Packaging

By uniaxially or biaxially stretching the polyethylene resin layer, combined with the design of the heat sealing layer, the problem of heat welding of the outermost layer of the packaging film during the heat sealing process is solved, and the recyclability and thermal stability of the packaging body are improved. Sealing properties, enhanced mechanical properties and formability.

CN114423610BActive Publication Date: 2024-10-11MITSUI CHEM TOHCELLO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080064876.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-20
Filing Date
2020-09-16
Publication Date
2024-10-11
Estimated Expiration
2040-09-16

AI Technical Summary

Technical Problem

The existing polyethylene resin layer packaging film easily causes thermal welding of the outermost layer during the heat sealing process, affecting the recyclability of the packaging body.

Method used

By uniaxially or biaxially stretching the outermost polyethylene resin layer, heat welding is suppressed, and a heat sealing layer is provided in the packaging body to ensure the heat sealability and recyclability of the packaging film.

Benefits of technology

It achieves the suppression of thermal welding of the outermost layer, improves the recyclability and heat sealability of the packaging body, reduces the complexity of raw material separation, and enhances the mechanical properties and formability of the packaging film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114423610B_ABST
    Figure CN114423610B_ABST
Patent Text Reader

Abstract

The packaging body is a packaging body (10) composed of a packaging film, the outermost layer of which is a polyethylene resin layer, and the polyethylene resin layer is uniaxially or biaxially stretched.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to packaging. Background Art

[0002] For example, packaging bags represented by bags used as packaging materials for food, toiletries, pharmaceuticals, automotive products such as vehicle oil, cleaning fluid, cooling water, industrial lubricants, oil, water and other thermal media are composed of packaging materials including a heat seal layer and a base layer.

[0003] As a technology regarding a packaging bag including a heat seal layer and a substrate layer, for example, the technology described in Patent Document 1 (Japanese Patent Application Laid-Open No. 2018-154133) can be cited.

[0004] Patent Document 1 describes a packaging bag using a laminated film comprising: a single-layer film formed of a polyethylene resin composition or a multi-layered sealing film including at least one layer formed of the polyethylene resin composition; and a base film.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-154133 Summary of the invention

[0008] Problems to be solved by the invention

[0009] As environmental awareness has increased in recent years, packaging films have been required to be easily recyclable.

[0010] From the viewpoint of making the packaging film easy to recycle, for example, it is conceivable to make the packaging film from a single raw material (single material) as much as possible.

[0011] The inventors of the present application have found out from the research that from the viewpoint of achieving single material, a packaging body formed of a packaging film having a polyethylene-based resin layer as a base layer has the following problems.

[0012] First, if Figure 2 and Figure 3 As shown in FIG. 1 , when a packaging body 1 is produced using a packaging film having a polyethylene resin layer 4 as a base layer, there is a step of heat-melting the heat-sealing layers 2. At this time, for example, at the bottom 3 of the packaging body 1, the polyethylene resin layers 4 as the outermost layers are in contact with each other. Moreover, according to the research of the inventors of the present application, it is known that in the step of heat-melting the heat-sealing layers 2, the polyethylene resin layers 4 as the outermost layers are heat-melted with each other. In addition, it is also known that the polyethylene resin layer is melted to the heat-sealing rod heated for heat sealing.

[0013] Thus, the inventors of the present application have found that a packaging body having a polyethylene resin layer as its outermost layer may cause heat fusion of the outermost layer during its production process.

[0014] The present invention has been made in view of the above circumstances, and provides a packaging body in which heat fusion of the outermost layer is suppressed.

[0015] Means for solving problems

[0016] The inventors of the present application have repeatedly conducted in-depth research to achieve the above-mentioned problem. As a result, they have found that in a packaging body whose outermost layer is a polyethylene resin layer, by uniaxially or biaxially stretching the polyethylene resin layer, a packaging body in which heat fusion of the outermost layer is suppressed can be achieved, thereby completing the present invention.

[0017] That is, according to the present invention, there is provided the following packaging body.

[0018] [1] a packaging body, which is a packaging body composed of a packaging film,

[0019] The outermost layer is a polyethylene resin layer.

[0020] The polyethylene resin layer is stretched uniaxially or biaxially.

[0021] [2] The packaging body according to [1] above, wherein

[0022] The melting point of the polyethylene resin layer constituting the polyethylene resin layer is 100° C. or higher and 150° C. or lower.

[0023] [3] The packaging body according to [1] or [2] above, wherein:

[0024] The innermost layer of the packaging body is provided with a heat seal layer.

[0025] [4] The packaging body according to any one of [1] to [3] above, wherein

[0026] The heat seal layer contains a polyethylene resin.

[0027] [5] The packaging body according to [4] above, wherein

[0028] The polyethylene resin constituting the heat seal layer has a melting point of 90° C. or higher and 140° C. or lower.

[0029] [6] The packaging body according to [5] above, wherein

[0030] When the entire packaging body is defined as 100% by mass, 90% by mass or more of the packaging body is the polyethylene-based resin.

[0031] Effects of the Invention

[0032] According to the present invention, it is possible to provide a packaging body in which heat fusion of the outermost layer is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a perspective view schematically showing an example of the structure of a package according to an embodiment of the present invention.

[0034] Figure 2 This is a front view schematically showing an example of the structure of a conventional package.

[0035] Figure 3 yes Figure 2 XX' cross-sectional view of the packaging body shown. DETAILED DESCRIPTION

[0036] Hereinafter, the embodiments of the present invention will be described using the accompanying drawings. It should be noted that the drawings are schematic diagrams and do not correspond to actual dimensional ratios. In addition, unless otherwise specified, "A to B" in a numerical range means greater than A and less than B.

[0037] <Packaging>

[0038] Figure 1 It is a perspective view schematically showing an example of the structure of the package 10 according to the embodiment of the present invention.

[0039] The packaging body 10 of the present embodiment is a packaging body composed of a packaging film, and the outermost layer is a polyethylene resin layer, and the polyethylene resin layer is uniaxially or biaxially stretched.

[0040] Thus, in a package whose outermost layer is a uniaxially or biaxially stretched polyethylene resin layer, in the process of heat-sealing the heat-sealing layers, the heat-sealing of the polyethylene resin layers as the outermost layers can be suppressed. In addition, in the heat-sealing process, the polyethylene resin layer as the outermost layer can be suppressed from being fused to the heat-sealing rod.

[0041] In this embodiment, the packaging body is a packaging bag itself or a material containing articles in the bag, for example, for storing articles such as food, medicines, health products, daily necessities, industrial products, automotive products such as vehicle oil, cleaning fluid, cooling water, industrial lubricants, oil, water and other heat media. In addition, the packaging form of the packaging body of this embodiment can include, for example, a three-side sealed bag or a four-side sealed bag having a heat-sealed portion formed by heat welding on all or part of the periphery, a pillow bag, a palm bag, a rod bag, a gusset bag (gazette bag), a bag body, etc. In addition, in addition to the articles, a deoxidizer, etc., can be added to the inside of the packaging body.

[0042] The package 10 of the present embodiment usually has a heat seal layer in the innermost layer of the package (the outermost layer on the inner side of the package). Therefore, the package 10 of the present embodiment can be produced by heat-sealing the heat seal layers of the packaging film.

[0043] For the packaging body 10 of the present embodiment, from the viewpoint of improving recyclability, when the entire packaging body is set to 100 mass %, it is preferred that more than 90 mass % of the packaging body is polyethylene resin, more preferably more than 95 mass % of the packaging body is polyethylene resin, further preferably more than 98 mass % of the packaging body is polyethylene resin, and further preferably more than 99 mass % of the packaging body is polyethylene resin.

[0044] Thus, since the package body 10 is substantially composed of a single raw material (single material), the work of separating the raw materials constituting the package body 10 is reduced, and the recyclability of the package body 10 can be improved.

[0045] <Packaging film>

[0046] As the packaging film of this embodiment, for example, a film including a polyethylene resin layer containing a polyethylene resin and a heat seal layer provided on at least one surface of the polyethylene resin layer can be used. Here, the polyethylene resin layer may be one layer or two or more layers.

[0047] The thickness of the packaging film of this embodiment can be arbitrarily set according to the desired purpose such as water vapor barrier property, cost, mechanical strength, transparency, recyclability, appearance, formability, lightness, etc., and is not particularly limited. The thickness is usually 10 μm to 220 μm, preferably 15 μm to 190 μm, and more preferably 20 μm to 175 μm.

[0048] When the thickness of the packaging film of the present embodiment is within the above range, the packaging film has a better balance among mechanical properties, handling properties, appearance, moldability, lightness, and the like.

[0049] Hereinafter, each layer constituting the packaging film of the present embodiment will be described.

[0050] [Polyethylene resin layer]

[0051] The polyethylene resin layer (also referred to as a base material layer) of the present embodiment is formed by, for example, uniaxially stretching or biaxially stretching a film composed of a resin composition containing a polyethylene resin.

[0052] The thickness of the polyethylene resin layer of the present embodiment can be arbitrarily set according to the desired purpose such as water vapor barrier, cost, mechanical strength, transparency, recyclability, appearance, formability, lightness, etc., and is therefore not particularly limited. It is usually between 0.5 μm and 100 μm, preferably between 1.0 μm and 75 μm, and more preferably between 1.5 μm and 50 μm.

[0053] When the thickness of the polyethylene resin layer is within the above range, mechanical properties, handling properties, appearance, moldability, lightness, and the like are more well-balanced.

[0054] The polyethylene resin layer of the present embodiment only needs to include at least a uniaxially or biaxially stretched outermost layer, and may be a single layer consisting of only the outermost layer, or may be a laminated structure of a plurality of layers consisting of a resin composition containing a polyethylene resin.

[0055] In the case of a structure in which a plurality of layers composed of a resin composition containing a polyethylene resin are stacked, as layers other than the layer located on the outer surface of the packaging body (also referred to as the outermost layer), for example, a core layer, a laminating layer, etc. can be cited. From the viewpoint of the formability of the film and the web handling during winding, it is preferred to provide a core layer and a laminating layer. The core layer is a layer located between the outermost layer and the laminating layer in the polyethylene resin layer, and the laminating layer is a layer located on the surface opposite to the outermost layer in the polyethylene resin layer. The polyethylene resin layer may consist of only the outermost layer and the laminating layer. In addition, in the polyethylene resin layer, at least the outermost layer is subjected to uniaxial stretching or biaxial stretching, and the core layer and the laminating layer may or may not be subjected to stretching treatment.

[0056] The thickness of the outermost layer is, for example, 0.05 μm to 10 μm, specifically, 1.0 μm to 6 μm. The thickness of the core layer is, for example, 0.4 μm to 49.9 μm, specifically, 1 μm to 48 μm. The thickness of the laminate layer is, for example, 0.05 μm to 10 μm, specifically, 1.0 μm to 6 μm.

[0057] Furthermore, as a method for stacking multiple layers composed of a resin composition containing a polyethylene resin, for example: a dry lamination method; an extrusion lamination method; a heat welding method such as a method of extruding a resin and laminating the extruded resin on a surface layer; a method of using a dry lamination method, an extrusion lamination method, and a heat welding method in combination, etc.

[0058] (Polyethylene resin composition)

[0059] The polyethylene resin composition of the present embodiment contains a polyethylene resin.

[0060] When the entire polyethylene resin composition is set to 100 mass%, the content of the polyethylene resin contained in the polyethylene resin composition (i.e., polyethylene resin layer) of the present embodiment is preferably 90 mass% to 100 mass%, more preferably 95 mass% to 100 mass%, further preferably 98 mass% to 100 mass%, and particularly preferably 99 mass% to 100 mass%. Thus, the balance of water vapor barrier properties, cost, mechanical strength, transparency, recyclability, appearance, moldability, lightness, etc. can be improved.

[0061] (Polyethylene resin)

[0062] As the polyethylene resin constituting the polyethylene resin layer of the present embodiment, there can be listed one or more polyethylene resins such as high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear polyethylene, ultra-high molecular weight polyethylene, etc. Among them, one or more of high-density polyethylene, medium-density polyethylene, low-density polyethylene and linear polyethylene are preferred, and linear polyethylene monomers, or linear polyethylene containing 20% ​​by mass or more and containing at least one of high-density polyethylene, medium-density polyethylene, and low-density polyethylene are further preferred.

[0063] From the viewpoint of suppressing whitening and improving the transparency of the package, it is preferred to combine two or more polyethylene resins. Whitening is caused by the crystallization of polyethylene. By using two or more polyethylene resins in combination, the polyethylene resin layer is easily amorphous, so crystallization can sometimes be suppressed to suppress whitening. As a viewpoint of combining two or more polyethylene resins, MFR, density, melting point, etc. can be listed. Specifically, when combining two or more polyethylene resins, it is preferred to meet at least any one of the following (i) to (iii) (the method for measuring MFR and density will be described later).

[0064] (i) Two polyethylene resins having MFRs different by 0.5 g / 10 min or more are used together. In this case, it is preferred to make the ratio of the two resins equal in terms of mass ratio, or to increase the ratio of the one with a smaller MFR.

[0065] (ii) The combined density difference is 10 kg / m 3 At this time, it is preferred to make the ratio of the two resins the same in terms of mass ratio, or to increase the amount of the one with a smaller density.

[0066] (iii) Combining polyethylene resins having melting points different by 1° C. or more. In this case, it is preferred to make the ratio of the two resins the same by mass ratio, or to increase the amount of the one with the lower melting point.

[0067] When the polyethylene resin layer is a multilayer structure as described above (for example, a three-layer structure of an outermost layer, a core layer, and a laminating layer), only one layer may contain two or more polyethylene resins, or two or more layers may each contain two or more polyester resins. Of course, each layer in the polyethylene resin layer may also be composed of only one polyethylene resin.

[0068] From the viewpoint of achieving a better balance among heat resistance, transparency, mechanical properties, rigidity, fluidity and formability, the melting point of the polyethylene resin is preferably above 100°C, more preferably above 120°C, further preferably above 125°C, and preferably below 150°C, more preferably below 140°C, further preferably below 135°C.

[0069] When the melting point of the polyethylene resin is above the lower limit, thermal fusion of the polyethylene resin layers as the outermost layers in the package 10 can be further suppressed. When the melting point of the polyethylene resin is below the upper limit, interlayer strength, fluidity and moldability can be improved.

[0070] From the viewpoint of achieving a better balance among heat resistance, transparency, mechanical properties, rigidity, fluidity, and moldability, the density of the polyethylene resin is preferably 920 kg / m 3 More preferably 923 kg / m 3 More preferably, 925 kg / m 3 Above, and preferably 970kg / m 3 Below, more preferably 965kg / m 3 Below, more preferably 960kg / m 3 Below, particularly preferably 950kg / m 3 Here, in the present embodiment, the density of the polyethylene-based resin can be measured in accordance with JIS K 7112 (1999).

[0071] When the density of the polyethylene resin is greater than or equal to the lower limit, thermal fusion of the polyethylene resin layers as the outermost layers in the package 10 can be further suppressed. When the density of the polyethylene resin is less than or equal to the upper limit, interlayer strength, fluidity, and moldability can be improved.

[0072] The melt flow rate (MFR) of the polyethylene resin measured at 190°C and a load of 2.16 kg in accordance with ASTM D1238 is preferably 0.5 g / 10 min or more, more preferably 1 g / 10 min or more, and further preferably 2 g / 10 min or more from the viewpoint of fluidity and moldability, and is preferably 30 g / 10 min or less, more preferably 20 g / 10 min or less, and further preferably 10 g / 10 min or less from the viewpoint of further stabilizing the moldability.

[0073] The method for producing the polyethylene resin is not particularly limited, and the polyethylene resin can be produced by a known method. In addition, commercially available polyethylene can be used as the polyethylene.

[0074] (Other ingredients)

[0075] Within the scope that does not impair the purpose of the present embodiment, various additives such as tackifiers, heat stabilizers, weather stabilizers, antioxidants, ultraviolet absorbers, lubricants, slip agents, nucleating agents, anti-blocking agents, antistatic agents, anti-fogging agents, pigments, dyes, inorganic or organic fillers, etc. can be added to the polyethylene resin composition of the present embodiment as needed.

[0076] (Method for preparing polyethylene resin composition)

[0077] The polyethylene resin composition of the present embodiment can be prepared by mixing or melt-kneading the components using methods / apparatus such as dry blending, tumble mixer, Banbury mixer, single-screw extruder, twin-screw extruder, high-speed twin-screw extruder, and hot roll.

[0078] [Heat seal layer]

[0079] In order to impart heat sealability to the packaging film of this embodiment, it is preferred that a heat seal layer be provided on at least a portion of one surface of the polyethylene resin layer. The heat seal layer may be provided only at the intended heat-sealable portion of the packaging film of this embodiment, or may be provided on the entire surface of the polyethylene resin layer.

[0080] In the packaging film of this embodiment, the thickness of the heat seal layer is preferably 0.1 μm to 200 μm, more preferably 0.2 μm to 170 μm, further preferably 0.5 μm to 150 μm, particularly preferably 1 μm to 120 μm.

[0081] When the thickness of the heat seal layer is equal to or greater than the above lower limit, the heat sealability of the packaging film can be improved.

[0082] In addition, by making the thickness of the heat seal layer below the upper limit, the fusion of the outermost layer during heat sealing can be particularly suppressed. Generally, the thicker the heat seal layer, the higher the temperature required for sealing.

[0083] In the packaging film of the present embodiment, the heat seal layer provided on one surface is preferably a single layer. This can simplify the manufacturing process of the packaging film, that is, the manufacturing process of the packaging body 10 of the present embodiment.

[0084] In addition, the heat seal layer can be formed by stretching the film in the state before the polyethylene resin layer is stretched. Thus, the packaging film can be made using a laminated film made by a molding method such as coextrusion molding, i.e., one-step molding. Therefore, the manufacturing process of the packaging film, i.e., the manufacturing process of the package body 10 of the present embodiment, can be simplified. Therefore, the heat seal layer can be stretched uniaxially or biaxially.

[0085] (Polyolefin)

[0086] The heat seal layer of the present embodiment is composed of, for example, a polyolefin resin composition containing polyolefin. Examples of the polyolefin constituting the heat seal layer include homopolymers or copolymers of α-olefins such as ethylene, propylene, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene; polyethylene resins such as high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear polyethylene, and ultra-high molecular weight polyethylene; polypropylene; propylene·α-olefin random copolymer; ethylene·vinyl acetate copolymer (EVA); ionomer resins, etc.

[0087] Among them, as the polyolefin constituting the heat seal layer, polyethylene resin is preferred from the viewpoint of improving recyclability and making the balance of adhesion and heat sealability with the polyethylene resin layer excellent. Thus, since the package body is generally composed of a single raw material (single material), it is easy to separate the raw materials constituting the package body 10, and the recyclability of the package body 10 can be improved.

[0088] (Polyethylene resin)

[0089] As the polyethylene resin constituting the heat seal layer of the present embodiment, for example, high density polyethylene, medium density polyethylene, low density polyethylene, linear low density polyethylene, ultra high molecular weight polyethylene, etc. can be cited. Among them, low density polyethylene and linear low density polyethylene are preferred, and linear low density polyethylene is more preferred. One polyethylene can be used, or two or more can be used in combination.

[0090] The melting point of the polyethylene resin is preferably 90° C. or higher, more preferably 95° C. or higher, and is preferably 140° C. or lower, more preferably 120° C. or lower.

[0091] When the melting point of the polyethylene resin is not less than the above lower limit, stickiness of the surface of the heat seal layer can be suppressed, and the blocking resistance of the packaging film can be improved.

[0092] Moreover, when the melting point of the polyethylene resin is below the above upper limit, the heat-sealing property of the packaging film can be further improved.

[0093] The melt flow rate (MFR) of the polyethylene resin measured at 190°C and a load of 2.16 kg in accordance with ASTM D1238 is preferably 0.5 g / 10 min or more, more preferably 1 g / 10 min or more, and further preferably 2 g / 10 min or more from the viewpoint of fluidity and moldability, and is preferably 30 g / 10 min or less, more preferably 20 g / 10 min or less, and further preferably 10 g / 10 min or less from the viewpoint of further stabilizing the moldability.

[0094] The method for producing the polyethylene resin is not particularly limited, and the polyethylene resin can be produced by a known method. In addition, commercially available polyethylene can be used as the polyethylene.

[0095] When the entire polyolefin resin composition is set to 100% by mass, the content of the polyolefin resin in the polyolefin resin composition of the present embodiment (i.e., in the heat seal layer) is preferably 90% by mass or more and 100% by mass or less, more preferably 95% by mass or more and 100% by mass or less, further preferably 98% by mass or more and 100% by mass or less, and particularly preferably 99% by mass or more and 100% by mass or less. Thus, the balance of recyclability, adhesion to the polyethylene resin layer, heat sealability, etc. can be made better.

[0096] (Other ingredients)

[0097] In the polyolefin resin composition constituting the heat seal layer of the present embodiment, various additives such as heat stabilizers, weather stabilizers, antioxidants, ultraviolet absorbers, lubricants, slip agents, nucleating agents, antiblocking agents, antistatic agents, antifogging agents, pigments, dyes, inorganic or organic fillers can be added as needed within the scope of not damaging the purpose of the present embodiment.

[0098] On the other hand, from the viewpoint of single material, the polyolefin-based resin composition preferably does not substantially contain these various additives.

[0099] (Method for preparing polyolefin resin composition)

[0100] The polyolefin resin composition of the present embodiment can be prepared by mixing or melt-kneading the components using dry blending, a tumble mixer, a Banbury mixer, a single-screw extruder, a twin-screw extruder, a high-speed twin-screw extruder, a heat roll, or the like.

[0101] <Method for producing packaging film>

[0102] The packaging film of the present embodiment can be obtained, for example, by uniaxially or biaxially stretching a laminated film obtained by co-extruding the polyethylene resin composition for forming the polyethylene resin layer and the polyolefin resin composition for forming the heat seal layer into a film shape using a known stretch film production method.

[0103] As forming device and forming condition, there is no particular limitation, and known forming device and forming condition can be used. As forming device, multilayer T-die extruder or multilayer inflation molding machine etc. can be used. The conditions of biaxial stretching can, for example, adopt the manufacturing conditions of known stretched film.

[0104] The conditions for producing the stretched film are not particularly limited, and examples thereof include the following conditions.

[0105] Extrusion setting temperature: 190-250℃, processing speed: 20-60m / min

[0106] Longitudinal stretching temperature: 100-130℃

[0107] Longitudinal stretching ratio: 3.5-7.5 times

[0108] Transverse stretching temperature: 100-150℃

[0109] Transverse stretching ratio: 4-12 times

[0110] The packaging film of the present embodiment can also be obtained by dry lamination in which a polyethylene resin layer and a heat seal layer which are uniaxially stretched or biaxially stretched only or contain the outermost layer are separately formed and then laminated with an adhesive etc. Furthermore, the packaging film of the present embodiment can also be obtained by extruding a resin of a heat seal layer on a uniaxially stretched or biaxially stretched polyethylene resin layer and molding by lamination molding etc.

[0111] As mentioned above, although embodiment of this invention was described with reference to drawings, these are illustrations of this invention, and various structures other than the above-mentioned can also be adopted.

[0112] Example

[0113] Hereinafter, the present embodiment will be described in detail with reference to Examples and Comparative Examples. It should be noted that the present embodiment is not limited at all by the description of these Examples.

[0114] 1. Raw materials

[0115] The raw materials used in Examples and Comparative Examples are as follows.

[0116] (1) Polyethylene resin

[0117] PE1: Polyethylene (MFR: 0.8g / 10min, density: 926kg / m 3 , melting point: 124°C)

[0118] PE2: Polyethylene (MFR: 2.8g / 10min, density: 942kg / m 3 , melting point: 129°C)

[0119] PE3: Polyethylene (MFR: 1.8g / 10min, density: 927kg / m 3 , melting point: 127°C)

[0120] PE4: Polyethylene (MFR: 3.8g / 10min, density: 918kg / m 3 , melting point: 116°C)

[0121] PE5: Polyethylene (MFR: 1.1g / 10min, density: 950kg / m 3 , melting point: 132°C)

[0122] 2. Measurement and evaluation methods

[0123] (1) MFR of polyethylene resin

[0124] The measurement was performed in accordance with ASTM D1238 at 190°C and a load of 2.16 kg.

[0125] (2) Melting point of polyethylene resin

[0126] The temperature of the maximum melting peak of the DSC curve of the polyethylene resin obtained using DSC (differential scanning calorimeter) is defined as the melting point. Specifically, the temperature of the maximum melting peak of the DSC curve of the 2nd run when the following 1st run and 2nd run are performed is defined as the melting point.

[0127] 1st run: Heat up to 200℃ at 10℃ / min, hold for 10 minutes, cool down to -50℃ at 10℃ / min

[0128] 2nd run: After the 1st run, the temperature is raised to 200℃ at 10℃ / min.

[0129] (3) Density of polyethylene resin

[0130] The density of the polyethylene resin was measured in accordance with JIS K 7112 (1999).

[0131] (4) Evaluation of thermal weldability

[0132] The outermost layers of two packaging films cut into 15 mm width were heat-sealed at 130°C, 2.0 kgf pressure, and 1 second sealing time to obtain a laminated film. Next, the two packaging films were peeled off at 15 mm width, 180 degrees, and a peeling speed of 300 mm / min, and the peel strength at this time was taken as the heat seal strength.

[0133] Next, the thermal fusion properties of the packaging films were evaluated based on the following criteria.

[0134] ◎(Very good): Heat seal strength is less than 2.0N / 15mm

[0135] ○ (good): heat seal strength is 2.0 N / 15 mm or more and less than 5.0 N / 15 mm

[0136] △ (poor): heat seal strength is 5.0N / 15mm or more and less than 10.0N / 15mm

[0137] × (very poor): heat seal strength is 10.0N / 15mm or more

[0138] (5) Presence of whitening (transparency)

[0139] The packaging film was visually observed and judged according to the following criteria.

[0140] 〇 (Good): Sufficiently transparent, and as a packaging film, there is no problem with the visibility of the packaged product

[0141] × (poor): The film is matte and has a problem in visibility of the packaged product as a packaging film.

[0142] [Examples 1 to 13]

[0143] Each layer was co-extruded and then stretched to produce packaging films. The thermal fusion properties were evaluated. The molding machine used was as shown below.

[0144] Multilayer extruder: 260 mm wide multilayer T-die extruder (L / D = 27, manufactured by Screw Seiki Co., Ltd.)

[0145] In addition, the stretching ratio is as follows.

[0146] Examples 1, 2, and 4: Biaxial stretching 4.0 to 7.5 times in the longitudinal direction and 7.5 to 14 times in the transverse direction

[0147] Example 3: Uniaxial stretching at 8 to 14 times in the transverse direction

[0148] [Comparative Example 1]

[0149] The layers were co-extruded to form a packaging film according to the layer structure shown in Table 1 (no stretching treatment was performed in Comparative Example 1). Then, the heat-welding property was evaluated. The molding machine used is shown below.

[0150] Multilayer extrusion molding machine: Multilayer T-die extrusion molding machine (L / D=30)

[0151] [Table 1]

[0152]

[0153] This application claims the benefit of priority based on Japanese patent application No. 2019-171374, filed on September 20, 2019, the disclosure of which is incorporated herein in its entirety.

[0154] Description of Reference Numerals

[0155] 1. Packaging

[0156] 2 Heat seal layer

[0157] 3 Bottom

[0158] 4 Polyethylene resin layer

[0159] 10 Packaging

Claims

1. A packaging body, which is a packaging body composed of a packaging film, The outermost layer is a polyethylene resin layer. The polyethylene resin layer is biaxially stretched. The packaging body is a packaging bag, The polyethylene resin constituting the polyethylene resin layer includes two or more polyethylene resins. The two or more polyethylene resins satisfy at least one of the following (i) to (iii): (i) using two polyethylene resins having MFRs that differ by 0.5 g / 10 min or more, in which case the ratio of the two resins is made equal in terms of mass ratio, or the one with a smaller MFR is increased; (ii) The combined density difference is 10 kg / m 3 The above polyethylene resins, in this case, make the ratio of the two resins the same by mass ratio, or increase the one with a smaller density; (iii) Combining polyethylene resins having melting points different by 1°C or more, in which case the ratio of the two resins is made equal in terms of mass ratio, or the one with the lower melting point is increased.

2. The packaging body according to claim 1, wherein: The polyethylene resin constituting the polyethylene resin layer has a melting point of 100° C. or higher and 150° C. or lower.

3. The packaging body according to claim 1 or 2, wherein: The innermost layer of the packaging body is provided with a heat-sealing layer.

4. The packaging body according to claim 3, wherein: The heat seal layer includes a polyethylene-based resin.

5. The packaging body according to claim 4, wherein: The polyethylene resin constituting the heat seal layer has a melting point of 90° C. or higher and 140° C. or lower.

6. The packaging body according to claim 5, wherein: When the entire packaging body is defined as 100% by mass, 90% by mass or more of the packaging body is the polyethylene-based resin.