A nano-TiB reinforced titanium-based composite powder and preparation method thereof
Nano-TiB reinforced titanium-based composite powder is prepared through vacuum reaction hot pressing and heating rotation processing, which solves the problems of poor uniformity and high cost in the preparation of titanium-based composite powder, and achieves high-quality and uniform nano-scale powder.
Patent Information
- Application Number
- CN202210078260.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-01-24
AI Technical Summary
Existing powder preparation methods for titanium-based composite materials have problems such as poor uniformity, high cost, high oxidation risk, and low powder quality. In particular, when introducing ceramic reinforcements, high-energy ball milling is required, resulting in powder deformation and uneven particle size.
By mixing titanium alloy powder and reinforcement powder and performing vacuum reaction and hot-pressing sintering to form a sintered body, the sintered body is then heated and rotated to melt and condense into nano-TiB reinforced titanium-based composite powder. Rapid cooling and surface tension are used to form spherical powder, which avoids The spheres stick together and control the particle size range.
The nano-TiB reinforced titanium-based composite powder has a high sphericity, a narrow particle size range and a uniform distribution of reinforcement phases, reducing material costs and oxidation risks, and improving the quality and uniformity of the powder.
Smart Images

Figure CN114406275B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal-based composite materials, and in particular to a nano-TiB reinforced titanium-based composite powder and a preparation method thereof. Background Art
[0002] Titanium-based composite materials have excellent properties such as high specific strength and high temperature resistance, and are important materials for future applications in the field of aerospace technology. Titanium-based composite materials are mainly made of a mechanical mixture of titanium alloy powder and ceramic reinforcement powder as raw materials, but there is no ceramic phase inside the powder of the mechanical mixture, and the ceramic particles are only attached to the surface of the titanium alloy powder, which limits the scope of the titanium-based composite material organization regulation and the strengthening effect of the ceramic reinforcement, and greatly reduces the plasticity of the material. In the prior art, if ceramic reinforcement is to be introduced into the mechanical mixed powder, it is necessary to use extremely fine titanium alloy powder as raw material and apply very high ball milling energy to achieve this, but this not only increases the material cost, but also increases the risk of powder oxidation. The final powder will also be deformed due to the high energy, and the sphericity will decrease.
[0003] The Chinese patent with publication number CN110340371A discloses a method for preparing a powder for particle-reinforced titanium-based composite material additive manufacturing, wherein a titanium-based composite material block material is first prepared by a smelting method, and then a titanium-based composite powder is prepared by a gas atomization powder making method. However, this method has three disadvantages: first, the uniformity of the titanium-based composite material is poor during the smelting process, and it is easy to form a macroscopically uneven organization, which will lead to poor uniformity of the titanium-based composite powder obtained subsequently; if the uniformity is to be improved, multiple smelting is required, which not only prolongs the preparation cycle, but also increases the difficulty of preparation, and also increases the risk of oxidation of the titanium-based composite material; second, the block of the titanium-based composite material after smelting needs to be forged and machined into a rod, which increases the powder making step and also causes material waste; third, the cooling rate of the gas atomization powder making is low, the powder obtained is very easy to form sphere adhesion, and the powder quality is low, holes are easy to appear inside, and the obtained powder particle size range is also wide and uneven. Summary of the invention
[0004] The embodiment of the present invention provides a nano-TiB reinforced titanium-based composite powder and a preparation method thereof. The provided nano-TiB reinforced titanium-based composite powder has high sphericity, a narrow particle size range, and uniform distribution of internal reinforcement phases.
[0005] In a first aspect, the present invention provides a method for preparing a nano-TiB reinforced titanium-based composite powder, comprising the following steps:
[0006] Step 1: uniformly mixing titanium alloy powder and reinforcement powder to obtain a mixture;
[0007] Step 2: subjecting the mixture to vacuum reaction hot pressing sintering treatment to obtain a sintered body;
[0008] Step three: heating and rotating the sintered body to rotate the heated and melted sintered body to obtain molten droplets, and cooling the molten droplets to obtain the nano-TiB reinforced titanium-based composite powder.
[0009] Preferably, in step one, the titanium alloy powder is TC4 titanium alloy powder or TA15 titanium alloy powder, and the reinforcement powder is TiB2 powder or boron powder.
[0010] Preferably, the particle size of the titanium alloy powder is 100-200 μm, the particle size of the TiB2 powder is 3-5 μm, and the particle size of the boron powder is 0.5-1 μm.
[0011] Preferably, in step one, it includes:
[0012] The titanium alloy powder and the reinforcement powder are ball-milled in an argon environment for 4-8 hours, the rotation speed of the ball-milling is 200-250 r / min, and the ball-to-material ratio is (3-5):1.
[0013] Preferably, in step 2, the temperature of the vacuum reaction hot pressing sintering treatment is 1150-1300°C, the pressure is 20-30Mpa, and the vacuum degree is less than 5×10 -2 Pa, time is 0.5-2h.
[0014] Preferably, in step three, the heating temperature of the heating and rotating treatment is 2800-3400° C., and the rotating speed is 20000-30000 r / min.
[0015] Preferably, in step 2, it includes: placing the mixture into a matching mold and performing vacuum reaction hot pressing sintering;
[0016] In step three, the process includes: fixing the sintered body on a rotary clamp of a plasma rotating electrode atomizing powder making device, wherein the rotary clamp is used to rotate the sintered body;
[0017] The size of the matching mold matches the size of the rotary clamp so that the sintered body can be fixed on the rotary clamp.
[0018] Preferably, the matching mold is made of graphite.
[0019] Preferably, in step three, it includes:
[0020] The sintered body is fixed on the rotary clamp, and under an argon environment, the current of the plasma rotary electrode atomization powder making equipment is adjusted to 600-800A, the rotation speed of the rotary clamp is set to 20000-30000r / min, and the feed speed of the sintered body is set to 1.5-3mm / s, so that the heated and molten sintered body is rotated out to obtain molten droplets;
[0021] The molten liquid droplets are cooled to obtain the nano-TiB reinforced titanium-based composite powder.
[0022] In a second aspect, the present invention provides a nano-TiB reinforced titanium-based composite powder prepared according to any one of the preparation methods described in the first aspect.
[0023] Compared with the prior art, the present invention has at least the following beneficial effects:
[0024] In the present invention, titanium alloy powder and reinforcement powder are first mixed uniformly to make the titanium alloy powder and reinforcement powder uniformly mixed on a macro scale and obtain a mechanical mixture, and then the mechanical mixture is subjected to vacuum reaction hot pressing sintering treatment to make the boron element in the reinforcement powder react with the titanium element in situ to obtain a sintered body including a micron-sized reinforcement phase.
[0025] In the present invention, a sintered body is heated to melt the surface of the sintered body, and then the sintered body is rotated so that the molten sintered body is thrown out under the action of centrifugal force to form a plurality of molten droplets. The molten droplets are condensed to obtain nano-TiB-reinforced titanium-based composite powder. Since the nano-TiB-reinforced titanium-based composite powder is formed by condensation of molten droplets, the droplets agglomerate into a sphere due to surface tension. Therefore, the generated powder is spherical, thereby avoiding the situation where multiple spheres adhere to each other. Since the particles of the powder are formed by condensation of molten droplets, the particle size range of the formed powder is narrow. The molten droplets are rapidly cooled, and the cooling rate can reach 10 3 -10 4 ℃ / s, when the droplets are rapidly condensed, the nucleation rate of titanium is high, titanium is preferentially nucleated and crystallized, and the B element is pushed to the grain boundary and reacts to form TiB. Due to the fast cooling rate and the small size of the reinforcement phase, particles with nano-scale reinforcement phase inside are obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1This is a surface microscopic image of a nano-TiB reinforced titanium-based composite powder having a reinforcing phase content of 1 vol% provided in an embodiment of the present invention;
[0028] Figure 2 This is a surface microscopic image of another nano-TiB reinforced titanium-based composite powder with a reinforcing phase content of 1 vol% provided in an embodiment of the present invention;
[0029] Figure 3 This is a surface microscopic image of another nano-TiB reinforced titanium-based composite powder with a reinforcing phase content of 1 vol% provided in an embodiment of the present invention;
[0030] Figure 4 This is a cross-sectional microscopic image of a nano-TiB reinforced titanium-based composite powder having a reinforcing phase content of 1 vol% provided in an embodiment of the present invention;
[0031] Figure 5 This is a cross-sectional microscopic image of another nano-TiB reinforced titanium-based composite powder having a reinforcing phase content of 1 vol% provided in an embodiment of the present invention;
[0032] Figure 6 This is a cross-sectional microscopic image of another nano-TiB reinforced titanium-based composite powder with a reinforcing phase content of 1 vol% provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0034] The embodiment of the present invention provides a method for preparing nano-TiB reinforced titanium-based composite powder, comprising the following steps:
[0035] Step 1: uniformly mixing titanium alloy powder and reinforcement powder to obtain a mixture;
[0036] Step 2: subjecting the mixture to vacuum reaction hot pressing sintering treatment to obtain a sintered body;
[0037] Step three: heating and rotating the sintered body to rotate the heated and melted sintered body to obtain molten droplets, and cooling the molten droplets to obtain the nano-TiB reinforced titanium-based composite powder.
[0038] In the present invention, titanium alloy powder and reinforcement powder are first mixed uniformly to make the titanium alloy powder and reinforcement powder uniformly mixed on a macro scale and obtain a mechanical mixture, and then the mechanical mixture is subjected to a vacuum reaction hot pressing sintering treatment to make the non-metallic elements in the reinforcement powder react with the titanium element in situ to obtain a sintered body including a micron-sized reinforcement phase.
[0039] In the present invention, a sintered body is heated to melt the surface of the sintered body, and then the sintered body is rotated so that the molten sintered body is thrown out under the action of centrifugal force to form a plurality of molten droplets. The molten droplets are condensed to obtain nano-TiB-reinforced titanium-based composite powder. Since the nano-TiB-reinforced titanium-based composite powder is formed by condensation of molten droplets, the droplets agglomerate into a sphere due to surface tension. Therefore, the generated powder is spherical, thereby avoiding the situation where multiple spheres adhere to each other. Since the particles of the powder are formed by condensation of molten droplets, the particle size range of the formed powder is narrow. The molten droplets are rapidly cooled, and the cooling rate can reach 10 3 -10 4 ℃ / s, when the droplets are rapidly condensed, the nucleation rate of titanium is high, titanium is preferentially nucleated and crystallized, and the B element is pushed to the grain boundary and reacts to form TiB. Due to the fast cooling rate and the small size of the reinforcement phase, particles with nano-scale reinforcement phase inside are obtained.
[0040] It should be noted that the method provided in this application can be used to prepare nano-TiB reinforced titanium-based composite powder with a reinforcing phase content of 0.001-10 vol%. The mass ratio of titanium alloy powder and reinforcing body powder in the mixture needs to be adjusted according to the obtained reinforcing phase content.
[0041] According to some preferred embodiments, in step one, the titanium alloy powder is TC4 titanium alloy powder or TA15 titanium alloy powder, and the reinforcement powder is TiB2 powder or boron powder.
[0042] In the present invention, TC4 titanium alloy powder or TA15 titanium alloy powder is selected as the matrix of the composite material, wherein TA15 titanium alloy has excellent high temperature resistance, and the type of titanium alloy powder can be selected according to the use requirements.
[0043] In the present invention, after the reinforcing body containing boron element is mixed and melted with titanium alloy, an in-situ autogenous reaction can occur during the condensation process to form a stable TiB reinforcing phase.
[0044] According to some preferred embodiments, the particle size of the titanium alloy powder is 100-200μm (for example, it can be 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm or 200μm), the particle size of the TiB2 powder is 3-5μm (for example, it can be 3μm, 4μm or 5μm), and the particle size of the boron powder is 0.5-1μm (for example, it can be 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm or 1μm).
[0045] In the present invention, the particle sizes of the titanium alloy powder and the reinforcement powder are selected within the above range, so that the two can be mixed evenly after low-energy ball milling.
[0046] According to some preferred embodiments, in step 1, it includes:
[0047] The titanium alloy powder and the reinforcement powder are ball-milled in an argon environment for 4-8 hours (for example, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours), the ball-milling rotation speed is 200-250 r / min (for example, 200 r / min, 210 r / min, 220 r / min, 230 r / min, 240 r / min or 250 r / min), and the ball-to-material ratio is (3-5):1 (for example, 3:1, 4:1, or 5:1).
[0048] In the present invention, the titanium alloy powder and the reinforcement powder can be fully and uniformly mixed by ball milling, and the argon gas environment can protect the titanium alloy powder and the reinforcement powder from being oxidized.
[0049] It should be noted that, in the scheme of the present invention, low-energy ball milling with a rotation speed of 200-250r / min can meet the uniformity requirements of the present invention. Of course, the present invention can also choose high-energy ball milling, but under the premise that low-energy ball milling can meet the use requirements, in line with the principle of cost saving, low-energy ball milling can be selected in this step.
[0050] According to some preferred embodiments, in step 2, the temperature of the vacuum reaction hot pressing sintering treatment is 1150-1300°C (for example, 1150°C, 1200°C, 1250°C or 1300°C), the pressure is 20-30Mpa (20Mpa, 21Mpa, 22Mpa, 23Mpa, 24Mpa, 25Mpa, 26Mpa, 27Mpa, 28Mpa, 29Mpa or 30Mpa), and the vacuum degree is less than 5×10 - 2Pa, the time is 0.5-2h (for example, it can be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h or 2h).
[0051] In the present invention, the mixture is placed at 1150-1300°C, 20-30MPa and a vacuum degree of less than 5×10 -2 Pa environment, and then vacuum reaction hot pressing sintering treatment is carried out for 0.5-2h, so that the obtained sintered body has excellent density, reduces its risk of oxidation, and improves its uniformity; at the same time, during the vacuum reaction hot pressing sintering process, the non-metallic elements in the reinforcement phase powder react in situ with the titanium element in the titanium alloy to obtain a micron-sized reinforcement phase.
[0052] According to some preferred embodiments, in step three, the heating temperature of the heating and rotating treatment is 2800-3400°C (for example, it can be 2800°C, 2900°C, 3000°C, 3100°C, 3200°C, 3300°C or 3400°C), and the rotation speed is 20000-30000r / min (for example, it can be 20000r / min, 21000r / min, 22000r / min, 23000r / min, 24000r / min, 25000r / min, 26000r / min, 27000r / min, 28000r / min, 29000r / min or 30000r / min).
[0053] In the present invention, heating the sintered body to the above temperature can melt the surface of the sintered body, and rotating the sintered body at the above speed can cause the molten sintered body to be thrown out in the form of droplets under the action of centrifugal force.
[0054] According to some preferred embodiments, in step 2, it includes: loading the mixture into a matching mold to perform vacuum reaction hot pressing sintering;
[0055] In step three, the process includes: fixing the sintered body on a rotary clamp of a plasma rotating electrode atomizing powder making device, wherein the rotary clamp is used to rotate the sintered body;
[0056] The size of the matching mold matches the size of the rotary clamp so that the sintered body can be fixed on the rotary clamp.
[0057] In the present invention, the size of the matching mold matches the size of the rotary clamp, and the mixture is loaded into the matching mold for vacuum reaction hot pressing sintering to obtain a sintered body, so that the obtained sintered body can be directly loaded and fixed on the rotary clamp without processing, eliminating the step of secondary processing, avoiding the waste of raw materials, and further simplifying the preparation process of nano-TiB reinforced titanium-based composite powder.
[0058] In the present invention, before step three and after step two, the method further includes: polishing the surface of the sintered body to remove pollutants on the surface and make the surface smooth.
[0059] It should be noted that the treatment described in step three may not be performed immediately after the sintered body is obtained in step two. Therefore, there may be contaminants on the surface of the sintered body that has been stored for a period of time. In order to avoid the subsequent preparation of nano-TiB reinforced titanium-based composite powder being doped with contaminants, the surface of the sintered body needs to be polished before performing step three.
[0060] According to some preferred embodiments, the matching mold is made of graphite.
[0061] In the present invention, graphite is selected as the material for making the matching mold. Graphite has excellent thermal conductivity and thermal stability. Of course, steel can also be selected as the material for preparing the matching mold, but graphite has a lower cost than steel.
[0062] According to some preferred implementations, in step three, it includes:
[0063] The sintered body is fixed on the rotary clamp, and under an argon environment, the current of the plasma rotary electrode atomization powder making device is adjusted to 600-800A (for example, 600A, 650A, 700A, 750A or 800A), and the rotation speed of the rotary clamp is set to 20000-30000r / min (for example, 20000r / min, 21000r / min, 22000r / min, 23000r / min, 24000r / min, 25000r / min, 26000r / min, 27000r / min, etc. in, 28000r / min, 29000r / min or 30000r / min), setting the feeding speed of the sintered body to 1.5-3mm / s (for example, it can be 1.5mm / s, 1.6mm / s, 1.7mm / s, 1.8mm / s, 1.9mm / s, 2mm / s, 2.1mm / s, 2.2mm / s, 2.3mm / s, 2.4mm / s, 2.5mm / s, 2.6mm / s, 2.7mm / s, 2.8mm / s, 2.9mm / s or 3mm / s) so that the heated and molten sintered body is spun out to obtain molten droplets;
[0064] The molten liquid droplets are cooled to obtain the nano-TiB reinforced titanium-based composite powder.
[0065] It should be noted that the high-temperature molten droplets can be naturally cooled quickly after being spun out, and the cooling rate can reach 10 3 -10 4 ℃ / s.
[0066] In the present invention, a plasma rotating electrode atomizing powder making device is selected to heat and rotate the sintered body, and the current of the plasma rotating electrode atomizing powder making device is adjusted to release high-temperature plasma, and the surface of the sintered body is melted by the high-temperature plasma, and the sintered body is rotated by rotating clamping. At the same time, the particle size of the molten droplets can also be controlled by controlling the rotation speed and the feed speed of the sintered body.
[0067] The embodiment of the present invention further provides a nano-TiB reinforced titanium-based composite powder, which is prepared according to any of the above-mentioned preparation methods.
[0068] The nano-TiB reinforced titanium-based composite powder provided by the invention has high sphericity, a narrow particle size range, and the reinforcement phase can be evenly distributed inside the powder.
[0069] In order to more clearly illustrate the technical solution and advantages of the present invention, a nano-TiB reinforced titanium-based composite powder and a preparation method thereof are described in detail below through several embodiments.
[0070] Example 1
[0071] 130 μm TC4 titanium alloy powder and 4 μm TiB2 powder were ball-milled for 5 hours in an argon environment to obtain a mixture; wherein the mass fraction of TC4 titanium alloy powder was 99.4 wt%, the mass fraction of TiB2 was 0.6 wt%, the speed of ball milling was 220 r / min, and the ball-to-material ratio was 5:1;
[0072] The mixture was placed in a matching mold made of graphite, and then the matching mold containing the mixture was heated at 1200°C, 25 MPa and a vacuum degree of 4×10 -2 Pa environment, vacuum reaction hot pressing sintering treatment was performed for 1.5 h to obtain a sintered body;
[0073] The sintered body is polished and fixed on a rotary clamp in a plasma rotating electrode atomizing powder making device under an argon environment. The surface of the sintered body is melted by adjusting the current of the plasma rotating electrode atomizing powder making device to 750A. The rotation speed of the rotary clamp is set to 28000r / min to rotate the sintered body. The feed speed of the sintered body is set to 2.5mm / s at the same time, so that molten droplets are rotated out of the surface of the molten sintered body under the action of centrifugal force. After the molten droplets are condensed, a nano-TiB reinforced titanium-based composite powder with a reinforcing phase TiB content of 1vol% is obtained.
[0074] Example 2
[0075] 180 μm TA15 titanium alloy powder and 3 μm TiB2 powder were ball-milled for 6 hours in an argon environment to obtain a mixture; wherein the mass fraction of TA15 titanium alloy powder was 97.1 wt%, the mass fraction of TiB2 was 2.9 wt%, the speed of ball milling was 200 r / min, and the ball-to-material ratio was 3:1;
[0076] The mixture was placed in a matching mold made of graphite material, and then the matching mold containing the mixture was heated at 1180°C, 23 MPa and a vacuum degree of 4.6×10 -2 Pa environment, vacuum reaction hot pressing sintering treatment was performed for 2 h to obtain a sintered body;
[0077] The sintered body was polished and fixed on a rotary clamp in a plasma rotating electrode atomizing powder making device under an argon environment. The surface of the sintered body was melted by adjusting the current of the plasma rotating electrode atomizing powder making device to 760A. The rotation speed of the rotary clamp was set to 29000r / min to rotate the sintered body. The feed speed of the sintered body was set to 2.1mm / s at the same time, so that molten droplets were rotated out of the surface of the molten sintered body under the action of centrifugal force. After the molten droplets were condensed, a nano-TiB reinforced titanium-based composite powder with a reinforcing phase content of 5vol% was obtained.
[0078] Example 3
[0079] 160 μm TC4 titanium alloy powder and 0.6 μm boron powder were ball-milled for 5.5 hours in an argon environment to obtain a mixture; wherein the mass fraction of TA15 titanium alloy powder was 99.8wt%, the mass fraction of boron powder was 0.2wt%, the speed of ball milling was 250 r / min, and the ball-to-material ratio was 4:1;
[0080] The mixture was placed in a matching mold made of graphite material, and then the matching mold containing the mixture was heated at 1200°C, 25 MPa and a vacuum degree of 4×10 -2 Pa environment, vacuum reaction hot pressing sintering treatment was performed for 1.5 h to obtain a sintered body;
[0081] The sintered body is polished and fixed on a rotary clamp in a plasma rotating electrode atomizing powder making device under an argon environment. The surface of the sintered body is melted by adjusting the current of the plasma rotating electrode atomizing powder making device to 750A. The rotation speed of the rotary clamp is set to 28000r / min to rotate the sintered body. The feed speed of the sintered body is set to 2mm / s at the same time, so that molten droplets are rotated out of the surface of the molten sintered body under the action of centrifugal force. After the molten droplets are condensed, a nano-TiB reinforced titanium-based composite powder with a reinforcing phase content of 1vol% is obtained.
[0082] Example 4
[0083] Example 4 is basically the same as Example 3, except that the titanium alloy powder is TA15 titanium alloy powder (particle size is 200 μm), the mass fraction of TA15 titanium alloy powder is 99.8wt%, the mass fraction of boron powder is 0.2wt%; and the particle size of the boron powder is 0.5μm.
[0084] Example 5
[0085] 100 μm TC4 titanium alloy powder and 1 μm boron powder were ball-milled for 4 hours in an argon environment to obtain a mixture; wherein the mass fraction of TA15 titanium alloy powder was 99.8wt%, the mass fraction of boron powder was 0.2wt%, the speed of ball milling was 250 r / min, and the ball-to-material ratio was 5:1;
[0086] The mixture was placed in a matching mold made of graphite material, and then the matching mold containing the mixture was heated at 1150°C, 20 MPa and a vacuum degree of 4×10 -2 The vacuum reaction hot pressing sintering treatment was carried out in an environment of Pa for 0.5 h to obtain a sintered body.
[0087] The sintered body is polished and fixed on a rotary clamp in a plasma rotating electrode atomizing powder making device under an argon environment. The surface of the sintered body is melted by adjusting the current of the plasma rotating electrode atomizing powder making device to 600A. The rotation speed of the rotary clamp is set to 20000r / min to rotate the sintered body. The feed speed of the sintered body is set to 1.5mm / s at the same time, so that molten droplets are rotated out of the surface of the molten sintered body under the action of centrifugal force. After the molten droplets are condensed, a nano-TiB reinforced titanium-based composite powder with a reinforcing phase content of 1vol% is obtained.
[0088] Example 6
[0089] 200 μm TA15 titanium alloy powder and 5 μm TiB2 powder were ball-milled for 8 hours in an argon environment to obtain a mixture; wherein the mass fraction of TA15 titanium alloy powder is 97.1wt%, the mass fraction of TiB2 is 2.9wt%, the speed of ball milling is 200 r / min, and the ball-to-material ratio is 5:1;
[0090] The mixture was placed in a matching mold made of graphite material, and then the matching mold containing the mixture was heated at 1300°C, 30 MPa and a vacuum degree of 4.9×10 -2 Pa environment, vacuum reaction hot pressing sintering treatment was performed for 2 h to obtain a sintered body;
[0091] The sintered body is polished and fixed on a rotary clamp in a plasma rotating electrode atomizing powder making device under an argon environment. The surface of the sintered body is melted by adjusting the current of the plasma rotating electrode atomizing powder making device to 800A. The rotation speed of the rotary clamp is set to 30000r / min to rotate the sintered body. The feed speed of the sintered body is set to 3mm / s at the same time, so that molten droplets are rotated out of the surface of the molten sintered body under the action of centrifugal force. After the molten droplets are condensed, a nano-TiB reinforced titanium-based composite powder with a reinforcing phase content of 5vol% is obtained.
[0092] The nano-TiB-enhanced titanium-based composite powders prepared in Examples 1-6 were sieved to obtain powders of three different particle sizes, namely, less than 100 mesh, 100-200 mesh, and greater than 200 mesh. Among them, powders less than 100 mesh accounted for only 9% of the prepared powders, powders of 100-200 mesh accounted for 56%, and fine powders greater than 200 mesh accounted for 35%. It can be seen that the nano-TiB-enhanced titanium-based composite powders provided in this application have a narrow particle size range and a high fine powder acquisition rate.
[0093] Figure 1-6 This is a microscopic image of a nano-TiB reinforced titanium-based composite powder with a reinforcing phase content of 1 vol% prepared in Example 1. Figure 1-3 It can be seen that the nano-TiB reinforced titanium-based composite powder is spherical, has no spherical adhesion phenomenon, no flat particles, uniform particle size, and high powder quality; at the same time, according to Figure 4-6 It can be seen that there are no hole defects in the cross section of the nano-TiB reinforced titanium-based composite powder, and Figure 6 Nanoscale TiB whiskers can be observed at the grain boundaries, with a length of less than 500 nm and a diameter of less than 100 nm.
[0094] It should be noted that in order to facilitate the observation of the subgrain boundaries of the hypoeutectic structure under a microscope, the powder is corroded so that the subgrain boundaries are corroded for easy observation. The network of dark cracks in the figure are the subgrain boundaries after corrosion.
[0095] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing nano-TiB reinforced titanium-based composite powder, characterized in that: The steps include: Step 1: uniformly mixing titanium alloy powder and reinforcement powder to obtain a mixture; Step 2: subjecting the mixture to vacuum reaction hot pressing sintering treatment to obtain a sintered body; Step 3: heating and rotating the sintered body to rotate the heated and melted sintered body to obtain molten droplets, cooling the molten droplets to obtain the nano-TiB reinforced titanium-based composite powder, wherein the reinforcement powder is TiB2 powder or boron powder, the particle size of the TiB2 powder is 3-5 μm, and the particle size of the boron powder is 0.5-1 μm; In step 3, the heating temperature of the heating and rotating treatment is 2800-3400° C., and the rotating speed is 20000-30000 r / min; In step three, the process includes: fixing the sintered body on a rotary clamp of a plasma rotating electrode atomizing powder making device, wherein the rotary clamp is used to rotate the sintered body; The current of the plasma rotating electrode atomizing powder making equipment is adjusted to 600-800A, and the feeding speed of the sintered body is set to 1.5-3mm / s, so that the heated and molten sintered body can be rotated out to obtain molten droplets.
2. The preparation method according to claim 1, characterized in that: In step one, the titanium alloy powder is TC4 titanium alloy powder or TA15 titanium alloy powder.
3. The preparation method according to claim 2, characterized in that: The particle size of the titanium alloy powder is 100-200 μm.
4. The preparation method according to claim 1, characterized in that: In step one, include: The titanium alloy powder and the reinforcement powder are ball-milled in an argon environment for 4-8 hours, the rotation speed of the ball-milling is 200-250 r / min, and the ball-to-material ratio is (3-5):
1.
5. The preparation method according to claim 1, characterized in that: In step 2, the temperature of the vacuum reaction hot pressing sintering treatment is 1150-1300°C, the pressure is 20-30Mpa, and the vacuum degree is less than 5×10 -2 Pa, time is 0.5-2h.
6. The preparation method according to claim 1, characterized in that: In step 2, it includes: placing the mixture into a matching mold and performing vacuum reaction hot pressing sintering; The size of the matching mold matches the size of the rotary clamp so that the sintered body can be fixed on the rotary clamp.
7. The preparation method according to claim 6, characterized in that: The matching mold is prepared by graphite.
8. A nano-TiB reinforced titanium-based composite powder, characterized in that: Prepared according to any one of the preparation methods described in claims 1-7.