A polyether ester, its preparation method and application

By optimizing the dosage of catalyst and polymerization inhibitor during the synthesis of polyethylene glycol monoether, and adding dropwise glycidyl methacrylate solution, the problems of solvent waste and low conversion rate were solved, and efficient and low-cost polymerization was achieved. Ether ester synthesis is suitable for preparing high-performance polycarboxylate water-reducing agent.

CN114437337BActive Publication Date: 2024-10-18LIAONING OXIRANCHEM INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202011204245.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-02
Publication Date
2024-10-18
Estimated Expiration
2040-11-02

AI Technical Summary

Technical Problem

The existing synthesis process of polyethylene glycol monoether (meth)acrylate requires a large amount of alkane solvent, resulting in resource waste and low conversion rate, and there are problems with solvent recycling.

Method used

Use polyethylene glycol monomethyl ether, catalyst and polymerization inhibitor as the base material, add glycidyl methacrylate solution dropwise, and react to obtain polyethylene glycol monomethyl ether hydroxypropyl methacrylate. Control the reaction temperature and time. , optimize the dosage of catalyst and polymerization inhibitor to increase conversion rate and reduce cost.

Benefits of technology

The polyether ester synthesis with high conversion rate is achieved, the production process is simplified, the cost is reduced, and the product quality is improved. It is suitable for preparing high-performance polycarboxylate water-reducing agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002756490320000041
    Figure BDA0002756490320000041
  • Figure BDA0002756490320000071
    Figure BDA0002756490320000071
  • Figure BDA0002756490320000081
    Figure BDA0002756490320000081
Patent Text Reader

Abstract

The present invention provides a polyether ester and a preparation method and application thereof. The preparation method of the polyether ester comprises: using polyethylene glycol monomethyl ether, a catalyst and a polymerization inhibitor as a base material, dripping a glycidyl methacrylate solution, and reacting to obtain polyethylene glycol monomethyl ether hydroxypropyl methacrylate. The preparation method of the present invention has a simple process, is not easy to self-polymerize, has few side reactions, has a high product yield, and greatly reduces the cost; the obtained polyether ester can be used to synthesize a polycarboxylic acid water reducer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer preparation, and in particular to a polyether ester and a preparation method and application thereof. Background Art

[0002] Polyethylene glycol (meth) acrylate is an important intermediate. The functional polymer materials synthesized with it as a macromonomer have shown broad application prospects in the fields of thermosensitive polymer materials, temperature-sensitive polymer materials, conductive polymer materials, dental materials, artificial lenses, concrete water reducers (MAPEG products) and self-dispersing inks.

[0003] At present, MAPEG polyether products are still the mainstream products for the synthesis of polycarboxylic acid water-reducing agents in Europe, the United States and other countries. Both literature reports and production practices have shown that water-reducing agents synthesized using MAPEG ester polyether products have good workability, which is mainly reflected in the improvement of the construction performance of concrete, such as wide applicability, no water seepage, good wrapping, easy pumping, etc., which meets the functional and integrated performance development needs of polycarboxylic acid water-reducing agents.

[0004] The existing synthesis route of polyethylene glycol monoether (meth)acrylate mainly uses polyethylene glycol monoether and (meth)acrylic acid, (meth)acrylate as raw materials and synthesizes through esterification, transesterification and other methods.

[0005] CN101289533A discloses a method for synthesizing polyethylene glycol monomethyl ether methacrylate, wherein alkali metal alkoxide is used as a catalyst, phenothiazine is used as a polymerization inhibitor, and hydrocarbon substances are used as solvents to synthesize polyethylene glycol monomethyl ether methacrylate through an ester exchange reaction between methyl methacrylate and polyethylene glycol monomethyl ether.

[0006] CN101092478A discloses a method for preparing alkyl polyoxyethylene ether methacrylate, wherein a solid acid is used as a catalyst, an alkane is used as an azeotropic solvent, and methacrylic acid and alkyl polyoxyethylene ether are used as reaction reagents to synthesize the polyether macromonomer.

[0007] Although the above esterification or transesterification reaction successfully synthesizes methacrylate polyethylene glycol macromonomer, a large amount of alkane is required as solvent during the synthesis process, the proportion of acid ether is large, the conversion rate is low, and there are problems of resource waste and solvent recycling. Summary of the invention

[0008] The main purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for synthesizing acrylate polyoxyethylene ether, thereby saving solvents, simplifying the production process, reducing production costs and improving product quality.

[0009] In order to achieve the above object, the present invention adopts the following technical solution:

[0010] A method for preparing polyether ester, comprising:

[0011] Polyethylene glycol monomethyl ether, a catalyst and a polymerization inhibitor are used as base materials, and a glycidyl methacrylate solution is added dropwise to react to obtain polyethylene glycol monomethyl ether hydroxypropyl methacrylate.

[0012] In some embodiments, the molecular weight of the polyethylene glycol monomethyl ether is 800-3000.

[0013] In some embodiments, the catalyst is selected from one or more of sodium hydroxide, potassium hydroxide, metallic sodium, sodium methoxide, potassium methoxide, calcium acetate, potassium acetate, sodium carbonate, boron trifluoride, sodium p-toluenesulfonate, tin tetrachloride, and zinc chloride.

[0014] In some embodiments, the amount of the catalyst used is 0.01%-2% by mass of the polyethylene glycol monomethyl ether.

[0015] In some embodiments, the polymerization inhibitor is selected from one or more of hydroquinone, p-hydroxyanisole, methylhydroquinone, phenothiazine, and 2,2,6,6-tetramethylpiperidinyl nitroxide free radical.

[0016] In some embodiments, the amount of the polymerization inhibitor in the base material is 0.05%-1% of the mass of the polyethylene glycol monomethyl ether.

[0017] In some embodiments, the glycidyl methacrylate solution is a mixture of glycidyl methacrylate and the polymerization inhibitor, and the amount of the polymerization inhibitor in the glycidyl methacrylate solution is 0.05%-1% of the mass of the glycidyl methacrylate, and the molar ratio of the glycidyl methacrylate to the polyethylene glycol monomethyl ether is 1.001:1-1.005:1.

[0018] In some embodiments, the reaction temperature is 40-200° C., and the dripping time of the glycidyl methacrylate solution is 3-6 hours.

[0019] In another aspect, the present invention provides a polyether ester prepared by the above preparation method.

[0020] In another aspect, the present invention provides use of the polyether ester in preparing a polycarboxylate water-reducing agent.

[0021] The preparation method of the invention has simple process, is not easy to self-polymerize, has few side reactions, has high product yield, and greatly reduces the cost. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is further described below according to specific embodiments. The protection scope of the present invention is not limited to the following embodiments, which are listed only for illustrative purposes and do not limit the present invention in any way.

[0023] The preparation method of the polyether ester of the present invention comprises:

[0024] Polyethylene glycol monomethyl ether, a catalyst and a polymerization inhibitor are used as base materials, and a glycidyl methacrylate solution is added dropwise to react to obtain polyethylene glycol monomethyl ether hydroxypropyl methacrylate.

[0025] In the preparation method of the present invention, the molecular weight of the polyethylene glycol monomethyl ether used is 800-3000.

[0026] In the preparation method of the present invention, the catalyst used is selected from one or more of sodium hydroxide, potassium hydroxide, metallic sodium, sodium methoxide, potassium methoxide, calcium acetate, potassium acetate, sodium carbonate, boron trifluoride, sodium p-toluenesulfonate, tin tetrachloride and zinc chloride.

[0027] In the preparation method of the present invention, the polymerization inhibitor used is selected from one or more of hydroquinone, p-hydroxyanisole, methyl hydroquinone, phenothiazine, and 2,2,6,6-tetramethylpiperidinyl nitroxide free radical.

[0028] In the preparation method of the present invention, the amount of the catalyst is 0.01%-2% of the mass of the polyethylene glycol monomethyl ether, preferably 0.02%-0.1%; the amount of the inhibitor in the base material is 0.05%-1% of the mass of the polyethylene glycol monomethyl ether.

[0029] In the preparation method of the present invention, the glycidyl methacrylate solution is a mixture of glycidyl methacrylate and a polymerization inhibitor, and the polymerization inhibitor in the glycidyl methacrylate solution and the polymerization inhibitor in the base material can be the same or different. The amount of the polymerization inhibitor in the glycidyl methacrylate solution is 0.05%-1% of the mass of glycidyl methacrylate, and the molar ratio of glycidyl methacrylate to polyethylene glycol monomethyl ether is 1.001:1-1.005:1.

[0030] In the preparation method of the present invention, the reaction temperature is 40-200° C., preferably 60-140° C. The dripping time of the glycidyl methacrylate solution is 3-6 hours.

[0031] The polyethylene glycol monomethyl ether hydroxypropyl methacrylate prepared by the invention can be used for synthesizing polycarboxylic acid water reducing agent.

[0032] Unless otherwise defined, the terms used in the present invention have the meanings commonly understood by those skilled in the art.

[0033] The present invention is further described in detail below by way of examples.

[0034] Example

[0035] Unless otherwise specified, the experimental methods used in the following embodiments and application examples are conventional methods.

[0036] The raw materials used in the embodiments and application examples are all commercially available.

[0037] In the examples, the indicators of the ester polyether were measured by the following methods.

[0038] (1) Determination of weight average molecular weight and molecular weight distribution

[0039] A multi-angle laser scatterer, an eighteen-angle laser scatterer coupling system, a Shodex RI101 differential detector, and experimental conditions: Shodex gel column, mobile phase: dimethylformamide, column temperature: 35°C.

[0040] (2) Determination of the content of unsaturated carbon-carbon double bonds

[0041] After the unsaturated carbon-carbon double bonds in the ester polyether react with 0.1 mol / L tribromo compound, potassium iodide solution is added to replace the unreacted bromine with iodine. The iodine in the solution is titrated with a sodium thiosulfate standard solution through back titration to calculate the content of the unsaturated double bonds.

[0042] (3) Epoxy value is determined in accordance with GB / T 1677-2008 "Determination of epoxy value of plasticizers"

[0043] (4) Calculation of esterification rate of glycidyl methacrylate

[0044]

[0045] Example 1

[0046] Add 800g of polyethylene glycol monomethyl ether (average molecular weight 800) into a three-necked flask, add 8g of KOH as a catalyst, and 0.072g of phenothiazine as an inhibitor. Heat to 120°C, and dropwise add glycidyl methacrylate solution (142.29g of glycidyl methacrylate, 0.072g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical). The dropping time is controlled within 3h, and after the dropping is completed, mature for 30min.

[0047] After aging, the epoxy value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0048] Example 2

[0049] Add 1000g of polyethylene glycol monomethyl ether (average molecular weight 1000) into a three-necked flask, add 10g of sodium methoxide as a catalyst, 5g of phenothiazine, and 5g of p-methylphenol as an inhibitor, raise the temperature to 120°C, and add dropwise glycidyl methacrylate solution (142.29g of glycidyl methacrylate, 0.144g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical). The dropping time is controlled within 3h, and after the dropping is completed, mature for 30min.

[0050] After aging, the epoxy value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0051] Example 3

[0052] Add 1200g of polyethylene glycol monomethyl ether (average molecular weight 1200) into a three-necked flask, add 12g of NaOH as a catalyst, 12g of phenothiazine and 6g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical as an inhibitor, raise the temperature to 120°C, and add glycidyl methacrylate solution (142.43g of glycidyl methacrylate, 0.072g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical) dropwise. The dropping time is controlled within 3h. After the dropping is completed, mature for 30min.

[0053] After aging, the epoxy value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0054] Example 4

[0055] Add 1500g of polyethylene glycol monomethyl ether (average molecular weight 1500) into a three-necked flask, add 10g of KOH and 5g of sodium carbonate as catalysts, and 15g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical as an inhibitor. Heat to 130°C, and dropwise add glycidyl methacrylate solution (142.45g of glycidyl methacrylate, 0.072g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical). The dropping time is controlled within 4h, and after the dropping is completed, mature for 30min.

[0056] After aging, the epoxy value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0057] Example 5

[0058] Add 2000g of polyethylene glycol monomethyl ether (average molecular weight 2000) into a three-necked flask, add 20g of KOH as a catalyst, 10g of phenothiazine and 15g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical as an inhibitor, raise the temperature to 130°C, and add dropwise methacrylate glycidyl methacrylate solution (142.57g of methacrylate glycidyl methacrylate, 0.72g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical). The dropping time is controlled within 3h, and after the dropping is completed, mature for 30min.

[0059] After aging, the epoxy value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0060] Example 6

[0061] Add 2400g of polyethylene glycol monomethyl ether (average molecular weight 2400) into a three-necked flask, add 12g of KOH and 12g of sodium carbonate as catalysts, 12g of phenothiazine and 15g of 2,2,6,6-tetramethylpiperidine nitroxide free radical, and 5g of p-hydroxyanisole as an inhibitor, raise the temperature to 140°C, and add dropwise methacrylate glycidyl methacrylate solution (142.60g of methacrylate glycidyl methacrylate, 0.072g of 2,2,6,6-tetramethylpiperidine nitroxide free radical). The dropping time is controlled within 3h, and after the dropping is completed, mature for 30min.

[0062] After aging, the epoxy value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0063] Example 7

[0064] Add 3000g of polyethylene glycol monomethyl ether (average molecular weight 3000) into a three-necked flask, add 15g of KOH and 15g of potassium acetate as catalysts, 10g of phenothiazine, 30g of 2,2,6,6-tetramethylpiperidine nitroxide free radical, and 5g of methylhydroquinone as inhibitors, raise the temperature to 120°C, and add glycidyl methacrylate solution (142.86g of glycidyl methacrylate, 0.072g of 2,2,6,6-tetramethylpiperidine nitroxide free radical) dropwise. The addition time is controlled within 3h. After the addition is completed, mature for 30min.

[0065] After aging, the epoxy value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0066] Example 8

[0067] Add 1200g of polyethylene glycol monomethyl ether (average molecular weight 1200) into a three-necked flask, add 8g of tin tetrachloride and 4g of sodium p-toluenesulfonate as catalysts, and 12g of phenothiazine as an inhibitor. Heat to 120°C, and add glycidyl methacrylate solution (142.30g of glycidyl methacrylate, 1.432g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical) dropwise. The addition time is controlled within 3h. After the addition is completed, mature for 30min.

[0068] After aging, the epoxy value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0069] Example 9

[0070] Add 800g of polyethylene glycol monomethyl ether (average molecular weight 800) into a three-necked flask, add 8g of KOH as a catalyst, and 0.072g of phenothiazine as an inhibitor. Heat to 60°C, and dropwise add glycidyl methacrylate solution (142.4g of glycidyl methacrylate, 0.072g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical). The dropping time is controlled within 3h, and after the dropping is completed, mature for 30min.

[0071] After aging, the epoxy value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0072] Example 10

[0073] Add 3000g of polyethylene glycol monomethyl ether (average molecular weight 800) into a three-necked flask, add 15g of boron trifluoride and 15g of tin tetrachloride as catalysts, 10g of phenothiazine and 20g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical as inhibitors, raise the temperature to 70°C, and add dropwise methacrylate glycidyl methacrylate solution (142.3g of methacrylate glycidyl methacrylate, 0.072g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical). The dropping time is controlled within 3h, and the mixture is matured for 30min after the dropping is completed.

[0074] After aging, the epoxy value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0075] Comparative Example

[0076] Add 1200g of polyethylene glycol monomethyl ether (average molecular weight 1200) into a three-necked flask, add 8g of tin tetrachloride and 4g of sodium p-toluenesulfonate as catalysts, and 12g of phenothiazine as an inhibitor. Heat to 120°C, and drop methacrylic acid solution (142.30g of glycidyl methacrylate, 1.432g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical). The dropping time is controlled within 3h. During the dropping process, the water produced in the reaction is continuously removed by fractional distillation. After the dropping is completed, mature for 30min.

[0077] After aging, the acid value, saponification value, weight average molecular weight, molecular weight distribution, unsaturation and other indicators were tested and calculated. The results are shown in Table 1.

[0078] Table 1 Test results of Examples 1-10

[0079]

[0080]

[0081] The unsaturation degree is calculated by (1-acid value / saponification value)*100%.

[0082] It can be seen from Table 1 that the conversion rates of polyethylene glycol monomethyl ether hydroxypropyl methacrylate in Examples 1-10 of the present invention are all above 98%, which is significantly improved compared with the conversion rate of the comparative example.

[0083] Application Examples

[0084] In a 1L round-bottom flask, add 271g of deionized water, fully evacuate with nitrogen and continue to add nitrogen to keep the system in a nitrogen protection environment. Turn on stirring and heating to raise the temperature of the deionized water in the flask to 88-90°C. Add the pre-prepared A material and B material dropwise into the flask.

[0085] A material preparation method: ester ether: water: MAS = 100g: 266.45g: 2.241g, wherein the ester ether is obtained in Example 3, (MAS is sodium methyl allyl sulfonate)

[0086] Material B preparation method: APS: water = 2.075g: 39.4g (APS is ammonium persulfate).

[0087] The water used was deionized water.

[0088] Material A was dripped at a constant speed for 3 hours, and material B was dripped at the same time as material A for 3.5 hours. After the addition of material B, it was aged at 88-90℃ for 1 hour. The temperature was lowered to 30℃, and a sodium hydroxide solution with a mass concentration of 30% was added to adjust the pH value of the system to 6.5-7.5, and the material was discharged to obtain a water reducer.

[0089] The test indicators of the water reducing agent are as follows: pH value: 6.5-7.5 Water content: 20% Weight average molecular weight: 42500 Molecular weight distribution coefficient: 2.380. Then, the performance and state of the concrete were tested in accordance with GB8076-2008 "Concrete Admixtures". The results are shown in Table 2.

[0090] Table 2 Performance test results of water reducing agent prepared in application example

[0091]

[0092] It can be seen from Table 2 that after the polyethylene glycol monomethyl ether hydroxypropyl methacrylate prepared by the present invention is used to prepare the water reducer, the obtained water reducer has excellent performance test, good packaging, good workability, and fully meets the daily use requirements.

[0093] In summary, the preparation method of the present invention has simple process, high conversion rate, few side reactions, and saves solvent, and can simplify the production process, reduce production costs, and improve product quality.

[0094] Those skilled in the art should note that the embodiments described in the present invention are merely exemplary, and various other substitutions, changes and improvements may be made within the scope of the present invention. Therefore, the present invention is not limited to the above embodiments, but only to the claims.

Claims

1. A method for preparing a water reducing agent, characterized in that: Including the preparation of polyether ester and the preparation of water reducing agent; The preparation method of polyether ester comprises: Add 1200g of polyethylene glycol monomethyl ether with an average molecular weight of 1200 into a three-necked flask, add 12g of NaOH as a catalyst, 12g of phenothiazine and 6g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical as a polymerization inhibitor, raise the temperature to 120°C, dropwise add a methacrylate glycidyl methacrylate solution including 142.43g of methacrylate glycidyl methacrylate and 0.072g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical, control the dropwise addition time to 3h, and ripen for 30min after the dropwise addition is completed to obtain a polyether ester; The preparation method of the water reducing agent comprises: In a 1L round-bottom flask, add 271g of deionized water, fully evacuate with nitrogen and continue to add nitrogen to keep the system in a nitrogen protection environment; start stirring and heating to raise the temperature of the deionized water in the flask and maintain it at 88-90°C; dropwise add the pre-configured material A and material B into the flask; A material preparation method: ester ether: water: MAS = 100g: 266.45g: 2.241g, wherein the ester ether is prepared by the above-mentioned preparation method of polyether ester, and MAS is sodium methyl allyl sulfonate; Material B preparation method: APS: water = 2.075g: 39.4g, APS is ammonium persulfate; All water used was deionized water; Material A is added dropwise at a constant speed for 3 hours, and material B is added dropwise at the same time as material A for 3.5 hours; after the addition of material B is completed, it is aged at 88-90°C for 1 hour; the temperature is lowered to 30°C, a sodium hydroxide solution with a mass concentration of 30% is added, the pH value of the system is adjusted to 6.5-7.5, and the material is discharged to obtain a water reducer.

Citation Information

Patent Citations

  • Method for preparing alkyl polyethenoxy ether acrylic ester, or alkyl polyethenoxy ether methyl acrylic ester

    CN101092478A

  • Method for synthesizing polyethyleneglycol monomethyl ether metacrylic acid ester

    CN101289533A

  • Polyalkylene glycol-based polymer

    JP2011132364A

  • Method for producing polyalkylene glycol monomer

    JP2012057030A