Cyanide on demand
By using the macro structure of structured catalysts and conductive materials in the reactor system for resistance heating, the high investment and high risk of hydrogen cyanide production process is solved, and compact and efficient hydrogen cyanide and nitrile production is achieved, reducing the number of Storage and transportation needs and environmental emissions.
Patent Information
- Application Number
- CN202080067396.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-06
- Filing Date
- 2020-09-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-09-24
AI Technical Summary
The existing hydrogen cyanide (HCN) production process has high investment and is highly dangerous, and it is difficult to achieve on-demand production, resulting in an increase in storage and transportation demand, and a large emissions that are harmful to the climate.
A reactor system was designed to utilize the macro structure of structured catalysts and conductive materials to realize the BMA reaction through resistance heating to produce hydrogen cyanide and nitrile. The system includes a pressure-resistant shell, a thermal insulation layer and a conductor, allowing the raw gas to be in the catalyst. The reaction is carried out on and the catalyst is heated to high temperature by electrical connection.
The compact and efficient hydrogen cyanide and nitrile production is achieved, reducing storage and transportation needs, reducing environmental hazards, and can be quickly started and shut down, suitable for non-fixed facilities and reduce processing risks.
Smart Images

Figure CN114430699B_ABST
Abstract
Description
Technical Field
[0001] A reactor system and method for producing hydrogen cyanide and / or nitrile by a BMA (hydrocyanic acid from methane and ammonia; also known as the Degussa process) reaction and / or nitrile synthesis from a feed gas comprising an alkane such as methane and ammonia is provided, wherein heat for the endothermic BMA reaction is provided by resistive heating. Background Art
[0002] Hydrogen cyanide is used in the chemical industry to produce intermediate chemicals such as acrylonitrile, methyl methacrylate and adiponitrile. However, hydrogen cyanide HCN is difficult to produce and often requires high temperature chemistry. A simple way to produce cyanide is the BMA (hydrocyanic acid from methane and ammonia) process, in which methane and ammonia are reacted at around 1200-1300°C, usually in a combustion reaction unit.
[0003] However, due to the high investment in the process compared to the relatively small demand for hydrogen cyanide, there is little industrial application of the process, with only four plants in operation in 2003. Due to the high toxicity of hydrogen cyanide, strict regulations apply to its production, storage and transportation.
[0004] It is therefore desirable to produce hydrogen cyanide in an "on-demand" manner at the location where it is needed. Ideally, HCN production would use readily available starting materials that are cheap, safe, and common in industrial chemical plants. In this way, storage and transportation of hydrogen cyanide could be reduced or even completely eliminated. In addition, the possibility of rapid startup and shutdown would also reduce the need for HCN storage.
[0005] It is also desirable that the reactor system be compact and operational equipment that allows for less hazardous handling of hydrogen cyanide and / or nitrile.Another advantage of the technology is that overall emissions of carbon dioxide and other climate-damaging emissions can be greatly reduced, especially if the electricity used in the reactor system comes from renewable sources.
[0006] Systems and methods for steam methane reforming are described in co-pending patent application PCT / EP2019 / 062423. Systems and methods for performing endothermic catalytic reactions are described in co-pending patent application PCT / EP2019 / 062424. Summary of the invention
[0007] Thus, in a first aspect, the present invention relates to a reactor system for reacting a feed gas comprising alkanes, in particular methane, and ammonia, in the presence of a catalyst, in particular a BMA catalyst, for example under BMA reaction conditions, in particular a BMA reaction, to produce hydrogen cyanide and / or nitrile, the reactor system comprising:
[0008] - a source of feed gas comprising an alkane such as methane and ammonia;
[0009] - a structured catalyst arranged to catalyze a reaction of the feed gas, the structured catalyst comprising macrostructures of an electrically conductive material, the macrostructures supporting a ceramic coating, wherein the ceramic coating supports a catalytically active material;
[0010] - a pressure-resistant shell containing the structured catalyst, the pressure-resistant shell comprising an inlet for the feed gas to enter and an outlet for the product gas to exit, wherein the inlet is located so that the feed gas enters the structured catalyst at a first end of the structured catalyst and the product gas leaves the structured catalyst from a second end of the structured catalyst;
[0011] - a thermal insulation layer between the structured catalyst and the pressure shell;
[0012] - at least two conductors electrically connected to the structured catalyst and to a power source disposed outside the pressure vessel, wherein the power source is sized to heat at least a portion of the structured catalyst to a temperature of at least 500° C. by passing an electric current through the macrostructure, wherein the at least two conductors are connected to the structured catalyst at a location on the structured catalyst closer to the first end of the structured catalyst than to the second end of the structured catalyst, and wherein the structured catalyst is configured to direct an electric current from one conductor substantially toward the second end of the structured catalyst and back to a second of the at least two conductors;
[0013] - an outlet for a product stream comprising hydrogen cyanide and / or nitrile.
[0014] In another aspect, there is provided a method for reacting a feed gas comprising an alkane such as methane and ammonia in the presence of a catalyst (e.g., under BMA reaction conditions) to produce hydrogen cyanide and / or nitrile in a reactor system, the reactor system comprising a pressure vessel containing a structured catalyst, the structured catalyst being arranged to catalyze the endothermic reaction of the feed gas, the structured catalyst comprising macrostructures of an electrically conductive material, the macrostructures supporting a ceramic coating, wherein the ceramic coating supports a catalytically active material; wherein the reactor system is provided with a thermal insulation layer between the structured catalyst and the pressure vessel; the method comprising the steps of:
[0015] - pressurizing the raw gas,
[0016] - supplying the pressurized feed gas to the pressure shell through an inlet, the inlet being located so that the feed gas enters the structured catalyst at a first end of the structured catalyst; reacting the feed gas on the structured catalyst; and discharging product gas from the pressure shell, wherein the product gas leaves the structured catalyst from a second end of the structured catalyst;
[0017] - providing electrical power via an electrical conductor connected from a power source positioned outside the pressure vessel to the structured catalyst, allowing electrical current to run through the macrostructure, thereby heating at least a portion of the structured catalyst to a temperature of at least 500° C., wherein the at least two conductors are connected to the structured catalyst at a location on the structured catalyst closer to the first end of the structured catalyst than to the second end of the structured catalyst, and wherein the structured catalyst is configured to direct electrical current from one conductor substantially toward the second end of the structured catalyst and back to a second of the at least two conductors, thereby heating at least a portion of the structured catalyst to a temperature sufficient to cause the feed gas to undergo a BMA reaction on the structured catalyst, and
[0018] - product gas comprising hydrogen cyanide and / or nitrile is discharged from the reactor system.
[0019] In another aspect, a method is provided for rapidly switching a metal-catalyzed reaction of a feed gas comprising an alkane such as methane and ammonia from a first steady-state reaction condition (A) to a second steady-state reaction condition (B) or from a second steady-state reaction condition (B) to a first steady-state reaction condition (A) in a reactor system as described herein; the method comprising the steps of:
[0020] In the first steady-state reaction condition (A):
[0021] - supplying the feed gas to the reactor system at a first total flow rate, and
[0022] - providing a first electrical power via an electrical conductor connecting a power source placed outside the pressure vessel to the structured catalyst, thereby allowing a first current to flow through the conductive material,
[0023] thereby heating at least a portion of the structured catalyst to a first temperature at which the feed gas is converted over the structured catalyst under the first steady-state reaction condition (A) into a first product gas mixture; and exhausting the first product gas from the reactor system;
[0024] And, in the second steady-state reaction condition (B):
[0025] - supplying the feed gas to the reactor system at a second total flow rate,
[0026] - providing a second electrical power via an electrical conductor connecting a power source placed outside the pressure vessel to the structured catalyst, thereby allowing a second current to flow through the conductive material,
[0027] Thereby, at least a portion of the structured catalyst is heated to a second temperature; at the second temperature, the feed gas is converted into a second product gas mixture on the structured catalyst under the second steady-state reaction condition (B); and the second product gas is discharged from the reactor system; wherein the second electrical power is higher than the first electrical power; and / or the second total flow rate is higher than the first total flow rate.
[0028] Further aspects of the invention are set out in the following detailed description, examples and appended claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1a shows a cross-section of one embodiment of a reactor system of the present invention having a structured catalyst comprising an array of macrostructures in cross-section;
[0030] Figure 1b Shows Figure 1a A reactor system wherein a portion of the pressure vessel and thermal insulation are removed;
[0031] Figure 2 is an enlarged view of a portion of a reactor system;
[0032] Figure 3a and 3b shows a schematic cross-section of one embodiment of a reactor system of the present invention comprising a structured catalyst;
[0033] Figure 4 and 5 An embodiment of a structured catalyst having an array of macrostructures is shown viewed from above and from the side, respectively;
[0034] Figure 6 An embodiment of a structured catalyst according to the present invention is shown;
[0035] Figure 7 and 8 An embodiment of a structured catalyst having a connector is shown;
[0036] Fig. 9 The equilibrium composition of CH4 (and NH3) and HCN is shown as a function of temperature when equimolar CH4 and NH3 feed gases are used at 5 barg. DETAILED DESCRIPTION
[0037] The present technology describes how electrically heated reactors can facilitate the task of producing hydrogen cyanide and / or nitrile via reactions in an on-demand process in a compact design.
[0038] The present technology can be used to synthesize hydrogen cyanide (HCN) and / or nitrile (RCN, where R is an alkyl group). When the alkane is methane, the catalyst is a BMA catalyst, and the product stream comprises hydrogen cyanide.
[0039] However, when the alkane is ethane or propane, nitrile can be produced under a similar principle, for example:
[0040]
[0041]
[0042] If the feed gas contains a mixture of methane and other alkanes, a product gas containing hydrogen cyanide and / or nitrile is obtained. Below, the present invention will be described for the synthesis of HCN via the BMA reaction. However, as mentioned above, the technology is also applicable to the synthesis of nitrile from alkanes.
[0043] The BMA reaction can be summarized as:
[0044]
[0045] Where ΔH R = 251 kJ / mol. Usually, a platinum (Pt) catalyst is used as the catalytically active material. The BMA process does not require O2 (as required by the Andrussow process, for example). Therefore, in the present technology, the feed gas usually does not contain oxygen.
[0046] The compact electroreactor using a monolithic catalyst can be easily operated and produces HCN when needed using an easy start-up principle. This provides a relatively inexpensive facility where HCN is produced only in the required amount, with little to no need for HCN storage, while also reducing or completely eliminating HCN transportation. The simple reactor equipment and simple operation of the BMA process make HCN production attractive in non-stationary facilities, which reduces the risk of HCN handling.
[0047] In addition, using electricity as a heat source allows for rapid startup and shutdown (on the order of minutes). This almost instantaneous switchover from standby to HCN production and back also reduces the need for HCN storage.
[0048] Thus, there is provided a reactor system for reacting a feed gas comprising an alkane such as methane and ammonia in the presence of a catalyst such as a BMA catalyst (e.g., under BMA reaction conditions) to produce hydrogen cyanide and / or nitrile, the reactor system comprising:
[0049] - a source of feed gas comprising alkanes and ammonia;
[0050] - a structured catalyst arranged to catalyze a reaction of the feed gas, the structured catalyst comprising macrostructures of an electrically conductive material, the macrostructures supporting a ceramic coating, wherein the ceramic coating supports a catalytically active material;
[0051] - a pressure-resistant shell containing the structured catalyst, the pressure-resistant shell comprising an inlet for the feed gas to enter and an outlet for the product gas to exit, wherein the inlet is located so that the feed gas enters the structured catalyst at a first end of the structured catalyst and the product gas leaves the structured catalyst from a second end of the structured catalyst;
[0052] - a thermal insulation layer between the structured catalyst and the pressure shell;
[0053] - at least two conductors electrically connected to the structured catalyst and to a power source disposed outside the pressure vessel, wherein the power source is sized to heat at least a portion of the structured catalyst to a temperature of at least 500° C. by passing an electric current through the macrostructure, wherein the at least two conductors are connected to the structured catalyst at a location on the structured catalyst closer to the first end of the structured catalyst than to the second end of the structured catalyst, and wherein the structured catalyst is configured to direct an electric current from one conductor substantially toward the second end of the structured catalyst and back to a second of the at least two conductors;
[0054] - An outlet for a product stream comprising hydrogen cyanide and / or nitrile.
[0055] In a preferred aspect, the alkane is methane, the catalyst is a BMA catalyst, and the product stream comprises hydrogen cyanide.
[0056] The layout of the reactor system allows for feeding pressurized feed gas to the reactor system at the inlet and directing the gas into the pressure vessel of the reactor system. Inside the pressure vessel, an arrangement of thermal insulation layers and inert materials are arranged to direct the feed gas through the structured catalyst where it will come into contact with the catalyst material, wherein the catalytically active material will promote the BMA reaction. Furthermore, heating of the structured catalyst will supply the required heat for the endothermic reaction. The product gas from the heated structured catalyst is directed to the reactor system outlet.
[0057] The close proximity between the catalytically active material and the electrically conductive material enables efficient heating of the catalytically active material by close proximity heat conduction from the electrically conductive material of the resistive heating. Thus, an important feature of the resistive heating process is that the energy is supplied within the object itself, rather than from an external heat source via thermal conduction, convection, and radiation. In addition, the hottest portion of the reactor system will be located within the pressure vessel of the reactor system. Preferably, the power source and the size of the structured catalyst are configured so that at least a portion of the structured catalyst reaches a temperature of at least 700°C, preferably at least 900°C, and more preferably at least 1000°C. The surface area of the electrically conductive material, the proportion of the electrically conductive material coated with the ceramic coating, the type and structure of the ceramic coating, and the amount and composition of the catalytically active catalyst material can be tailored to the specific reaction under given operating conditions.
[0058] The conductive material is suitably a macrostructure. As used herein, the term "macrostructure" is intended to mean a structure large enough to be seen with the naked eye without the need for a magnifying device. The size of the macrostructure is typically in the range of centimeters or even meters. It is advantageous to make the size of the macrostructure correspond at least in part to the internal dimensions of the pressure shell containing the structured catalyst, leaving room for the thermal insulation layer and the conductor. Two or more macrostructures can be connected to provide a macrostructure array, at least one of whose external dimensions is in the meter range, such as 2m or 5m. Such two or more macrostructures can be represented as a "macrostructure array". In this case, it is advantageous to make the size of the macrostructure array correspond at least in part to the internal dimensions of the pressure shell containing the structured catalyst (leaving room for the thermal insulation layer). A conceivable macrostructure array can occupy 0.1 to 10m 3 Or even larger volumes. The structured catalyst may comprise a single macrostructure or an array of macrostructures, wherein (one or more) macrostructures support a ceramic coating, and the ceramic coating supports a catalytically active material. In the array of macrostructures, the macrostructures may be electrically connected to each other; however, optionally, the macrostructures are not electrically connected to each other. Thus, the structured catalyst may comprise two or more macrostructures positioned adjacent to each other. (One or more) macrostructures may be extruded and sintered structures or 3D printed structures. 3D printed macrostructures may be provided with or without subsequent sintering.
[0059] The physical dimensions of the macrostructures may be any suitable dimensions; thus, the height may be smaller than the width of the macrostructure, or vice versa.
[0060] The macrostructure supports a ceramic coating, wherein the ceramic coating supports a catalytically active material. The term "macrostructure supporting a ceramic coating" means that the macrostructure is coated with a ceramic coating on at least a portion of the surface of the macrostructure. Thus, the term does not mean that all surfaces of the macrostructure are coated with the ceramic coating; in particular, there is no coating on at least the portion of the macrostructure that is electrically connected to the conductor. The coating is a ceramic material having pores in the structure that allow the catalytically active material to be supported on and within the coating. Advantageously, the catalytically active material comprises catalytically active particles having a size ranging from about 2 nm to about 250 nm.
[0061] Preferably, the macrostructure has been manufactured by extruding a mixture of powdered metal particles and a binder into an extruded structure and subsequently sintering the extruded structure to provide a material with a high geometric surface area per volume. Preferably, the extruded structure is sintered in a reducing atmosphere to provide the macrostructure. Alternatively, the macrostructure is 3D printed, a metal additive manufacturing melting process, i.e. a 3D printing process that does not require subsequent sintering, such as a powder bed fusion or direct energy deposition process. Examples of such powder bed fusion or direct energy deposition processes are laser beam, electron beam or plasma 3D printing processes. As another option, the macrostructure can be manufactured as a 3D metal structure by means of a binder-based metal additive manufacturing process and then sintered at a first temperature T1 in a non-oxidizing atmosphere, where T1>1000°C, to provide the macrostructure.
[0062] A ceramic coating, which may contain a catalytically active material, is provided to the macrostructure, followed by a second sintering in an oxidizing atmosphere to form a chemical bond between the ceramic coating and the macrostructure. Alternatively, the catalytically active material may be impregnated onto the ceramic coating after the second sintering. When a chemical bond is formed between the ceramic coating and the macrostructure, it is possible to have a particularly high thermal conductivity between the electrically heated macrostructure and the catalytically active material supported by the ceramic coating, thereby providing close and almost direct contact between the heat source and the catalytically active material of the structured catalyst. Due to the close proximity between the heat source and the catalytically active material, heat transfer is efficient, and thus the structured catalyst can be heated very efficiently. Therefore, a compact reactor system is possible in terms of gas processing per reactor system volume, and therefore the reactor system accommodating the structured catalyst can be compact.
[0063] As used herein, the terms "3D printing" and "3D printing" are intended to refer to metal additive manufacturing processes. Such metal additive manufacturing processes cover 3D printing processes in which material is joined to a structure under computer control to create a three-dimensional object, wherein the structure will be solidified, such as by sintering, to provide a macrostructure. Moreover, such metal additive manufacturing processes cover 3D printing processes that do not require subsequent sintering, such as powder bed fusion or direct energy deposition processes. Examples of such powder bed fusion or direct energy deposition processes are laser beam, electron beam or plasma 3D printing processes.
[0064] The reactor system does not require a furnace, which significantly reduces the overall size of the reactor.
[0065] The conductive material comprises Fe, Ni, Cu, Co, Cr, Al, Si or an alloy thereof. Such alloys may contain further elements, such as Mn, Y, Zr, C, Co, Mo or a combination thereof. Preferably, the conductive material comprises Fe, Cr, Al or an alloy thereof. Such alloys may contain further elements, such as Si, Mn, Y, Zr, C, Co, Mo or a combination thereof. Preferably, the catalytically active material is a particle having a size of 2 nm to 250 nm. Preferably, the conductor and the conductive material are made of a material different from the conductive material. The conductor may be, for example, iron, nickel, aluminum, copper, silver or an alloy thereof. The ceramic coating is an electrically insulating material, the thickness of which is typically in the range of about 100 μm, for example 10-500 μm.
[0066] The conductive material is advantageously a coherent or always internally connected material, so as to realize the conductivity in the whole conductive material, thereby realize the thermal conductivity in the whole structured catalyst, and particularly provide the heating of the catalyst material. Through the coherent or always internally connected material, it is possible to ensure the uniform distribution of electric current in the conductive material, and therefore ensure the uniform distribution of heat in the structured catalyst. Throughout the text, the term "coherent (coherent)" means a synonym of cohesive (cohesive), and therefore refers to the material that is always internally connected or always coupled. The structured catalyst is a coherent or always internally connected material that controls the connectivity in the material of the structured catalyst and therefore obtains the conductivity of the conductive material. It should be noted that even if the conductive material is further modified, such as providing a slit in multiple parts of the conductive material or applying an insulating material in the conductive material, it is still represented that the conductive material is a coherent or always internally connected material.
[0067] The gas flow over the structured catalyst may be axial or coaxial with the current path through the structured catalyst, perpendicular to the current path, or have any other suitable direction relative to the current path.
[0068] The BMA reaction is highly endothermic. High temperatures, typically in excess of 800-850°C, are required to achieve acceptable conversions of the methane in the feed.
[0069] The feedstocks for the BMA reaction are preferably substantially pure ammonia and methane streams. Alternatively, the methane is provided in the form of a hydrocarbon mixture provided from, for example, natural gas or town gas, with an upstream upgrading step expected to remove a major portion of the higher hydrocarbons and possible sulfur compounds typically present in such feedstocks. Furthermore, the feedstock for the process may include a recycle stream from a unit operation downstream of the reactor system. Such a recycle may be a hydrogen-rich waste gas produced, for example, from an upgrading unit arranged to purify HCN in the product stream.
[0070] The feedstock for nitrile synthesis is preferably a substantially pure alkane such as ethane, propane or butane mixed with a substantially pure ammonia stream.
[0071] In one embodiment, the alkane feedstock is a mixture of several alkanes mixed with a substantially pure ammonia stream.
[0072] The term "conductive" is intended to mean a resistivity of 10 -5 Up to 10 -8 Thus, the conductive material is, for example, a metal such as copper, silver, aluminum, chromium, iron, nickel, or an alloy of the metal. Furthermore, the term "electrically insulating" is intended to mean a material with a resistivity higher than 10 Ω·m at 20°C, for example a material with a resistivity of 10 Ω·m at 20°C. 9 Up to 10 25 In the range of Ω·m.
[0073] When the reactor system includes a thermal insulation layer located between the structured catalyst and the pressure shell, appropriate thermal and electrical insulation is obtained between the structured catalyst and the pressure shell. The presence of a thermal insulation layer between the pressure shell and the structured catalyst helps to avoid excessive heating of the pressure shell and helps to reduce heat loss to the surrounding environment. The temperature of the structured catalyst can reach about 1300°C, at least in some parts thereof, but by using a thermal insulation layer between the structured catalyst and the pressure shell, the temperature of the pressure shell can be maintained at a significantly lower temperature, such as 500°C or even 100°C, which is advantageous because typical construction steel is generally not suitable for pressure applications at temperatures above 1000°C. In addition, the thermal insulation layer between the pressure shell and the structured catalyst helps to control the current within the reactor system because the thermal insulation layer is also electrically insulating. The thermal insulation layer can be one or more layers of solid material, such as ceramics, inert materials, fibrous materials, bricks or gas barriers or combinations thereof. Therefore, it is also conceivable that the purge gas or the limiting gas constitutes or forms part of the thermal insulation layer.
[0074] Furthermore, it should be noted that the term "thermal insulating material" refers to a material having a thermal conductivity of about 10 W·m -1 ·K -1 Materials with a thermal conductivity of 2000 Å or less. Examples of thermal insulating materials are ceramics, bricks, alumina-based materials, zirconia-based materials, and the like.
[0075] Advantageously, any relevant gaps between the structured catalyst, the thermal insulation layer, the pressure shell and / or any other components in the reactor system are filled with inert materials, for example in the form of inert granules. Such gaps are, for example, the gap between the bottom of the structured catalyst and the pressure shell and the gap between the side of the structured catalyst and the insulating layer covering the inner side of the pressure shell. The inert material can be, for example, a ceramic material in the form of granules or tiles. The inert material helps control the gas distribution through the reactor system and controls the gas flow through the structured catalyst. Moreover, the inert material usually has a thermal insulation effect.
[0076] The pressure shell has a design pressure of 2 bar to 30 bar appropriately. The actual operating pressure will depend on aspects such as the endothermic reaction, the size of the facility. Since the hottest part of the reactor system is a conductive material, the conductive material will be surrounded by a thermal insulation layer and located in the pressure shell of the reactor system, so the temperature of the pressure shell can be kept significantly lower than the maximum process temperature. This allows the pressure shell to have a relatively low design temperature, for example, the design temperature of the pressure shell is 700 ° C or 500 ° C or preferably 300 ° C or 100 ° C, while having a maximum process temperature of 400 ° C or even 900, or even 1100 ° C, or even up to 1300 ° C on the structured catalyst. At lower temperatures among these temperatures, the material strength is higher (corresponding to the design temperature of the pressure shell mentioned above). This provides an advantage when designing a chemical reactor. Suitably, the design pressure of the pressure shell is 2 bar to 30 bar or 30 to 200 bar. As a compromise between process economy and thermodynamic constraints, preferably about 30 bar.
[0077] The resistivity of the conductive material is suitably 10 -5 Ω·m to 10 -7 Ω·m. Materials with resistivity in this range provide efficient heating of the structured catalyst when powered by a power source. The resistivity of graphite at 20°C is about 10 -5 Ω·m, the resistivity of kanthal at 20℃ is about 10 -6 Ω·m, while the resistivity of stainless steel at 20°C is about 10 -7 Ω·m. The conductive material may have a resistivity of about 1.5·10 at 20°C, for example. -6 Ω·m FeCr alloy.
[0078] Typically, the pressure vessel includes an inlet for admitting process gas and an outlet for discharging product gas, wherein the inlet is located proximate to a first end of the pressure vessel and the outlet is located proximate to a second end of the pressure vessel, and wherein at least two conductors are connected to the structured catalyst at a location on the structured catalyst closer to the inlet than to the outlet. Thus, the at least two conductors can be placed in a significantly cooler portion of the reactor system, because the temperature of the inlet gas will be lower than the temperature of the product gas, the conductive material will be cooler at the most upstream portion of the material due to the heat consumed by the chemical reaction process, and the feed gas fed through the inlet can cool the at least two conductors, and then be heated by the heated structured catalyst further along the path of the gas on the heated structured catalyst. Advantageously, the temperature of all conductive elements other than the conductive material is kept low to protect the connection between the conductor and the structured catalyst. When the temperature of the conductor and other conductive elements other than the conductive material is relatively low, there are fewer restrictions on the materials suitable for the conductor and other conductive elements other than the conductive material. When the temperature of the conductive element increases, its resistivity increases; therefore, it is desirable to avoid unnecessary heating of all other components in the reactor system other than the conductive material. The term "conductive elements other than conductive material" is intended to encompass associated conductive elements arranged to connect a power source to the structured catalyst other than the conductive structured catalyst itself.
[0079] It should be noted that the systems of the present invention may include any suitable number of power sources and any suitable number of conductors connecting the power source(s) and the conductive material(s) of the structured catalyst.
[0080] Suitably, at least two conductors are guided through the pressure hull in a sleeve so that the at least two conductors are electrically insulated from the pressure hull. The sleeve may be made in part of a plastic and / or ceramic material. The term "sleeve" is intended to indicate a device that allows two pieces of hardware to be mechanically connected in a pressure-bearing configuration. Thus, the pressure within the pressure hull may be maintained even if the at least two conductors are guided through the pressure hull. Non-limiting examples of sleeves may be an electrically insulating sleeve, a dielectric sleeve, a dynamic compression seal, a compression sleeve or a flange. The pressure hull typically comprises side walls, end walls, flanges and possibly other parts. The term "pressure hull" is intended to cover any of these components.
[0081] The pressure shell may also include one or more inlets near or in combination with at least one sleeve to allow cooling gas to flow on, around, near or inside at least one conductor in the pressure shell. Therefore, the conductor is cooled, so the temperature experienced by the sleeve remains very low. If cooling gas is not used, the conductor can be heated by the feed gas fed to the reactor system, the resistance heating of the conductor due to the applied current, and / or the heat conduction from the structured catalyst. The cooling gas may be, for example, hydrogen, argon, nitrogen, methane, ammonia or a mixture thereof. The temperature of the cooling gas entering the pressure shell may be, for example, about 100°C or 200°C or 250°C. In one embodiment, (one or more) conductors are hollow so that the cooling gas can flow through the (one or more) conductors and cool it (them) from the inside. By keeping the temperature of the sleeve at a relatively low level, for example, at about 100-200°C, it is easier to achieve a leakproof configuration. Typically, a portion of the feed gas, such as one of the reactants, is fed into the pressure shell as a cooling gas. In another embodiment, a portion of the feed gas or a gas having the same composition as the feed gas is used as a cooling gas.
[0082] The reactor system may also include an inner tube in a heat exchange relationship with the structured catalyst, wherein the inner tube is adapted to extract product gas from the structured catalyst so that the product gas flowing through one or more inner tubes is in a heat exchange relationship with the gas flowing on the structured catalyst, but is electrically separated from the structured catalyst. This is a layout represented herein as a bayonet reactor system. In this layout, the product gas in the inner tube helps to heat the process gas flowing on the structured catalyst. The electrical insulation between the inner tube and the structured catalyst may be a gas in the form of a gap or distance between the inner tube and the structured catalyst, or an inert material loaded around the inner tube and the structured catalyst. The gas may pass through the structured catalyst in an upward flow or downward flow direction.
[0083] The connection between the structured catalyst and the at least two conductors can be a mechanical connection, a welded connection, a brazed connection, or a combination thereof. The structured catalyst can include terminals physically and electrically connected to the structured catalyst to facilitate electrical connection between the conductive material and the at least two conductors. The term "mechanical connection" is intended to mean a connection in which two components are mechanically held together, such as by threading or by clamping, so that current can flow between the components.
[0084] The conductive materials placed in the conductive material array can be electrically connected to each other. The connection between two or more conductive materials can be by mechanical connection, clamping, soldering, welding or any combination of these connection methods. Each conductive material can include a terminal to facilitate electrical connection. Two or more conductive materials can be connected to a power source in series or in parallel. The electrical connection between two or more conductive materials is advantageously coherent and uniform along the connection surface between the two or more conductive materials, so that the two or more conductive materials act as a single coherent or always connected material; therefore, uniform conductivity throughout the two or more conductive materials is promoted. Alternatively or additionally, the structured catalyst may include an array of conductive materials that are not electrically connected to each other. Instead, two or more conductive materials are placed together in a pressure-resistant shell, but are not electrically connected to each other. In this case, the structured catalyst therefore includes conductive materials connected in parallel to the power source.
[0085] Ceramic coatings with or without catalytically active materials can be added directly to the metal surface of the conductive material by wash coating. Wash coating of metal surfaces is a well-known process; descriptions are given, for example, in Cybulski, A., and Moulijn, JA, "Structured catalysts and reactors", Marcel Dekker, Inc, New York, 1998, Chapter 3 and references therein. The ceramic coating can be added to the surface of the conductive material and the catalytically active material can be added subsequently; alternatively, the ceramic coating containing the catalytically active material is added to the macrostructure or conductive material. The ceramic coating can be, for example, an oxide containing Al, Zr, Mg, Ce and / or Ca. Exemplary coatings are calcium aluminate or magnesium aluminum spinel. Such ceramic coatings can contain additional elements, such as La, Y, Ti, K or combinations thereof. The ceramic coating is an electrically insulating material whose thickness is typically in the range of about 100 μm, say 10-500 μm.
[0086] Extruded and sintered or 3D printed macrostructures result in homogeneous and coherent macrostructures, which can then be coated with a ceramic coating.
[0087] The conductive material and the ceramic coating may have been sintered in an oxidizing atmosphere to form a chemical bond between the ceramic coating and the conductive material; this provides a particularly high thermal conductivity between the conductive material and the catalytically active material supported by the ceramic coating. Thus, the structured catalyst is compact in terms of heat transfer to the active catalytic sites, and the reactor system housing the structured catalyst can be compact and limited primarily by the chemical reaction rate.
[0088] In one embodiment, the structured catalyst has at least one electrically insulating component arranged to increase the current path between the conductors to a length greater than the maximum dimension of the structured catalyst. Providing a current path between the conductors that is greater than the maximum dimension of the structured catalyst can be achieved by providing (one or more) electrically insulating components located between the conductors and preventing the current from flowing through a portion of the structured catalyst. Such electrically insulating components are arranged to increase the current path and thus increase the resistance through the structured catalyst. Therefore, the current path through the structured catalyst can be longer than the maximum dimension of the structured catalyst, for example, by 50%, 100%, 200%, 1000% or even more than 10000%.
[0089] In addition, such an electrically insulating member is arranged to direct current from a conductor closer to the first end of the structured catalyst than to the second end toward the second end of the structured catalyst and back to a second conductor closer to the first end of the structured catalyst than to the second end. Preferably, the current is arranged to flow from the first end of the structured catalyst to the second end and back to the first end. As shown in the accompanying drawings, the first end of the structured catalyst is its top end. Figure 5-7 The arrow indicated as "z" in the figure represents the z-axis along the length of the structured catalyst. The main current path running through the structured catalyst will have a positive or negative value of the z-coordinate of the accompanying current density vector along most of the length of the current path. The main current path means the path of electrons through the macrostructure of the structured catalyst with the highest current density. The main current path can also be understood as the path with the minimum length through the macrostructure of the structured catalyst. Geometrically, the main current path can be quantified as the maximum current density vector in a plane perpendicular to the gas flow direction of the coherent part of the macrostructure. As shown in the figure, at the bottom of the structured catalyst, the current will turn, and the z-coordinate of the accompanying current density vector here will be zero.
[0090] As used herein, the term coherent portion is intended to refer to a cross-sectional area of a macrostructure wherein all walls of the coherent portion are geometrically connected to one or more other walls of the coherent portion in the same plane.
[0091] In one embodiment, the structured catalyst has at least one electrically insulating component arranged to conduct an electric current through the structured catalyst so as to ensure that for at least 70% of the length of the structured catalyst, the current density vector of the main current path has a non-zero component value parallel to the length of the structured catalyst. Thus, for at least 70% of the length of the structured catalyst, the current density vector will have a positive or negative component value parallel to the length of the structured catalyst. Thus, for at least 70%, for example 90% or 95% of the length of the structured catalyst, i.e. Figure 5As seen in Figure 10, along the z-axis of the structured catalyst, the current density vector of the main current path will have a positive or negative value along the z-axis. This means that the current is forced to flow from the first end of the structured catalyst to the second end, and then forced to flow to the first end again. The temperature of the gas entering the first end of the structured catalyst and the endothermic BMA reaction occurring on the structured catalyst absorb heat from the structured catalyst. To this end, the first end of the structured catalyst remains colder than the second end, and by ensuring that the current density vector of the main current path has a non-zero component value parallel to the length of the structured catalyst, this occurs with a substantially continuously increasing temperature curve, which gives a controllable reaction front. In one embodiment, the current density vector has a non-zero component value parallel to the length of the structured catalyst in 70%, preferably 80%, more preferably 90%, and even more preferably 95% of the length of the structured catalyst. It should be noted that the term "length of the structured catalyst" is intended to represent the size of the structured catalyst in the direction of gas flow. In the structured catalyst shown in the accompanying drawings, the length is longitudinal, that is, its longest dimension. This is shown by arrows representing z in some drawings.
[0092] Non-limiting examples of insulating components are cutouts, slits or holes in the structure. Optionally, solid insulating materials, such as ceramics, in the cutouts or slits in the structure can be used. In the case where the solid insulating material is a porous ceramic material, the catalytically active material can be advantageously incorporated into the hole by, for example, impregnation. The solid insulating material in the cutout or slit helps to keep the parts of the structured catalyst on the sides of the cutout or slit separate from each other. As used herein, the term "maximum dimension of the structured catalyst" is intended to represent the maximum internal dimension of the geometric form occupied by the structured catalyst. If the structured catalyst is box-shaped, the maximum dimension will be the diagonal from one corner to the farthest corner, also referred to as the space diagonal.
[0093] It should be noted that even though the current through the structured catalyst may be arranged to have a tortuous or curved path through the structured catalyst due to the electrically insulating components arranged to increase the current path, the gas passing through the reactor system enters at one end of the reactor system and passes over the structured catalyst once before being discharged from the reactor system. Inert material is advantageously present in the associated gap between the structured catalyst and the rest of the reactor system to ensure that the gas within the reactor system passes over the structured catalyst and catalyst material herein.
[0094] The length of the gas channel through the structured catalyst is suitably less than the length of the current channel from one electrode through the structured catalyst and to the next electrode. The ratio of gas channel length to current channel length may be less than 0.6, or 0.3, 0.1, or even as low as 0.002.
[0095] Typically, the structured catalyst has an electrical insulating component that is arranged to make the current path through the structured catalyst a zigzag path. Here, the terms "zigzag path" and "zigzag approach" are intended to represent a path with a corner that tracks the path from one conductor to another conductor at a variable angle. A zigzag path is, for example, a path that goes up, turns, and then goes down. A zigzag path can have many turns, going up and then down through the structured catalyst multiple times, even if one turn is enough to make the path a zigzag path.
[0096] It should be noted that an insulating component arranged to increase the current path is not necessarily associated with a ceramic coating on a conductive material. Although such a ceramic coating is also considered to be electrically insulating, it does not change the length of the current path between the conductors connected to the conductive material.
[0097] The macrostructure can have multiple parallel channels, multiple non-parallel channels and / or multiple labyrinth channels, wherein the channels have walls defining the channels. Therefore, several different forms of macrostructures can be used, as long as the surface area of the structured catalyst exposed to the gas is as large as possible. In a preferred embodiment, the macrostructure has parallel channels because such parallel channels give the structured catalyst a very small pressure drop. In a preferred embodiment, the parallel longitudinal channels are inclined in the longitudinal direction of the macrostructure. In this way, the gas molecules flowing through the macrostructure will mostly tend to hit the walls in the channel, rather than just flowing directly through the channel without contacting the wall. In order to provide a macrostructure with sufficient resistivity, the size of the channel should be appropriate. For example, the channel can be square (as seen in a cross section perpendicular to the channel) and the side length of the square is 1 to 3 mm; however, it is conceivable that the channel has a maximum range of up to about 4 cm in the cross section. The thickness of the wall can be, for example, 0.2 to 2 mm, for example, about 0.5 mm, and the thickness of the ceramic coating supported by the wall is 10 μm to 500 μm, for example, 50 μm to 200 μm, for example, 100 μm. In another embodiment, the macrostructure of the structured catalyst is cross-corrugated.
[0098] Typically, when macrostructures are extruded or 3D printed, the pressure drop from the inlet to the outlet of the reactor system can be significantly reduced compared to reactors where the catalyst material is in pellet form.
[0099] Suitably, the reactor system also includes a bed of second catalyst material upstream of the structured catalyst within the pressure shell. Here, the term "upstream" is viewed from the direction of flow of the feed gas. Therefore, the term "upstream" is intended here to mean that the feed gas is directed through the bed of second catalyst material before reaching the structured catalyst. This provides a situation in which the second catalyst material can be arranged to pretreat the feed stream. There is no need to provide specific heating to the second catalyst material bed; however, if the second catalyst material bed is in close proximity to the structured catalyst, the second catalyst material bed can be heated indirectly. Alternatively, the second catalyst material can be heated. In order to clarify the terms used herein, it should be noted that the term "structured catalyst" may also be expressed as "first catalyst material" to distinguish it from the second and / or third and / or fourth catalyst material.
[0100] The reactor system may further include a third catalyst material in the form of catalyst pellets, extrudates or particles loaded into the channels of the macrostructure. In this embodiment, the reactor system will therefore have a catalytically active material in the coating of the macrostructure and a third catalyst material in the form of catalyst pellets, extrudates or particles in the channels of the macrostructure. Pellets are, for example, prepared to a size that loosely matches the channel size to form a single pellet string stacked on each other in the channels of the macrostructure. Alternatively, pellets, extrudates or particles can be prepared to a size significantly smaller than the channel size to form a packed bed in each channel. As used herein, the term "pellet" is intended to represent any well-defined structure with a maximum external dimension in the range of millimeters or centimeters, while "extrudate" and "particle" are intended to define a catalyst material with a maximum external dimension defined within a range.
[0101] A bed of a fourth catalyst material may be placed within the pressure shell and downstream of the structured catalyst. This fourth catalyst material may be in the form of catalyst pellets, extrudates or granules.
[0102] Thus, the first, second, third, and fourth catalyst materials can be catalyst materials suitable for use in a BMA reaction. In one embodiment, this catalyst is Pt / Al2O3. In another embodiment, it is CoSn / Al2O3. In a configuration that includes a combination of the second, third, and fourth catalyst materials in the reactor system, the catalyst for each catalyst material can be different.
[0103] The geometric surface area of the macrostructure can range from 100 to 3000 m 2 / m 3 , e.g. 500 to 1100m 2 / m 3 Typically, the material of the macrostructure is chosen to provide 500W / m 2 Up to 50000W / m2 Preferably, the resistive heating of the material provides 5 kW / m 2 Up to 12kW / m 2 , for example 8kW / m 2 Up to 10kW / m 2 The heat flux is given as heat / geometric surface area of the surface exposed to the gas.
[0104] In one embodiment, the structured catalyst includes a first portion arranged to generate a first heat flux and a second portion arranged to generate a second heat flux, wherein the first heat flux is lower than the second heat flux, and wherein the first portion is located upstream of the second portion. Here, the term "the first portion is located upstream of the second portion" is intended to indicate that the gas fed to the reactor system arrives at the first portion before the gas arrives at the second portion. The first portion and the second portion of the structured catalyst can be two different macro structures supporting a ceramic coating (which supports a catalytically active material), wherein the two different macro structures can be arranged to generate different heat fluxes for a given current and voltage. For example, the first portion of the structured catalyst can have a large surface area, while the second portion of the structured catalyst has a smaller surface area. This can be achieved by providing a structured catalyst in a second portion having a cross-sectional area less than the cross-sectional area of the first portion. Alternatively, the current path through the first portion of the structured catalyst can be straighter than the current path through the second portion of the structured catalyst, so that the current is more tortuous or bent through the second portion than through the first portion of the structured catalyst, thereby generating more heat in the second portion of the structured catalyst than in the first portion. As previously mentioned, the slits or cuts in the macrostructure can make the current path through the macrostructure zigzag. It should be noted that the first and second parts of the structured catalyst can experience different currents and voltages so that different heat fluxes can be provided. However, due to the different physical properties of the first and second parts as described above, the different heat fluxes of the first and second parts can also be achieved by providing the same current and voltage in / on the first and second parts. In a further embodiment, the structured catalyst includes a third part arranged to generate a third heat flux, wherein the third heat flux is lower than the first and / or second heat flux, and wherein the third part is downstream of the first and / or second part.
[0105] The predetermined temperature range of the gas leaving the pressure vessel / reactor system is 200 to 1300° C. The product gas outlet temperature from the structured catalyst is measured directly below or on the most downstream surface of the structured catalyst. The measurement technique can be a thermocouple (by voltage drop), a resistance temperature detector or infrared detection. The measurement point can be separated from the structured catalyst and embedded in an inert material / catalyst downstream, or directly on a surface with an insulating surface covering.
[0106] The structured catalyst in the reactor system suitably has a ratio of the area equivalent diameter of the horizontal cross section through the structured catalyst to the height of the structured catalyst in the range of 0.1 to 2.0. The area equivalent diameter of the cross section through the reactor system is defined as the diameter of a circle having an area equivalent to the cross-sectional area. When the ratio of the area equivalent diameter to the height of the structured catalyst is 0.1 to 2.0, the pressure shell containing the structured catalyst can be relatively small compared to other reactor systems for endothermic reactions (e.g., tubular reformers currently used for steam methane reforming).
[0107] Typically, the gas flows through the reactor system in an upward or downward flow direction so that the gas flows through the channels therein along the height of the structured catalyst. When the structured catalyst includes a plurality of macrostructures or an array of macrostructures, the individual macrostructures within the array may be placed side by side, stacked one on top of the other, or in combination thereof. It should be emphasized that when the structured catalyst includes more than one macrostructure, the size of the structured catalyst is the size of the more than one macrostructure. Thus, as an example, if the structured catalyst includes two macrostructures stacked one on top of the other, each having a height h, the height of the structured catalyst is 2h.
[0108] The volume of the structured catalyst is selected taking into account the desired feed conversion rate and / or the temperature exiting the reactor system in relation to the heat generating capacity of the conductive material.
[0109] Suitably, the height of the reactor system is from 0.5 to 7 m, more preferably from 0.5 to 3 m. Exemplary values for the height of the reactor system are heights of less than 5 meters, preferably less than 2 m or even 1 m. The size of the reactor system and the size of the structured catalyst within the reactor system are related; of course, the pressure hull and thermal insulation make the reactor system slightly larger than the structured catalyst itself.
[0110] The reactor system may further include an upgrading unit arranged to receive the product stream comprising hydrogen cyanide and separate it into an upgraded hydrogen cyanide stream and an off-gas stream.
[0111] In contrast to a combustion BMA reactor, the above reaction system is not an isolated system. Since heat is not transferred across the pressure-bearing wall, the risk of mechanical failure is not high. Temporary overheating is not a problem from the catalyst point of view, it is just the production of very hot gases. This means that start-up is relatively fast and in practice the invention can be started by applying a given voltage and the system will then work towards thermal equilibrium to reach steady state without any additional operator input.
[0112] A method is provided for reacting a feed gas containing an alkane (e.g., methane) and ammonia in the presence of a catalyst (e.g., a BMA catalyst) (e.g., under BMA reaction conditions) in a reactor system to produce hydrogen cyanide and / or nitrile, the reactor system comprising a pressure-resistant shell accommodating a structured catalyst, the structured catalyst being arranged to catalyze the endothermic reaction of the feed gas, the structured catalyst comprising a macrostructure of a conductive material, the macrostructure supporting a ceramic coating, wherein the ceramic coating supports a catalytically active material; wherein the reactor system is provided with a thermal insulation layer between the structured catalyst and the pressure-resistant shell.
[0113] The method comprises the following steps:
[0114] - pressurizing the raw gas,
[0115] - supplying the pressurized feed gas to the pressure shell through an inlet, the inlet being located so that the feed gas enters the structured catalyst at a first end of the structured catalyst; reacting the feed gas on the structured catalyst; and discharging product gas from the pressure shell, wherein the product gas leaves the structured catalyst from a second end of the structured catalyst;
[0116] - providing electrical power via an electrical conductor connected from a power source positioned outside the pressure vessel to the structured catalyst, allowing electrical current to flow through the macrostructure, thereby heating at least a portion of the structured catalyst to a temperature of at least 500° C., wherein the at least two conductors are connected to the structured catalyst at a location on the structured catalyst closer to the first end of the structured catalyst than to the second end of the structured catalyst, and wherein the structured catalyst is configured to direct electrical current from one conductor substantially toward the second end of the structured catalyst and back to a second of the at least two conductors, thereby heating at least a portion of the structured catalyst to a temperature sufficient to cause the feed gas to undergo a BMA reaction on the structured catalyst,
[0117] - product gas comprising hydrogen cyanide and / or nitrile is discharged from the reactor system.
[0118] Whenever possible, all details of the system given above relate to the method described above.
[0119] In one aspect, the feed gas is pressurized to a pressure of 2 to 30 bar. The feed gas may be pressurized to a pressure of 30 to 200 bar. Suitably, at least a portion of the structured catalyst is heated to a temperature of at least 700°C, preferably at least 900°C, more preferably at least 1000°C. The maximum temperature to which the structured catalyst is heated is about 1400°C.
[0120] One aspect of the method further comprises the step of introducing a cooling gas through the pressure vessel via the inlet so as to allow the cooling gas to flow over the at least one conductor.
[0121] Suitably, in the process of the present invention, the alkane is methane, the catalyst is a BMA catalyst and the product stream comprises hydrogen cyanide.
[0122] The method may further comprise the step of feeding the product stream comprising hydrogen cyanide to an upgrading unit and separating it into an upgraded hydrogen cyanide stream and an off-gas stream. The upgrading unit may be arranged such that the off-gas stream is recycled and mixed with the supplied feed gas before passing over the structured catalyst.
[0123] The upgrading unit may include a combination of an absorber, a scrubber, a stripper, and a condenser. In one embodiment, the process gas from the reactor system is passed through a monoammonium phosphate solution to remove ammonia. The resulting stream is then passed to an HCN adsorber using cold water to retain the HCN, and the solution is sent to an HCN stripper for product purification. In another embodiment, the process gas from the reactor system is passed through a sulfuric acid scrubber to remove ammonia. The resulting stream is then passed to an HCN adsorber using cold water to retain the HCN, and the solution is sent to an HCN stripper for product purification.
[0124] In one aspect, the method further comprises the step of feeding the upgraded hydrogen cyanide stream from the upgrading unit to a downstream facility to convert HCN into an upgraded product, wherein the production of HCN is equal to the consumption of HCN in the downstream facility. This means that HCN is produced "on demand" and therefore there is no intermediate inventory of HCN to store or transport. Examples of upgraded products include acetone cyanohydrin, adiponitrile, sodium cyanide, methionine, and cyanuric chloride.
[0125] Therefore, a method is provided for quickly switching a metal-catalyzed reaction of a feed gas containing methane and ammonia from a first steady-state reaction condition (A) to a second steady-state reaction condition (B) or from a second steady-state reaction condition (B) to a first steady-state reaction condition (A) in a reactor system as described herein.
[0126] Achieving steady-state conditions is defined as when central process parameters (eg, feed flow rates, outlet temperatures, and reactant conversions) reach values within ±15% of the average process value for the given process parameter over the subsequent hour.
[0127] Condition A or B of the present invention relates to a state in which the load is 300 Nm 3 / h to 100 000Nm 3 / h total flow rate, with a feedstock comprising methane and ammonia and any of hydrogen, nitrogen, argon or oxygen, at a pressure of 5 barg to 150 barg, with a balanced electrical heating system's catalyst to heat the product gas outlet temperature from the structured catalyst to a temperature of 300 to 1300° C. As the feedstock passes through the monolith, it reacts towards the equilibrium of the reaction.
[0128] In one embodiment of the present invention, the method comprises initial reaction conditions A, wherein the feedstock consists of 49.6% CH4, 49.6% NH3, 0.2% N2 and 0.6% H2, with a total flow rate of 547 Nm 3 / h, the temperature is 430℃, the pressure is 6.7barg. Providing 100kW of first electrical power produces an almost balanced gas composed of 46.3% CH4, 46.3% NH3, 0.2% N2, 5.6% H2 and 1.7% HCN, with a total flow rate of 566Nm 3 / h, temperature is 600℃, pressure is 6.6barg. In about 90min, it switches to condition B, and at the same time applies a second electric power of 1090kW, producing an almost balanced gas composed of 5.0% CH4, 5.0% NH3, 0.1% N2, 67.6% H2 and 22.4% HCN, with a total flow rate of 992Nm 3 / h, temperature is 1130℃, pressure is 6.6barg.
[0129] In one embodiment of the present invention, the method comprises initial reaction conditions A, wherein the feedstock consists of 48.4% CH4, 48.4% NH3, 0.8% N2 and 2.4% H2, with a total flow rate of 127 Nm 3 / h, the temperature is 430℃, the pressure is 34.3barg. The first electrical power of 200kW is provided to produce an almost balanced gas composed of 13.0% CH4, 13.0% NH3, 0.5% N2, 55.5% H2 and 18.0% HCN, with a total flow rate of 199Nm 3 / h, temperature of 1150 ° C, pressure of 34.0 barg. In about 25 minutes, switch to condition B, apply a second electric power of 580 kW, and increase the total feed flow rate to 381 Nm 3 / h, producing an almost balanced gas consisting of 14.0% CH4, 14.0% NH3, 0.5% N2, 54.1% H2 and 17.5% HCN, with a total flow of 586Nm 3 / h, temperature is 1135℃, pressure is 34barg.
[0130] The term "vice versa" is used to indicate that the method is equally applicable when switching from the first reaction condition (A) to the second reaction condition (B) as when switching from the second reaction condition (B) to the first reaction condition (A). It is worth noting that the switch from condition A to condition B is considered complete when the process value of the system reaches within 85% of the steady-state condition.
[0131] The reactor system is as described above; that is, it comprises a pressure vessel containing a structured catalyst arranged to catalyze a reaction of a feed gas comprising methane and ammonia, the structured catalyst comprising a macrostructure of an electrically conductive material, the macrostructure supporting a ceramic coating, wherein the ceramic coating supports a catalytically active material, and wherein the reactor system is provided with a thermal insulation layer between the structured catalyst and the pressure vessel. All details described above with respect to the reactor system are relevant to the present technology.
[0132] The method of this aspect of the invention comprises the following steps:
[0133] In the first steady-state reaction condition (A):
[0134] - supplying the feed gas to the reactor system at a first total flow rate, and
[0135] - providing a first electrical power via an electrical conductor connecting a power source placed outside the pressure vessel to the structured catalyst, thereby allowing a first current to flow through the conductive material,
[0136] thereby heating at least a portion of the structured catalyst to a first temperature at which the feed gas is converted over the structured catalyst under the first steady-state reaction condition (A) into a first product gas mixture; and exhausting the first product gas from the reactor system;
[0137] And, in the second steady-state reaction condition (B):
[0138] - supplying the feed gas to the reactor system at a second total flow rate,
[0139] - providing a second electrical power via an electrical conductor connecting a power source placed outside the pressure vessel to the structured catalyst, thereby allowing a second current to flow through the conductive material,
[0140] thereby heating at least a portion of the structured catalyst to a second temperature; converting the feed gas to a second product gas mixture over the structured catalyst at the second steady-state reaction condition (B) at the second temperature; and exhausting the second product gas from the reactor system;
[0141] To achieve the first and second steady-state reaction conditions (A) and (B), the second electrical power is higher than the first electrical power; and / or the second total flow rate is higher than the first total flow rate.
[0142] It is noteworthy that an increase in the total flow rate will increase the input of cold feed gas, thereby cooling the structured catalyst and reducing reactivity, thereby achieving the second steady-state reaction condition (B). Significant changes in flow rate will change the energy required for the process.
[0143] Changes in total flow may include changes in total flow without compositional changes or changes in composition, such as increasing recycle flow or changing a portion of the feedstock.
[0144] In one embodiment, the ratio (A:B) of the total gas feed flow rate in the first reaction condition A and the second reaction condition B is at least 1:10. Therefore, switching between conditions A and B allows a significant increase / reduction in the output of product gas. When the present invention is used for energy storage, for example, this is advantageous, wherein excess electrical energy from an energy grid is available, and in this way can be stored as chemical energy, and vice versa, to increase the availability of electrical energy in the grid when electrical energy is needed elsewhere. In addition, this embodiment allows the use of the present invention to supply a large amount of product gas during the period when the downstream process needs it, and in other cases the present invention is operated under standby conditions. If there is no continuous demand for product gas, this is advantageous.
[0145] In another embodiment, the product gas outlet temperature from the structured catalyst in reaction conditions B is 50°C to 800°C higher than the product gas outlet temperature from the structured catalyst in reaction conditions A, for example 100°C to 500°C higher, preferably 150°C to 400°C higher. This allows for rapid startup of the reactor system from a cold state to operating conditions. This is advantageous in the case of system startup, where the startup procedure comprises the following steps:
[0146] Heating process equipment in non-condensing gases to a temperature above the condensation point of the facility under steady-state conditions at full load,
[0147] Pressurize the raw gas components,
[0148] feeding a raw gas component into the reactor system while applying a first electrical power,
[0149] • Switching to a higher operating temperature by applying a second electrical power.
[0150] In this way, all steps of the startup procedure are relatively quick.
[0151] The product gas outlet temperature from the structured catalyst in reaction condition B is typically no more than 50°C higher than the product gas outlet temperature from the structured catalyst in reaction condition A. This allows for rapid changes between conditions A and B without significantly changing the composition of the product gas from the system. In this way, product gas requirements for downstream processes of the reactor system can be easily supplied in different amounts without significantly disturbing the chemical environment of these.
[0152] In one embodiment, the switching between reaction conditions A and B comprises a gradual change in the total gas feed flow rate from the first total flow rate to the second total flow rate, and a simultaneous gradual change in the potential applied to the conductive material from the first electrical power to the second electrical power. In this way, the product gas composition can also remain almost constant during the transition phase. In one embodiment, the gradual change is performed in such a way that the flow rate is increased in small steps while the electrical power is increased to maintain an almost constant product gas outlet temperature from the structured catalyst.
[0153] In one embodiment, the reactor system also includes a control system, which is arranged to control the power supply to ensure that the temperature of the gas leaving the pressure shell is within a predetermined range and / or to ensure that the conversion rate of the feed gas is within a predetermined range. The control of the power supply is the control of the electrical output from the power supply. The control of the power supply can be performed, for example, as a control of the voltage and / or current from the power supply, as a control of whether the power supply is turned on or off, or as a combination thereof. The power provided to the structured catalyst can be in the form of alternating current or direct current.
[0154] According to one embodiment, a proportional-integral-derivative (PID) controller controls the potential based on feedback readings from a process value of the product gas outlet temperature of the structured catalyst.
[0155] The methods described herein allow for rapid switching between conditions A and B. Thus, suitably, switching between reaction conditions A and B occurs within a time period of less than 3 hours, such as less than 2 hours, such as less than 60 min, preferably less than 30 min, even more preferably less than 15 min.
[0156] In one embodiment, switching between reaction conditions A and B comprises supplying a second electrical power to the structured catalyst. This suitably occurs whilst maintaining the total flow rate substantially constant.
[0157] In one aspect, the switching between reaction conditions A and B comprises a transition state between said reaction conditions A and B; said transition state comprises a first period of time, in which the power is cut off; followed by a second period of time, in which the structured catalyst is supplied with said second electrical power of condition B. This allows a more rapid establishment of a stable state.
[0158] In one aspect, the transition between reaction conditions A and B comprises a transition state between the reaction conditions A and B; the transition state comprises a first period of time in which the third electrical power is supplied to the structured catalyst; followed by a second period of time in which the second electrical power of condition B is supplied to the structured catalyst, the third electrical power being higher than the second electrical power. This allows a more rapid establishment of a stable state.
[0159] The method may include subjecting the product gas comprising hydrogen cyanide to other steps such as purification, pressurization, heating, cooling, etc. to provide a final product gas for use downstream of the reactor system of the present invention.
[0160] It should be noted that the feed gas may include separate feed gases, and the step of pressurizing the feed gas may include pressurizing the individual feed gases separately. Also, it should be noted that the order in which the method steps are written is not necessarily the order in which the method steps occur, as two or more steps may occur simultaneously, or the order may be different from the order shown above.
[0161] In one embodiment, the process comprises the step of pressurizing the gas upstream of the pressure vessel up to a pressure of at least 2 bar.The selected operating pressure is determined by the endothermic reaction and the integration of the reactor in surrounding process steps.
[0162] In one embodiment of the process according to the invention, the temperature of the feed gas entering the reactor system is from 100° C. to 700° C. However, in all embodiments, the temperature and pressure of the feed gas are adjusted to ensure that the feed gas is above the dew point.
[0163] In one embodiment of the process of the invention, the structured catalyst is heated so that the maximum temperature of the structured catalyst is between 200°C and 1300°C. The temperature used will depend on the endothermic reaction. The maximum temperature of the structured catalyst depends on the material of the conductive material; thus, if the conductive material is a FeCr alloy, which melts at a temperature between 1380°C and 1490°C (depending on the actual alloy), if the melting point of the conductive material is about 1400°C, then the maximum temperature should be slightly below the melting point, for example about 1300°C, because the material will become soft and ductile when approaching the melting point. The maximum temperature may be further limited by the durability of the catalyst material, the coating and the catalytically active material.
[0164] In one embodiment, the method according to the invention further comprises the step of introducing a cooling gas through the pressure vessel via the inlet to allow the cooling gas to flow through the at least one conductor and / or the sleeve. The cooling gas may advantageously be hydrogen, nitrogen, ammonia, methane or any other gas suitable for cooling the area or zone around the at least one conductor. A portion of the feed gas may be fed into the pressure vessel as cooling gas.
[0165] In one embodiment according to the invention, the method further comprises the step of introducing a cooling gas through the pressure hull via the inlet to allow the cooling gas to flow through at least one conductor and / or the sleeve. The cooling gas may be any suitable gas; examples of such gases are hydrogen, nitrogen, ammonia, methane or mixtures thereof. The cooling gas may flow through the conductor(s) and cool it(them) from the inside; in this case, the conductor(s) need to be hollow to accommodate the cooling gas flowing therein.
[0166] The catalyst material used for the reaction can be Pt / Al2O3, Pt / ZrO2, Ru / Al2O3, Rh / Al2O3, Pt / MgAl2O3 or CoSn / Al2O3. The catalytically active material can be Pt, Ru, Rh, Ir, Co, Sn or a combination thereof, and the ceramic coating can be Al2O3, ZrO2, MgAl2O3, CaAl2O3 or a combination thereof and may be mixed with oxides of Y, Ti, La or Ce. The maximum temperature of the reactor can be between 850-1300°C. The pressure of the feed gas can be 2-180 bar, preferably about 25 bar. In one embodiment, the macrostructure is made of an alloy of Fe Cr Al, supports a ceramic coating of a mixture of ZrO2 and Al2O3, and Pt is used as the catalytically active material.
[0167] Detailed description with drawings
[0168] In the following description of the figures, the BMA reaction is described. However, the details of the reactor system etc. are also applicable to the nitrile synthesis.
[0169] The same reference numerals refer to the same elements throughout the drawings.
[0170] Figure 1a A cross section through one embodiment of a reactor system 100 according to the present invention is shown. The reactor system 100 includes a structured catalyst 10, which is arranged as an array of macrostructures 5. Each macrostructure 5 in the array is coated with a ceramic coating impregnated with a catalytically active material. Moreover, the reactor system 100 includes conductors 40, 40' connected to a power source (not shown in the figure) and the structured catalyst 10 (i.e., the array of macrostructures). The conductors 40, 40' are guided through the wall of the pressure vessel 20 containing the structured catalyst via a sleeve 50 and through the insulating material 30 on the inside of the pressure vessel. The conductor 40' is connected to the array of macrostructures 5 by a conductor contact rail 41.
[0171] In one embodiment, the power supply supplies a voltage of 26 V and a current of 1200 A. In another embodiment, the power supply supplies a voltage of 5 V and a current of 240 A. The current is conducted through the electrical conductors 40, 40' to the conductor contact rails 41, and the current flows from a conductor contact rail 41, for example from Figure 1a The conductor rail, seen on the left in the middle, flows through the structured catalyst 10 to another conductor rail 41, for example Figure 1a The conductor rail is seen on the right in the figure. The current can be either alternating current, i.e. running in both directions alternately, or direct current and running in either direction.
[0172] The macrostructure 5 is made of an electrically conductive material. Particularly preferred is kanthal, an alloy consisting of aluminum, iron and chromium. The ceramic coating applied to the structured catalyst 5, such as an oxide, is impregnated with a catalytically active material. The conductors 40, 40' are made of materials such as iron, aluminum, nickel, copper or alloys thereof.
[0173] During operation, a feed gas comprising methane and ammonia enters the reactor system 100 from above as indicated by arrow 11. A product stream exits the reactor system from its base as indicated by arrow 12.
[0174] Figure 1b Shows Figure 1a The reactor system 100, wherein a portion of the pressure vessel 20 and the thermal insulation layer 30 are removed, Figure 2 is an enlarged view of a portion of the reactor system 100. Figure 1b and 2 The connection ratio between the conductor 40' and the conductor contact rail 41 is Figure 1a It is shown more clearly. Furthermore, it can be seen that the conductor 40 is guided through the wall of the pressure hull in the sleeve 50 and that one conductor 40 is divided into three conductors 40' inside the pressure hull. It should be noted that the number of conductors 40' can be any suitable number, for example less than three or even more than three.
[0175] exist Figure 1a , 1b 2, the conductors 40, 40' are guided through the wall of the pressure vessel 20 containing the structured catalyst and through the insulating material 30 on the inner side of the pressure vessel via the sleeve 50. The feed gas for the BMA reaction enters the reactor system 100 via the inlet on the upper side of the reactor system 100 as shown by the arrow 11, and the converted product stream leaves the reactor system 100 via the outlet at the bottom of the reactor system 100 as shown by the arrow 12. In addition, one or more additional inlets ( Figures 1a to 2The cooling gas may be hydrogen, nitrogen, methane or a mixture thereof. The temperature of the cooling gas when entering the pressure vessel may be, for example, about 100° C.
[0176] exist Figures 1a to 2 In the reactor system 100 shown, the inert material ( Figure 1a-2 The inert material (not shown) is advantageously present between the lower side of the structured catalyst 10 and the bottom of the pressure-resistant shell. Moreover, the inert material is advantageously present between the outer side of the structured catalyst 10 of the macrostructure 5 and the insulating material 30. Therefore, one side of the insulating material 30 faces the inner side of the pressure-resistant shell 20, while the other side of the insulating material 30 faces the inert material. The inert material is, for example, a ceramic material and can be in the form of a granular material. The inert material helps to control the pressure drop across the reactor system 100 and control the flow of the gas through the reactor system 100 so that the gas flows on the surface of the structured catalyst 10.
[0177] Figure 3a and 3b A schematic cross-section of one embodiment of a reactor system 100', 100" of the present invention including a structured catalyst 10' is shown. The structured catalyst 10' may be composed of a single macrostructure having a ceramic coating supporting a catalytically active material, or it may include two or more macrostructures. Each of the reactor systems 100', 100" includes a pressure shell 20 and a thermal insulation layer 80 between the structured catalyst 10' and the pressure shell 20. An inert material 90 may be used to fill the gap between the structured catalyst 10' and the thermal insulation layer or the pressure shell 20. Figure 3a and 3b In the figure, inert material 90 is represented by the dashed area; inert material 90 can be in any suitable form, such as in the form of inert granules, and it is, for example, a ceramic material. Inert material 90 helps control the pressure drop through the reactor system and control the gas flow through the reactor system. Moreover, the inert material generally has a thermal insulation effect.
[0178] from Figure 3a and 3bAs can be seen, the reactor system 100', 100" also includes inner tubes 15 in heat exchange relationship with the structured catalyst 10'. The inner tubes 15 are adapted to draw product gas from the structured catalyst 10' such that the product gas flowing through the one or more inner tubes is in heat exchange relationship with the gas flowing over the structured catalyst; however, the inner tubes 15 are electrically insulated from the structured catalyst 10' by thermal insulation layers 80, inert materials 90, gaps, or a combination. This is an arrangement that is denoted as a bayonet reactor system. In this arrangement, the product gas within the inner tubes assists in heating the process gas flowing over the macrostructure. Figure 3a and 3b In the illustrated arrangement, the feed gas enters the reactor system 100', 100" as indicated by arrow 11 and continues into the structured catalyst 10' as indicated by arrow 13. As the feed gas passes over the structured catalyst 10', it undergoes a BMA reaction. The gas exiting the structured catalyst 10' is at least partially converted to hydrogen cyanide. The at least partially converted gas flows from the structured catalyst 10' into the inner tube 15 as indicated by arrow 14 and exits the inner tube as indicated by arrow 12. Even though there is a thermal insulation layer 80 between the inner tube 15 and the structured catalyst 10', some heat transfer will occur from the gas within the inner tube 15 and the gas within or upstream of the structured catalyst 10'. Figure 3a and 3b In the embodiment shown, the feed gas flows downward through the structured catalyst 10 ′ and upward through the inner tube 15 ; however, it is contemplated that the configuration could be reversed so that the feed gas flows upward through the structured catalyst 10 ′ and downward through the inner tube 15 .
[0179] Figure 4 and 5 One embodiment of a structured catalyst comprising an array of macrostructures is shown viewed from above and from the side, respectively. Figure 4 A structured catalyst 10 comprising an array of macrostructures 5 is shown as seen from above, i.e. as seen from Figure 1a and 1b As seen by arrow 11 in FIG. 1 . The array has 6 rows (i.e. Figure 1a , 1b , 1c, 1d, 1e and 1f). The macrostructures 5 in each row are connected to the adjacent macrostructures (one or more) in the same row, and the two outermost macrostructures in each row are connected to the conductor contact rail 41. Adjacent macrostructures 5 in a row of macrostructures are connected to each other by means of connecting pieces 3.
[0180] Figure 5 Shown from the side Figure 4 A structured catalyst 10 having an array of macrostructures 5. Figure 5It can be seen that each macrostructure 5 is perpendicular to Figure 4 The cross section shown extends longitudinally. Each macrostructure 5 has a slit 60 cut into it along its longitudinal direction (see Figure 5 ). Thus, when powered by a power source, current enters the array of macrostructures 5 via the conductor contact rail 41, is directed downward through the first macrostructure 5 to the lower limit of the slit 60, and is then directed upward toward the connector 3. Current is directed downward and upward through each macrostructure 5 in each row 1a-1f of macrostructures 5 in the array 10 via a corresponding zigzag path. This configuration advantageously increases the electrical resistance on the structured catalyst 10.
[0181] Figure 6 The structured catalyst 10 according to the present invention is shown in a perspective view. The structured catalyst 10 comprises a macrostructure coated with a ceramic coating impregnated with a catalytically active material. Within the structured catalyst are channels 70 extending in the longitudinal direction of the macrostructure 5 (by Figure 6 The passage is defined by a wall 75. Figure 6 In the embodiment shown, the walls 75 define a plurality of parallel square channels 70 when viewed in the direction of flow indicated by arrow 12. When viewed from above, the structured catalyst 10 has a substantially square perimeter defined by side lengths e1 and e2. However, the perimeter may also be circular or other shapes.
[0182] The walls 75 of the structured catalyst 10 are made of an extruded or 3D printed material coated with a ceramic coating, such as an oxide, which has been applied to the macrostructure. In the figure, the ceramic coating is not shown. The ceramic coating is impregnated with a catalytically active material. The ceramic coating and therefore the catalytically active material are present on each wall within the structured catalyst 10 over which the gas flow flows during operation and interacts with the heated surface and catalytically active material of the structured catalyst.
[0183] Thus, during use in the reactor system to conduct a BMA reaction, the feed gas flows through the channels 70 and interacts with the heated surface of the structured catalyst and the catalytically active material supported by the ceramic coating.
[0184] exist Figure 6 In the structured catalyst 10 shown, a slit 60 has been cut into the structured catalyst 10. In this case, the slit 60 forces the current to take a zigzag route downwards and then upwards within the macrostructure, thereby increasing the current path and therefore increasing the resistance and therefore the heat dissipated within the macrostructure. The slits 60 within the macrostructure may be provided with an embedded insulating material to ensure that no current flows in the lateral direction of the slits 60.
[0185] The channels 70 in the structured catalyst 10 are open at both ends. When the structured catalyst is used in a reactor system, the feed gas flows along Figure 1a and 1b The BMA flows through the cell in the direction indicated by arrows 11 and 12 and is heated by contact with the wall 75 of the channel 70 and by heat radiation. The heat induces the desired BMA reaction. The wall 75 of the channel 70 may have a thickness of, for example, 0.5 mm, and the ceramic coating applied to the wall 75 may have a thickness of, for example, 0.1 mm. Although arrows 11 and 12 (see Figure 1a and 1b ) shows that the flow of the raw gas is downward, but the opposite flow direction, i.e., upward flow, is also conceivable.
[0186] Figure 7 The perspective view shows the connector 7 attached. Figure 1a and 1b The structured catalyst 10 is provided with a plurality of connectors 7. The connectors 7 each connect a portion of the structured catalyst 10 to the conductors 40. The conductors 40 are all connected to a power source (not shown). Each connector 7 is connected to the upper portion of the structured catalyst. When the conductors 40 are connected to the power source, the current is guided to the corresponding connector 7 via the conductors and flows through the structured catalyst 10. The slits 60 block the current from flowing in the lateral direction ( Figure 7 Therefore, the current flows in the partially structured catalyst along the slits 60 in a manner as follows: Figure 7 Run in the downward direction as shown, then Figure 7 It is shown running transversely from below the slit 60 to the longitudinal direction and finally the current runs upward in the longitudinal direction of the structured catalyst to another connector 7 . Figure 7 The connector 7 in the structured catalyst is mechanically fastened to the structured catalyst by means of mechanical fastening means such as screws and bolts. However, additional or alternative fastening means are conceivable. In one embodiment, the power supply generates a voltage of 3 V and a current of 400 A. The connector 7 is made of a material such as iron, aluminum, nickel, copper or an alloy thereof, for example.
[0187] As described above, the structured catalyst 10 is coated with a ceramic coating, such as an oxide, that supports a catalytically active material. However, the portion of the structured catalyst 10 that is connected to the connector 7 should not be coated with an oxide. Instead, the macrostructure of the structured catalyst should be exposed to or directly connected to the connector 7 in order to obtain a good electrical connection between the macrostructure and the connector.
[0188] When the connector 7 and thus the conductor 40 are connected to the same end of the structured catalyst 10, i.e. to the Figure 7At the upper end shown, the feed gas entering the reactor system containing the structured catalyst 10 will be able to cool the connector 7 and the conductor 40. For example, the feed gas entering such a reactor system may have a temperature of 200°C or 400°C, thus preventing the connector 7 and the conductor 40 from reaching a temperature much higher than that.
[0189] Figure 8 Another embodiment of a structured catalyst 10'' with a connector 7'' is shown. The structured catalyst 10'' is, for example, Figure 6 Each connector 7'" has three holes on its upper side for connecting conductors (not shown). A piece of electrically insulating material 61 is located between the slits 60 (see Figure 6 )Inside.
[0190] Fig. 9 The equilibrium composition of CH4 (and NH3) and HCN is shown as a function of temperature when an equimolar feed gas of CH4 and NH3 is used at 5 barg. This illustrates the change in the thermodynamic equilibrium composition with temperature. Note that only methane is shown as a reactant, but since the feed gas is equimolar, the concentration is equivalent to the ammonia concentration due to the 1:1 stoichiometric ratio. According to the figure, the reaction temperature should be above 1000°C to achieve high methane conversion, with the remaining methane mole fraction still being 10.3%. Ideally, the reaction temperature is even higher than 1200°C to produce a gas composition of 2.4% methane, 2.4% ammonia and 23.8% hydrogen cyanide, with the balance being hydrogen.
[0191] It should be noted that even though the structured catalyst shown in the figures is shown as having channels with square cross-sections, as seen perpendicular to the z-axis, any suitable shape of the channel cross-section is conceivable. Thus, the channels of the structured catalyst may alternatively be, for example, triangular, hexagonal, octagonal or circular, with triangular, square and hexagonal shapes being preferred.
[0192] Although the present invention has been illustrated by the description of various embodiments and examples and these embodiments and examples have been described in considerable detail, it is not the intention of the applicant to limit or in any way restrict the scope of the appended claims to such details. Additional advantages and modifications will readily occur to those skilled in the art. Therefore, the present invention in its broader aspects is not limited to the specific details, representative methods and illustrative examples shown and described. Therefore, these details may be deviated from without departing from the spirit or scope of the applicant's overall inventive concept.
[0193] Invention Project
[0194] 1. A reactor system for reacting a feed gas containing an alkane and ammonia in the presence of a catalyst to produce hydrogen cyanide and / or nitrile, the reactor system comprising:
[0195] - a source of feed gas comprising alkanes and ammonia;
[0196] - a structured catalyst arranged to catalyze a reaction of the feed gas, the structured catalyst comprising macrostructures of an electrically conductive material, the macrostructures supporting a ceramic coating, wherein the ceramic coating supports a catalytically active material;
[0197] - a pressure-resistant shell containing the structured catalyst, the pressure-resistant shell comprising an inlet for the feed gas to enter and an outlet for the product gas to exit, wherein the inlet is located so that the feed gas enters the structured catalyst at a first end of the structured catalyst and the product gas leaves the structured catalyst from a second end of the structured catalyst;
[0198] - a thermal insulation layer between the structured catalyst and the pressure shell;
[0199] - at least two conductors electrically connected to the structured catalyst and to a power source disposed outside the pressure vessel, wherein the power source is sized to heat at least a portion of the structured catalyst to a temperature of at least 500° C. by passing an electric current through the macrostructure, wherein the at least two conductors are connected to the structured catalyst at a location on the structured catalyst closer to the first end of the structured catalyst than to the second end of the structured catalyst, and wherein the structured catalyst is configured to direct an electric current from one conductor substantially toward the second end of the structured catalyst and back to a second of the at least two conductors;
[0200] - an outlet for a product stream comprising hydrogen cyanide and / or nitrile.
[0201] 2. The reactor system according to item 1, wherein the power supply is sized to heat at least a portion of the structured catalyst to a temperature of at least 700°C, preferably at least 900°C, more preferably at least 1000°C.
[0202] 3. A reactor system according to any of the preceding items, wherein the feed gas additionally comprises H2, N2 or Ar.
[0203] 4. The reactor system according to any one of the preceding items, wherein the design pressure of the pressure vessel is 2 to 30 bar.
[0204] 5. The reactor system according to any one of items 1 to 3, wherein the design pressure of the pressure shell is 30 to 200 bar.
[0205] 6. A reactor system according to any one of the preceding items, wherein the resistivity of the conductive material is 10 -5 Ω·m to 10 -7 Ω·m.
[0206] 7. The reactor system according to any of the preceding clauses, wherein the at least two conductors are guided through the pressure vessel in a sleeve such that the at least two conductors are electrically insulated from the pressure vessel.
[0207] 8. The reactor system of item 7, wherein the pressure vessel further comprises one or more inlets proximate to or in combination with at least one sleeve to allow cooling gas to flow on, around, near or within at least one conductor within the pressure vessel.
[0208] 9. A reactor system according to any of the preceding items, wherein the reactor system further comprises an inner tube in heat exchange relationship with the structured catalyst but electrically insulated, the inner tube being adapted to draw product gas from the structured catalyst such that the product gas flowing through the inner tube is in heat exchange relationship with the gas flowing over the structured catalyst.
[0209] 10. The reactor system according to any of the preceding items, wherein the connection between the structured catalyst and the at least two conductors is a mechanical connection, a welded connection, a brazed connection or a combination thereof.
[0210] 11. A reactor system according to any of the preceding items, wherein the conductive material comprises a 3D printed or extruded and sintered macrostructure, the macrostructure supporting a ceramic coating, wherein the ceramic coating supports a catalytically active material.
[0211] 12. The reactor system according to any of the preceding clauses, wherein the structured catalyst comprises an array of macrostructures electrically connected to each other.
[0212] 13. A reactor system according to any of the preceding clauses, wherein the structured catalyst has an electrically insulating component arranged to increase the length of the main current path between the at least two conductors to a length greater than the maximum dimension of the structured catalyst.
[0213] 14. A reactor system according to any of the preceding items, wherein the structured catalyst has at least one electrically insulating component, and the at least one electrically insulating component is arranged to guide current through the structured catalyst so as to ensure that for at least 70% of the length of the structured catalyst, the current density vector of the main current path has a non-zero component value parallel to the length of the structured catalyst.
[0214] 15. The reactor system according to any of the preceding items, wherein the macrostructure has a plurality of parallel channels, a plurality of non-parallel channels and / or a plurality of labyrinthine channels.
[0215] 16. A reactor system according to any of the preceding items, wherein the reactor system further comprises a third catalyst material loaded into the channels of the macrostructure, the third catalyst material being in the form of catalyst pellets, extrudates or granules.
[0216] 17. The reactor system according to any of the preceding clauses, wherein the reactor system further comprises a fourth catalyst material bed within the pressure shell downstream of the structured catalyst.
[0217] 18. A reactor system according to any of the preceding clauses, wherein the material of the macrostructure is selected to be arranged to generate 500 to 50,000 W / m 2 The heat flux of the material.
[0218] 19. A reactor system according to any of the preceding items, wherein the structured catalyst comprises a first portion arranged to generate a first heat flux and a second portion arranged to generate a second heat flux, wherein the first heat flux is lower than the second heat flux, and wherein the first portion is located upstream of the second portion.
[0219] 20. A reactor system according to any of the preceding items, wherein the structured catalyst comprises a third portion arranged to generate a third heat flux, wherein the third heat flux is lower than the first heat flux and / or the second heat flux, and wherein the third portion is downstream of the first portion and / or the second portion.
[0220] 21. A reactor system according to any one of the preceding items, wherein the reactor system further comprises a control system, which is arranged to control the power supply to ensure that the temperature of the gas leaving the pressure vessel is within a predetermined range and / or to ensure that the conversion rate of the feed gas is within a predetermined range.
[0221] 22. The reactor system according to any of the preceding items, wherein the structured catalyst within the reactor system has a ratio of the area equivalent diameter of a horizontal cross-section through the structured catalyst to the height of the structured catalyst in the range of 0.1 to 2.0.
[0222] 23. The reactor system according to any of the preceding items, wherein the height of the reactor system is from 0.5 to 7 m, more preferably from 0.5 to 3 m.
[0223] 24. The reactor system according to any of the preceding clauses, wherein the alkane is methane, the catalyst is a BMA catalyst, and the product stream comprises hydrogen cyanide.
[0224] 25. A method for reacting a feed gas comprising alkanes and ammonia in the presence of a catalyst in a reactor system to produce hydrogen cyanide and / or nitrile, the reactor system comprising a pressure vessel containing a structured catalyst, the structured catalyst being arranged to catalyze the endothermic reaction of the feed gas, the structured catalyst comprising macrostructures of conductive material, the macrostructures supporting a ceramic coating, wherein the ceramic coating supports a catalytically active material; wherein the reactor system is provided with a thermal insulation layer between the structured catalyst and the pressure vessel; the method comprising the steps of:
[0225] - pressurizing the raw gas,
[0226] - supplying the pressurized feed gas to the pressure shell through an inlet, the inlet being located so that the feed gas enters the structured catalyst at a first end of the structured catalyst; allowing the feed gas to react on the structured catalyst and exhausting product gas from the pressure shell, wherein the product gas leaves the structured catalyst from a second end of the structured catalyst;
[0227] - providing electrical power via an electrical conductor connected from a power source positioned outside the pressure vessel to the structured catalyst, allowing current to flow through the macrostructure, thereby heating at least a portion of the structured catalyst to a temperature of at least 500° C., wherein the at least two conductors are connected to the structured catalyst at a location on the structured catalyst closer to the first end of the structured catalyst than to the second end of the structured catalyst, and wherein the structured catalyst is configured to direct current from one conductor to flow substantially toward the second end of the structured catalyst and back to a second of the at least two conductors, thereby heating at least a portion of the structured catalyst to a temperature sufficient to cause the feed gas to undergo a BMA reaction on the structured catalyst, thereby heating at least a portion of the structured catalyst to a temperature sufficient to cause the feed gas to undergo a BMA reaction on the structured catalyst,
[0228] - product gas comprising hydrogen cyanide and / or nitrile is discharged from the reactor system.
[0229] 26. The method according to item 25, wherein the feed gas is pressurized to a pressure of 2 to 30 bar.
[0230] 27. The method according to item 25, wherein the feed gas is pressurized to a pressure of 30 to 200 bar.
[0231] 28. The process according to any one of items 25 to 27, wherein at least a portion of the structured catalyst is heated to a temperature of at least 700°C, preferably at least 900°C, more preferably at least 1000°C.
[0232] 29. The method according to any one of items 25 to 28, further comprising the step of introducing a cooling gas through the pressure vessel via an inlet so as to allow the cooling gas to flow over at least one conductor.
[0233] 30. The process according to any one of items 25-29, wherein the alkane is methane, the catalyst is a BMA catalyst, and the product stream comprises hydrogen cyanide.
[0234] 31. The process of claim 30, wherein the process further comprises the step of feeding the product stream comprising hydrogen cyanide to an upgrading unit and separating it into an upgraded hydrogen cyanide stream and a waste gas stream.
[0235] 32. The method according to item 31, wherein the upgrading unit is arranged so that the exhaust gas stream is recirculated and mixed with the supplied feed gas before passing over the structured catalyst.
[0236] 33. The method according to item 31 or 32, wherein the method further comprises the step of feeding the upgraded hydrogen cyanide stream from the upgrading unit to a downstream facility to convert HCN into an upgraded product, and wherein the production of HCN is equal to the consumption of HCN in the downstream facility.
[0237] 34. A method for rapidly switching a metal-catalyzed reaction of a feed gas containing alkanes and ammonia from a first steady-state reaction condition (A) to a second steady-state reaction condition (B) or from a second steady-state reaction condition (B) to a first steady-state reaction condition (A) in a reactor system according to any one of claims 1 to 24; the method comprising the following steps:
[0238] In the first steady-state reaction condition (A):
[0239] - supplying the feed gas to the reactor system at a first total flow rate, and
[0240] - providing a first electrical power via an electrical conductor connecting a power source placed outside the pressure vessel to the structured catalyst, thereby allowing a first current to flow through the conductive material,
[0241] thereby heating at least a portion of the structured catalyst to a first temperature at which the feed gas is converted over the structured catalyst under the first steady-state reaction condition (A) into a first product gas mixture; and exhausting the first product gas from the reactor system;
[0242] And, in the second steady-state reaction condition (B):
[0243] - supplying the feed gas to the reactor system at a second total flow rate,
[0244] - providing a second electrical power via an electrical conductor connecting a power source placed outside the pressure vessel to the structured catalyst, thereby allowing a second current to flow through the conductive material,
[0245] thereby heating at least a portion of the structured catalyst to a second temperature; converting the feed gas to a second product gas mixture over the structured catalyst at the second steady-state reaction condition (B) at the second temperature; and exhausting the second product gas from the reactor system;
[0246] The second electric power is higher than the first electric power; and / or the second total flow is higher than the first total flow.
[0247] 35. A method according to item 34, wherein the at least two conductors are connected to the structured catalyst at a position on the structured catalyst closer to the first end of the structured catalyst than to the second end of the structured catalyst, and wherein the structured catalyst is configured to direct current from one conductor to flow substantially toward the second end of the structured catalyst and back to the second of the at least two conductors.
[0248] 36. The method according to any one of items 34-35, wherein the ratio of the total gas feed flow in the first reaction condition A to the second reaction condition B (A:B) is at least 1:10.
[0249] 37. The process according to any one of items 34 to 36, wherein the outlet temperature of the product gas from the structured catalyst in reaction conditions B is 50°C to 800°C higher than the outlet temperature of the product gas from the structured catalyst in reaction conditions A, for example 100°C to 500°C higher, preferably 150°C to 400°C higher.
[0250] 38. A method according to any one of items 34-37, wherein the switching between reaction conditions A and B includes gradually changing the total gas feed flow rate from the first total flow rate to the second total flow rate and simultaneously gradually changing the potential applied to the conductive material from the first electric power to the second electric power.
[0251] 39. The process according to any one of items 34 to 38, wherein the product gas outlet temperature from the structured catalyst in reaction conditions B is no more than 50°C higher than the product gas outlet temperature from the structured catalyst in reaction conditions A.
[0252] 40. The method according to any one of items 34-39, wherein a proportional-integral-derivative (PID) controller controls the potential based on feedback readings from a process value of the product gas outlet temperature of the structured catalyst.
[0253] 41. The method according to any one of items 34 to 40, wherein the product gas outlet temperature from the structured catalyst is measured directly below or on the most downstream surface of the structured catalyst.
[0254] 42. A method according to any one of items 34 to 41, wherein the switching between reaction conditions A and B occurs within a time period of less than 3 hours, such as less than 2 hours, such as less than 60 min, preferably less than 30 min, even more preferably less than 15 min.
[0255] 43. The method according to any one of items 34-42, wherein switching between reaction conditions A and B comprises providing a second electrical power to the structured catalyst.
[0256] 44. A method according to any one of items 34-43, wherein the switching between reaction conditions A and B includes a transition state between the reaction conditions A and B; the transition state includes a first time period in which power is cut off; followed by a second time period in which the second electrical power of condition B is supplied to the structured catalyst.
[0257] 45. A method according to any one of items 34-44, wherein the switching between reaction conditions A and B includes a transition state between the reaction conditions A and B; the transition state includes a first time period, wherein a third electrical power is supplied to the structured catalyst; followed by a second time period, wherein the second electrical power of condition B is supplied to the structured catalyst, and the third electrical power is higher than the second electrical power.
Claims
1. A reactor system for reacting a feed gas containing an alkane and ammonia in the presence of a catalyst to produce hydrogen cyanide and / or nitrile, the reactor system comprising: - a source of feed gas comprising alkanes and ammonia; - a structured catalyst arranged to catalyze a reaction of the feed gas, the structured catalyst comprising macrostructures of an electrically conductive material, the macrostructures supporting a ceramic coating, wherein the ceramic coating supports a catalytically active material; - a pressure-resistant shell containing the structured catalyst, the pressure-resistant shell comprising an inlet for the feed gas to enter and an outlet for the product gas to exit, wherein the inlet is located so that the feed gas enters the structured catalyst at a first end of the structured catalyst and the product gas leaves the structured catalyst from a second end of the structured catalyst; - a thermal insulation layer between the structured catalyst and the pressure shell; - at least two conductors electrically connected to the structured catalyst and to a power source disposed outside the pressure vessel, wherein the power source is sized to heat at least a portion of the structured catalyst to a temperature of at least 500° C. by passing an electric current through the macrostructure, wherein the at least two conductors are connected to the structured catalyst at a location on the structured catalyst closer to the first end of the structured catalyst than to the second end of the structured catalyst, and wherein the structured catalyst is configured to direct an electric current from one conductor to the second end of the structured catalyst and back to a second of the at least two conductors; - an outlet for a product stream comprising hydrogen cyanide and / or nitrile, wherein the current density vector of the primary current path has a non-zero component value parallel to the length of the structured catalyst, which occurs with a continuously increasing temperature profile; and The macrostructure has a plurality of parallel channels, a plurality of non-parallel channels and / or a plurality of labyrinth channels, wherein the channels have walls defining the channels.
2. The reactor system of claim 1, wherein the power source is sized to heat at least a portion of the structured catalyst to a temperature of at least 700°C.
3. The reactor system of claim 1, wherein the power source is sized to heat at least a portion of the structured catalyst to a temperature of at least 900°C.
4. The reactor system of claim 1, wherein the power source is sized to heat at least a portion of the structured catalyst to a temperature of at least 1000°C.
5. The reactor system according to any one of claims 1 to 4, wherein the feed gas additionally comprises H2, N2 or Ar.
6. The reactor system according to any one of claims 1 to 4, wherein the design pressure of the pressure vessel is 2 to 30 bar.
7. A method for reacting a feed gas comprising an alkane and ammonia in the presence of a catalyst in a reactor system to produce hydrogen cyanide and / or nitrile, the reactor system comprising a pressure resistant shell containing a structured catalyst, the structured catalyst being arranged to catalyze the reaction of the feed gas, the structured catalyst comprising macrostructures of an electrically conductive material, the macrostructures supporting a ceramic coating, wherein the ceramic coating supports a catalytically active material; The reactor system is provided with a thermal insulation layer between the structured catalyst and the pressure-resistant shell; the method comprises the following steps: - pressurizing the raw gas, - supplying the pressurized feed gas to the pressure shell through an inlet, the inlet being located so that the feed gas enters the structured catalyst at a first end of the structured catalyst; allowing the feed gas to react on the structured catalyst and exhausting product gas from the pressure shell, wherein the product gas leaves the structured catalyst from a second end of the structured catalyst; - providing electrical power via electrically connecting a power source disposed outside the pressure vessel to at least two conductors of the structured catalyst, allowing current to flow through the macrostructure, thereby heating at least a portion of the structured catalyst to a temperature of at least 500° C., wherein the at least two conductors are connected to the structured catalyst at a location on the structured catalyst closer to the first end of the structured catalyst than to the second end of the structured catalyst, and wherein the structured catalyst is configured to direct current from one conductor to the second end of the structured catalyst and back to a second of the at least two conductors, thereby heating at least a portion of the structured catalyst to a temperature sufficient to cause the feed gas to undergo a BMA reaction on the structured catalyst, - allowing a product gas comprising hydrogen cyanide and / or nitrile to be discharged from the reactor system, wherein the structured catalyst has a continuously increasing temperature profile parallel to the length of the structured catalyst; and The macrostructure has a plurality of parallel channels, a plurality of non-parallel channels and / or a plurality of labyrinth channels, wherein the channels have walls defining the channels.
8. The process of claim 7, wherein the alkane is methane, the catalyst is a BMA catalyst, and the product stream comprises hydrogen cyanide.
9. The process of claim 8, wherein the process further comprises the step of feeding the product stream comprising hydrogen cyanide to an upgrading unit and separating it into an upgraded hydrogen cyanide stream and an off-gas stream.
10. The method according to claim 9, wherein the upgrading unit is arranged so that the exhaust gas stream is recirculated and mixed with the supplied feed gas before passing over the structured catalyst.
11. The process according to claim 9 or 10, wherein the process further comprises the step of feeding the upgraded hydrogen cyanide stream from the upgrading unit to a downstream facility to convert HCN into upgraded products, and wherein the production of HCN is equal to the consumption of HCN in the downstream facility.
12. A method for rapidly switching a metal-catalyzed reaction of a feed gas containing alkanes and ammonia from a first steady-state reaction condition (A) to a second steady-state reaction condition (B) or from a second steady-state reaction condition (B) to a first steady-state reaction condition (A) in a reactor system according to any one of claims 1 to 6; the method comprising the following steps: In the first steady-state reaction condition (A): - supplying the feed gas to the reactor system at a first total flow rate, and - providing a first electrical power via an electrical conductor connecting a power source placed outside the pressure vessel to the structured catalyst, thereby allowing a first current to flow through the conductive material, thereby heating at least a portion of the structured catalyst to a first temperature at which the feed gas is converted over the structured catalyst under the first steady-state reaction condition (A) into a first product gas mixture; and exhausting the first product gas from the reactor system; And, in the second steady-state reaction condition (B): - supplying the feed gas to the reactor system at a second total flow rate, - providing a second electrical power via an electrical conductor connecting a power source placed outside the pressure vessel to the structured catalyst, thereby allowing a second current to flow through the conductive material, thereby heating at least a portion of the structured catalyst to a second temperature; converting the feed gas to a second product gas mixture over the structured catalyst at the second steady-state reaction condition (B) at the second temperature; and exhausting the second product gas from the reactor system; The second electric power is higher than the first electric power; and / or the second total flow is higher than the first total flow.
Citation Information
Patent Citations
Steam reforming heated by resistance heating
WO2019228797A1
Endothermic reactions heated by resistance heating
WO2019228798A1
Process for preparing charcoal / charcoal component by electrothermy orienting infiltration
CN101157563A
Electrically heated reactor and process for carrying out gas reactions at a high temperature using this reactor
CN1774291A
Process and apparatus for the production of hydrogen cyanide
GB722025A