application, the thickness of the first bonding layer and the thickness of the second bonding layer can be regulated by means known to those skilled in the art. For example, when the first bonding layer slurry is coated on the surface of the first ceramic layer away from the base film, the coating amount of the first bonding layer slurry is increased on the basis of a certain solid content of the first bonding layer slurry to increase the thickness of the first bonding layer; when the second bonding layer slurry is coated on the surface of the second ceramic layer away from the base film, the coating amount of the second bonding layer slurry is increased on the basis of a certain solid content of the second bonding layer slurry to increase the thickness of the first bonding layer. This application is not particularly limited, as long as the purpose of this application can be achieved.

[0049] In some embodiments of the present application, the first binder includes at least one of styrene-butadiene latex, styrene-acrylic latex, polymethyl methacrylate, polybutyl methacrylate, polyethyl acrylate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate or polyurethane, and the second binder includes at least one of polyvinylidene fluoride or vinylidene fluoride and hexafluoropropylene copolymer. By selecting the above-mentioned first binder and second binder, the bonding force of the second bonding layer is stronger than that of the first bonding layer, and the ion conductivity of the first bonding layer has better electrode interface bonding than the second bonding layer, and further optimizes the ion conduction between the interfaces. While strengthening the interface between the first diaphragm and the positive electrode sheet and the first diaphragm and the negative electrode sheet, the first diaphragm can absorb more electrolyte facing the negative electrode side, thereby improving the liquid storage capacity of the diaphragm facing the negative electrode side, and can be supplied in time when the negative electrode sheet containing silicon elements needs electrolyte. While taking into account the safety performance of secondary batteries, it reduces the risk of ion conduction bridge breaking at the negative electrode interface in the late cycle due to insufficient electrolyte, and the risk of lithium plating or even cycle water drop caused by the destruction of the SEI film due to the cyclic expansion of silicon particles, and the inability to replenish the electrolyte in time. The SEI film cannot be regenerated, thereby improving the cycle performance of secondary batteries.

[0050] In some embodiments of the present application, the electrode assembly is a laminated structure. When the electrode assembly is of the above structure, since the laminated structure has no interface corner area, the positive and negative pole pieces are evenly distributed, which is conducive to reducing the excessive corner stress caused by the volume expansion of the negative pole piece containing silicon elements in the electrode assembly of the winding structure, thereby causing the overall structure of the electrode assembly to deform or even cause the risk of internal tearing of the pole piece. The porosity of the first coating on the negative electrode side of the first diaphragm is larger, and the first diaphragm can absorb more electrolyte on the negative electrode side, thereby improving the liquid storage capacity of the diaphragm facing the negative electrode side, and can supply electrolyte in time when the negative pole piece containing silicon elements needs electrolyte, thereby reducing the negative electrode interface ion conduction bridge breakage caused by insufficient electrolyte in the late cycle, and the electrolyte cannot be replenished in time after the SEI film is destroyed by the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, thereby leading to the risk of lithium precipitation or even cycle diving, thereby improving the cycle performance of the secondary battery.

[0051] In some embodiments of the present application, the electrode assembly further includes a second diaphragm, the electrode piece includes two outer electrode pieces and a plurality of inner electrode pieces, the two outer electrode pieces are respectively located on the outermost sides of the electrode assembly, the first diaphragm is at least arranged between the outer electrode piece and the inner electrode piece adjacent to the outer electrode piece, and the second diaphragm is arranged between two adjacent inner electrode pieces. For example, Figure 3 As shown, the electrode assembly 01 further includes a second diaphragm 21, the pole piece 10 includes two outer pole pieces 101 and an inner pole piece 102, the two outer pole pieces 101 are respectively located on the outermost sides of the electrode assembly 01, the first diaphragm 20 is arranged between the outer pole piece 101 and the inner pole piece 102 adjacent to the outer pole piece 101, and the second diaphragm 21 is arranged between two adjacent inner pole pieces 102. In a conventional laminated electrode assembly, the outer pole piece has a small resistance and a large current density, and its ability to consume and transmit electrolyte is greater than that of the inner pole piece. Through the above arrangement, the liquid storage capacity of the diaphragm facing the negative electrode side is improved, and the electrolyte can be supplied in time when the negative electrode plate containing silicon elements needs it. At the same time, the liquid storage capacity of the outside of the electrode assembly is also improved, thereby reducing the risk of lithium deposition on the outer electrode plate due to insufficient electrolyte on the outer side of the electrode assembly during the cycle, and the negative electrode interface ion conduction bridge breaking in the late cycle due to insufficient electrolyte, and the cyclic expansion of silicon particles that causes the SEI film to be destroyed and the electrolyte cannot be replenished in time, and the SEI film cannot be regenerated, which leads to the risk of lithium deposition and even cycle water diving, thereby improving the cycle performance of the secondary battery.

[0052] In some embodiments of the present application, the number of layers of the first diaphragm is m, the total number of layers of the first diaphragm and the second diaphragm is n, and 1 / 5≤m / n≤1. For example, the value of m / n can be 1 / 5, 3 / 10, 2 / 5, 1 / 2, 3 / 5, 7 / 10, 4 / 5, 9 / 10, 1 or a range consisting of any two of these values. By regulating the value of m / n within the above range, the ion conduction bridge of the negative electrode interface in the late cycle caused by insufficient electrolyte is reduced, and the electrolyte cannot be replenished in time after the SEI film is destroyed due to the cyclic expansion of silicon particles, and the SEI film cannot be regenerated, which leads to the risk of lithium precipitation or even cycle diving. While improving the cycle performance of the secondary battery, it takes into account the operational difficulty and processing cost in the actual production process, and further improves the energy density of the secondary battery.

[0053] The present application has no particular restrictions on the material of the base film, as long as the purpose of the present application can be achieved. For example, the material of the base film may include at least one of polyimide, polyamide, polysulfone, polyacrylonitrile, cellulose, polyetheretherketone, polyphenylene sulfide, polyacrylate, polyethylene terephthalate, polyphenylamide, polyarylethersulfoneketone, aramid, aromatic sulfone or polyolefin, and the polymerization monomer of the polyolefin includes at least one of ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 4-methyl-1-pentene, cyclobutene, cyclopentene or cyclohexene. In the present application, a commercially available base film of the desired material can be selected. The present application has no particular restrictions, as long as the purpose of the present application can be achieved.

[0054] The present application has no particular restrictions on the second diaphragm, as long as the purpose of the present application can be achieved. For example, the second diaphragm includes a basement membrane. Optionally, the second diaphragm may also include a third coating, which may be disposed on one surface of the basement membrane or on both surfaces of the basement membrane. The second diaphragm may also be selected from commercially available diaphragms. For example, the second diaphragm may be selected from a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane, etc.

[0055] In some embodiments of the present application, the first separator is in a Z-shaped folded structure in the electrode assembly, and the Z-shaped first separator separates the adjacent positive electrode sheet from the negative electrode sheet. Figure 4 As shown, the first separator 20 is in a Z-shaped folded structure in the electrode assembly 01, and the Z-shaped first separator 20 separates the adjacent positive electrode sheet 11 from the negative electrode sheet 12. Through the above arrangement, the stability of the electrode assembly stacking structure is further improved, while taking into account the operational difficulty and processing cost in the actual production process, and having a higher stacking efficiency.

[0056] In one embodiment of the present application, the negative electrode material layer includes a negative electrode active material, the negative electrode active material includes a silicon-based material, and the silicon-based material includes at least one of a silicon-carbon composite material, a silicon-oxygen composite material, or a pure silicon material. By selecting the above-mentioned silicon-based materials, the energy density of the secondary battery is improved while taking into account the cycle performance of the secondary battery.

[0057] In one embodiment of the present application, the negative electrode active material further comprises at least one of artificial graphite, natural graphite, hard carbon or MCMB mesophase carbon microspheres. By selecting the above-mentioned types of negative electrode active materials, it is beneficial to improve the structural stability of the negative electrode plate, so that the volume expansion of the negative electrode plate during charging and discharging is moderate.

[0058] In one embodiment of the present application, the first ceramic layer also includes a first ceramic layer binder, and the second ceramic layer also includes a second ceramic layer binder. The present application has no particular restrictions on the types of the first ceramic layer binder and the second ceramic layer binder, as long as the purpose of the present application can be achieved. For example, the first ceramic layer binder and the second ceramic layer binder are each independently selected from at least one of styrene-butadiene rubber, polyvinyl alcohol, polyvinylidene fluoride, polyacrylic acid, polymethyl methacrylate, polybutyl acrylate or polyacrylonitrile. The present application has no particular restrictions on the content of the first ceramic particles and the first ceramic layer binder in the first ceramic layer, and the content of the second ceramic particles and the second ceramic layer binder in the second ceramic layer. Those skilled in the art can make a selection according to actual needs, as long as the purpose of the present application can be achieved.

[0059] In one embodiment of the present application, the first adhesive layer may further include a first thickener, and the second adhesive layer may further include a second thickener. Applying the first thickener to the first adhesive layer and the second thickener to the second adhesive layer is beneficial to increase the stability of the first adhesive layer slurry and the second adhesive layer slurry, and prevent the sedimentation of each component in the first adhesive layer slurry and the second adhesive layer slurry. The present application has no particular restrictions on the types of the first thickener and the second thickener, as long as the purpose of the present application can be achieved. For example, the first thickener and the second thickener are each independently selected from at least one of hydroxyethyl cellulose, methyl hydroxyethyl cellulose, sodium carboxymethyl cellulose, polyacrylamide or sodium alginate. The present application has no particular restrictions on the content of the first thickener in the first adhesive layer and the content of the second thickener in the second adhesive layer. Those skilled in the art can make a selection according to actual needs, as long as the purpose of the present application can be achieved.

[0060] The present application has no particular restrictions on the preparation method of the first diaphragm, as long as the purpose of the present application can be achieved. For example, the preparation method of the first diaphragm includes but is not limited to the following steps: (1) adding the first ceramic particles and the first ceramic layer binder to the solvent and mixing them evenly to obtain the first ceramic layer slurry, adding the second ceramic particles and the second ceramic layer binder to the solvent and mixing them evenly to obtain the second ceramic layer slurry; (2) coating the first ceramic layer slurry on one surface of the base film, and after drying, forming a first coating on one surface of the base film; (3) coating the second ceramic layer slurry on the other surface of the base film, and after drying, forming a second coating on one surface of the first base film, so as to obtain the first diaphragm.

[0061] In another embodiment of the present application, the preparation method of the first diaphragm may include but is not limited to the following steps: (1) adding the first ceramic particles and the first ceramic layer binder to the solvent and mixing them evenly to obtain a first ceramic layer slurry, adding the second ceramic particles and the second ceramic layer binder to the solvent and mixing them evenly to obtain a second ceramic layer slurry; (2) mixing the first binder and the first thickener evenly to obtain a first bonding layer slurry, mixing the second binder and the second thickener evenly to obtain a second bonding layer slurry; (3) coating the first ceramic layer slurry on one surface of the base film, and after drying, forming a first ceramic layer on one surface of the base film, coating the first bonding layer slurry on the surface of the first ceramic layer away from the base film, and after drying, obtaining a first coating layer including a first ceramic coating and a first bonding layer; (4) coating the second ceramic layer slurry on the other surface of the base film, and after drying, forming a second ceramic layer on one surface of the base film, coating the second bonding layer slurry on the surface of the second ceramic layer away from the base film, and after drying, obtaining a second coating layer including a second ceramic coating and a second bonding layer, thereby obtaining the first diaphragm.

[0062] The present application does not limit the above-mentioned solvents, as long as the purpose of the present application can be achieved.

[0063] In the present application, the negative electrode plate also includes a negative electrode current collector, and the negative electrode material layer is arranged on at least one surface of the negative electrode current collector. The above-mentioned "negative electrode material layer is arranged on at least one surface of the negative electrode current collector" means that the negative electrode material layer can be arranged on one surface of the negative electrode current collector along its own thickness direction, or it can be arranged on two surfaces of the negative electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of ​​the surface of the negative electrode current collector, or it can be a partial area of ​​the surface of the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved. Figure 1 As shown, the negative electrode plate 12 further includes a negative electrode current collector 121 , and a negative electrode material layer 122 is disposed on two surfaces of the negative electrode current collector 121 along its thickness direction Z direction.

[0064] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, it can contain copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or composite current collector. For example, the composite current collector can be a lithium copper composite current collector, a carbon copper composite current collector, a nickel copper composite current collector, a titanium copper composite current collector, etc. In the present application, there is no particular restriction on the thickness of the negative electrode current collector and the negative electrode material layer, as long as the purpose of the present application can be achieved. Optionally, the negative electrode material layer may also include a conductive agent and a negative electrode binder. The present application has no particular restrictions on the type of conductive agent in the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, flake graphite, graphene, metal materials or conductive polymers, and the conductive carbon black may include but is not limited to at least one of acetylene black or Ketjen black. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The carbon fiber may include but is not limited to vapor grown carbon fiber (VGCF) and / or nano carbon fiber. The metal material may include but is not limited to metal powder and / or metal fiber. Specifically, the metal may include but is not limited to at least one of copper, nickel, aluminum or silver. The conductive polymer may include but is not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole. The present application does not particularly limit the type of negative electrode binder in the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the negative electrode binder may include but is not limited to polyacrylic acid, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyvinyl alcohol, carboxymethyl cellulose, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, polyimide, polyamide-imide, styrene-butadiene rubber or polyvinylidene fluoride. Optionally, the negative electrode material layer also includes a thickener, and the present application does not particularly limit the type of thickener, as long as the purpose of the present application can be achieved. For example, the thickener may include at least one of carboxymethyl cellulose or sodium carboxymethyl cellulose. The present application has no particular restriction on the mass ratio of the negative electrode active material, the conductive agent, the binder and the thickener in the negative electrode material layer. Those skilled in the art can select the ratio according to actual needs as long as the purpose of the present application can be achieved.

[0065] The present application has no special restrictions on the positive electrode plate, as long as the purpose of the present application can be achieved. For example, the positive electrode plate includes a positive current collector and a positive electrode material layer disposed on at least one surface of the positive current collector. The above-mentioned "positive electrode material layer disposed on at least one surface of the positive current collector" means that the positive electrode material layer can be disposed on one surface of the positive current collector along the thickness direction of itself, or on two surfaces of the positive current collector along the thickness direction of itself. It should be noted that the "surface" here can be the entire area of ​​the surface of the positive current collector, or it can be a partial area of ​​the surface of the positive current collector. The present application has no special restrictions, as long as the purpose of the present application can be achieved. As Figure 1 As shown, the positive electrode sheet 11 includes a positive electrode current collector 111 and a positive electrode material layer 112 disposed on two surfaces of the positive electrode current collector 111 along its thickness direction Z direction.

[0066] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector). The positive electrode material layer of the present application includes a positive electrode active material. The present application has no particular restrictions on the type of positive electrode active material, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include lithium nickel cobalt manganese oxide (LiNi 0.90 Co 0.05 Mn 0.05 O2 (NCM955), NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium manganate or lithium iron manganese phosphate, etc. In the present application, the positive electrode active material may also contain non-metallic elements, for example, the non-metallic elements include at least one of fluorine, phosphorus, boron, chlorine, silicon or sulfur. In the present application, there is no particular restriction on the thickness of the positive electrode current collector and the positive electrode material layer, as long as the purpose of the present application can be achieved. In the present application, the positive electrode material layer may also include a positive electrode binder and a conductive agent. The present application does not particularly limit the type of the positive electrode binder in the positive electrode material layer, as long as the purpose of the present application can be achieved, for example, the positive electrode binder may be the same type as the negative electrode binder in the above-mentioned negative electrode material layer. The present application does not particularly limit the type of the conductive agent in the positive electrode material layer, as long as the purpose of the present application can be achieved, for example, the conductive agent may be the same type as the conductive agent in the above-mentioned negative electrode material layer. The present application has no particular restriction on the mass ratio of the positive electrode active material, the conductive agent, and the positive electrode binder in the positive electrode material layer. Those skilled in the art can select the ratio according to actual needs as long as the purpose of the present application can be achieved.

[0067] In the present application, the secondary battery also includes an electrolyte, and the electrolyte includes a lithium salt and a non-aqueous solvent. The present application has no particular restrictions on lithium salts, as long as the purpose of the present application can be achieved. For example, the lithium salt may include but is not limited to at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalate borate) (LiBOB) or lithium difluoroborate. The present application has no particular restrictions on the content of lithium salts in the electrolyte, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on non-aqueous solvents, as long as the purpose of the present application can be achieved, for example, non-aqueous solvents may include but are not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of chain carbonate compounds, cyclic carbonate compounds or fluorocarbonate compounds. The above-mentioned linear carbonate compound may include but is not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or methyl ethyl carbonate (MEC). The above-mentioned cyclic carbonate may include but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). Fluorinated carbonate compounds may include but are not limited to at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate or trifluoromethylethylene carbonate. The above-mentioned carboxylate compounds may include but are not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valerolactone or caprolactone. The above-mentioned ether compounds may include but are not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methylcyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate. The present application does not particularly limit the content of the non-aqueous solvent in the electrolyte, as long as the purpose of the present application can be achieved.

[0068] For example, Figure 3 and Figure 4 As shown, the secondary battery 001 also includes a shell 02 for accommodating a positive electrode plate, a first diaphragm or a first diaphragm and a second diaphragm, a negative electrode plate and an electrolyte, and other components known in the field of secondary batteries. This application does not limit the above-mentioned other components. This application has no special restrictions on the shell, and it can be a shell known in the art, as long as the purpose of this application can be achieved. For example, the shell can be a hard shell shell or a flexible shell. The material of the hard shell shell can be metal. This application does not limit the type of metal, and a metal hard shell shell known in the art can be used, as long as the purpose of this application can be achieved. The flexible shell can be a metal plastic film, such as an aluminum plastic film, a steel plastic film, etc.

[0069] The secondary battery of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction. In some embodiments of the present application, the secondary battery may include, but is not limited to, a lithium ion secondary battery (lithium ion battery), a lithium polymer secondary battery, or a lithium ion polymer secondary battery, etc.

[0070] The preparation process of the secondary battery of the present application is well known to those skilled in the art, and there is no particular limitation in the present application. For example, the preparation process of the secondary battery may include but is not limited to the following steps: stacking the positive electrode sheet, the first diaphragm, and the negative electrode sheet in order, and winding, folding, and other operations as needed to obtain an electrode assembly of a winding structure, placing the electrode assembly in a shell, injecting an electrolyte into the shell and sealing it to obtain a secondary battery. Alternatively, stacking the positive electrode sheet, the first diaphragm or the first diaphragm and the second diaphragm, and the negative electrode sheet in order, and then fixing the four corners of the entire laminated structure with tape to obtain an electrode assembly of a laminated structure, placing the electrode assembly in a shell, injecting an electrolyte into the shell and sealing it to obtain a secondary battery. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the shell as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.

[0071] The second aspect of the present application provides an electronic device, which includes the secondary battery in any of the above embodiments. The secondary battery of the present application has good cycle performance, so the electronic device of the present application has a long service life.

[0072] The electronic device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. For example, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.

[0073] Example

[0074] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0075] Test methods and equipment:

[0076] Sampling method for the first diaphragm:

[0077] The lithium-ion batteries in the tested embodiments and comparative examples were disassembled, the first diaphragm was taken out, and it was soaked in dimethyl carbonate (DMC) for 20 minutes to remove the electrolyte residue. Then, the first diaphragm was placed in an oven and dried at 60°C for 12 hours to obtain the first diaphragm sample. Among them, the ceramic layer on the surface of the diaphragm facing the negative electrode plate is the first ceramic layer, and the ceramic layer on the surface of the diaphragm facing the positive electrode plate is the second ceramic layer. If the first coating has only one layer, the first coating is the first ceramic layer, and if the second coating has only one layer, the second coating is the second ceramic layer. If a bonding layer is provided on the surface of the ceramic layer, the bonding layer provided on the surface of the first ceramic layer is the first bonding layer, and the bonding layer provided on the surface of the second ceramic layer is the second bonding layer.

[0078] Test of mass percentage of silicon element:

[0079] The lithium-ion battery discharged at 0.5C to 3.0V was disassembled, the negative electrode was removed, and it was soaked in dimethyl carbonate (DMC) for 20 minutes, and then rinsed with DMC and acetone in turn. Then the negative electrode was placed in an oven and baked at 80°C for 12 hours to obtain the negative electrode. The negative electrode was dried in a vacuum oven at 100°C for 24 hours, and 1g of the powdered sample of the negative electrode material layer on the negative electrode was scraped off with a blade, and then the mass percentage W of the silicon element in the negative electrode material layer was tested using an inductively coupled plasma (ICP) analyzer.

[0080] Test of the porosity P1 of the first coating and the porosity P2 of the second coating:

[0081] Take the first diaphragm sample, use N-methylpyrrolidone (NMP) solvent to wipe off the second coating of the first diaphragm, and obtain a single-sided first diaphragm sample with only a base film and the first coating, and first test the porosity Pa of the single-sided sample; wipe off the first coating again to obtain a sample with only a base film, and test the porosity Pb ​​of the base film sample; at the same time, use argon ion polishing to obtain the diaphragm cross-section, and use a field emission scanning electron microscope to measure the thickness Ta of the single-sided sample, the sample thickness Tb of the base film, and the sample thickness Tc of the first coating, Ta = Tb + Tc; it is easy to obtain Tb / Ta×Pb+Tc / Ta×P1=Pa, P1=(Tb×Pa-Ta×Pb) / Tc.

[0082] The first coating of the first diaphragm is wiped off with NMP solvent to obtain a single-sided diaphragm sample with only a base film and a second coating. Referring to the above test steps and calculation logic, the porosity P2 of the second coating can be obtained.

[0083] Test of the average particle size of the first ceramic particles and the average particle size of the second ceramic particles:

[0084] The cross-section of the first diaphragm along the thickness direction is prepared by argon ion polishing, and the cross-sections of the first ceramic layer and the second ceramic layer are observed respectively by scanning electron microscopy (SEM). Ten first ceramic particles and ten second ceramic particles are randomly selected, and the equivalent diameters of the ten first ceramic particles and the ten second ceramic particles are measured respectively (i.e., a particle with an irregular cross-section is converted into a circle of equal area, and the diameter of the circle), and the average value is calculated to obtain the average particle size D1 of the first ceramic particles and the average particle size D2 of the second ceramic particles.

[0085] Thickness of the first bonding layer and thickness of the second bonding layer test:

[0086] The first diaphragm is subjected to argon ion polishing to obtain the cross section of the first diaphragm. The cross-sectional morphology of the first diaphragm along the thickness direction is observed by a field emission scanning electron microscope (Philips, XL-30 model) and scanning electron microscope photographs are taken. The thickness T1 of the first bonding layer and the thickness T2 of the second bonding layer are measured by scanning electron microscopy.

[0087] Lithium deposition performance test:

[0088] The lithium-ion battery in the embodiment and the comparative example is placed in a constant temperature box at 10°C. After 60 minutes, it is charged to 4.45V at 2C constant current, charged to 0.025C at 4.45V constant voltage, and left to stand for 5 minutes. Then, it is discharged to 2.75V at 0.5C constant current. This is one cycle. After 100 cycles of the above charge and discharge process, it is charged to 4.45V at 2C constant current, charged to 0.025C at 4.45V constant voltage, and left to stand for 5 minutes. After that, the lithium-ion battery is disassembled, the negative electrode sheet in the electrode assembly is taken out, and the lithium deposition state on the surface of the negative electrode sheet is observed. The non-lithium deposition area on the surface of the negative electrode sheet is golden yellow, and the lithium deposition area is grayish white.

[0089] The criteria for judging the degree of lithium deposition in lithium-ion batteries are as follows: a lithium deposition area of ​​0% means no lithium deposition, i.e., the degree of lithium deposition is zero; a lithium deposition area greater than 0 and less than or equal to 2% means mild lithium deposition, i.e., the degree of lithium deposition is mild; a lithium deposition area greater than 2% and less than or equal to 20% means moderate lithium deposition, i.e., the degree of lithium deposition is moderate; a lithium deposition area greater than 20% and less than or equal to 100% means severe lithium deposition, i.e., the degree of lithium deposition is severe, wherein the percentage of the lithium deposition area is calculated based on the total area of ​​the negative electrode material layer of the negative electrode plate.

[0090] Cycle performance test:

[0091] Place the lithium-ion battery in a 25℃ constant temperature test box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature of 25℃. Charge to 4.45V at 1C constant current, charge to 0.025C at 4.45V constant voltage, let stand for 5 minutes, and discharge to 2.75V at 0.2C constant current. This is the first cycle, and the initial discharge capacity is recorded as C0. Perform charge and discharge cycles on the lithium-ion battery according to the above process. When the cycle reaches 500 cycles (cls), stop the test and record the discharge capacity after 500 cycles (cls) as C1. Calculate the 500cls capacity retention rate as an indicator for evaluating the cycle performance of lithium-ion batteries.

[0092] 500cls capacity retention rate (%) = C1 / C0×100%.

[0093] The higher the 500cls capacity retention rate, the better the cycle performance of the lithium-ion battery.

[0094] Drop test:

[0095] The lithium-ion batteries in the embodiments and comparative examples were placed in a 25°C environment and allowed to stand for 30 minutes, and then charged in the following steps: charged to 4.53V at a constant current of 0.5C, and then charged to 0.05C at a constant voltage. After standing for 60 minutes, the voltage of the lithium-ion battery before the drop test was tested; the lithium-ion battery was loaded into a fixture and freely dropped from a position 1.5m above the ground using a drop device in the following order: head-tail-head right corner-tail right corner-head left corner-tail left corner (angle: 45±15°), and repeated 6 rounds. After the drop, it was allowed to stand at room temperature for 24 hours, and the voltage of the lithium-ion battery was measured and recorded. The appearance of the lithium-ion battery was checked and photographed before and after the test. The drop test passing criteria: voltage drop <30mV (20 lithium-ion batteries were prepared and tested for each group of embodiments or comparative examples, the number of lithium-ion batteries that passed the test was X, and the test pass rate was X / 20×100%.)

[0096] The higher the drop test pass rate, the better the drop performance of the lithium-ion battery pack.

[0097] Example 1-1

[0098] <Preparation of First Separator>

[0099] A polyethylene (PE) film with a thickness of 10 μm was used as the base film, and the porosity of the first base film was 60%.

[0100] The first ceramic particle boehmite and the first ceramic layer binder polyvinylidene fluoride were mixed in a mass ratio of 95:5, and then deionized water was added as a solvent. After mixing evenly, a first ceramic layer slurry was obtained.

[0101] The second ceramic particle boehmite and the second ceramic layer binder polyvinylidene fluoride were mixed in a mass ratio of 95:5, and then deionized water was added as a solvent, and the mixture was evenly mixed to obtain a second ceramic layer slurry.

[0102] A first ceramic layer slurry is coated on one surface of the base film, and after drying at 60°C, a first coating is formed on one surface of the first base film; a second ceramic layer slurry is coated on the other surface of the base film, and after drying at 60°C, a second coating is formed on the other surface of the first base film, thereby obtaining a first diaphragm.

[0103] The average particle size of the first ceramic particles is 1.5 μm, that is, D1 is 1.5 μm, and the average particle size of the second ceramic particles is 0.33 μm, that is, D2 is 0.33 μm. The coating weight of the first ceramic layer is 0.75 mg / 1540.25 mm 2 The coating weight of the second ceramic layer is 0.75mg / 1540.25mm 2 The porosity P1 of the first coating layer is 55%, and the porosity P2 of the second coating layer is 22%.

[0104] <Preparation of positive electrode sheet>

[0105] The positive electrode active material lithium cobalt oxide, the conductive agent conductive carbon black and the positive electrode binder polyvinylidene fluoride are mixed in a mass ratio of 97:1.5:1.5, N-methylpyrrolidone (NMP) is added as a solvent, and the mixture is stirred and evenly mixed to form a positive electrode slurry with a solid content of 75wt%. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 110°C to obtain a positive electrode sheet with a single-sided coating of a positive electrode material layer with a thickness of 55μm. The positive electrode slurry is coated on the other surface of the positive electrode current collector aluminum foil, and after drying, a positive electrode sheet with a total thickness of 120μm is obtained. The positive electrode sheet after coating is cold pressed, and then cut into a specification of 70mm×40mm for standby use. Among them, the compaction density of the positive electrode material layer is 4.23g / cm 3 .

[0106] <Preparation of negative electrode sheet>

[0107] The negative electrode active material artificial graphite, silicon-carbon composite material SiC, conductive agent carbon nanotubes and negative electrode binder polyacrylic acid are mixed in a mass ratio of 41.1:42.9:1:5, and then deionized water is added as a solvent. After stirring evenly, a negative electrode slurry with a solid content of 35wt% is obtained. The negative electrode slurry is coated on one surface of a negative electrode current collector copper foil with a thickness of 10μm, and dried at 110°C to obtain a negative electrode sheet with a negative electrode material layer coated with a thickness of 40μm. The negative electrode slurry is coated on the other surface of the negative electrode current collector copper foil, and after drying, a negative electrode sheet with a total thickness of 90μm is obtained. The negative electrode sheet after coating is cold pressed, and then cut into a specification of 74mm×42mm for standby use. Among them, the compaction density of the negative electrode material layer is 1.5g / cm 3 Based on the mass of the negative electrode material layer, the mass percentage W of the silicon element is 30%.

[0108] <Preparation of Electrolyte>

[0109] In a glove box filled with dry argon atmosphere, propylene carbonate (PC), diethyl carbonate (DEC), and ethylene carbonate (EC) are mixed at a mass ratio of 1:1:1 to obtain a base solvent, and then lithium hexafluorophosphate (LiPF6) is added to the base solvent to dissolve and mix well to obtain an electrolyte. Among them, based on the mass of the electrolyte, the mass percentage of LiPF6 is 4.5%, and the balance is the base solvent.

[0110] <Preparation of lithium-ion batteries>

[0111] The single-sided positive electrode sheet in <Preparation of positive electrode sheet> is placed on the outermost side of the electrode assembly as the outermost electrode sheet of the electrode assembly. The remaining positive electrode sheets in the electrode assembly are all double-sided positive electrode sheets.

[0112] The outer positive electrode sheet, the first diaphragm, the outer negative electrode sheet, the first diaphragm, the second outer positive electrode sheet, the first diaphragm, the inner negative electrode sheet, the first diaphragm, the inner positive electrode sheet, the first diaphragm, the inner negative electrode sheet, the first diaphragm, the inner positive electrode sheet, the first diaphragm, the inner negative electrode sheet, the first diaphragm, the inner positive electrode sheet, the first diaphragm, the inner negative electrode sheet, the first diaphragm, the inner positive electrode sheet, the first diaphragm, the inner negative electrode sheet, the first diaphragm, the inner positive electrode sheet, the first diaphragm, the inner negative electrode sheet, the first diaphragm, the inner positive electrode sheet, the first diaphragm, the inner negative electrode sheet, the first diaphragm, the second outer positive electrode sheet, the first diaphragm, the outer negative electrode sheet, the first diaphragm, and the outer positive electrode sheet are stacked in sequence, wherein the first diaphragm is continuous and uninterrupted and presents a Z-shaped folding structure in the electrode assembly. Then, the four corners of the entire laminate structure are fixed with tape to obtain the electrode assembly of the laminate structure, and the electrode assembly is placed in an aluminum-plastic film packaging bag, placed in an 80°C vacuum oven for 12 hours to remove moisture, and the prepared electrolyte is injected, and a lithium-ion battery is obtained after vacuum packaging, standing, formation, degassing, trimming and other processes. The design potential range of the lithium-ion battery is 2.75V to 4.45V.

[0113] Example 1-2 to Example 1-13

[0114] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1. Among them, when the average particle size of the same ceramic particles changes, the grinding time is adjusted so that the value of the average particle size is as shown in Table 1. When the mass percentage of silicon element changes, the mass percentage of the conductive carbon nanotubes and the negative electrode binder remains unchanged, and the mass ratio of artificial graphite and silicon-carbon composite material SiO is adjusted so that the mass percentage of silicon element is as shown in Table 1. In Example 1-7, Example 1-8 and Example 1-11, the silicon-carbon composite material SiC is replaced with pure silicon, the mass percentage of the conductive carbon nanotubes and the negative electrode binder remains unchanged, and the mass ratio of artificial graphite and pure silicon is adjusted so that the mass percentage of silicon element is as shown in Table 1.

[0115] Examples 1-14

[0116] Except for preparing the first separator according to the following steps, the rest is the same as Example 1-1.

[0117] A polyethylene (PE) film with a thickness of 10 μm was used as the base film, and the porosity of the first base film was 60%.

[0118] The first ceramic particle boehmite and the first ceramic layer binder polyvinylidene fluoride were mixed in a mass ratio of 95:5, and then deionized water was added as a solvent. After mixing evenly, a first ceramic layer slurry was obtained.

[0119] The second ceramic particle boehmite and the second ceramic layer binder polyvinylidene fluoride were mixed in a mass ratio of 95:5, and then deionized water was added as a solvent, and the mixture was evenly mixed to obtain a second ceramic layer slurry.

[0120] The first adhesive styrene-butadiene latex and the first thickener sodium carboxymethyl cellulose were mixed in a mass ratio of 98.5:1.5, and then deionized water was added as a solvent. After mixing evenly, a first adhesive layer slurry was obtained.

[0121] The second binder, vinylidene fluoride homopolymer, and the second thickener, sodium carboxymethyl cellulose, were mixed in a mass ratio of 98.5:1.5, and then deionized water was added as a solvent. After mixing evenly, a second bonding layer slurry was obtained.

[0122] A first ceramic layer slurry is coated on one surface of the base film, and after drying at 60°C, a first ceramic layer is formed on one surface of the first base film. A first bonding layer slurry is coated on the surface of the first ceramic layer away from the base film, and after drying at 60°C, a first coating layer including a first ceramic coating layer and a first bonding layer is obtained. A second ceramic layer slurry is coated on the other surface of the base film, and after drying at 60°C, a second ceramic layer is formed on the other surface of the base film. A second bonding layer slurry is coated on the surface of the second ceramic layer away from the base film, and after drying at 60°C, a second coating layer including a second ceramic coating layer and a second bonding layer is obtained, and a first diaphragm is obtained.

[0123] The average particle size of the first ceramic particles is 1.5 μm, that is, D1 is 1.5 μm, and the average particle size of the second ceramic particles is 0.33 μm, that is, D2 is 0.33 μm. The coating weight of the first ceramic layer is 0.75 mg / 1540.25 mm 2 The coating weight of the second ceramic layer is 0.75mg / 1540.25mm 2 The porosity P1 of the first coating layer is 55%, and the porosity P2 of the second coating layer is 22%. The thickness T1 of the first bonding layer is 1 μm, and the thickness T2 of the second bonding layer is 1.2 μm.

[0124] Example 1-15 to Example 1-20

[0125] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1. When the thickness of the adhesive layer changes, the coating amount is adjusted so that the thickness of the adhesive layer is as shown in Table 1.

[0126] Example 2-1

[0127] Except that the positive electrode sheet is cut into a size of 70 mm × 800 mm in <Preparation of positive electrode sheet>, the negative electrode sheet is cut into a size of 74 mm × 824 mm in <Preparation of negative electrode sheet>, and the lithium-ion battery is prepared according to the following steps, the rest is the same as Example 1-1.

[0128] <Preparation of lithium-ion batteries>

[0129] The first separator, negative electrode sheet, first separator, and positive electrode sheet prepared above are stacked in order, ensuring that the first coating of the first separator faces the negative electrode sheet and the second coating of the first separator faces the positive electrode sheet, and are wound in order to obtain an electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, and after drying, the prepared electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, formation, degassing, trimming, and other processes.

[0130] Example 2-2

[0131] Except for preparing the lithium-ion battery and the second separator according to the following steps, the rest is the same as Example 1-1.

[0132] <Preparation of Second Separator>

[0133] A polyethylene (PE) film with a thickness of 10 μm was used as the base film, and the porosity of the base film was 60%.

[0134] The ceramic particles of boehmite and the ceramic layer binder polyvinylidene fluoride were mixed in a mass ratio of 95:5, and then deionized water was added as a solvent. After mixing evenly, a third ceramic layer slurry was obtained.

[0135] The third ceramic layer slurry is coated on one surface of the base film and dried at 60°C to form a third ceramic layer on one surface of the base film; the above operation is repeated on the other surface of the base film to obtain a second diaphragm.

[0136] The average particle size of the ceramic particles is 0.33 μm, the porosity of the third coating is 22%, and the coating weight of the third ceramic layer is 0.75 mg / 1540.25 mm 2 .

[0137] <Preparation of lithium-ion batteries>

[0138] The single-sided positive electrode sheet in <Preparation of positive electrode sheet> is placed on the outermost side of the electrode assembly as the outermost electrode sheet of the electrode assembly. The remaining positive electrode sheets in the electrode assembly are all double-sided positive electrode sheets.

[0139] Stack the outer positive electrode sheet, the first separator, the outer negative electrode sheet, the first separator, the second outer positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the second outer positive electrode sheet, the first separator, the outer negative electrode sheet, the first separator, and the outer positive electrode sheet in sequence. Then, the four corners of the entire laminate structure are fixed with tape to obtain the electrode assembly of the laminate structure, and the electrode assembly is placed in an aluminum-plastic film packaging bag, placed in an 80°C vacuum oven for 12 hours to remove moisture, and the prepared electrolyte is injected, and a lithium-ion battery is obtained after vacuum packaging, standing, formation, degassing, trimming and other processes. The design potential range of the lithium-ion battery is 2.75V to 4.45V.

[0140] Example 2-3

[0141] Except for preparing the lithium ion battery according to the following steps, the rest is the same as Example 2-2.

[0142] <Preparation of lithium-ion batteries>

[0143] The single-sided positive electrode sheet in <Preparation of positive electrode sheet> is placed on the outermost side of the electrode assembly as the outermost electrode sheet of the electrode assembly. The remaining positive electrode sheets in the electrode assembly are all double-sided positive electrode sheets.

[0144] Stack the outer positive electrode sheet, the first separator, the outer negative electrode sheet, the first separator, the second outer positive electrode sheet, the first separator, the inner negative electrode sheet, the first separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the second separator, the inner negative electrode sheet, the second separator, the inner positive electrode sheet, the first separator, the inner negative electrode sheet, the first separator, the second outer positive electrode sheet, the first separator, the outer negative electrode sheet, the first separator, and the outer positive electrode sheet in sequence. Then, the four corners of the entire laminate structure are fixed with tape to obtain the electrode assembly of the laminate structure, and the electrode assembly is placed in an aluminum-plastic film packaging bag, placed in an 80°C vacuum oven for 12 hours to remove moisture, and the prepared electrolyte is injected, and a lithium-ion battery is obtained after vacuum packaging, standing, formation, degassing, trimming and other processes. The design potential range of the lithium-ion battery is 2.75V to 4.45V.

[0145] Embodiment 2-4

[0146] Except that the first separator is used in <Preparation of lithium-ion battery>, the rest is the same as Example 2-2.

[0147] Comparative Example 1

[0148] Except that the preparation steps of the first coating layer are exactly the same as the preparation steps of the second coating layer in Example 1-1, the rest are the same as Example 1-1.

[0149] Comparative Example 2

[0150] Except that the preparation steps of the second coating layer are exactly the same as the preparation steps of the first coating layer in Example 1-1, the rest are the same as Example 1-1.

[0151] Comparative Example 3

[0152] Except that the preparation steps of the first coating layer are exactly the same as the preparation steps of the second coating layer in Example 1-1, and the preparation steps of the second coating layer are exactly the same as the preparation steps of the first coating layer in Example 1-1, the rest are the same as Example 1-1.

[0153] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 and 2.

[0154]

[0155]

[0156] From Examples 1-1 to 1-20 and Comparative Examples 1 to 3, it can be seen that by adjusting the porosity of the first coating to be greater than the porosity of the second coating, the degree of lithium precipitation of the negative electrode sheet in the electrode assembly is relatively light, the 500cls capacity retention rate of the lithium ion battery is improved, and the drop test pass rate is relatively high, indicating that the lithium ion battery of the present application can reduce the risk of deterioration of the negative electrode interface due to insufficient electrolyte, and the lithium ion battery has good cycle performance while taking into account drop performance and safety performance. The porosity of the first coating and the second coating of the first diaphragm of the electrode assembly in Comparative Examples 1 and 2 is the same; the various parameters of the first coating and the second coating in Comparative Example 3 are exactly opposite to the various parameters of the first coating and the second coating in Example 1-1; the degree of lithium precipitation of the negative electrode sheet in the lithium ion battery in Comparative Examples 1 to 3 is heavier; the 500cls capacity retention rate is lower; and / or, the drop test pass rate is lower. The lithium ion batteries in Examples 1-1 to 1-20 have a lower degree of lithium plating on the negative electrode sheets, a higher 500cls capacity retention rate, and a higher drop test pass rate, indicating that the risk of deterioration of the negative electrode sheets due to insufficient electrolyte during the cycle is lower. While taking into account both drop performance and safety performance, the lithium ion batteries have good cycle performance.

[0157] The value of W usually affects the cycle performance of lithium-ion batteries. It can be seen from Examples 1-1 to 1-11 that when the value of W is within the range of this application, the degree of lithium precipitation of the negative electrode sheet in the lithium-ion battery is relatively light, the 500cls capacity retention rate is relatively high, and the drop test pass rate is relatively high, indicating that the risk of deterioration of the negative electrode sheet due to insufficient electrolyte during the cycle is relatively low, and the lithium-ion battery has good cycle performance while taking into account both drop performance and safety performance.

[0158] The values ​​of P1 / P2 and P1 usually affect the cycle performance of lithium-ion batteries. It can be seen from Example 1-1 to Example 1-11 that when the values ​​of P1 / P2 and P1 are within the scope of this application, the degree of lithium precipitation of the negative electrode sheet in the lithium-ion battery is relatively light, the 500cls capacity retention rate is high, and the drop test pass rate is high, indicating that the risk of deterioration of the negative electrode sheet due to insufficient electrolyte during the cycle is low, and the lithium-ion battery has good cycle performance while taking into account drop performance and safety performance. Among them, the values ​​of P1 / P2 and P1 in Example 1-11 are relatively large, at this time the liquid storage capacity of the diaphragm on the positive side is relatively weak, the liquid storage capacity of the diaphragm on the negative side is relatively strong, and the liquid storage amount on both sides is relatively different, resulting in a decrease in the 500cls capacity retention rate of the lithium-ion battery, and at the same time, there is more free electrolyte in the shell, which reduces the drop test pass rate of the lithium-ion battery, and the cycle performance and drop performance of the lithium-ion battery are affected.

[0159] The correspondence between P1 / P2 and W usually affects the cycle performance of lithium-ion batteries. It can be seen from Examples 1-1 to 1-10 that when the correspondence between P1 / P2 and W meets the requirements of this application, the degree of lithium precipitation of the negative electrode sheet in the lithium-ion battery is relatively light, the 500cls capacity retention rate is high, and the drop test pass rate is high, indicating that the risk of deterioration of the negative electrode sheet due to insufficient electrolyte during the cycle is low, and the lithium-ion battery has good cycle performance while taking into account drop performance and safety performance. Among them, in Examples 1-10, the values ​​of P1 / P2 and P1 are relatively large relative to the value of W. At this time, the liquid storage capacity of the diaphragm on the positive electrode side is relatively weak, and the liquid storage amount on both sides differs greatly, resulting in a decrease in the 500cls capacity retention rate of the lithium-ion battery, and the cycle performance of the lithium-ion battery is affected.

[0160] The average particle size of the first ceramic particles and the average particle size of the second ceramic particles usually affect the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1 to 1-11 that when the average particle size of the first ceramic particles and the average particle size of the second ceramic particles are within the range of this application, the degree of lithium precipitation of the negative electrode sheet in the lithium-ion battery is relatively light, the 500cls capacity retention rate is relatively high, and the drop test pass rate is relatively high, indicating that the risk of deterioration of the negative electrode sheet due to insufficient electrolyte during the cycle is relatively low, and the lithium-ion battery has good cycle performance while taking into account both drop performance and safety performance.

[0161] The type of the first ceramic particles and the type of the second ceramic particles usually affect the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-12 and 1-13 that when the first ceramic particles and the second ceramic particles within the scope of the present application are selected, the lithium ion battery negative electrode sheet has a lower degree of lithium precipitation, a higher 500cls capacity retention rate, and a higher drop test pass rate, indicating that the risk of deterioration of the negative electrode sheet due to insufficient electrolyte during the cycle is lower, and the lithium-ion battery has good cycle performance while taking into account drop performance and safety performance.

[0162] The type of the first binder and the type of the second binder usually affect the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-14 and 1-17 that when the first binder and the second binder within the scope of the present application are selected, the lithium plating degree of the negative electrode sheet in the lithium-ion battery is relatively light, the 500cls capacity retention rate is relatively high, and the drop test pass rate is relatively high, indicating that the risk of deterioration of the negative electrode sheet due to insufficient electrolyte during the cycle is relatively low, and the lithium-ion battery has good cycle performance while taking into account drop performance and safety performance.

[0163] The thickness T1 of the first adhesive layer usually affects the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-18 to 1-20 that when the thickness T1 of the first adhesive layer is within the scope of this application, the degree of lithium precipitation of the negative electrode sheet in the lithium-ion battery is relatively light, the 500cls capacity retention rate is relatively high, and the drop test pass rate is relatively high, indicating that the risk of deterioration of the negative electrode sheet due to insufficient electrolyte during the cycle is relatively low. While taking into account both drop performance and safety performance, the lithium-ion battery has good cycle performance. Among them, the thickness of the first adhesive layer in Example 1-20 is relatively large, and the porosity of the first coating is reduced. At this time, the resistance encountered during the lithium ion transmission process during the cycle increases, and the ion transmission capacity is affected, resulting in a decrease in the 500cls capacity retention rate of the lithium-ion battery and the cycle performance of the lithium-ion battery.

[0164] Table 2

[0165] Electrode assembly structure n m m / n Lithium precipitation degree 500cls capacity retention rate (%) Drop test pass rate (%) Example 1-1 Lamination / / 1 No lithium precipitation 85 100 Example 2-1 Winding / / 1 No lithium precipitation 76 100 Example 2-2 Lamination 16 4 1 / 4 Moderate lithium precipitation 75 100 Example 2-3 Lamination 16 8 1 / 2 Mild lithium deposition 80 100 Embodiment 2-4 Lamination 16 16 1 No lithium precipitation 85 95

[0166] Note: “ / ” in Table 2 indicates no relevant preparation parameters.

[0167] The structure of the electrode assembly usually affects the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1, 2-1 and 2-4 that when the structure of the electrode assembly meets the requirements of this application, the negative electrode sheet in the lithium-ion battery has a relatively light lithium deposition degree, a high 500cls capacity retention rate, and a high drop test pass rate, indicating that the risk of deterioration of the negative electrode sheet due to insufficient electrolyte during the cycle is relatively low, and the lithium-ion battery has good cycle performance while taking into account both drop performance and safety performance.

[0168] The value of m / n usually affects the cycle performance of lithium-ion batteries. It can be seen from Examples 1-1, 2-2 and 2-4 that when the value of m / n meets the requirements of this application, the negative electrode sheet in the lithium-ion battery has a relatively light lithium deposition degree, a high 500cls capacity retention rate, and a high drop test pass rate, indicating that the risk of deterioration of the negative electrode sheet due to insufficient electrolyte during the cycle is relatively low, and the lithium-ion battery has good cycle performance while taking into account drop performance and safety performance.

[0169] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method or article including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method or article.

[0170] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0171] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A secondary battery, comprising an electrode assembly, the electrode assembly comprising an electrode sheet and a first separator, the electrode sheet comprising a positive electrode sheet and a negative electrode sheet, the negative electrode sheet comprising a negative electrode material layer, the negative electrode material layer comprising silicon, based on the mass of the negative electrode material layer, the mass percentage of the silicon element is W, W ≥ 3%; The first separator includes a base film, a first coating layer and a second coating layer. Along the thickness direction of the first separator, the base film includes a first surface and a second surface. The first surface faces the negative electrode sheet, and the second surface faces the positive electrode sheet. The first coating layer is disposed on the first surface, and the second coating layer is disposed on the second surface. The porosity of the first coating layer is P1, the porosity of the second coating layer is P2, and P1>P2.

2. The secondary battery according to claim 1, wherein 3%≤W≤80%。 3. The secondary battery according to claim 1, wherein The first coating layer includes a first ceramic layer, and the second coating layer includes a second ceramic layer.

4. The secondary battery according to claim 3, wherein 1<P1 / P2≤5, 30%≤P1≤70%.

5. The secondary battery according to claim 4, wherein 0.6P1 / P2≤0.04W×100+0.98≤1.5P1 / P2.

6. The secondary battery according to claim 4, wherein 3%≤W≤10%, 1<P1 / P2≤1.5, 30%≤P1≤40%.

7. The secondary battery according to claim 4, wherein 10%<W≤30%, 1.5<P1 / P2≤2.5, 40%<P1≤55%.

8. The secondary battery according to claim 4, wherein 30%<W≤80%, 2.5<P1 / P2≤5, 55%<P1≤70%.

9. The secondary battery according to claim 3, wherein: The first ceramic layer includes first ceramic particles, the second ceramic layer includes second ceramic particles, the first ceramic particles and the second ceramic particles are each independently selected from at least one of aluminum oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide or boehmite; The average particle size of the first ceramic particles is D1 μm, 0.5≤D1≤3; The average particle size of the second ceramic particles is D2 μm, and 0.25≤D2≤0.

45.

10. The secondary battery according to claim 3, wherein The first coating layer further comprises a first bonding layer, the first bonding layer and the first ceramic layer are sequentially stacked on the first surface, and the first ceramic layer is located between the first bonding layer and the base film; the second coating layer further comprises a second bonding layer, the second bonding layer and the second ceramic layer are sequentially stacked on the second surface, and the second ceramic layer is located between the second bonding layer and the base film; The first adhesive layer includes a first adhesive, and the second adhesive layer includes a second adhesive. The first adhesive and the second adhesive are each independently selected from at least one of styrene-butadiene latex, styrene-acrylic latex, polymethyl methacrylate, polybutyl methacrylate, polyethyl acrylate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate, polyurethane, polyvinylidene fluoride, or a copolymer of vinylidene fluoride and hexafluoropropylene.

11. The secondary battery according to claim 10, wherein The first adhesive layer has a thickness of 0.5 μm to 3 μm.

12. The secondary battery according to claim 10, wherein The first binder includes at least one of styrene-butadiene latex, styrene-acrylic latex, polymethyl methacrylate, polybutyl methacrylate, polyethyl acrylate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate or polyurethane, and the second binder includes at least one of polyvinylidene fluoride or a copolymer of vinylidene fluoride and hexafluoropropylene.

13. The secondary battery according to claim 1, wherein The electrode assembly is a laminate structure.

14. The secondary battery according to claim 13, wherein The electrode assembly also includes a second diaphragm, the electrode pieces include two outer electrode pieces and a plurality of inner electrode pieces, the two outer electrode pieces are respectively located on the outermost sides of the electrode assembly, the first diaphragm is at least arranged between the outer electrode piece and the inner electrode piece adjacent to the outer electrode piece, and the second diaphragm is arranged between two adjacent inner electrode pieces.

15. The secondary battery according to claim 14, wherein The number of layers of the first diaphragm is m, the total number of layers of the first diaphragm and the second diaphragm is n, and 1 / 5≤m / n≤1.

16. The secondary battery according to claim 13, wherein The first separator is in a Z-shaped folded structure in the electrode assembly, and the Z-shaped first separator separates the adjacent positive electrode sheet from the negative electrode sheet. 17 . An electronic device comprising the secondary battery according to claim 1 .

Citation Information

Patent Citations

  • Separator, electrochemical device, and electronic apparatus

    CN116315459A

  • High security lithium cell and diaphragm thereof

    CN205248350U

  • Battery monomer, battery and electric device

    CN220774471U

  • Electrochemical device with improved safety

    KR1020170003020A

  • A Section Reducing Member and a Fixing Frame for Concrete Structure and a Construction Method thereof

    KR1020230046923A

Cited By

  • Diaphragm and preparation method thereof, battery and electric device

    CN121076411A

  • Secondary battery and electronic device

    CN122315276A

  • Secondary battery and electronic device

    WO2026066426A1

  • Battery cell, separator, battery device and electrical device

    WO2026153268A1

  • Battery cell, battery apparatus and electrical apparatus

    WO2026174877A1