A wear-resistant catalyst for producing high-yield low-carbon olefins and its preparation method
By using components such as zirconium sol and phosphorus-aluminum inorganic binders in the catalyst, the strength of the catalyst and the selectivity of low-carbon olefins are improved, and the problem of poor performance of phosphorus-aluminum binders is solved, and high conversion rate and high Selective catalytic cracking effect.
Patent Information
- Application Number
- CN202011103672.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-15
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-10-15
AI Technical Summary
The performance of phosphorus-aluminum adhesives in existing catalytic cracking catalysts is poor, resulting in poor catalyst strength, low conversion rate and insufficient selectivity of low-carbon olefins.
The catalysts with a high yield of low-carbon olefins include 10-60% cracking active components, 20-60% binder and 0-70% second clay, and the binder is 1-50% zirconium sol, 50-99% phosphorus-aluminum inorganic binder and 0-45% third binder, zirconium sol contains ZrO2, stabilizers and alkali cations, and phosphorus-aluminum inorganic binder contains alumina, phosphoric acid and clay, through Specific preparation methods improve the strength and selectivity of the catalyst.
The strength, conversion rate and low-carbon olefin selectivity of the catalyst are significantly improved, the yields of propylene and ethylene are increased, the wear index is reduced, and the coke selectivity is improved.
Smart Images

Figure BDA0002726236590000131 
Figure BDA0002726236590000141 
Figure BDA0002726236590000161
Abstract
Description
Technical Field
[0001] The present invention relates to a catalytic cracking catalyst, and more particularly to a catalytic cracking catalyst with excellent anti-wear performance and a preparation method thereof. Background Art
[0002] In recent years, the demand for propylene has grown rapidly, and the growth rate of global propylene consumption will average about 5%, which is higher than the growth rate of ethylene by 3.5%. However, the propylene / ethylene ratio of steam cracking cannot be flexibly adjusted, and its reaction temperature is as high as 800℃, and its energy consumption accounts for about 40% of the energy consumption of the petrochemical industry. Therefore, increasing the production of propylene through FCC is an effective and efficient way to meet the growth in demand.
[0003] Microporous zeolite catalytic materials are widely used in petroleum refining and chemical processing industries due to their excellent shape-selective catalytic performance and high cracking reaction activity. At present, catalytic cracking catalysts mostly use aluminum sol and peptized pseudo-boehmite as binders, which have low matrix activity, poor selectivity and poor strength. In recent years, phosphate aluminum sol has begun to be introduced as a binder in the preparation of catalytic cracking catalysts.
[0004] CN1076714A discloses a phosphorus-containing hydrocarbon cracking catalyst prepared using phosphorus-containing aluminum sol as a binder. The phosphorus-containing aluminum sol used is prepared according to the method disclosed in CN170384A and CN170385A. However, the performance of the phosphorus-containing aluminum sol catalyst still needs to be improved.
[0005] CN102847547A discloses an inorganic binder containing phosphorus aluminum compounds and a preparation method thereof, wherein the binder contains 15-40 wt% Al2O3, 45-80 wt% P2O5 and 1-40 wt% clay, wherein the P / Al weight ratio is 1-6, the pH value is 1-3.5, and the solid content is 15-60 wt%. The preparation method comprises: dispersing aluminum hydroxide and / or aluminum oxide and clay that can be colloided by acid with decationized water into a slurry with a solid content of 15-45 wt%, adding concentrated phosphoric acid to the slurry at a weight ratio of P / Al=1-6 under stirring, and then reacting at 50-99°C for 15-90 minutes. The preparation method disclosed in the disclosure can avoid the curing of the binder caused by the uneven local instantaneous violent reaction of the material, the exothermic overtemperature, and the obtained binder can improve the wear resistance, activity and selectivity of the FCC catalyst. However, the binder has poor performance in some cases.
[0006] CN102211039B provides a catalytic cracking catalyst and a preparation method thereof, comprising mixing and slurrying a molecular sieve, a zirconium oxide powder and an aluminum binder, adding the zirconium oxide powder to the slurry for slurrying, adjusting the pH value of the slurry to 2-5 with an inorganic acid, and then spray drying, wherein the zirconium oxide powder is prepared by mixing an aqueous solution of a zirconium salt with ammonia water. The catalyst prepared by the method has a strong ability to resist calcium pollution, is used for cracking of calcium-containing hydrocarbon oil, and has a high propylene yield. However, this method introduces zirconium in the form of oxide, which is difficult to be peptized again, which will affect the strength improvement of the catalyst. When the method uses a phosphoaluminum glue binder, the effect is limited. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide a catalytic cracking catalyst with good strength, high conversion rate and high selectivity for light olefins in view of the poor performance of the catalytic cracking catalyst using phosphate aluminum gel binder as a matrix in the prior art.
[0008] The present invention provides a catalytic cracking catalyst for producing more light olefins, comprising: 10% to 60% by weight of a cracking active component on a dry basis, 20% to 60% by weight of a binder on a dry basis, and 0% to 70% by weight of a second clay on a dry basis; wherein, based on the dry basis weight of the binder, the binder comprises 1% to 50% by weight of a zirconium sol, 50% to 99% by weight of an inorganic phosphorus aluminum binder, and 0% to 45% by weight of a third binder;
[0009] The cracking active component comprises a first molecular sieve and an optional second molecular sieve, wherein the first molecular sieve is a five-membered ring structure molecular sieve; on a dry basis, the first molecular sieve accounts for more than 70% of the cracking active component; preferably, the cracking active component contains 70-100% by weight of the first molecular sieve and 0-30% by weight of the second molecular sieve;
[0010] The zirconium sol comprises 0.5 mass % to 20 mass % of ZrO2, a stabilizer, an alkali cation and water, wherein the molar ratio of the stabilizer to Zr is 1 to 6, and the pH value of the zirconium sol is 1 to 7;
[0011] The phosphorus-aluminum inorganic binder contains 15-40 wt% of alumina source components in terms of Al2O3, 45-80 wt% of phosphorus components in terms of P2O5, and 0-40 wt% of first clay in terms of dry basis, with a P / Al weight ratio of 1-6, a pH value of 1-3.5, and a solid content of 15-60 wt%.
[0012] According to the catalytic cracking catalyst described in the above technical solution, the third binder is selected from one or more of silica sol, alumina sol, silica-alumina gel, acidified alumina, and metal-modified alumina.
[0013] According to any of the above technical solutions, the catalytic cracking catalyst, wherein the method for preparing the phosphorus-aluminum inorganic binder comprises:
[0014] (1) slurrying an alumina source, a first clay and water to form a slurry with a solid content of 8-45 wt %; the alumina source is aluminum hydroxide and / or aluminum oxide that can be colloided by acid, and the weight ratio of the first clay calculated on a dry basis to the alumina source calculated on Al2O3 is 0-40:15-40;
[0015] (2) Add concentrated phosphoric acid to the slurry obtained in step (1) at a weight ratio of P / Al=1-6 under stirring; wherein the concentration of the concentrated phosphoric acid is, for example, 50-98% by weight.
[0016] (3) reacting the slurry obtained in step (2) at a temperature of 50-99° C. for 15-90 minutes.
[0017] According to the catalytic cracking catalyst described in any of the above technical solutions, preferably, based on the dry weight of the phosphorus-aluminum inorganic binder, the phosphorus-aluminum inorganic binder contains 15-35 weight % of Al2O3 derived from the alumina source, 50-75 weight % of P2O5 and 0-35 weight % of the first clay on a dry basis, such as 5-30 weight % of the first clay.
[0018] According to the catalytic cracking catalyst described in any of the above technical solutions, the P / Al weight ratio is preferably 2-5.
[0019] According to the catalytic cracking catalyst described in any of the above technical solutions, the alumina source can be one or more of ρ-alumina, χ-alumina, η-alumina, γ-alumina, κ-alumina, δ-alumina, θ-alumina, gibbsite, diaspore, boehmite, diaspore, boehmite and pseudo-boehmite.
[0020] According to the catalytic cracking catalyst described in any of the above technical solutions, the first clay is one or more of kaolin, montmorillonite, diatomite, halloysite, pseudo-halloysite, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite, preferably one or more of kaolin, sepiolite, attapulgite, rectorite, montmorillonite and diatomite.
[0021] According to the catalytic cracking catalyst described in any of the above technical solutions, the second clay can be one or more of kaolin, montmorillonite, diatomaceous earth, halloysite, pseudo-halloysite, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite.
[0022] According to the catalytic cracking catalyst described in any of the above technical solutions, preferably, the size of the zirconium sol particles is between 5nm and 15nm, the average particle size is about 10nm, and the concentration is more than 90%. The about 10nm refers to 10±2nm. The concentration is the ratio of the number of particles with a particle size of about 10nm in the measured particles in the zirconium sol sample to the total number of measured particles, which can be obtained by obtaining the zirconium sol sample image through TEM and computer image analysis. The particle size refers to the diameter of the largest circumscribed circle in the particle projection diagram, and the average particle size is the arithmetic mean of the sample particle size.
[0023] According to the catalytic cracking catalyst described in any of the above technical solutions, preferably, the zirconium sol is dried at 100°C for 6 hours and calcined at 600°C for 2-6 hours for heat treatment, and the obtained product has coexistence of monoclinic and tetragonal phases, and the ratio of monoclinic phase to tetragonal phase is preferably 0.05-0.6:1; and / or the zirconium sol is dried at 100°C for 6 hours and calcined at 800°C for 2-6 hours for heat treatment, and ZrO2 in the obtained product exists in the tetragonal phase.
[0024] According to the catalytic cracking catalyst described in any of the above technical solutions, in the zirconium sol, the stabilizer is an organic acid. In one embodiment, the stabilizer is preferably at least one of glycolic acid, oxalic acid, acetic acid, malonic acid, malic acid, tartaric acid, succinic acid, adipic acid, maleic acid, itaconic acid, citric acid, etc., more preferably one or more of acetic acid, oxalic acid or citric acid.
[0025] According to the catalytic cracking catalyst described in any of the above technical solutions, in the zirconium sol, the alkali cation (also called basic cation) is preferably a nitrogen-containing cation, such as an ammonium ion or a nitrogen-containing cation formed by hydrolysis of a water-soluble organic base, and the water-soluble organic base is, for example, one or more of methylamine, dimethylamine, trimethylamine, methanolamine, dimethanolamine, trimethanolamine, triethylamine, ethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetraisopropylammonium hydroxide, tetrabutylammonium hydroxide, monomethyltriethylammonium hydroxide, monomethyltriethanolammonium hydroxide, monomethyltributylammonium hydroxide, etc.
[0026] According to the catalytic cracking catalyst described in any of the above technical solutions, in the zirconium sol, the molar ratio of the alkali cation to Zr is preferably 1-8.
[0027] According to the catalytic cracking catalyst described in any of the above technical solutions, preferably, the zirconium sol further contains inorganic acid radicals and / or alcohols, and the molar ratio of the inorganic acid radicals and / or alcohols to Zr is preferably 1-6, for example, 1-4: 1. The inorganic acid radicals are one or more of sulfate, chloride, and nitrate, and the alcohols are one or more of methanol, ethanol, propanol, and butanol.
[0028] According to the catalytic cracking catalyst described in any of the above technical solutions, the pH value of the zirconium sol is preferably 1.5-5, more preferably 2-4, and further preferably 2-3.
[0029] According to any of the above technical solutions, a method for preparing the zirconium sol comprises the following steps:
[0030] (1) preparing a zirconium source solution, wherein the concentration of the zirconium source solution is 0.5 mass % to 20 mass % based on ZrO2, for example, 1 to 18 mass % or 5 to 15 mass %; the zirconium source solution can be prepared at room temperature; the room temperature can be 15 to 40°C;
[0031] (2) adding a stabilizer to the zirconium source solution to obtain a first mixed solution, preferably, stirring at room temperature to 90° C. for 0.5-3 hours to allow it to react sufficiently to obtain a first mixed solution; wherein the molar ratio of the stabilizer to the zirconium is 1-6:
[0032] (3) At room temperature-50° C., adding alkali solution to the first mixed solution to obtain zirconium sol, wherein the amount of alkali solution is such that the pH value of the zirconium sol is 1-7.
[0033] According to the above technical scheme, the method for preparing zirconium sol, slowly adding alkali solution to the first mixed solution to obtain clear and transparent zirconium sol. The slowly adding, for example, can be dripping, or controlling a certain adding speed, for example, the adding speed is 0.05ml-50ml / minute / L first mixed solution, for example, 0.1-30ml alkali solution / minute / L first mixed solution or 1-35ml alkali solution / minute / L first mixed solution or 0.05ml-10ml / minute / L first mixed solution or 0.1ml-5ml / minute / L first mixed solution. In one embodiment, alkali solution is slowly added to the first mixed solution with a pump, and the pump is, for example, a peristaltic pump. Preferably, the amount of alkali solution added makes the pH value of the zirconium sol 1.5-5, for example, 2-4, and more preferably 2-3.
[0034] According to any of the above technical solutions, in the zirconium sol preparation method, the zirconium source is one or more of inorganic zirconium salts or organic zirconium salts, the inorganic zirconium salts are, for example, one or more of zirconium tetrachloride, zirconium oxychloride, zirconium acetate, zirconium nitrate, zirconium oxynitrate, zirconium oxy sulfate and zirconium oxy carbonate; the organic zirconium salt is, for example, one or more of zirconium n-propoxide, zirconium isopropoxide, zirconium ethanol and zirconium butoxide.
[0035] According to any of the above technical schemes, in the zirconium sol preparation method, the stabilizer is an organic acid that can form a coordination polymer with zirconium, and the stabilizer is preferably at least one of glycolic acid, acetic acid, oxalic acid, malonic acid, malic acid, tartaric acid, succinic acid, adipic acid, maleic acid, itaconic acid, citric acid, etc., and more preferably one or more of acetic acid, oxalic acid or citric acid.
[0036] According to any of the above technical schemes, in the zirconium sol preparation method, the alkali solution is selected from ammonia water or an aqueous solution of a water-soluble organic base, and the water-soluble organic base is, for example, methylamine, dimethylamine, trimethylamine, methanolamine, dimethanolamine, trimethanolamine, triethylamine, ethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetraisopropylammonium hydroxide, tetrabutylammonium hydroxide, monomethyltriethylammonium hydroxide, monomethyltriethanolammonium hydroxide, and monomethyltributylammonium hydroxide. One or more.
[0037] The present invention also provides a method for preparing the catalytic cracking catalyst, comprising: forming a slurry from cracking active components, a binder, water and optional clay, and spray drying.
[0038] The present invention provides a catalytic cracking method, comprising the step of contacting and reacting heavy oil with the catalytic cracking catalyst described in any one of the above technical solutions or a catalyst obtained by the catalytic cracking catalyst preparation method described in any one of the technical solutions.
[0039] The catalytic cracking catalyst provided by the present invention has at least one of the following beneficial effects, and preferably has multiple or all of the following beneficial effects:
[0040] (1) The catalyst provided by the present invention is used for catalytic cracking of hydrocarbon oil and has high hydrocarbon oil conversion activity.
[0041] (2) The catalyst provided by the present invention is used for catalytic cracking conversion and has high selectivity for light olefins.
[0042] (3) The catalyst provided by the present invention is used for catalytic cracking conversion of hydrocarbon oil, has a high propylene yield, and a high propylene concentration in the liquefied gas.
[0043] (4) The catalyst provided by the present invention is used for catalytic cracking conversion of hydrocarbon oil, and the ethylene concentration in the dry gas is relatively high.
[0044] (5) The catalyst provided by the present invention has good strength and low wear index.
[0045] (6) When using modified NSY molecular sieve, the coke selectivity of the catalyst is better.
[0046] The catalyst preparation method provided by the present invention has one or more of the following advantages:
[0047] (1) The phosphoaluminum gel of the present invention has a good stabilizing effect on the five-membered ring molecular sieve.
[0048] (2) The present invention uses the newly developed zirconium oxide sol, which, when containing the phosphoaluminum sol, can further improve the wear strength of the catalyst.
[0049] (3) The present invention introduces zirconium and P elements in the form of sol. The zirconium sol and the phosphorus-aluminum inorganic binder synergistically compensate for the weak adhesion of the P-Al glue and improve the propylene selectivity of ZSM-5, thereby improving the heavy oil conversion rate and low-carbon olefin selectivity.
[0050] (4) The preparation method of the catalytic cracking catalyst provided by the present invention introduces zirconium and P elements in the form of sol, and contains a newly developed modified NSY molecular sieve active component, so that the catalyst has higher activity, thereby improving the heavy oil conversion rate and light olefin selectivity. DETAILED DESCRIPTION
[0051] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0052] According to the catalytic cracking catalyst of the present invention, the first molecular sieve is a molecular sieve with a five-membered ring, and the molecular sieve with a five-membered ring is one or more of MFI structure molecular sieve (or MFI type molecular sieve), BEA structure molecular sieve, mordenite, etc., preferably one or more of BEA structure molecular sieve and MFI structure molecular sieve. The MFI structure molecular sieve includes at least one of rare earth-containing MFI molecular sieve, phosphorus-containing MFI molecular sieve, and transition metal-containing MFI molecular sieve. The phosphorus-containing MFI molecular sieve may further contain a transition metal, and the transition metal is preferably one or more of Fe, Co, Ni, Cu, Mn, Zn, Sn, and Bi, and more preferably one or more of Fe, Co, Ni, Zn, and Cu; the BEA structure molecular sieve, such as Beta molecular sieve, can be a BEA structure molecular sieve obtained by amine-free crystallization, or a BEA structure molecular sieve obtained by calcining a molecular sieve prepared by a template method; mordenite may include at least one of high-silicon mordenite or low-silicon mordenite. Preferably, the first molecular sieve includes an MFI structure molecular sieve.
[0053] The catalytic cracking catalyst according to the present invention optionally contains a second molecular sieve, and the content of the second molecular sieve is preferably 0-18 wt%, 1-15 wt%, 2-10 wt%, or 5-10 wt%.
[0054] According to any of the above technical solutions, in the catalytic cracking catalyst provided by the present invention, the second molecular sieve is preferably a macroporous molecular sieve, and the second molecular sieve is preferably a Y-type molecular sieve, which may or may not contain rare earth elements, and the rare earth content in the Y-type molecular sieve is 0-20% by weight in terms of RE2O3. The unit cell constant of the Y-type molecular sieve may be 2.430nm-2.480nm.
[0055] According to the catalytic cracking catalyst provided by the present invention, the Y-type molecular sieve is preferably one or more of DASY molecular sieve, DASY molecular sieve containing rare earth, USY molecular sieve, USY molecular sieve containing rare earth, REY molecular sieve, HY molecular sieve, REHY molecular sieve, and Y-type molecular sieve synthesized by in-situ crystallization of modified kaolin.
[0056] According to the catalytic cracking catalyst provided by the present invention, in one embodiment, the Y-type molecular sieve is an ultra-stable Y-type molecular sieve, the rare earth content in the ultra-stable Y-type molecular sieve is 0-12% by weight, for example, 1-12% by weight, calculated as RE2O3, the sodium oxide content does not exceed 2% by weight, and the unit cell constant measured by X-ray diffraction is 2.435-2.460nm.
[0057] According to the method for preparing a catalytic cracking catalyst of the present invention, in one embodiment, the catalyst provided by the present invention contains a second molecular sieve, and the second molecular sieve comprises a Y-type molecular sieve synthesized by in-situ crystallization of modified kaolin, and the sodium oxide content of the Y-type molecular sieve synthesized by in-situ crystallization of the modified kaolin is preferably less than 2% by weight, and preferably, the Y-type molecular sieve synthesized by in-situ crystallization of the modified kaolin is a modified NSY-type molecular sieve. The NSY molecular sieve synthesized by in-situ crystallization of kaolin is subjected to a modification treatment to obtain a modified NSY-type molecular sieve, and the modification treatment includes ultrastabilization treatment and / or ion exchange treatment. The sodium oxide content of the modified NSY-type molecular sieve is less than 2% by weight. The rare earth content in the modified NSY molecular sieve is 0% by weight-20% by weight in terms of RE2O3.
[0058] In one embodiment, the modified NSY molecular sieve is an ion-modified ultra-stable NSY molecular sieve, the rare earth content of which is 0% by weight to 12% by weight in terms of RE2O3, and the unit cell constant is 2.435-2.460 nm.
[0059] In one embodiment, the modified NSY molecular sieve is an ion-modified ultrastable NSY molecular sieve, and the content of the ion-modified ultrastable NSY molecular sieve in the catalytic cracking catalyst is, for example, 1-10 wt% or 5-10 wt% on a dry basis. The ion modification is, for example, ammonium exchange and / or rare earth exchange.
[0060] According to the catalytic cracking catalyst of the present invention, in a preferred embodiment, the Y molecular sieve is a modified NSY molecular sieve, which is obtained by modifying the NSY molecular sieve synthesized by in-situ crystallization of kaolin (hereinafter referred to as the NSY molecular sieve synthesized by in-situ crystallization). The modification treatment is, for example, ion exchange and / or ultra-stabilization treatment. The modification treatment reduces the sodium oxide content in the NSY molecular sieve synthesized by in-situ crystallization of kaolin to less than 2% by weight. The NSY molecular sieve synthesized by in-situ crystallization of kaolin is measured by X-ray diffraction method, and the crystallinity of the peak height method is ≥60%, and the ratio of the crystallinity to the peak area method is K1, K1=0.76-0.89; the silicon-aluminum ratio measured by the unit cell constant a0 is 5.0-5.5, and the ratio to the silicon-aluminum ratio measured by the chemical method is K2, K2=0.87-0.93, and the silicon-aluminum ratio is the molar ratio of silicon oxide to aluminum oxide.
[0061] According to the common sense of crystallization, the difference between the crystallinity measured by the peak height method and the crystallinity measured by the peak area method is related to the size of the crystal grains. The Y-type molecular sieve composite material of the present invention (hereinafter referred to as the composite material) sets the crystal factor K1, K1 = S 峰高 / S 峰面积, which is the ratio of the crystallinity measured by the peak height method to the crystallinity measured by the peak area method. The size of the K1 value indicates the size of the grains. The larger the K1 value, the larger the grain size.
[0062] The molar ratio of silicon oxide to aluminum oxide calculated by the unit cell constant a0 is the framework silicon-aluminum ratio of the molecular sieve, and the molar ratio of silicon oxide to aluminum oxide determined by the chemical method is the overall silicon-aluminum ratio of the composite material. The NSY molecular sieve synthesized by kaolin in-situ crystallization of the present invention has a framework silicon-aluminum ratio of 5.0-5.5, preferably 5.2-5.5, determined by the unit cell constant a0, and the overall silicon-aluminum ratio determined by the chemical method is the macroscopic silicon-aluminum ratio of the entire material. The two values of the framework silicon-aluminum ratio and the overall silicon-aluminum ratio are related to the framework integrity and purity of the molecular sieve in the composite material. The NSY molecular sieve synthesized by kaolin in-situ crystallization of the present invention is obtained by crystallization of metakaolin, in which a part of the metakaolin is in the intermediate of crystallization to Y-type molecular sieve, therefore, the intermediate system coefficient K2 is set, i.e., K2=framework silicon-aluminum ratio / overall silicon-aluminum ratio. The size of the K2 value indicates the degree of compositeness of the composite material, and the smaller the K2 value, the more intermediates are contained. The preferred K2 is 0.87-0.92, more preferably = 0.88-0.90.
[0063] The NSY molecular sieve (also called Y-type molecular sieve composite material) synthesized by in-situ crystallization of kaolin described in the present invention preferably has K1=0.77-0.88, for example, K1=0.81-0.88 or K1=0.86-0.88 and K2=0.87-0.91.
[0064] According to the catalytic cracking catalyst of the present invention, preferably, the NSY molecular sieve synthesized by in-situ crystallization of kaolin has a spherical shape of 5-20 microns, wherein the crystallinity measured by the peak height method is ≥60%, that is, the mass percentage of the NaY molecular sieve is at least 60%. Preferably, the crystallinity measured by the peak height method is greater than 75%, more preferably ≥80%.
[0065] According to the catalytic cracking catalyst of the present invention, wherein the K1=0.80-0.89.
[0066] According to the catalytic cracking catalyst of the present invention, wherein the K1=0.80-0.85.
[0067] According to the catalytic cracking catalyst of the present invention, wherein the K2=0.87-0.92.
[0068] According to the catalytic cracking catalyst of the present invention, wherein the K2=0.88-0.90.
[0069] The catalytic cracking catalyst according to any of the above technical solutions, wherein K1=0.77-0.88, K2=0.87-0.91.
[0070] In the present invention, pores with a pore diameter greater than 0.8 nm are defined as medium and macropores. The NSY molecular sieve synthesized by in-situ crystallization of kaolin described in the present invention has a suitable medium and macropore ratio, wherein the macropore ratio is 10-20%.
[0071] According to the catalytic cracking catalyst of the present invention, the NSY molecular sieve synthesized by in-situ crystallization of kaolin comprises the following steps:
[0072] (1) calcining and dehydrating kaolin at 500-900° C. to convert it into metakaolin, and crushing it into metakaolin powder with a particle size of less than 10 μm;
[0073] (2) adding a directing agent, sodium silicate, sodium hydroxide solution and water to the metakaolin powder to prepare a reaction raw material A, wherein the mass ratio of the directing agent to the metakaolin is 0.01-1.0, and the ratio of the reaction raw material A is (1-2.5) Na2O:Al2O3:(4-9)SiO2:(40-100)H2O in molar ratio;
[0074] (3) crystallizing the reaction raw material A at 88-98° C. for 1-70 h under stirring, and then adding a second silicon source to obtain a reaction raw material B, wherein the second silicon source accounts for 0.1-10% by weight of the total silicon feed, calculated as silicon oxide;
[0075] (4) The reaction material B is crystallized under stirring at 88-98°C and the product is recovered.
[0076] According to the preparation method of the catalytic cracking catalyst provided by the present invention, the sodium content in the NSY molecular sieve synthesized by in-situ crystallization of kaolin can be reduced by any method that can reduce the sodium content in the NSY molecular sieve so that the sodium oxide content therein does not exceed 2% by weight, for example, by ion exchange to obtain a modified NSY molecular sieve. The ion exchange can be carried out using ammonium salt and / or rare earth salt solution, and the present invention has no special requirements. In one embodiment, the ion exchange makes the rare earth content in the obtained modified NSY molecular sieve be 10% to 20% by weight, for example, 10% to 20% by weight or 1-15% by weight or 4-12% by weight in terms of RE2O3, and the sodium oxide content is less than 2% by weight. In one embodiment, the NSY molecular sieve synthesized by in-situ crystallization of kaolin is mixed with an exchange solution and stirred at 20-90°C for 10-120 minutes. The above process can be carried out once or multiple times, and the exchange solution exchanged each time can contain ammonium ions, rare earth ions, or both ammonium ions and rare earth ions. Preferably, the concentration of ammonium salt in the exchange solution is 5-700 g / L, for example, 5-100 g / L and / or the concentration of rare earth salt is 2-450 g / L, for example, 5-200 g / L or 5-400 g / L in terms of RE2O3. The ammonium salt is, for example, one or more of ammonium chloride, ammonium nitrate, and ammonium sulfate. The rare earth salt is, for example, one or more of rare earth chloride and rare earth nitrate. The rare earth may include one or more of lanthanide rare earths and actinide rare earths, for example, one or more of La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, TB, Dy, Ho, Er, Tm, Yb, and Lu.
[0077] According to the preparation method of the catalytic cracking catalyst provided by the present invention, the NSY molecular sieve synthesized by in-situ crystallization of kaolin may further include one or more steps of filtration, washing, drying and calcination after ion exchange. These steps may refer to the filtration, washing, drying and calcination methods well known to those skilled in the art.
[0078] According to the method for preparing the catalytic cracking catalyst of the present invention, the method for preparing the modified NSY molecular sieve comprises the following steps:
[0079] (1) calcining kaolin at 500-900° C. to dehydrate and convert it into metakaolin, and crushing it to prepare metakaolin powder with a particle size of less than 10 μm;
[0080] (2) adding sodium silicate, a directing agent, a sodium hydroxide solution and water to the metakaolin powder to prepare a reaction raw material A with a ratio of (1-2.5) Na2O:Al2O3:(4-9)SiO2:(40-100)H2O, wherein the mass ratio of the directing agent to the metakaolin is 0.01-1.0;
[0081] (3) crystallizing the reaction raw material A at 88-98° C. under stirring, and adding a second silicon source after the crystallization time reaches 1-70 hours to obtain the reaction raw material B, wherein the second silicon source accounts for 0.1% to 10% by weight of the total silicon feed, calculated as silicon oxide;
[0082] (4) crystallizing the reaction raw material B at 88-98° C. under stirring and recovering the product to obtain the NSY molecular sieve synthesized by in-situ crystallization of kaolin;
[0083] (5) Recovering the product and subjecting it to ion exchange and / or ultrastabilization treatment.
[0084] According to the preparation method of the catalytic cracking catalyst of the present invention, in the preparation method of the modified NSY molecular sieve, the directing agent can be synthesized according to a conventional method, such as according to the preparation methods of USP3574538, USP3639099, USP3671191, USP4166099, and EUP0435625. The molar composition of the directing agent is: (10-17) SiO2: (0.7-1.3) Al2O3: (11-18) Na2O: (200-350) H2O. During the synthesis, the raw materials are aged at 4-35°C, preferably 4-20°C to obtain the directing agent.
[0085] According to the preparation method of the catalytic cracking catalyst of the present invention, wherein, in the preparation method of the modified NSY molecular sieve, the sodium content of the second silicon source is 0.01 wt%-10 wt% in terms of Na2O, preferably <1 wt%. The second silicon source may be a solid silicon source and / or a liquid silicon source. Considering the cost control factor, the preferred second silicon source is solid silica gel. The solid silica gel is included in the total synthesis ratio, and the solid silica gel used may be solid silica gel of different pore sizes. According to the pore size, there are fine-pore silica gel, coarse-pore silica gel and medium-pore silica gel between the two. It is customary to call silica gel with an average pore size of less than 1.5-2.0nm as fine-pored silica gel (e.g., type A solid silica gel from Qingdao Ocean Chemical Group Special Silica Gel Factory), and silica gel with an average pore size of more than 4.0-5.0nm as coarse-pored silica gel (e.g., type C solid silica gel from Qingdao Ocean Chemical Group Special Silica Gel Factory); in addition, silica gel with an average pore size of more than 10.0nm is called extra coarse-pored silica gel, and silica gel with an average pore size of less than 0.8nm is called extra fine-pored silica gel (e.g., type B solid silica gel from Qingdao Ocean Chemical Group Special Silica Gel Factory). The second silicon source may also be liquid silica gel. When liquid silica gel is used as the second silicon source, preferably, the mass content of SiO2 therein is at least 30%.
[0086] According to the method for preparing the catalytic cracking catalyst of the present invention, in the method for preparing the modified NSY molecular sieve, the second silicon source accounts for 4-10 weight % of the total silicon feed, calculated as silicon oxide.
[0087] According to the preparation method of the catalytic cracking catalyst provided by the present invention, in the preparation method of the modified NSY molecular sieve, sodium silicate and the second silicon source are added into the synthesis preparation system in different processes, and the second silicon source is added during the crystal growth period. The present invention combines the means of adding different silicon sources at different stages of the crystallization process to control the synthesis ratio technology and the kaolin in-situ crystallization synthesis technology (using natural minerals as the main aluminum source and silicon source), changes the crystal growth environment through the silicon source, and adopts two completely different material ratios in the crystal nucleation period and the crystal growth period. In the crystal nucleation period, the method of the present invention adopts a larger sodium-silicon ratio (Na2O / SiO2) in the material, which is conducive to the rapid nucleation of the Y-type molecular sieve, and in the crystal growth period, a low-sodium or sodium-free silicon source is added to increase the silicon-aluminum ratio (SiO2 / A12O3) in the synthetic material, while reducing the sodium-silicon ratio (Na2O / SiO2) in the material, and on the premise of shortening the crystallization time, it is conducive to the improvement of the product silicon-aluminum ratio, and the skeleton silicon-aluminum ratio is increased to 5.0-5.5.
[0088] According to the preparation method of the catalytic cracking catalyst provided by the present invention, in the preparation method of the modified NSY molecular sieve, a multi-level pore Y-type molecular sieve composite material product containing certain medium and large pores is obtained by crystallization under stirring, and the crystallization stirring speed can be, but is not limited to, 50-1000 rpm, preferably 300-500 rpm, and the time is 16-48 hours, preferably 24-32 hours. The drying temperature of the zeolite after crystallization is 100-120°C.
[0089] According to the preparation method of the catalytic cracking catalyst provided by the present invention, in step (4) of the preparation method of the modified NSY molecular sieve, the product is recovered after the crystallization is completed to obtain the NSY molecular sieve synthesized by in-situ crystallization of kaolin. The recovery generally includes the step of filtering, and optionally, may also include one or more processes of washing, drying, and roasting.
[0090] According to the method for preparing the catalytic cracking catalyst of the present invention, the ion exchange in the preparation step (5) of the method for preparing the modified NSY molecular sieve may be ammonium ion exchange and / or rare earth ion exchange.
[0091] According to the method for preparing a catalytic cracking catalyst of the present invention, wherein the ion exchange comprises rare earth ion exchange, the rare earth content in the modified NSY molecular sieve obtained in step (5) is 0 wt%-20 wt% in terms of RE2O3, and the sodium oxide content is less than 2 wt%.
[0092] In one embodiment, the modified NSY molecular sieve is obtained by subjecting the NSY molecular sieve synthesized by in-situ crystallization of kaolin to ultra-stabilization treatment and ion exchange treatment to obtain an ion-modified ultra-stable NSY molecular sieve.
[0093] The NSY molecular sieve synthesized by in-situ crystallization of kaolin is subjected to ultrastabilization treatment and ion exchange treatment to obtain an ion-modified ultrastable NSY molecular sieve. The ultrastabilization treatment is, for example, hydrothermal ultrastabilization and gas phase ultrastabilization; the ion exchange is one or more of ammonium ion exchange and rare earth ion exchange. There is no requirement for the order of ultrastabilization treatment and ion exchange, for example, ultrastabilization treatment can be performed first and then ion exchange, or ion exchange can be performed first and then ultrastabilization treatment, or ultrastabilization treatment and ion exchange can be performed alternately one or more times.
[0094] The hydrothermal ultra-stabilization method can be based on existing methods. In one embodiment, the NSY molecular sieve synthesized by in-situ crystallization of kaolin may be subjected to or not subjected to ion exchange, and then contacted with water vapor at a temperature of 550-750° C. for treatment, and the contact time may be, for example, 0.5-20 hours. For example, the hydrothermal ultra-stabilization treatment may be performed with reference to the methods disclosed in patent documents CN108928833A and CN108927211A.
[0095] The gas phase ultra-stabilization method can refer to the existing gas phase ultra-stabilization method. In one embodiment, the NSY molecular sieve synthesized by in-situ crystallization with or without ion exchange is contacted with silicon tetrachloride gas at 200-600°C for treatment, and the contact time can be, for example, 0.5-20 hours. For example, the gas phase ultra-stabilization treatment can be carried out by referring to the methods disclosed in patent documents CN1382525A, CN1194941A, CN1683244A, and CN111013328A.
[0096] The ion exchange can be carried out using ammonium salt and / or rare earth salt solution, and can be carried out with reference to the existing ion exchange method. The present invention has no special requirements. In one embodiment, the ion exchange is to mix the NSY molecular sieve synthesized by in-situ crystallization of kaolin or the NSY molecular sieve synthesized by in-situ crystallization of kaolin treated with ultra-stabilization with an exchange solution, and stir for 10-120 minutes at 20-90°C. The above process can be carried out once or multiple times, and the exchange solution of each exchange can contain ammonium ions, rare earth ions, or both ammonium ions and rare earth ions. Preferably, the exchange solution contains ammonium salt and / or rare earth salt, and the concentration of ammonium salt in the exchange solution is 5-700g / L, such as 5-100g / L, and / or the concentration of rare earth salt is 2-450g / L, such as 5-400g / L or 5-200g / L in terms of RE2O3.
[0097] The ammonium salt is, for example, one or more of ammonium chloride, ammonium nitrate, and ammonium sulfate.
[0098] The rare earth salt is, for example, one or more of rare earth chloride and rare earth nitrate.
[0099] The rare earth may include one or more of lanthanide rare earths and actinide rare earths, for example, one or more of La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, TB, Dy, Ho, Er, Tm, Yb, and Lu.
[0100] Step (5) may also include a washing step, wherein the washing may be performed with water or with an ammonium salt to remove the exchanged sodium ions.
[0101] Preferably, the rare earth content in the ion-modified ultrastable NSY molecular sieve obtained in step (5) is 0%-12% by weight in terms of RE2O3, the sodium oxide content is less than 2% by weight, and the unit cell constant is 2.435-2.460 nm. The unit cell constant can be measured by X-ray diffraction.
[0102] According to the method for preparing a catalytic cracking catalyst of the present invention, the ion exchange product obtained in step (5) of the method for preparing the modified NSY molecular sieve is further calcined.
[0103] According to the preparation method of the catalytic cracking catalyst provided by the present invention, the NSY molecular sieve synthesized by in-situ crystallization of kaolin may further include one or more steps of filtration, washing, drying and calcination after ion exchange. These steps may refer to the filtration, washing, drying and calcination methods well known to those skilled in the art.
[0104] According to one embodiment of the present invention, the method for preparing the catalytic cracking catalyst comprises the following steps:
[0105] (S1) obtaining a molecular sieve slurry,
[0106] (S2) obtaining a second clay slurry,
[0107] (S3) obtaining zirconium sol,
[0108] (S4) obtaining a phosphorus aluminum inorganic binder,
[0109] (S5) mixing the molecular sieve slurry, the second clay slurry, the zirconium sol, the phosphorus aluminum inorganic binder and an optional third binder;
[0110] (S6) spray drying the slurry obtained in step (S5).
[0111] The preparation method of the catalytic cracking catalyst according to the present invention comprises mixing a molecular sieve slurry, a second clay slurry, a zirconium sol, a phosphorus aluminum inorganic binder and an optional third binder to form a slurry, wherein the solid content of the slurry may be 15-45 wt % and preferably 20-40 wt %; and then spray drying the slurry. The spray drying method may adopt an existing method.
[0112] In the method for preparing the catalytic cracking catalyst provided by the present invention, the catalyst microspheres obtained by spray drying can also be washed and / or calcined. There is no special requirement for the order of washing and calcining. The washing and calcining methods of the existing catalytic cracking catalysts can be referred to.
[0113] The present invention will be described in detail below through examples.
[0114] The element content in the catalyst was determined by XRF, and the specific surface area and pore volume were determined by low-temperature nitrogen adsorption-desorption method. The wear index of the catalyst was determined by the RIPP29-90 method in "Petrochemical Analysis Method, RIPP Test Method" (edited by Yang Cuiding, Science Press, published in 1990).
[0115] The specifications of raw materials used in the preparation of zirconium sol, molecular sieve and catalyst are as follows:
[0116] Pseudo-boehmite: purchased from Shandong Aluminum Company, solid content 75 wt%;
[0117] Zirconium oxychloride: purchased from Aldrich Company, analytical grade, content 98.5 wt%;
[0118] Kaolin: solid content 75% by weight, produced by China Kaolin Co., Ltd. (Suzhou);
[0119] DASY molecular sieve: Sinopec Catalyst Qilu Branch, Na2O content is 1.02% by weight, rare earth content (calculated as RE2O3) is 2.3% by weight, silicon-aluminum ratio (SiO2 / Al2O3 molar ratio) is 10.4.
[0120] ZSP-3 molecular sieve: Sinopec Catalyst Qilu Branch, P2O5 content is 3.02% by weight, (SiO2 / Al2O3) is 45, and Na2O content is 0.02% by weight.
[0121] Alumina sol: produced by Shandong Aluminum Plant, solid content 25% by weight.
[0122] Glacial acetic acid: Sinopharm Group, analytical grade, 99 wt%.
[0123] Ammonia water: Sinopharm Group, analytical grade, 28 wt%.
[0124] Oxalic acid: Sinopharm Group, analytical grade, 99% by weight
[0125] Zirconium isopropoxide: Sinopharm Group, analytical grade, 99 wt%
[0126] Triethanolamine: Sinopharm Group, analytical grade, 99 wt%
[0127] Sodium hydroxide: Sinopharm Group, analytical grade, 99% by weight
[0128] Hydrochloric acid: Sinopharm Group, analytical grade, 36% by weight
[0129] The content of NaY zeolite in the composite material in the example is determined according to the RIPP146-90 standard method (the RIPP standard method is shown in "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990, the same below).
[0130] The unit cell constant a0 is determined according to the RIPP 145-90 standard method. The framework silicon-aluminum ratio is calculated from the unit cell constant a0 according to the following formula: SiO2 / Al2O3 (molar ratio) = 2×(25.858-a0) / (a0-24.191).
[0131] The specific surface area was determined by the nitrogen adsorption method (GB / T5816-1995); the pore volume was determined by the nitrogen adsorption method (RIPP151-90). In the nitrogen adsorption method, pores larger than 0.8 nm were defined as medium and macropores. The formula for calculating the medium and macroporosity was (V 总孔 -V 微孔 ) / V 总孔 ×100%.
[0132] In the molecular sieve preparation examples and comparative examples, the preparation of the directing agent is as follows: 250 kg of sodium silicate solution (containing 20.05 wt% SiO2 and 6.41 wt% Na2O) is slowly added with 120 kg of sodium aluminate solution (containing 3.15 wt% Al2O3 and 21.1 wt% Na2O) at 30°C under rapid stirring, stirred for 1 hour, aged at 20°C for 48 hours to obtain the directing agent. The directing agent composition is 16Na2O:Al2O3:15SiO2:320H2O.
[0133] Zirconium sol preparation example 1
[0134] Add 130 g of deionized water to a beaker, then add 125 g of zirconium oxychloride, stir for 10 min, add 93 g of acetic acid, stir for 30 min, and obtain a mixed solution; then use a peristaltic pump to slowly add ammonia water to the above solution, control the pump speed (i.e., the feeding speed of ammonia water) at 5 ml / min, and control the pH value to 2.5 to obtain a clear and transparent zirconium sol A1.
[0135] Zirconium sol preparation example 2
[0136] Add 130 g of deionized water to a beaker, then add 125 g of zirconium oxychloride, stir for 10 min, add 70 g of oxalic acid, stir for 30 min, and obtain a mixed solution; then use a peristaltic pump to slowly add ammonia water to the above solution, control the pump speed at 5 ml ammonia water / min, and control the pH value to 2.5 to obtain a clear and transparent zirconium sol A2.
[0137] Zirconium sol preparation example 3
[0138] Add 170 g of deionized water to a beaker, then add 176 g of zirconium isopropoxide, stir for 10 min, add 70 g of oxalic acid, stir for 30 min, and obtain a mixed solution; then slowly add triethanolamine to the above solution with a pump, control the pump speed at 5 ml / min, control the pH to 2.5, and obtain a clear and transparent zirconium sol A3.
[0139] Zirconium sol preparation comparative example 1
[0140] Add 130 g of deionized water to a beaker, then add 125 g of zirconium oxychloride, stir for 10 min, and then slowly add ammonia water to the above solution using a peristaltic pump with the pump speed controlled at 5 ml / min to generate a precipitate suspension with a pH of 1.2, recorded as D1.
[0141] Zirconium sol preparation comparative example 2
[0142] 35.38 g of ZrOCl2·8H2O was added to a beaker, and 9.77 g of a 45 wt % sodium hydroxide solution was added in a molar ratio of Zr to sodium hydroxide of 1:1, and then stirred at 60°C for 60 min to obtain a first contact product after the reaction, and then heated at 40°C in a ratio of Zr:H + =1:1.5 ratio, add 19.41g of hydrochloric acid with a concentration of 31% by weight, and then stir at a temperature of 40°C for 60min to obtain a second contact material, and then heat at a temperature of 40°C according to Zr:H + =1:1.5 ratio, add 19.41g of hydrochloric acid with a concentration of 31wt% (wt% means weight%) to the second contact material, stir at 40°C for 60min, and obtain zirconium sol D2.
[0143] Zirconium sol preparation comparative example 3
[0144] Zirconium sol D1 was prepared according to the preparation method of zirconium sol preparation comparative example 1, dried at 120° C. / 12 h, and then calcined at 600° C. for 4 h to obtain zirconium oxide powder D3.
[0145] The properties of the zirconium sols prepared in the zirconium sol preparation examples 1-3 and the zirconium sol preparation comparative examples 1-3 are shown in Table 1.
[0146] Table 1
[0147] Zirconium sol preparation example number 1 2 3 Comparative Example 1 Comparative Example 2 Zirconium sol number A1 A2 A3 D1 D2 <![CDATA[ZrO2, mass %]]> 10.8 11.9 11.3 13.4 16.3 pH 2.5 2.5 2.5 1.2 2.5 Molar ratio of alkali cation to Zr 2 1.67 1.74 0.6 1 Molar ratio of stabilizer to Zr 4 4 4 0 0 Average particle size, nm 10 9.8 9.7 Particle size range, nm 8-10 8-10 8-10 Concentration, % 95 93 92 Ratio of monoclinic to tetragonal phase* 0.4:1 0.35:1 0.3:1
[0148] * Samples were dried at 100°C for 6 h and calcined at 600°C for 4 h.
[0149] Catalyst Preparation Examples 1-3
[0150] The catalyst was prepared according to the following method. The catalyst formula is shown in Table 2:
[0151] (1) Preparation of phosphate aluminum colloid: Pseudoboehmite, kaolin and water are slurried and dispersed into a slurry with a solid content of 15 wt% (the weight ratio of clay on a dry basis to pseudoboehmite on an Al2O3 basis is 1:1); concentrated phosphoric acid (H3PO4 concentration of 85 wt%) is added to the slurry at a weight ratio of P / Al=3 while stirring, and the mixture is reacted at 70°C for 30 minutes to obtain a phosphate aluminum sol.
[0152] (2) First, kaolin is slurried to obtain a kaolin slurry with a solid content of 20 wt %, and DASY molecular sieve and ZSP-3 molecular sieve are taken, slurried separately with water, and dispersed with a homogenizer to obtain DASY molecular sieve slurry with a solid content of 35 wt % and ZSP-3 molecular sieve slurry with a solid content of 35 wt %, respectively; the kaolin slurry, DASY molecular sieve slurry, molecular sieve slurry and molecular sieve slurry are mixed and stirred, and then acidified aluminum stone with a solid content of 10 wt % (wherein the molar ratio of HCl to pseudo-boehmite calculated as Al2O3 (acid-aluminum ratio) is 0.2) is added, and stirred for 10 min to obtain a first catalyst mixed slurry; zirconium sol and phosphoaluminum sol are mixed, and then added to the above-mentioned first catalyst mixed slurry, and stirred for 30 min to obtain a second catalyst slurry; the second catalyst slurry is spray-dried to obtain catalyst microspheres, and the obtained catalyst microspheres are calcined at 500° C. for 2 hours, and then washed once with ammonium sulfate with a catalyst dry weight of 6% to obtain a catalytic cracking catalyst.
[0153] Catalyst Preparation Examples 4-6 were prepared according to the following method:
[0154] The catalyst formula is shown in Table 2:
[0155] (1) Preparation of phosphoaluminum gel: Pseudoboehmite, kaolin and water are slurried and dispersed into a slurry with a solid content of 15 wt% (the weight ratio of clay on a dry basis to pseudoboehmite on an Al2O3 basis is 1:1). Concentrated phosphoric acid (concentration 85 wt%) is added to the slurry at a weight ratio of P / Al=4 under stirring, and the mixture is reacted at 80°C for 20 minutes to obtain phosphoaluminum gel.
[0156] (2) First, slurry the kaolin to prepare a slurry with a solid content of 20% by weight, take DASY molecular sieve and ZSP-3 molecular sieve, add water to slurry respectively, disperse with a homogenizer, and obtain DASY molecular sieve slurry and ZSP-3 molecular sieve slurry with a solid content of 35% by weight; mix the kaolin slurry, DASY molecular sieve slurry and ZSP-3 molecular sieve slurry, stir, then add acidified aluminum stone with a solid content of 10% by weight (acidified with hydrochloric acid, acid-aluminum ratio of 0.2), stir for 10 minutes, and obtain a slurry containing molecular sieve and kaolin; after mixing zirconium sol and phosphorus aluminum sol, add them to the above slurry containing molecular sieve and kaolin, stir for 30 minutes, and obtain a catalyst slurry. The catalyst slurry is spray-dried, and the obtained catalyst microspheres are roasted at 500°C for 2 hours, and then washed once with ammonium sulfate with a catalyst dry weight of 6% to obtain a catalytic cracking catalyst.
[0157] Table 2
[0158] Catalyst No. C1 C2 C3 C4 C5 C6 DB1 DB2 DB3 DB4 DB5 DB6 Kaolin 30 30 30 30 40 20 40 40 40 40 40 40 DASY 1 5 9 5 5 5 5 5 5 5 5 5 ZSP-3 29 25 21 25 20 35 20 20 20 20 20 20 aluminite 5 10 8 10 15 8 30 25 20 15 15 15 Zirconium sol number A1 A2 A3 A2 A1 A3 A1 D1 D2 D3 Zirconium sol 5 5 10 20 5 12 5 5 5 5 Phosphate aluminum gel 25 17 18 5 10 10 10 10 10 10 Aluminum sol 5 8 4 5 5 10 5 5 5 5 5 5
[0159] The formula in Table 2 is in parts by weight, wherein zirconium sol is calculated as ZrO2, aluminum oxide and aluminum sol are calculated as Al2O3, and other components are calculated on a dry basis.
[0160] Catalyst Preparation Comparative Examples 1-6
[0161] The catalyst was prepared according to the method of catalyst preparation examples 4-6. The formulation is shown in Table 2. The physicochemical properties and evaluation results of the catalyst are shown in Table 3.
[0162] Catalyst Evaluation:
[0163] The catalyst was deactivated by aging at 800°C and 100% steam for 12 hours. The evaluation was conducted on a fixed fluidized bed microreactor ACE. The feedstock oil was Wu-mixed feedstock oil (composition and physical properties are shown in Table 3). The evaluation conditions were: reaction temperature of 550°C, catalyst-to-oil ratio (weight) of 6, and WHSV of 16h. -1 The results are listed in Table 4.
[0164] Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield
[0165] Light olefin selectivity = (ethylene yield + propylene yield) / conversion rate
[0166] Ethylene concentration = ethylene yield / dry gas yield
[0167] Propylene concentration = Propylene yield / Liquefied gas yield
[0168] Table 3
[0169]
[0170]
[0171] From the results in Table 4, it can be seen that the catalytic cracking catalyst provided by the present invention has a significantly smaller wear index, that is, the wear strength is improved. In the catalytic cracking reaction, the conversion rate is further improved, the selectivity of light olefins is increased, and the concentrations of ethylene and propylene are increased.
[0172] Molecular sieve preparation example 1
[0173] 100 kg of pulverized metakaolin powder was stirred and added with 400 kg of sodium silicate solution (containing 20.05 wt% SiO2, 6.41 wt% Na2O), 60 kg of directing agent and 100 kg of 5 wt% sodium hydroxide solution. The mixture was heated to 95°C and stirred at a constant temperature. After 8 hours, 10 kg of solid silica gel (Type A, from Qingdao Ocean Chemical Group Special Silica Gel Factory) was added and crystallized for 12 hours. The stirring speed during the addition and crystallization was 400 rpm. After the crystallization was completed, the crystallization tank was quenched, filtered and washed with water until the pH value of the washing liquid was less than 10. The mixture was dried at 120°C for 2 hours to obtain zeolite material Y-1. Y-1 was measured by X-ray diffraction method, and the crystallinity by peak height method, the K1 value of the ratio of the crystallinity by peak height method to the crystallinity by peak area method, the silicon-aluminum ratio determined by unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by unit cell constant a0 to the silicon-aluminum ratio determined by chemical method, and the medium and macro porosity are shown in Table B1.
[0174] Molecular sieve preparation example 2
[0175] According to the method of preparing the molecular sieve in Example 1, 100 kg of pulverized metakaolin powder was stirred and added with 380 kg of sodium silicate solution (containing 20.05% by weight of SiO2 and 6.41% by weight of Na2O), 60 kg of directing agent, and 100 kg of sodium hydroxide solution with a concentration of 5% by weight. The mixture was heated to 93°C and stirred at a constant temperature. After 8 hours, 15 kg of solid silica gel (special silica gel factory of Qingdao Ocean Chemical Group, type A) was added and crystallized for 14 hours. The stirring speed during the addition and crystallization was 400 rpm. After the crystallization was completed, the crystallization tank was quenched, filtered, and washed with water until the pH value of the washing liquid was less than 10. Dry at 120°C for 2 hours to obtain zeolite material Y-2. Y-2 was measured by X-ray diffraction method, and the crystallinity by peak height method, the K1 value of the ratio of the crystallinity by peak height method to the crystallinity by peak area method, the silicon-aluminum ratio determined by unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by unit cell constant a0 to the silicon-aluminum ratio determined by chemical method, and the medium and macro porosity are shown in Table B1.
[0176] Molecular sieve preparation example 3
[0177] According to the method of preparing the molecular sieve in Example 1, 100 kg of pulverized metakaolin powder was stirred and added with 360 kg of sodium silicate solution (containing 20.05 wt% SiO2, 6.41 wt% Na2O), 60 kg of directing agent, and 100 kg of sodium hydroxide solution with a concentration of 5 wt%. The mixture was heated to 95°C and stirred at a constant temperature. After 8 hours, 20 kg of solid silica gel (Special Silica Gel Factory of Qingdao Ocean Chemical Group, Type A) was added and crystallized for 16 hours. The stirring speed during the addition and crystallization was 400 rpm. After the crystallization was completed, the crystallization tank was quenched, filtered, and washed with water until the pH value of the washing liquid was less than 10. Dry at 120°C for 2 hours to obtain zeolite material Y-3. Y-3 was measured by X-ray diffraction method, and the crystallinity by peak height method, the K1 value of the ratio of the crystallinity by peak height method to the crystallinity by peak area method, the silicon-aluminum ratio determined by unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by unit cell constant a0 to the silicon-aluminum ratio determined by chemical method, and the medium and macro porosity are shown in Table B1.
[0178] Molecular sieve preparation comparative example 1
[0179] This comparative example illustrates the situation where two silicon sources are added into the reaction system at one time.
[0180] According to the method of preparing the molecular sieve in Example 1, 100 kg of pulverized metakaolin powder was stirred and added with 400 kg of sodium silicate solution (containing 20.05 wt% SiO2, 6.41 wt% Na2O), 60 kg of directing agent, 105 kg of 5 wt% sodium hydroxide solution, and 10 kg of solid silica gel (Qingdao Ocean Chemical Group Special Silica Gel Factory, Type A). The temperature was raised to 94°C and stirred at a constant temperature for 24 hours. The stirring speed during the addition and crystallization was 400 rpm. After the crystallization was completed, the crystallization tank was quenched, filtered, and washed with water until the pH value of the washing liquid was less than 10. Dry at 120°C for 2 hours to obtain the zeolite material DY-1. The crystallinity of DY-1 measured by X-ray diffraction method, the K1 value of the ratio of the crystallinity of the peak height method to the crystallinity of the peak area method, the silicon-aluminum ratio determined by the unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by the unit cell constant a0 to the silicon-aluminum ratio determined by the chemical method, and the medium-macro porosity are shown in Table B1. DY-1 has low crystallinity and contains impurities.
[0181] Molecular sieve preparation comparative example 2
[0182] This comparative example illustrates the case where no second silicon source is added.
[0183] According to the method of molecular sieve preparation example 1, 100 kg of pulverized metakaolin powder was stirred and added with 400 kg of sodium silicate solution (containing 20.05 wt% SiO2, 6.41 wt% Na2O), 60 kg of directing agent, and 100 kg of sodium hydroxide solution with a concentration of 5 wt%. The temperature was raised to 94°C and stirred at a constant temperature for 24 hours. The stirring speed during the addition and crystallization was 400 rpm. After the crystallization was completed, the crystallization tank was quenched, filtered, and washed with water until the pH value of the washing liquid was less than 10. Dry at 120°C for 2 hours to obtain zeolite DY-2. The crystallinity of DY-2 measured by the X-ray diffraction method, the K1 value of the ratio of the crystallinity of the peak height method to the crystallinity of the peak area method, the silicon-aluminum ratio determined by the unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by the unit cell constant a0 to the silicon-aluminum ratio determined by the chemical method, and the medium and macro porosity are shown in Table B1. The crystallinity of DY-2 is not bad, but the silicon-aluminum ratio is low.
[0184] Table B1
[0185]
[0186] Catalyst Preparation Example B1
[0187] (1) Preparation of ion-modified ultra-stable NSY molecular sieves:
[0188] The Y-1 molecular sieve prepared in the above molecular sieve preparation example 1 was contacted with silicon tetrachloride gas according to a weight ratio of SiCl4: Y-1 molecular sieve on a dry basis = 0.4:1, the reaction temperature was 450°C, the reaction time was 2 hours, washed and filtered, and a gas phase ultra-stable NSY type molecular sieve CY-1 with a unit cell constant of 2.456 was obtained; the CY-1 molecular sieve was slurried with deionized water to form a CY-1 molecular sieve slurry with a solid content of 10% by weight; lanthanum chloride was taken, and water was added to slurry to form a lanthanum chloride solution with a La2O3 concentration of 5% by weight; the lanthanum chloride solution was added to the CY-1 molecular sieve slurry, the weight ratio of lanthanum chloride (based on La2O3) to molecular sieve (based on a dry basis) was 1:20, stirred at 70°C for 1 hour, filtered, washed, dried at 150°C for 8 hours, and calcined at 500°C for 4 hours; then washed with an ammonium sulfate solution, wherein the weight ratio of ammonium sulfate to the molecular sieve dry basis was 1:20, and the obtained molecular sieve was recorded as UNSY-1;
[0189] (2) Preparation of phosphoaluminum gel: Pseudo-boehmite, kaolin and water are slurried to obtain a slurry with a solid content of 15 wt %. Concentrated phosphoric acid (concentration 85 wt %) is added to the slurry at a weight ratio of P / Al=3 under stirring, and the mixture is reacted at 70° C. for 30 minutes to obtain phosphoaluminum gel;
[0190] (3) Catalyst preparation: According to the catalyst formula in Table B2, kaolin was first slurried to prepare a kaolin slurry with a solid content of 20 wt %; rare earth modified ultrastable NSY molecular sieve UNSY-1 and ZSP-3 molecular sieve were taken, slurried separately with water, and dispersed with a homogenizer to obtain UNSY-1 molecular sieve slurry with a solid content of 35 wt % and ZSP-3 molecular sieve slurry with a solid content of 35 wt %; the kaolin slurry, UNSY-1 molecular sieve slurry and ZSP-3 molecular sieve slurry were mixed and stirred, and then acidified aluminum stone with a solid content of 10 wt % (acid-aluminum ratio 0.2 molar ratio) was added and stirred for 10 min, and then zirconium sol A1 and the above-mentioned aluminum phosphate gel were added, stirred for 30 min, and spray-dried to obtain catalyst microspheres, and the obtained catalyst microspheres were calcined at 500° C. for 2 hours to obtain catalytic cracking catalyst BC1.
[0191] Catalyst Preparation Examples B2-B3
[0192] The catalyst was prepared according to the method of Catalyst Example 1, and the catalyst formula is shown in Table B2.
[0193] Catalyst Example B4
[0194] (1) Preparation Example 4 of ion-modified ultrastable NSY molecular sieve:
[0195] The molecular sieve prepared in the above-mentioned NSY molecular sieve preparation example 1 was placed at 650°C and 100% by volume of water vapor for 12 hours to obtain an ultra-stable NSY type molecular sieve, which was recorded as CY-4, and the unit cell constant was 2.455nm; the CY-4 molecular sieve was added with deionized water to be slurried to obtain a slurry with a solid content of 10% by weight, lanthanum chloride was taken, water was added to be slurried to form a lanthanum chloride solution with a La2O3 concentration of 5% by weight, and the lanthanum chloride solution was added to the CY-4 molecular sieve slurry, the weight ratio of lanthanum chloride (calculated as La2O3) to molecular sieve (calculated on a dry basis) was 1:20, stirred at 70°C for 1h, filtered and washed, dried at 150°C for 8h, and calcined at 500°C for 4h. The rare earth modified ultra-stable NSY molecular sieve was obtained, and then an ammonium sulfate solution was added for washing, wherein the weight ratio of ammonium sulfate to the molecular sieve dry basis was 1:20, and the obtained molecular sieve was recorded as U-NSY4.
[0196] (2) Preparation of phosphate aluminum colloid: Pseudo-boehmite, kaolin and water are slurried and dispersed into a slurry with a solid content of 15 wt% (the weight ratio of clay on a dry basis to alumina source on an Al2O3 basis is 1:1). Concentrated phosphoric acid is added to the slurry at a weight ratio of P / Al=4 while stirring, and the reaction is carried out by stirring at 80°C for 20 minutes to obtain a phosphate aluminum sol.
[0197] (3) Catalyst preparation: According to the catalyst formula in Table 1, first slurry kaolin to obtain a kaolin slurry with a solid content of 40% by weight, and then add aluminum sol to slurry; take rare earth modified NSY molecular sieve and ZSP-3 molecular sieve, add water to slurry, disperse with a homogenizer, and obtain slurry solid contents of 35% by weight of NSY molecular sieve slurry and ZSP-3 molecular sieve slurry; mix and stir the kaolin slurry, NSY molecular sieve slurry and ZSP-3 molecular sieve, and then add the phosphorus aluminum sol obtained in step (2) and stir for 10 minutes. Finally, add the aluminum sol to the above catalyst mixed slurry, stir for 30 minutes, spray dry, and calcine the obtained catalyst microspheres at 500°C for 2 hours to obtain catalytic cracking catalyst BC4.
[0198] Catalyst Preparation Examples B5-B6
[0199] The catalyst was prepared according to the method of catalyst preparation example B4, and the formula is shown in Table B2, wherein the modified NSY molecular sieve was prepared, and its preparation method was similar to that of example B4 except for the different rare earth content.
[0200] Catalyst Preparation Comparative Examples B1 and B2
[0201] The catalyst was prepared according to the method of catalyst preparation example B4, and the catalyst formula is shown in Table B2. The modified NSY molecular sieve corresponds to the modified molecular sieve obtained by modifying the molecular sieve in the molecular sieve preparation comparative example.
[0202] Catalyst Evaluation:
[0203] The catalyst was deactivated by aging at 800°C and 100% steam for 12 hours. The catalyst was evaluated on a fixed fluidized bed microreactor ACE. The feedstock oil was Wu-mixed feedstock oil (composition and physical properties are shown in Table 3). The evaluation conditions were: reaction temperature of 550°C, catalyst-to-oil ratio (weight) of 6, WHSV = 16h -1 The results are listed in Table B3.
[0204] Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield
[0205] Light olefin selectivity = (propylene + ethylene) yield / conversion rate × 100%
[0206]
[0207] Table B3
[0208] catalyst BC1 BC2 BC3 BC4 BC5 BC6 BDB5 BDB6 Wear index, m% / h 0.8 0.6 0.7 0.6 0.9 1 3.9 4.8 Product distribution / weight % Dry gas 4.93 4.79 4.48 4.35 4.55 5.28 4.25 4.58 Liquefied gas 35.97 36.85 35.66 34.44 34.51 36.41 32.55 33.27 Ethylene 2.29 2.25 2.02 1.91 1.73 2.45 1.55 1.62 Propylene 19.58 19.52 18.83 18.16 17.92 22.35 14.63 14.27 <![CDATA[C5 + Gasoline]]> 31.46 35.03 34.67 33.94 32.93 32.42 29.67 28.71 Circulation oil 12.35 9.02 9.81 10.99 11.33 10.24 14.21 14.13 Oil slurry 10.11 8.13 9.15 9.85 10.86 9.04 11.87 11.77 Coke 5.18 6.18 6.23 6.43 5.82 6.61 7.45 7.54 Conversion rate 77.54 82.85 81.04 79.16 77.81 80.72 73.92 74.1 Light olefin selectivity 28.20 26.28 25.73 25.35 25.25 30.72 21.89 21.44 Propylene concentration 54.43 52.97 52.80 52.73 51.93 61.38 44.95 42.89 Ethylene concentration 46.45 46.97 45.09 43.91 38.02 46.40 36.47 35.37 Coke selectivity 6.68 7.46 7.69 8.12 7.48 8.19 10.08 10.18 Coke Factor 1.50 1.28 1.46 1.69 1.66 1.58 2.63 2.64
[0209] Coke factor (coking factor) = coke yield × (1-conversion rate) / conversion rate × 100.
[0210] It can be seen from Table B3 that the catalytic cracking catalyst provided by the present invention has a significantly smaller wear index, that is, high strength. When used in catalytic cracking reactions, the conversion rate is improved, the selectivity of light olefins is increased, the concentrations of propylene and ethylene are increased, the coke selectivity is improved, and the coke factor is reduced.
[0211] As can be seen from Table 4 and Table B3, the use of modified NSY molecular sieve has lower coke selectivity than the use of other Y molecular sieves when other compositions are similar, and the catalyst activity is higher, and the propylene concentration in the liquefied gas is higher.
Claims
1. A catalytic cracking catalyst for producing more light olefins, comprising: 10 wt%-60 wt% of cracking active components on a dry basis, 20 wt%-60 wt% of a binder on a dry basis, and 0 wt%-70 wt% of a second clay on a dry basis; wherein, based on the dry basis weight of the binder, the binder comprises 1 wt%-50 wt% of zirconium sol, 50 wt%-99 wt% of a phosphorus aluminum inorganic binder, and 0-45 wt% of a third binder; The cracking active component comprises a first molecular sieve and an optional second molecular sieve, wherein the first molecular sieve is a five-membered ring structure molecular sieve; on a dry basis, the cracking active component contains 70-100% by weight of the first molecular sieve and 0-30% by weight of the second molecular sieve; The zirconium sol comprises 0.5 mass % to 20 mass % ZrO2, a stabilizer, an alkali cation and water, wherein the molar ratio of the stabilizer to Zr is 1-6, the molar ratio of the alkali cation to Zr is 1-8, the pH value of the zirconium sol is 1.5-5, the alkali cation is an ammonium ion or a nitrogen-containing cation formed by hydrolysis of a water-soluble organic base, the stabilizer is one or more of glycolic acid, oxalic acid, acetic acid, malonic acid, malic acid, tartaric acid, succinic acid, adipic acid, maleic acid, itaconic acid and citric acid, the zirconium sol is dried at 100° C. for 6 hours, calcined at 600° C. for 2-6 hours for heat treatment, the monoclinic phase and the tetragonal phase of the obtained product coexist, and the ratio of the monoclinic phase to the tetragonal phase is 0.05-0.6:1; and / or the zirconium sol is dried at 100° C. for 6 hours, calcined at 800° C. for 2-6 hours for heat treatment, and ZrO2 in the obtained product exists in the tetragonal phase; The phosphorus-aluminum inorganic binder contains 15-40 wt% of an alumina source component in terms of Al2O3, 45-80 wt% of a phosphorus component in terms of P2O5, and 0-40 wt% of a first clay in terms of dry basis, with a P / Al weight ratio of 1-6, a pH value of 1-3.5, and a solid content of 15-60 wt%.
2. The catalytic cracking catalyst according to claim 1, characterized in that: The third binder is selected from one or more of silica sol, alumina sol, silica-alumina gel, acidified alumina, and metal-modified alumina.
3. The catalytic cracking catalyst according to claim 1, characterized in that: The first molecular sieve is one or more of MFI structure molecular sieve, BEA structure molecular sieve and mordenite.
4. The catalytic cracking catalyst according to claim 1, characterized in that: The second molecular sieve is a Y-type molecular sieve, and the rare earth content in the Y-type molecular sieve is 0-20% by weight.
5. The catalytic cracking catalyst according to claim 4, characterized in that: The rare earth content in the Y-type molecular sieve is 0-12% by weight.
6. The catalytic cracking catalyst according to claim 4, characterized in that: The Y-type molecular sieve is one or more of DASY molecular sieve, DASY molecular sieve containing rare earth, USY molecular sieve, USY molecular sieve containing rare earth, REY molecular sieve, HY molecular sieve, REHY molecular sieve, and Y-type molecular sieve synthesized by in-situ crystallization of modified kaolin.
7. The catalytic cracking catalyst according to claim 1, characterized in that: The second molecular sieve is an ion-modified ultra-stable NSY molecular sieve; based on the weight of the catalytic cracking catalyst, the content of the ion-modified ultra-stable NSY molecular sieve in the catalytic cracking catalyst is 1-10% by weight.
8. The catalytic cracking catalyst according to claim 1, characterized in that: The second clay is one or more of kaolin, montmorillonite, diatomite, halloysite, pseudo-halloysite, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite; the first clay is one or more of kaolin, montmorillonite, diatomite, halloysite, pseudo-halloysite, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite.
9. The catalytic cracking catalyst according to claim 1, characterized in that: The method for preparing the phosphorus-aluminum inorganic binder comprises: (1) Slurrying an alumina source, a first clay and water to form a slurry with a solid content of 8-45 wt %; the alumina source is aluminum hydroxide and / or aluminum oxide that can be colloided by acid, and the weight ratio of the first clay calculated on a dry basis to the alumina source calculated on Al2O3 is 0-40:15-40; (2) adding concentrated phosphoric acid to the slurry obtained in step (1) under stirring in a weight ratio of P / Al = 1-6; wherein the concentration of the concentrated phosphoric acid is 50 -98 wt %; (3) The slurry obtained in step (2) is reacted at 50-99°C for 15-90 minutes.
10. The catalytic cracking catalyst according to claim 9, characterized in that: The phosphorus-aluminum inorganic binder comprises 15-35 wt % of Al2O3 derived from the alumina source, 50-75 wt % of P2O5 and 5-30 wt % of the first clay on a dry basis.
11. The catalytic cracking catalyst according to claim 1, characterized in that: The P / Al weight ratio is 2-5.
12. The catalytic cracking catalyst according to claim 9, characterized in that: The alumina source is one or more of ρ-alumina, χ-alumina, η-alumina, γ-alumina, κ-alumina, δ-alumina, θ-alumina, gibbsite, diaspore, nordstromite, diaspore, boehmite and pseudo-boehmite.
13. The catalytic cracking catalyst according to claim 1, characterized in that: The particle size of the zirconium sol is between 5nm and 15nm, the average particle size is 10±2nm, and the concentration is above 90%.
14. The catalytic cracking catalyst according to claim 1, characterized in that: The stabilizer is one or more of oxalic acid, acetic acid or citric acid.
15. The catalytic cracking catalyst according to claim 1, characterized in that: The water-soluble organic base is one or more of methylamine, dimethylamine, trimethylamine, methanolamine, dimethanolamine, trimethanolamine, triethylamine, ethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetraisopropylammonium hydroxide, tetrabutylammonium hydroxide, monomethyltriethylammonium hydroxide, monomethyltriethanolammonium hydroxide, and monomethyltributylammonium hydroxide.
16. The catalytic cracking catalyst according to claim 1, characterized in that: The zirconium sol further contains inorganic acid radicals and / or alcohols, and the molar ratio of the inorganic acid radicals and / or alcohols to Zr is 1-6:
1.
17. The catalytic cracking catalyst according to claim 16, characterized in that: The inorganic acid radical is one or more of sulfate, chloride, and nitrate, and the alcohol is one or more of methanol, ethanol, propanol, and butanol.
18. The catalytic cracking catalyst according to claim 1, characterized in that: The pH value of the zirconium sol is 2-4.
19. The catalytic cracking catalyst according to claim 1, characterized in that: The zirconium sol is prepared by a preparation method comprising the following steps: (1) preparing a zirconium source solution, wherein the concentration of the zirconium source solution is 0.5 mass % to 20 mass % based on ZrO2; (2) adding a stabilizer to the zirconium source solution to obtain a first mixed solution; wherein the molar ratio of the stabilizer to zirconium is 1-6: (3) At room temperature-50° C., adding alkali solution to the first mixed solution to obtain zirconium sol, wherein the amount of alkali solution is such that the pH value of the zirconium sol is 1.5-5.
20. The catalytic cracking catalyst according to claim 7, characterized in that: The preparation method of the ion-modified ultrastable NSY molecular sieve comprises the following steps: (1) calcining kaolin at 500-900°C to dehydrate it and convert it into metakaolin, which is then crushed to produce metakaolin powder with a particle size of less than 10 microns; (2) adding sodium silicate, a directing agent, a sodium hydroxide solution and water to the metakaolin powder to prepare a reaction raw material A with a ratio of (1-2.5) Na2O:Al2O3:(4-9)SiO2:(40-100)H2O, wherein the mass ratio of the directing agent to the metakaolin is 0.01-1.0; (3) crystallizing the reaction material A at 88-98° C. under stirring, and adding a second silicon source after the crystallization time reaches 1-70 hours to obtain the reaction material B, wherein the second silicon source accounts for 0.1% to 10% by weight of the total silicon input, calculated as silicon oxide; (4) crystallizing the reaction raw material B at 88-98° C. under stirring and recovering the product to obtain the NSY molecular sieve synthesized by in-situ crystallization of kaolin; (5) The NSY molecular sieve synthesized by in-situ crystallization of kaolin is subjected to ion exchange and ultra-stabilization treatment.
21. A method for preparing the catalytic cracking catalyst according to any one of claims 1 to 20, comprising: The cracking active component, binder, water and optional clay are formed into a slurry and spray dried.
22. The method for preparing the catalytic cracking catalyst according to claim 21, characterized in that: The following steps are involved: (S1) obtaining a molecular sieve slurry, (S2) obtaining a second clay slurry, (S3) obtaining zirconium sol, (S4) obtaining a phosphorus-aluminum inorganic binder, (S5) mixing the molecular sieve slurry, the second clay slurry, the zirconium sol, the phosphorus-aluminum inorganic binder and an optional third binder; (S6) spray drying the slurry obtained in step (S5).
23. A catalytic cracking method, comprising the step of contacting heavy oil with the catalytic cracking catalyst according to any one of claims 1 to 20 for reaction.
Citation Information
Patent Citations
Pyrolysis catalyst and preparation method thereof
CN102211039B
Inorganic binder containing phosphorus and aluminum compounds
CN102847547A
P-containing hydrocarbon cracking catalyst and its preparation
CN1076714A
Catalytic cracking catalyst and preparation method thereof
CN108927211A
Modification method of molecular sieve, modified molecular sieve and application of modified molecular sieve
CN108928833A