Radio frequency heat dissipation plastic, preparation method thereof and repeater box using same
By using a polymer matrix, a silicon-based compound inorganic coating and a second filler in radio frequency heat dissipation plastics, the problem of performance degradation of existing materials in high-frequency signal transmission is solved, and the uniformity and efficient transmission characteristics of radio frequency heat dissipation plastics are achieved .
Patent Information
- Application Number
- CN202080066253.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-23
- Filing Date
- 2020-09-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-09-16
AI Technical Summary
While existing materials can achieve high-frequency transmission characteristics, low dielectric constant, mechanical strength and heat dissipation performance, they cannot express these characteristics uniformly across the entire area, resulting in performance degradation or loss of functionality of the repeater box in high-frequency signal transmission.
A radio frequency heat dissipation plastic containing a polymer matrix and a high-strength filler is used. A silicon-based compound inorganic coating is formed on the surface of the high-strength filler, and a second filler is dispersed in the polymer resin to improve the heat dissipation characteristics. The formed radio frequency heat dissipation plastic is used for Repeater box.
It achieves uniform expression of low dielectric constant, mechanical strength and heat dissipation performance over the entire area, minimizing performance degradation or loss of functions during high-frequency signal transmission, and is suitable for various items.
Smart Images

Figure CN114423816B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a radio frequency (RF) heat dissipation plastic, and more particularly to a radio frequency heat dissipation plastic, a preparation method thereof and a repeater box using the same. Background Art
[0002] A repeater for mobile communications is a device that receives a weakened signal in the middle of a communication system, amplifies it, and retransmits it, or shapes the waveform of a distorted signal and adjusts or reconfigures the transmission timing. This type of repeater was originally just for retransmitting signals, but recently, considering the service coverage, it can save equipment and operating costs, thus playing the role of a low-cost base station.
[0003] On the other hand, the signals sent and received by mobile communication repeaters are radio waves. 5G, which is about to be commercialized in recent years and whose network is being built, uses high-frequency bands of 3.5 GHz and 28 GHz. As a significantly higher high-frequency band is used than 4G, due to the communication characteristics of low diffraction characteristics (strong linearity) and short radio wave reach distance compared to 4G, more base stations or repeaters need to be installed than 4G.
[0004] However, since electrical signals have the characteristic that transmission loss increases as frequency increases, the development of materials with excellent high-frequency transmission characteristics is an essential element.
[0005] In the case of conventional materials with high-frequency transmission characteristics, it is not possible to simultaneously achieve the required levels of low dielectric constant and high mechanical strength, and there are technical limitations in expressing excellent heat dissipation performance, and these characteristics cannot be uniformly expressed over the entire area. Therefore, there is an urgent need to develop a material with high-frequency transmission characteristics that can minimize or prevent signal interference in the high-frequency band due to its low dielectric constant, exhibit excellent mechanical strength and excellent heat dissipation characteristics, and uniformly express low dielectric characteristics, mechanical strength, and heat dissipation characteristics over the entire area. Summary of the invention
[0006] Technical issues
[0007] The present invention is proposed in view of the above problems, and an object of the present invention is to provide a radio frequency heat dissipation plastic that can exhibit both low dielectric constant and excellent mechanical strength effects.
[0008] Furthermore, another object of the present invention is to provide a radio frequency heat dissipation plastic that exhibits excellent heat dissipation performance even though it is designed to have a low dielectric constant and excellent mechanical strength, and a repeater implemented using the same.
[0009] Furthermore, another object of the present invention is to provide a radio frequency heat dissipation plastic that uniformly exhibits low dielectric properties, excellent mechanical strength, and excellent heat dissipation properties over the entire area, and a repeater implemented using the same.
[0010] Furthermore, another object of the present invention is to provide a radio frequency heat dissipation plastic that can minimize the performance degradation or function loss of a repeater box that may be affected in receiving and transmitting high-frequency band signals according to the dielectric constant, and various articles in the entire industry including repeaters implemented therewith.
[0011] Means of solving the problem
[0012] In order to solve the above problems, the present invention provides a radio frequency heat dissipation plastic, which includes: a polymer matrix, which includes a polymer resin; and a first filler, which is dispersed in the above polymer matrix and includes a high-strength filler and an inorganic coating. The above high-strength filler is a polymer containing at least one hydroxyl group in a repeating unit, and the above inorganic coating is formed on at least a portion of the surface of the above high-strength filler.
[0013] According to an embodiment of the present invention, the high-strength filler may include at least one selected from the group consisting of cellulose nanofibrils and cellulose fibers.
[0014] Furthermore, the average cross-sectional diameter of the high-strength filler may be 10 nm to 20 μm, and the average thickness of the inorganic coating may be 5 nm to 30 nm.
[0015] Furthermore, the inorganic coating may be an inorganic coating in which a silicon-based compound is combined with the high-strength filler, wherein the silicon-based compound comprises one or more selected from the group consisting of an orthosilicic acid group, a linear silicic acid group formed by polymerization of two or more orthosilicic acid groups, a branched silicic acid group formed by polymerization of four or more orthosilicic acid groups, and a cyclic silicic acid group formed by polymerization of three or more orthosilicic acid groups.
[0016] Furthermore, in the first filler, at least one hydroxyl group of the silicon-based compound may be chemically bonded to a hydroxyl group of the high-strength filler.
[0017] Furthermore, the first filler may include 50 to 250 parts by weight of the inorganic coating layer relative to 100 parts by weight of the high-strength filler.
[0018] Furthermore, the first filler may be contained in an amount of 1 to 15 parts by weight based on 100 parts by weight of the polymer resin.
[0019] Furthermore, the polymer resin may include one compound selected from the group consisting of polycarbonate, polyamide, polyester, polyketone, liquid crystal polymer, polyolefin, polyphenylene sulfide (PPS), polyetheretherketone (PEEK), polyphenylene ether (PPO), polyethersulfone (PES), polyetherimide (PEI), polyimide (PI), polyphthalamide (PPA), polybutylene terephthalate (PBT), acrylonitrile butadiene styrene copolymer resin (ABS), polymethyl methacrylate (PMMA) and polyarylate (PAR), or a mixture or copolymer of two or more thereof.
[0020] Furthermore, the radio frequency heat dissipation plastic may further include a second filler dispersed in the polymer matrix to improve heat dissipation properties.
[0021] Furthermore, the average particle size of the second filler may be 5 μm to 300 μm.
[0022] Furthermore, the second filler may include one or more selected from a group consisting of non-insulating fillers and insulating fillers, the non-insulating filler including one or more selected from a group consisting of: one or more carbon-based fillers selected from a group consisting of carbon black, graphite and carbon nanomaterials; one or more metal-based fillers selected from a group consisting of copper, silver, nickel, gold, platinum and iron; and a non-insulating graphite composite, the insulating filler including one or more selected from a group consisting of magnesium oxide, yttrium oxide, zirconium oxide, titanium dioxide, aluminum nitride, silicon nitride, boron nitride, aluminum oxide, silicon dioxide, zinc oxide, barium titanate, strontium titanate, beryllium oxide, manganese oxide, talc, silicon carbide, silicon dioxide, single crystal silicon and insulating graphite composite.
[0023] Furthermore, 30 to 200 parts by weight of the second filler may be contained based on 100 parts by weight of the polymer resin.
[0024] Furthermore, the present invention provides a method for preparing a radio frequency heat dissipation plastic, which is characterized in that it comprises: step (1), preparing a first filler by treating at least a portion of the surface of a high-strength filler containing at least one hydroxyl group in a repeating unit with an inorganic coating precursor; and step (2), dispersing the first filler in a polymer resin.
[0025] According to an embodiment of the present invention, the inorganic coating precursor may include tetrahydroxysilane (TEOS).
[0026] Furthermore, in the above step (1), the high-strength filler and the inorganic coating precursor may be treated in a weight ratio of 1:10 to 50.
[0027] Furthermore, the above step (1) may include: step (1)-1, reacting the high-strength filler with the inorganic coating precursor for 3 hours to 13 hours; and step (1)-2, aging the reacted high-strength filler for 0.3 hours to 3 hours.
[0028] Furthermore, the present invention provides a repeater box body having a receiving portion, wherein a device for relaying radio frequency signals is received inside the receiving portion, and at least a portion of the box body is the radio frequency heat dissipation plastic.
[0029] Effects of the Invention
[0030] According to the present invention, since the RF heat dissipation plastic contains the first filler, it exhibits both low dielectric constant and excellent mechanical strength effects. Furthermore, even though it is designed to have a low dielectric constant and excellent mechanical strength, since it contains the second filler for improving the heat dissipation characteristics, it exhibits excellent heat dissipation performance. In addition, since the first filler and the second filler have excellent dispersibility, they exhibit uniform low dielectric properties, mechanical strength, and heat dissipation characteristics over the entire area. According to the RF heat dissipation plastic of the present invention that exhibits uniform low dielectric properties, mechanical strength, and heat dissipation characteristics over the entire area, it is possible to minimize the performance degradation or loss of function of a repeater box that may be affected in receiving and transmitting high-frequency band signals depending on the dielectric constant, and therefore can be widely used in various items throughout the industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A cross-sectional view of a radio frequency heat dissipation plastic according to an embodiment of the present invention.
[0032] Figure 2 It is a cross-sectional view of a radio frequency heat dissipation plastic according to another embodiment of the present invention.
[0033] Figure 3 FIG. 4 is a cross-sectional schematic diagram of a first filler according to an embodiment of the present invention.
[0034] Figure 4 This is an electron microscope photograph of the first filler according to one embodiment of the present invention.
[0035] Figure 5 It is an assembly stereogram of a repeater including a repeater box according to an embodiment of the present invention. DETAILED DESCRIPTION
[0036] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement them. The present invention can be implemented in various forms and is not limited to the embodiments described herein. In order to clearly describe the present invention in the accompanying drawings, parts not related to the description are omitted, and the same reference numerals are given to the same or similar structural elements throughout the specification.
[0037] like Figure 1 and Figure 3 As shown, the radio frequency heat dissipation plastic 100 of the present invention includes: a polymer matrix 10, which is made of a polymer resin; and a first filler 20, 20', which is dispersed in the above-mentioned polymer matrix 10, including a high-strength filler 20a and an inorganic coating 20b. The above-mentioned high-strength filler 20a is a polymer containing at least one hydroxyl group in a repeating unit, and the above-mentioned inorganic coating 20b is formed on at least a portion of the surface of the above-mentioned high-strength filler 20a.
[0038] First, the polymer matrix 10 described above will be described.
[0039] The polymer matrix 10 is a carrier for loading the first fillers 20, 20' described later, maintaining the shape of the radio frequency heat dissipation plastic and exhibiting a specified mechanical strength. The polymer resin forming the polymer matrix 10 can use organic compounds commonly used in the technical field without restriction. Preferably, it can be a compound selected from the group consisting of polycarbonate, polyamide, polyester, polyketone, liquid crystal polymer, polyolefin, polyphenylene sulfide (PPS), polyetheretherketone (PEEK), polyphenylene ether (PPO), polyethersulfone (PES), polyetherimide (PEI) and polyimide, or a mixture or copolymer of two or more thereof.
[0040] In this case, the polyamide may be a known polyamide compound, such as nylon 6, nylon 66, nylon 11, nylon 610, nylon 12, nylon 46, nylon 9T (PA-9T), Qiana, and aromatic polyamide.
[0041] As an example, the polyester may be a well-known polyester compound, such as polyethylene terephthalate (PET), trimethylene terephthalate (PTT), polybutylene terephthalate (PBT), polycarbonate, and the like.
[0042] As another example, the polyolefin may be a known polyolefin compound, such as polyethylene, polypropylene, polystyrene, polyisobutylene, ethylene vinyl alcohol, and the like.
[0043] As the liquid crystal polymer, any polymer that exhibits liquid crystallinity in a solution or dissolved state can be used without limitation, and any known type can be used, so the present invention is not particularly limited thereto.
[0044] On the other hand, since the repeater box body described later using the RF heat dissipation plastic should exhibit specified low dielectric properties and excellent mechanical strength, the RF heat dissipation plastic of an embodiment of the present invention can use the above-mentioned polymer resin as the polymer resin.
[0045] Next, the first fillers 20 and 20' will be described.
[0046] like Figure 3 and Figure 4 As shown, the first filler 20, 20' comprises: a high-strength filler 20a, which is a polymer containing at least one hydroxyl group in a repeating unit; and an inorganic coating 20b formed on at least a portion of the surface of the high-strength filler 20a.
[0047] As the above-mentioned high-strength filler 20a, any high-strength filler commonly used in the present technical field can be used without restriction, but preferably, it can be a cellulose-based filler comprising one or more selected from the group consisting of cellulose nanofibrils and cellulose fibers, and more preferably, it can be cellulose nanofibrils to exhibit the desired level of low dielectric properties and excellent mechanical strength.
[0048] Furthermore, the average cross-sectional diameter of the high-strength filler 20a may be 10 nm to 20 μm, preferably, the average cross-sectional diameter may be 20 nm to 10 μm. If the average cross-sectional diameter of the high-strength filler is less than 10 nm, the required level of mechanical strength cannot be exhibited, and if the average cross-sectional diameter exceeds 20 μm, the dispersibility is reduced, and thus uniform low dielectric properties, mechanical strength, and heat dissipation properties may not be exhibited.
[0049] The inorganic coating 20b improves the dispersibility of the first filler 20, 20', and when the high-strength filler 20a is a cellulose-based filler, it prevents yellowing and exerts a function of exhibiting low dielectric properties. The material that can generally form the inorganic coating in the technical field of the present invention can be used without restriction, but preferably, the inorganic coating is an inorganic coating in which a silicon-based compound is combined with the high-strength filler, and the silicon-based compound includes one or more selected from the group consisting of orthosilicic acid group, linear silicic acid group formed by polymerization of two or more orthosilicic acid groups, branched silicic acid group formed by polymerization of four or more orthosilicic acid groups, and cyclic silicic acid group formed by polymerization of three or more orthosilicic acid groups. This may be more conducive to improving the dispersibility of the first filler and preventing the occurrence of yellowing when the high-strength filler is a cellulose-based filler.
[0050] As an example of the silicon-based compound forming the above-mentioned inorganic coating 20b, the orthosilicic acid forming the above-mentioned orthosilicic acid group can be a compound represented by the following chemical formula 1, the linear silicic acid group formed by the above-mentioned two or more orthosilicic acid groups being polymerized with each other can be a compound represented by the following chemical formula 2, the branched silicic acid group formed by the above-mentioned four or more orthosilicic acid groups being polymerized with each other can be a compound represented by the following chemical formula 3, and the cyclic silicic acid group formed by the above-mentioned three or more orthosilicic acid groups being polymerized with each other can be a compound represented by the following chemical formula 4.
[0051] Chemical formula 1
[0052]
[0053] Chemical formula 2
[0054]
[0055] Chemical formula 3
[0056]
[0057] Chemical formula 4
[0058]
[0059] On the other hand, since the above-mentioned linear silicate groups, branched silicate groups and cyclic silicate groups can be respectively formed by further polymerizing the above-mentioned orthosilicic acid groups with the compounds represented by the above-mentioned Chemical Formulas 2 to 4, the above-mentioned linear silicate groups, branched silicate groups and cyclic silicate groups are not limited to the compounds represented by the above-mentioned Chemical Formulas 2 to 4.
[0060] In this case, since the silicon-based compound of the present invention contains a hydroxyl group like the compounds represented by the above Chemical Formulas 1 to 4, at least one hydroxyl group of the silicon-based compound can be chemically bonded to the hydroxyl group of the above-mentioned high-strength filler 20a. In particular, since a large number of hydroxyl groups are contained like the compounds represented by the above Chemical Formulas 1 to 4, it can be more easily chemically bonded to the hydroxyl group of the above-mentioned high-strength filler 20a, which may be very beneficial for improving the dispersibility of the first filler and preventing the occurrence of yellowing when the above-mentioned high-strength filler is a cellulose-based filler.
[0061] On the other hand, the average thickness of the inorganic coating layer 20b may be 5 nm to 30 nm, preferably, the average thickness may be 10 nm to 20 nm. If the average thickness of the inorganic coating layer is less than 5 nm or exceeds 30 nm, the dispersibility of the first filler cannot be improved to the desired level, and the yellowing of the high-strength filler when the cellulose-based filler is not prevented, and thus the low dielectric property cannot be exhibited.
[0062] Furthermore, the first filler 20, 20' may include 50 to 250 parts by weight, preferably 100 to 200 parts by weight, of the inorganic coating 20b relative to 100 parts by weight of the high-strength filler 20a. If the content of the inorganic coating is less than 50 parts by weight or exceeds 250 parts by weight relative to 100 parts by weight of the high-strength filler, the dispersibility of the first filler cannot be improved to a desired level, and yellowing cannot be prevented when the high-strength filler is a cellulose-based filler, and thus low dielectric properties cannot be exhibited.
[0063] The first filler 20, 20' may be contained in an amount of 1 to 15 parts by weight, preferably 1.5 to 13 parts by weight, relative to 100 parts by weight of the polymer resin. If the content of the first filler is less than 1 part by weight relative to 100 parts by weight of the polymer resin, the dielectric constant may increase and the mechanical strength may decrease. If it exceeds 15 parts by weight, the mechanical strength may decrease.
[0064] On the other hand, the first filler may be Figure 3 The fibrous shape shown may also be a granular shape formed by aggregation of fibrous fillers, and the present invention has no particular limitation on this.
[0065] On the other hand, Figure 2 As shown, the RF heat dissipation plastic 101 of another embodiment of the present invention includes: a polymer matrix 11, which is composed of a polymer resin; and a first filler 21, which is dispersed in the above-mentioned polymer matrix 11, and includes a high-strength filler and an inorganic coating. The above-mentioned high-strength filler is a polymer containing at least one hydroxyl group in a repeating unit, and the above-mentioned inorganic coating is formed on at least a portion of the surface of the above-mentioned high-strength filler. The above-mentioned RF heat dissipation plastic 101 may also include a second filler 22 dispersed in the above-mentioned polymer matrix 11 to improve the heat dissipation characteristics.
[0066] The second filler 22 serves to improve the heat dissipation characteristics of the RF heat dissipation plastic 101, and any filler commonly used in the technical field of the present invention for improving heat dissipation characteristics may be used without restriction. Preferably, the second filler 22 may include at least one selected from the group consisting of non-insulating fillers and insulating fillers, and the non-insulating filler includes at least one selected from the group consisting of: at least one carbon-based filler selected from the group consisting of carbon black, graphite and carbon nanomaterials; at least one metal-based filler selected from the group consisting of copper, silver, nickel, gold, platinum and iron; and a non-insulating graphite composite, and the insulating filler includes at least one selected from the group consisting of magnesium oxide, yttrium oxide, zirconium oxide, titanium dioxide, aluminum nitride, silicon nitride, boron nitride, aluminum oxide, silicon dioxide, zinc oxide, barium titanate, strontium titanate, beryllium oxide, manganese oxide, talc, silicon carbide, silicon dioxide, single crystal silicon and insulating graphite composite.
[0067] Furthermore, the second filler 22 may be in the form of spherical or plate-like particles. However, since the shape of the second filler may be changed according to the purpose, the present invention is not particularly limited thereto.
[0068] On the other hand, the graphite composite may include a graphite composite having graphite, nanoparticles bonded to the surface of the graphite, and a catecholamine layer, and may further include a polymer layer.
[0069] The above-mentioned graphite is a mineral in which the 6-membered rings of carbon atoms are infinitely connected on a plane to form a layer of planar macromolecules and are superimposed. It can be a type known in the art, specifically, it can be a natural graphite or artificial graphite among stamped graphite, highly crystalline graphite and earthy graphite. When the above-mentioned graphite is natural graphite, as an example, it can be expanded graphite obtained by expanding stamped graphite. The above-mentioned artificial graphite can be made by a known method. As an example, after a thermosetting resin such as polyimide is made into a film of less than 25 μm, it is graphitized at a high temperature of more than 2500°C to make graphite in a single crystal state, or hydrocarbons such as methane can be pyrolyzed at high temperature, and highly oriented graphite is prepared by chemical vapor deposition (CVD).
[0070] Furthermore, the graphite may be in a known shape such as spherical, plate-like, needle-like, or in an amorphous shape, such as a plate-like shape. The graphite may be high-purity graphite having a purity of 99% or more, which may be advantageous in exhibiting further improved physical properties.
[0071] The nanoparticles bonded to the surface of the graphite act as a medium capable of providing the catecholamine layer described later on the graphite. This is specifically explained as follows: Since the surface of the graphite has almost no functional groups capable of mediating chemical reactions, it is difficult to provide a catecholamine layer on the graphite surface that can improve the dispersibility of the graphite in heterogeneous materials. Even if the graphite is treated with catecholamines, there is still a problem that the amount of catecholamines remaining in the actual graphite is very small. In addition, in order to solve this problem, even if the graphite is modified to have functional groups on its surface, there is a limit to increasing the amount of catecholamines on the surface of the modified graphite. However, in the case of graphite having nanoparticles on its surface, since catecholamines are easily bonded to the surface of the nanoparticles, there is an advantage that catecholamines can be introduced into the graphite in a desired amount.
[0072] The nanoparticles may be metal or non-metal substances that exist in a solid form at room temperature when the graphite composite is a non-insulating graphite composite, and as non-limiting examples thereof, may be selected from alkali metals, alkaline earth metals, lanthanides, actinides, transition metals, post-transition metals, metalloids, etc. on the periodic table. As an example, the nanoparticles may be Ni, Si, Ti, Cr, Mn, Fe, Co, Cu, Sn, In, Pt, Au, Mg, and combinations thereof, preferably Cu, Ni, or Si.
[0073] Furthermore, when the above-mentioned graphite composite is an insulating graphite composite, the above-mentioned nanoparticles may include one or more selected from the group consisting of magnesium oxide, yttrium oxide, zirconium oxide, titanium dioxide, aluminum nitride, silicon nitride, boron nitride, aluminum oxide, silicon dioxide, zinc oxide, barium titanate, strontium titanate, beryllium oxide, manganese oxide, talc, silicon carbide, silicon dioxide, and single crystal silicon.
[0074] Then, the catecholamine layer can be arranged at least on the surface of the nanoparticles, thereby improving the excellent fluidity and dispersibility of graphite and the interface bonding characteristics between the graphite complex and the polymer compound in the heterogeneous polymer compound described later. In addition, the catecholamine layer itself has a reducing power, and the catechol functional groups on the surface of the layer form covalent bonds with the amine functional groups through the Michael addition reaction, so that the catecholamine layer can be used as a bonding material for secondary surface modification. As an example, in order to show further improved dispersibility in the polymer compound, it can act as a bonding material that can introduce the polymer layer into the graphite.
[0075] The catecholamines forming the catecholamine layer are single molecules having a hydroxyl group (-OH) as an ortho group of a benzene ring and various alkylamines as a para group. Non-limiting examples of various derivatives of these structures include dopamine, dopamine-quinone, epinephrine, alpha-methyldopamine, norepinephrine, alpha-methyldopa, droxidopa, indolamine, serotonin or 5-hydroxydopamine. As an example, the catecholamine layer may be a dopamine layer.
[0076] On the other hand, a polymer layer may be further coated on the catecholamine layer, and the polymer layer increases the compatibility with the polymer resin forming the radio frequency heat dissipation plastic, thereby achieving further improved dispersibility and interface bonding characteristics. The polymer layer may be the same as or different from the polymer resin, and its specific type may be known.
[0077] On the other hand, the average particle size of the second filler 22 may be 5 μm to 300 μm, preferably, the average particle size may be 10 μm to 250 μm. If the average particle size of the second filler is less than 5 μm, the heat dissipation filler may be detached from the surface, such as sticking out, and the dispersibility may be reduced, and the heat dissipation characteristics may be reduced. If the average particle size exceeds 300 μm, the surface quality of the RF heat dissipation plastic may be reduced, and the mechanical strength may be reduced.
[0078] Furthermore, relative to 100 parts by weight of the polymer resin, 30 to 200 parts by weight, preferably 50 to 150 parts by weight, of the second filler 22 may be further included. If the content of the second filler is less than 30 parts by weight relative to 100 parts by weight of the polymer resin, the heat dissipation characteristics may be relatively reduced, and if it exceeds 200 parts by weight, the surface characteristics of the RF heat sink may be reduced or the mechanical strength may be reduced.
[0079] On the other hand, as additives, the RF heat dissipation plastic of one embodiment of the present invention may also include one or more selected from the group consisting of antioxidants, impact modifiers, flame retardants, strength improvers, heat stabilizers, light stabilizers, plasticizers, antistatic agents, processing modifiers, ultraviolet (UV) absorbers, dispersants and coupling agents.
[0080] The above antioxidant is used to prevent the main chain of the polymer compound from breaking due to shearing during extrusion and injection molding, and to prevent thermal discoloration. As the above antioxidant, known antioxidants can be used without restriction, and as non-limiting examples, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, distearylpentaerythritol diphosphite or other similar organic phosphites; alkylated monophenol or polyphenol; alkylation reaction products of tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane or other similar dienes with polyphenols; butylation reaction products of p-cresol or dicyclopentadiene; alkylated hydroquinone; hydroxylated thiodiphenyl ether; alkylene-bisphenol ; benzyl compounds; esters of monohydric or polyhydric alcohols and β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid; esters of monohydric or polyhydric alcohols and β-(5-tert-butyl-4-hydroxy-3-methylphenyl)-propionic acid; esters of distearyl thiopropionate, dilauryl thiopropionate, tricosyl thiopropionate, octadecyl-3-(3,5-di-tert-butyl-1-4-hydroxyphenyl) propionate, pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate or other analogs of thioalkyl or thioaryl compounds; amides of β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid or other analogs or mixtures thereof. The content of the above antioxidant can be 0.01 to 0.5 parts by weight relative to 100 parts by weight of the polymer resin.
[0081] The impact modifier can be any known component that can improve the impact resistance by showing the flexibility and stress relaxation of the composite material. For example, it can be selected from thermoplastic polyurethane (TPU), thermoplastic polyolefin (TPO), maleic acid grafted ethylene propylene diene rubber (EPDM), core / shell structure elastic particles, rubber-based resins and polyamide-based materials. One or more components in the group consisting of the impact modifier. The thermoplastic polyolefin is a rubber-like material group, which is a linear polyolefin block copolymer having polyolefin blocks such as polypropylene and polyethylene and rubber blocks, or a blend of polypropylene and ethylene-propylene-diene monomer (EPDM) as a vinyl elastomer. Since the specific thermoplastic polyolefin can use the known one, the present invention will omit the description of its specific type. In addition, since the thermoplastic polyurethane can also use the known one, the description of its specific type will be omitted. Furthermore, as an example of the core / shell structured elastic particles, an allyl resin may be used as the core, and the shell portion may be a polymer resin having a functional group that can react to increase compatibility and bonding strength with a thermoplastic polymer resin.
[0082] Examples of the flame retardant include halogenated flame retardants, tretabromo bisphenol A oligomers such as BC58 and BC52, brominated polystyrene or poly(dibromostyrene), brominated epoxy resin, decabromodiphenyl ether, pentabromoacrylate monomer, pentabromobenzyl acrylate polymer, ethylene-bis(tetrabromophthalimide), bis(pentabromobenzyl)ethane, metal hydroxides such as Mg(OH)2 and Al(OH)3, melamine cyanurate, and poly(red phosphorus). The flame retardant may be a phosphorus-based FR system of a phosphorus-based FR system, polyphosphate melamine, phosphoric acid ester, metal phosphinate, ammonium polyphosphate, expandable graphite, sodium or potassium perfluorobutane sulfate, sodium or potassium perfluorooctane sulfate, sodium or potassium dibenzenesulfonate, sodium or potassium 2,4,6-trichlorobenzoate, N-(p-toluenesulfonyl)-p-toluenesulfonamide potassium salt, N-(N'-benzylaminocarbonyl)sulfonamide acyl potassium salt or a mixture thereof, but is not limited thereto. The content of the flame retardant may be 0.1 to 50 parts by weight based on 100 parts by weight of the polymer resin.
[0083] As the above-mentioned strength improver, known components that can improve the strength of the composite material can be used without restriction. As a non-limiting example of this, one or more components in the group consisting of glass fiber, glass beads, zirconium oxide, calcium silicate, gibbsite, boehmite, magnesium aluminate, dolomite, calcium carbonate, magnesium carbonate, mica, talc, silicon carbide, kaolin, calcium sulfate, barium sulfate, silicon dioxide, ammonium hydroxide, magnesium hydroxide and aluminum hydroxide can be included as a strength improver. As an example, the above-mentioned strength improver can be glass fiber. Relative to 100 parts by weight of the polymer resin, the content of the above-mentioned strength improver can be 5 parts by weight to 35 parts by weight, preferably 15 parts by weight to 35 parts by weight, and more preferably 25 parts by weight to 33.3 parts by weight.
[0084] On the other hand, when glass fiber is used as the above-mentioned strength improver, the length of the glass fiber can be 2mm to 8mm, preferably 2mm to 7mm, and most preferably 4mm, and the average fiber diameter can be 1μm to 30μm, preferably 3μm to 20μm, and most preferably 10μm.
[0085] And, as the above-mentioned heat stabilizer, a known heat stabilizer can be used without limitation, and as a non-limiting example, it includes: organic phosphites such as triphenyl phosphite, tris (2,6-dimethylphenyl) phosphite, tris- (mixed mono- and di-nonylphenyl) phosphate or the like; phosphates such as dimethyl phosphate or the like; phosphates such as trimethyl phosphate or the like; or mixtures thereof. The content of the heat stabilizer can be 0.01 to 0.5 parts by weight relative to 100 parts by weight of the polymer resin.
[0086] Furthermore, as the above-mentioned light stabilizer, known light stabilizers can be used without limitation, and as a non-limiting example, benzotriazoles such as 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)-benzotriazole and 2-hydroxy-4-n-octyloxybenzophenone or the like, or mixtures thereof, can be included.
[0087] And, as the above-mentioned plasticizer, known plasticizers can be used without limitation, and as a non-limiting example, phthalates such as dioctyl-4,5-epoxy-hexahydrophthalate, tris-(octyloxycarbonylethyl)isocyanurate, tristearate, epoxidized soybean oil (soybean oil) or the like or mixtures thereof can be included. The content of the plasticizer can be 0.5 to 3.0 parts by weight relative to 100 parts by weight of the polymer resin.
[0088] Furthermore, as the antistatic agent, known antistatic agents can be used without limitation, and non-limiting examples thereof include monostearate, sodium octadecylsulfonate, sodium dodecylbenzenesulfonate, polyether block amides or mixtures thereof, which can be obtained commercially from BASF under the trade name Irgastat, Arkema under the trade name PEBAX, and Sanyo Chemical Industries under the trade name Pelestat. The content of the antistatic agent can be 0.1 to 1.0 parts by weight relative to 100 parts by weight of the polymer resin.
[0089] Furthermore, as the processing modifier, known processing modifiers can be used without limitation, and as non-limiting examples, metal stearate, stearic acid stearate, pentaerythritol tetrastearate, beeswax, montan wax, paraffin, polyethylene wax or the like or a mixture thereof can be included. The content of the processing modifier can be 0.1 to 1.0 parts by weight relative to 100 parts by weight of the polymer resin.
[0090] Furthermore, as the above-mentioned ultraviolet absorber, a well-known ultraviolet absorber can be used without limitation, and non-limiting examples thereof include hydroxybenzophenone, hydroxybenzotriazole, hydroxybenzotriazine, cyanoacrylate, oxanilides, benzoxazinones, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)-phenol, 2-hydroxy-4-n-octyloxybenzophenone, 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-(octyloxy)-phenol, 2,2'-(1,4-phenylene)-1,3,5-triazine-2-yl]-5-(octyloxy)-phenol, 1,3-bis[(2-cyano-3,3-diphenylacryloxy)oxy]-2,2-bis[[(2-cyano-3,3-biphenylacryloxy)oxy]methyl]propane, 2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one), 1,3-bis[(2-cyano-3,3-diphenylacryloxy)oxy]-2,2-bis[[(2-cyano-3,3-diphenylacryloxy)oxy]methyl]propane, nano-sized inorganic substances such as titanium oxide, cerium oxide and zinc oxide with a particle size of less than 100 nm, or the like, or a mixture thereof. The content of the above-mentioned ultraviolet absorber can be 0.01 parts by weight to 3.0 parts by weight based on 100 parts by weight of the polymer resin.
[0091] Furthermore, as the above-mentioned dispersant and coupling agent, known dispersants and coupling agents may be used without limitation. Non-limiting examples of coupling agents include maleic acid grafted polypropylene, silane coupling agents, and the like for heat resistance.
[0092] On the other hand, the RF heat dissipation plastics 100, 101 of the present invention are prepared by a preparation method comprising the following steps: step (1), preparing a first filler 20 by treating at least a portion of the surface of a high-strength filler 20a containing at least one hydroxyl group in a repeating unit with an inorganic coating precursor; and step (2), dispersing the above-mentioned first filler 20 in a polymer resin.
[0093] In this case, as the above-mentioned inorganic coating precursor, any substance that can form the above-mentioned inorganic coating 20b can be used without restriction. Preferably, tetrahydroxysilane (TEOS) is used, which can be more conducive to improving the dispersibility of the first filler and preventing the occurrence of yellowing when the above-mentioned high-strength filler is a cellulose-based filler.
[0094] In the above step (1), the high-strength filler 20a and the inorganic coating precursor may be treated at a weight ratio of 1:10 to 50, preferably at a weight ratio of 1:15 to 45. If the weight ratio of the high-strength filler to the inorganic coating precursor is less than 1:10 or exceeds 1:50, the dispersibility of the first filler cannot be improved to a desired level, and yellowing cannot be prevented when the high-strength filler is a cellulose-based filler, and thus low dielectric properties cannot be exhibited.
[0095] On the other hand, the above step (1) may include: step (1)-1, reacting the high-strength filler with the inorganic coating precursor; and step (1)-2, aging the reacted high-strength filler.
[0096] The reaction step can be performed for 3 to 13 hours, preferably 4 to 12 hours. If the reaction step is performed for less than 3 hours or more than 13 hours, the dispersibility of the first filler cannot be improved to the desired level, and the yellowing of the high-strength filler when it is a cellulose-based filler cannot be prevented, so the low dielectric properties cannot be exhibited.
[0097] Furthermore, the aging step may be performed for 0.3 to 3 hours, preferably 0.5 to 2.5 hours. If the aging step is performed for less than 0.3 hours or more than 3 hours, the dispersibility of the first filler may not be improved to a desired level.
[0098] On the other hand, Figure 5 As shown, the present invention provides a repeater box body having a receiving portion, wherein a relay portion 300 including a device for relaying radio frequency signals is received inside the receiving portion. The present invention can be implemented as a repeater 1000 including a repeater box body, wherein at least a portion of the box body is the radio frequency heat dissipation plastic 102.
[0099] The radio frequency heat dissipation plastic 102 can be implemented as at least a part or the whole of the repeater box body, such as Figure 5 As shown, when implemented as at least one part, it can be composed of a first part as the radio frequency heat dissipation plastic 102 and a second part 200 as the other part.
[0100] In this case, the second portion 200 may be made of a known material used as a repeater box, and thus the present invention has no particular limitation thereto.
[0101] Furthermore, when the radio frequency heat dissipation plastic 102 is implemented as the entire repeater box body, the first part and the second part 200 of the radio frequency heat dissipation plastic 102 can be implemented by the same material.
[0102] On the other hand, the above-mentioned relay unit 300 can be an electrical / electronic device arranged in a well-known repeater. As an example, it can be a front end unit (FEU), a quad base radio (QBR), a router / site reference interface (SRI), a channel service unit (CSU), an optical terminal station equipment, a rectifier, etc.
[0103] Furthermore, the repeater 1000 may further include a heat sink (not shown) or a fan (not shown) inside or outside the repeater box to dissipate heat generated inside the repeater.
[0104] On the other hand, the repeater 1000 may further include other structures that can be further provided in a known repeater in addition to the above structures, and the present invention has no particular limitation on this.
[0105] Embodiments of the present invention
[0106] The present invention will be described more specifically through the following examples, but the following examples are not intended to limit the scope of the present invention but should be construed as helping to understand the present invention.
[0107] Preparation Example 1: Preparation of the First Filler
[0108] First, in order to prepare the first filler, cellulose nanofibrils as a high-strength filler and tetrahydroxysilane (TEOS) as an inorganic coating precursor were treated at a weight ratio of 1:30, reacted for 8 hours, and the high-strength filler after the reaction was aged for 1.5 hours to prepare a high-strength filler having an inorganic coating formed on the surface thereof. Figure 3 and Figure 4 In this case, in the prepared first filler, the average cross-sectional diameter of the high-strength filler is 10 μm, the average thickness of the inorganic coating is 15 nm, and the inorganic coating of the prepared first filler is 150 parts by weight relative to 100 parts by weight of the high-strength filler.
[0109] Preparation Example 2: Preparation of the Second Filler
[0110] First, in order to prepare the second filler, dopamine provided at a concentration of 2 mM, 13 parts by weight of sodium periodate (Na2S2O8) as an oxidant and 20 parts by weight of a buffer solution (Tris-base, Fisher) were mixed in a solvent containing 65 parts by weight of pure water (DI water) and 35 parts by weight of methanol at 23° C. and in the atmosphere to form a coating composition, graphite having nickel (Ni) nanoparticles formed on the surface was immersed therein, stirred for 2.5 hours, filtered, washed with pure water (DI water), and then dried at 23° C. to form a catecholamine layer on the graphite surface, thereby preparing the second filler as a graphite composite. In this case, the average particle size of the second filler was 150 μm.
[0111] Example 1: Preparation of radio frequency heat dissipation plastic
[0112] With respect to 100 parts by weight of polypropylene (PP) as the main resin, 7 parts by weight of the first filler prepared according to the above-mentioned Preparation Example 1 and 100 parts by weight of the second filler prepared according to the above-mentioned Preparation Example 2 were mixed and synthesized by 15 twin-screw extruder to prepare Figure 2 RF heat sink plastic shown.
[0113] Examples 2 to 21 and Comparative Examples 1 to 2
[0114] The preparation is carried out in the same manner as in Example 1, but by changing the average cross-sectional diameter of the high-strength filler in the first filler, the average thickness of the inorganic coating, the content of the inorganic coating, the content of the first filler, whether it is included or not, the average particle size, content and whether it is included or not of the second filler, etc., the RF heat dissipation plastics shown in Tables 1 to 4 are prepared.
[0115] Experimental example
[0116] The following physical properties of each radio frequency heat dissipation plastic prepared according to the embodiment and the comparative example were evaluated, and the results are shown in Tables 1 to 4.
[0117] 1. Heat dissipation performance evaluation
[0118] To prevent external influences, the performance evaluation was conducted in a sealed chamber with a width, length, and height of 30cm×30cm×30cm. Specifically, the planar heating element was attached to the RF heat dissipation plastic, and a current of 350mA was applied to make it heat up. After keeping it for 60 minutes, the heat dissipation performance was evaluated by measuring the temperature of the planar heating element.
[0119] In this case, a high measured temperature means poor heat dissipation performance, and a low measured temperature means excellent heat dissipation performance.
[0120] Furthermore, the measured temperatures of the remaining examples and comparative examples are shown in comparison with the measured temperature of Example 1 being 100 as a reference.
[0121] 2. Mechanical strength evaluation
[0122] The flexural strength of RF heat dissipation plastics was evaluated using an energy tensile tester (Utm).
[0123] In this case, the bending strength of Example 1 is set as 100 as a reference, and the bending strengths of the remaining Examples and Comparative Examples are shown in comparison.
[0124] 3. Dielectric constant and dielectric loss evaluation
[0125] For each RF heat dissipation plastic, the dielectric constant and dielectric loss were measured in the gigahertz (GHz) region using a network analyzer (E8364A (45 MHz to 50 GHz), Agilent Technologies) and a resonant cavity.
[0126] 4. Physical property uniformity evaluation
[0127] The uniformity of physical properties was evaluated by dividing each RF heat dissipation plastic into 10 equal parts with uniform width.
[0128] Specifically, when compared with the measured values measured in items 1 to 3 above, the error of at least one of the heat dissipation performance, mechanical strength, dielectric constant and dielectric loss of each RF heat dissipation plastic divided into 10 equal parts with a uniform width is represented by ○ when it is less than 1%, △ when the error is greater than 1% and less than or equal to 5%, and × when the error is greater than 5%, and the uniformity of the physical properties is evaluated.
[0129] 5. Surface quality assessment
[0130] For the RF heat dissipation plastic according to the embodiment and the comparative example, in order to confirm the surface quality, the surface is touched by hand to confirm whether there is unevenness or roughness. If there is a smooth feeling, it is represented by 5, if the rough part is less than 2% of the total area of the outer surface of the RF heat dissipation plastic, it is represented by 4, if the area exceeds 2% and is less than or equal to 5%, it is represented by 3, if the area exceeds 5% and is less than or equal to 10%, it is represented by 2, if the area exceeds 10% and is less than or equal to 20%, it is represented by 1, and if the area exceeds 20%, it is represented by 0.
[0131] Table 1
[0132]
[0133] Table 2
[0134]
[0135] Table 3
[0136]
[0137]
[0138] Table 4
[0139]
[0140] As can be seen from Tables 1 to 4 above, Examples 1, 3, 6, 7, 10, 11, 14, 15, 18 and 19 that meet all the items of the average cross-sectional diameter of the high-strength filler in the first filler of the present invention, the average thickness of the inorganic coating, the content of the inorganic coating, the content of the first filler, whether it is included or not, the average particle size, content and whether it is included or not of the second filler are compared with Examples 2, 4, 5, 8, 9, 12, 13, 16, 17, 20, 21 and Comparative Examples 1 to 2 in which at least one of the items is omitted, show excellent heat dissipation performance, mechanical strength, uniformity of physical properties and surface quality, and at the same time show the effect of significantly reducing the dielectric constant and dielectric loss.
[0141] An embodiment of the present invention is described above, but the concept of the present invention is not limited to the embodiment presented in this specification, and a person skilled in the art who understands the concept of the present invention can easily propose another embodiment within the same scope of the concept by adding, changing, deleting, or appending structural elements, but it can be said that this also falls within the scope of the concept of the present invention.
Claims
1. A radio frequency heat dissipation plastic, characterized in that: Include: The polymer matrix comprises a polymer resin; a first filler dispersed in the polymer matrix, comprising a high-strength filler and an inorganic coating, wherein the high-strength filler is a polymer containing at least one hydroxyl group in a repeating unit and is a cellulose-based filler having an average cross-sectional diameter of 20 nm to 10 μm, and the inorganic coating is formed on at least a portion of the surface of the high-strength filler and has an average thickness of 10 nm to 20 nm, and wherein the first filler comprises 100 to 200 parts by weight of the inorganic coating relative to 100 parts by weight of the high-strength filler; and The second filler is dispersed in the polymer matrix to improve the heat dissipation property, and has an average particle size of 5 μm to 300 μm.
2. The radio frequency heat dissipation plastic according to claim 1, characterized in that: The high-strength filler includes at least one selected from the group consisting of cellulose nanofibrils and cellulose fibers.
3. The radio frequency heat dissipation plastic according to claim 1, characterized in that: The above-mentioned inorganic coating is an inorganic coating combined with a silicon-based compound and the above-mentioned high-strength filler, and the above-mentioned silicon-based compound includes one or more selected from the group consisting of orthosilicic acid groups, straight-chain silicate groups formed by polymerization of more than two orthosilicic acid groups, branched silicate groups formed by polymerization of more than four orthosilicic acid groups, and cyclic silicate groups formed by polymerization of more than three orthosilicic acid groups.
4. The radio frequency heat dissipation plastic according to claim 3, characterized in that: In the first filler, at least one hydroxyl group of the silicon-based compound is chemically bonded to a hydroxyl group of the high-strength filler.
5. The radio frequency heat dissipation plastic according to claim 1, characterized in that: The first filler is contained in an amount of 1 to 15 parts by weight based on 100 parts by weight of the polymer resin.
6. The radio frequency heat dissipation plastic according to claim 1, characterized in that: The polymer resin comprises one compound selected from the group consisting of polycarbonate, polyamide, polyester, polyketone, liquid crystal polymer, polyolefin, polyphenylene sulfide, polyetheretherketone, polyphenylene ether, polyethersulfone, polyetherimide, polyimide, polyphthalamide, polybutylene terephthalate, acrylonitrile butadiene styrene copolymer resin, polymethyl methacrylate and polyarylate, or a mixture or copolymer of two or more thereof.
7. The radio frequency heat dissipation plastic according to claim 1, characterized in that: The second filler includes at least one selected from the group consisting of non-insulating fillers and insulating fillers, the non-insulating filler includes at least one selected from the group consisting of: at least one carbon-based filler selected from the group consisting of carbon black, graphite and carbon nanomaterials; at least one metal-based filler selected from the group consisting of copper, silver, nickel, gold, platinum and iron; and a non-insulating graphite composite, the insulating filler includes at least one selected from the group consisting of magnesium oxide, yttrium oxide, zirconium oxide, titanium dioxide, aluminum nitride, silicon nitride, boron nitride, aluminum oxide, silicon dioxide, zinc oxide, barium titanate, strontium titanate, beryllium oxide, manganese oxide, talc, silicon carbide, single crystal silicon and insulating graphite composite.
8. The radio frequency heat dissipation plastic according to claim 1, characterized in that: The second filler is further contained in an amount of 30 to 200 parts by weight based on 100 parts by weight of the polymer resin.
9. A method for preparing radio frequency heat dissipation plastic, characterized in that: include: Step (1), preparing a first filler by treating at least a portion of the surface of a high-strength filler containing at least one hydroxyl group in a repeating unit with an inorganic coating precursor so that an inorganic coating with a thickness of 10 nm to 20 nm is formed on at least a portion of the surface of the high-strength filler, wherein the high-strength filler is a polymer containing at least one hydroxyl group in a repeating unit and is a cellulose-based filler with an average cross-sectional diameter of 20 nm to 10 μm, and wherein the first filler contains 100 to 200 parts by weight of the inorganic coating relative to 100 parts by weight of the high-strength filler; and Step (2) is to disperse the first filler and the second filler having an average particle size of 5 μm to 300 μm in the polymer resin to improve the heat dissipation characteristics.
10. The method for preparing radio frequency heat dissipation plastic according to claim 9, characterized in that: The inorganic coating precursor contains tetrahydroxysilane.
11. The method for preparing radio frequency heat dissipation plastic according to claim 9, characterized in that: The above step (1) includes: Step (1)-1, reacting the high-strength filler with the inorganic coating precursor for 3 hours to 13 hours; and Step (1)-2, aging the high-strength filler after the reaction for 0.3 hours to 3 hours.
12. A repeater box, comprising a receiving portion, wherein a device for repeating radio frequency signals is received inside the receiving portion, wherein the repeater box is characterized in that at least a portion of the box is made of the radio frequency heat dissipation plastic according to any one of claims 1 to 8.