Modified conjugated diene polymer, preparation method thereof and rubber composition containing same
Through the continuous polymerization process of modified conjugated diene-based polymers, the dispersion and performance problems of the existing rubber composition are solved, and high modification rate, low glass transition temperature and excellent rubber composition performance are achieved.
Patent Information
- Application Number
- CN202180005563.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-20
- Filing Date
- 2021-01-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-01-18
AI Technical Summary
When the existing rubber composition reduces the tire driving resistance and improves wear resistance, poor dispersion leads to a decrease in overall physical properties and poor tensile and processability.
Modified conjugated diene polymers were used, and the molecular weight distribution curve was single peak shape by gel permeation chromatography, with narrow molecular weight distribution, high Si content and excellent cold flow properties. It was prepared by continuous polymerization to improve viscoelasticity and stability. sex.
High modification rate and low glass transition temperature are achieved, and the wear resistance, storage stability and molding stability of the rubber composition are improved while maintaining excellent rolling resistance.
Smart Images

Figure CN114450319B_ABST
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority from Korean Patent Application No. 10-2020-0007494, filed on January 20, 2020, which is hereby incorporated by reference in its entirety. Technical Field
[0004] The present invention relates to a modified conjugated diene polymer, a preparation method thereof and a rubber composition containing the same. Background Art
[0005] Recently, with the increasing attention paid to energy conservation and environmental protection, it is required to reduce the fuel consumption rate of automobiles. Therefore, materials having modulation stability represented by wet skid resistance, low running resistance, excellent wear resistance and tensile properties are required as rubber materials for tires.
[0006] In order to reduce the running resistance of tires, there is a method of reducing the hysteresis loss of vulcanized rubber, and the rebound resilience, tanδ, Goodrich heating at 50°C to 80°C are used as evaluation indicators of vulcanized rubber. That is, it is desirable to use a rubber material having high rebound resilience or low tanδ value or Goodrich heating at the above temperature.
[0007] As a method of meeting this requirement, a method of using inorganic fillers (such as silica and carbon black) in a rubber composition for forming a tire to reduce the heating performance of the tire has been proposed. However, the inorganic filler has poor dispersibility in the rubber composition, which may reduce the overall physical properties of the rubber composition (including wear resistance, crack resistance or processability).
[0008] In order to solve such a problem, a method for improving the dispersibility of inorganic fillers such as silica and carbon black in a rubber composition has been proposed, which uses a modifier containing a functional group capable of interacting with the inorganic filler to modify the polymerization active part of a conjugated diene-based polymer obtained by anionic polymerization using organic lithium. However, even if the low heat resistance is improved, the stretchability, wear resistance and processability are still poor. Summary of the invention
[0009] [Technical issues]
[0010] The present invention is made to solve the above-mentioned problems of the prior art, and its purpose is to provide a modified conjugated diene polymer and a preparation method thereof that simultaneously satisfies high modification rate and low glass transition temperature, wherein the polymer has a single-peak shape of a gel permeation chromatography molecular weight distribution curve, has a narrow molecular weight distribution of less than 1.70, a high Si content of more than 100 ppm and excellent cold flow properties.
[0011] Furthermore, an object of the present invention is to provide a rubber composition comprising a modified conjugated diene-based polymer having improved viscoelasticity at high and low temperatures and at the same time having wear resistance, in particular, maintaining rolling resistance at an excellent level, improving cold flow, and having excellent storage stability and molding stability.
[0012] [Technical solution]
[0013] To solve the above problems, according to one embodiment of the present invention, the present invention provides a modified conjugated diene polymer, which meets the following conditions: a) the molecular weight distribution curve of gel permeation chromatography (GPC) has a single peak shape; b) the molecular weight distribution (PDI; MWD) is greater than 1.00 and less than 1.70; c) the cold flow is less than 1.00; d) based on the total weight of the modified conjugated diene polymer, the Si content is greater than 100 ppm.
[0014] In addition, the present invention provides a method for preparing a modified conjugated diene polymer, which comprises: polymerizing a conjugated diene monomer in a hydrocarbon solvent in the presence of a polymerization initiator to prepare an active polymer (S1); reacting the active polymer prepared in step (S1) with a modifier (S2), wherein the polymerization reaction (S1) and the modification reaction (S2) are carried out continuously, and step (S1) is carried out in two or more polymerization reactors, and the polymerization conversion rate in the first polymerization reactor among these polymerization reactors is less than 50%, and the modifier comprises a first modifier and a second modifier, the first modifier is a modifier having more than five reactive functional groups capable of reacting with the active polymer, and the second modifier is a modifier having less than five reactive functional groups capable of reacting with the active polymer.
[0015] Furthermore, the present invention provides a rubber composition comprising the modified conjugated diene-based polymer and a filler.
[0016] [Beneficial Effects]
[0017] The modified conjugated diene polymer of the present invention satisfies both high modification rate and low glass transition temperature, and the gel permeation chromatography molecular weight distribution curve can have a single peak shape, a narrow molecular weight distribution of less than 1.70, a high Si content of 100 ppm or more, and excellent cold flowability.
[0018] The modified conjugated diene polymer of the present invention, although prepared by a continuous polymerization process, has excellent high and low temperature viscoelasticity due to its narrow molecular weight distribution and can be improved to an excellent level of wear resistance due to its low glass transition temperature. In addition, the modified conjugated diene polymer of the present invention has improved cold flowability, and when compounded with a rubber composition, can significantly improve storage stability and molding stability while maintaining rolling resistance at an excellent level.
[0019] Furthermore, the modified conjugated diene-based polymer of the present invention includes a functional group derived from a modifier, and stretchability and viscoelasticity can be further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings attached to this specification illustrate preferred examples of the present invention and are used together with the detailed description to enable a further understanding of the technical concept of the present invention. Therefore, the present invention should not be interpreted solely by the contents of the drawings.
[0021] Figure 1 The molecular weight distribution curve of the modified conjugated diene-based polymer of Example 1 according to the embodiment of the present invention is shown by gel permeation chromatography (GPC). DETAILED DESCRIPTION
[0022] Hereinafter, the present invention will be described in more detail to help understanding of the present invention.
[0023] It should be understood that the words or terms used in the description and claims of the present invention should not be interpreted as the meanings defined in commonly used dictionaries. It should also be understood that based on the principle that the inventor can appropriately define the meaning of words or terms to best explain the present invention, the words or terms should be interpreted as having a meaning consistent with the meaning of the technical idea of the present invention.
[0024] definition
[0025] The term "polymer" used in the present invention refers to a macromolecular compound prepared by polymerization of monomers of the same or different types. Similarly, the general term "polymer" includes the term "homopolymer" which is usually used to refer to a polymer prepared from only one monomer and the term "copolymer" which is usually used to refer to a polymer prepared from two or more monomers.
[0026] The term "vinyl content" used in the present invention refers to the mass (or weight) percentage of butadiene contained in positions 1 and 2 of the polymer chain based on the conjugated diene monomer (butadiene, etc.) portion (total weight of polymerized butadiene) in the polymer.
[0027] In the present invention, the term "monovalent hydrocarbon group" may refer to a monovalent atomic group obtained by bonding carbon and hydrogen in a monovalent alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, a cycloalkyl group containing one or more unsaturated bonds, and an aryl group, and the minimum carbon number of the substituent represented by the monovalent hydrocarbon may be determined according to the kind of each substituent.
[0028] In the present invention, the term "divalent hydrocarbon group" may refer to a divalent atomic group obtained by bonding carbon and hydrogen in a divalent alkylene group, an alkenylene group, an alkynylene group, a cycloalkylene group, a cycloalkylene group containing one or more unsaturated bonds, and an arylene group, and the minimum carbon number of the substituent represented by the divalent hydrocarbon may be determined according to the kind of each substituent.
[0029] In the present invention, the term "alkyl" may refer to a monovalent aliphatic saturated hydrocarbon and may include straight chain alkyl groups such as methyl, ethyl, propyl and butyl, and branched alkyl groups such as isopropyl, sec-butyl, tert-butyl and neopentyl.
[0030] In the present invention, the term "alkenyl" may refer to a monovalent aliphatic unsaturated hydrocarbon including one or two or more double bonds.
[0031] In the present invention, the term "alkynyl" may refer to a monovalent aliphatic unsaturated hydrocarbon including one or two or more triple bonds.
[0032] In the present invention, the term "alkylene group" may refer to a divalent aliphatic saturated hydrocarbon such as methylene, ethylene, propylene and butylene.
[0033] In the present invention, the term "aryl group" may refer to a cyclic aromatic hydrocarbon and may include a monocyclic aromatic hydrocarbon forming one ring and a polycyclic aromatic hydrocarbon combining two or more rings.
[0034] In the present invention, the term "heterocyclic group" is obtained by substituting a carbon atom in a cycloalkyl group or an aryl group with one or more hetero atoms, and may refer to a heterocycloalkyl group and a heteroaryl group.
[0035] The terms "including" and "having" and their derivatives in the present invention, whether specifically disclosed or not, are not intended to exclude the existence of optional additional components, steps or processes. In order to avoid any uncertainty, all compositions claimed using the term "comprising" may include optional additional additives, adjuvants or compounds, including polymers or any other materials, unless otherwise described to the contrary. In contrast, the term "essentially consisting of..." excludes content that is not necessary for the work and excludes optional other components, steps or processes outside the scope of the optional continuous description. The term "consisting of..." excludes optional components, steps or processes that are not specifically described or illustrated.
[0036] Measurement methods and conditions
[0037] In the present invention, the "1,2-vinyl bond content" is obtained as follows: the vinyl content in each polymer is measured and analyzed using a Varian VNMR S500 MHz NMR and using 1,1,2,2-tetrachloroethane as a solvent during the NMR measurement, and the 1,2-vinyl bond content in the total polymer is calculated by calculating 6.0 ppm as a solvent peak, 7.2-6.9 ppm as a random styrene peak, 6.9-6.2 ppm as a block styrene peak, 5.8-5.1 ppm as 1,4-vinyl and 1,2-vinyl peaks, and 5.1-4.5 ppm as a 1,2-vinyl peak.
[0038] In the present invention, "weight average molecular weight (Mw)", "number average molecular weight (Mn)" and "molecular weight distribution (MWD)" are measured by gel permeation chromatography (GPC) analysis and examination of the molecular weight distribution curve. Molecular weight distribution (PDI, MWD, Mw / Mn) is calculated based on each measured molecular weight. In particular, the GPC combination uses two PLgel Olexis columns (Polymer Laboratories Co.) and one PLgel mix-C column (Polymer Laboratories Co.), polystyrene (PS) is used as the GPC standard to calculate the molecular weight, and tetrahydrofuran mixed with 2 wt% amine compound is used as the GPC measurement solvent. The conditions used are: sample concentration 1-2 mg / mL (diluted with THF), flow rate 1 mL / min, injection volume 100 uL, column temperature 40°C, and the detector uses a refractive index.
[0039] In the present invention, Mooney viscosity (MV; (ML1+4, @100°C MU) is measured using MV-2000 (ALPHA Technologies Co.) using a large rotor at a rotor speed of 2±0.02 rpm at 100°C. In this case, the sample used is left to stand at room temperature (23±3°C) for 30 minutes or more, and then 27±3g of the sample is collected and put into the mold cavity, and then, the platen is operated for 4 minutes for measurement.
[0040] In the present invention, the glass transition temperature (Tg) is obtained as follows: using a modified conjugated diene polymer as a sample, based on ISO22768:2006, using a differential scanning calorimeter (product name "DSC3200S", manufactured by MacScience Inc.), helium is circulated at a rate of 50 ml / min, and the DSC curve is recorded while the temperature is raised from -100°C at a rate of 10°C / min, and the peak top (inflection point) of the DSC differential curve is measured as the glass transition temperature.
[0041] In the present invention, in order to obtain cold flow, a modified conjugated diene polymer is used as a sample, and a temperature dynamic equilibrium between the sample and the oven is reached in an oven at 50°C. After standing for 10 minutes, the protruding polymer sample is taken out and placed in a static state. Then, the polymer sample is extruded through a 1.4-inch orifice at a pressure of 34.6 kPa, and the extrusion amount of the polymer sample flowing out through the orifice is measured at intervals of 30 minutes for 90 minutes. The extrusion amount is calculated in grams per minute (mg / min) and displayed as cold flow. The smaller the value, the better the molding stability (storage stability).
[0042] In the present invention, "Si content" is measured using inductively coupled plasma optical emission spectroscopy (ICP-OES; Optima 7300DV) as an ICP analysis method. If inductively coupled plasma optical emission spectroscopy is used, the measurement is performed in the following manner: about 0.7 g of the sample is added to a platinum (Pt) crucible, about 1 mL of concentrated sulfuric acid (98 wt %, electronic grade) is added thereto, heated at 300° C. for 3 hours, and the sample is incinerated in an electric furnace (Thermo Scientific, Lindberg Blue M) according to the procedure of steps 1 to 3 below:
[0043] 1) Step 1: initial temperature 0°C, rate (temperature / hour): 180°C / hour, temperature (holding time): 180°C (1 hour);
[0044] 2) Step 2: initial temperature 180°C, rate (temperature / hour): 85°C / hour, temperature (holding time): 370°C (2 hours); and
[0045] 3) Step 3: initial temperature 370°C, rate (temperature / hour): 47°C / hour, temperature (holding time): 510°C (3 hours),
[0046] Add 1 mL of concentrated nitric acid (48 wt%) and 20 μl of concentrated hydrofluoric acid (50 wt%) to the residue, seal the platinum crucible, and shake for more than 30 minutes. Add 1 mL of boric acid to the sample, store at 0°C for more than 2 hours, dilute with 30 ml of ultrapure water, and incinerate.
[0047] In the present invention, "N content" can be obtained by measuring N content, for example, by NSX analysis method, and the measurement of NSX analysis method can use trace nitrogen quantitative analyzer (NSX-2100H). For example, when using trace nitrogen quantitative analyzer, turn on trace nitrogen quantitative analyzer (autosampler, horizontal furnace, PMT & nitrogen detector), set the carrier gas flow rate to Ar250ml / min, O 2350ml / min, ozone generator 300ml / min, heater is set to 800 ℃, analyzer is left to stand for about 3 hours to stabilize. After stabilizing the analyzer, a calibration curve of 5ppm, 10ppm, 50ppm, 100ppm and 500ppm calibration curve range is made using nitrogen standard sample (AccuStandard S-22750-01-5ml), and the area corresponding to each concentration is obtained. Then, a straight line is drawn using the ratio of concentration to area. Afterwards, a ceramic boat equipped with 20mg sample is placed in the automatic sampler of the analyzer and measured to obtain the area. Using the area and calibration curve of the sample thus obtained, N content is calculated. In this case, the sample is a modified conjugated diene polymer, and its solvent has been removed by placing the sample in hot water heated and stirred by steam, and can be a sample from which residual monomers, residual modifiers and oils have been removed.
[0048] The present invention provides a modified conjugated diene polymer having a combination of physical properties within a specific range and capable of simultaneously improving the mixing performance (especially viscoelasticity and wear resistance), storage stability and molding stability of the rubber composition when applied to the rubber composition.
[0049] According to one embodiment of the present invention, the present invention is characterized in that a modified conjugated diene polymer is provided, which satisfies the following conditions: a) the molecular weight distribution curve of gel permeation chromatography (GPC) has a single peak shape; b) the molecular weight distribution (PDI; MWD) is greater than 1.00 and less than 1.70; c) the cold flow is less than 1.00; d) based on the total weight of the modified conjugated diene polymer, the Si content is greater than 100 ppm.
[0050] According to one embodiment of the present invention, the modified conjugated diene polymer may include repeating units derived from conjugated diene monomers and functional groups derived from modifiers, wherein the repeating units derived from conjugated diene monomers may refer to repeating units formed by conjugated diene monomers during the polymerization process, and the functional groups derived from the modifier may refer to functional groups derived from the modifier present at at least one end of the active polymer through reaction or coupling between the active polymer (made by polymerization of conjugated diene monomers) and the modifier.
[0051] According to one embodiment of the present invention, the conjugated diene monomer may be one or more selected from 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, pentadiene, 3-butyl-1,3-octadiene, isoprene, 2-phenyl-1,3-butadiene and 2-halogeno-1,3-butadiene (halogeno refers to a halogen atom).
[0052] In addition, the modified conjugated diene polymer can be a copolymer further comprising repeating units derived from aromatic vinyl monomers, and in this case, can comprise 30 wt % or more, or 30 wt % to 50 wt % of repeating units derived from aromatic vinyl monomers. Preferably, the present invention may not include repeating units derived from aromatic vinyl monomers.
[0053] In the case where the polymer contains repeating units derived from aromatic vinyl monomers, the aromatic vinyl monomers can be, for example, one or more selected from styrene, α-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 1-vinylnaphthalene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene and 1-vinyl-5-hexylnaphthalene.
[0054] In another embodiment, in addition to the repeating units derived from conjugated diene monomers, the modified conjugated diene polymer can be a copolymer further comprising repeating units derived from diene monomers having 1 to 10 carbon atoms. The repeating units derived from diene monomers can be repeating units derived from diene monomers different from the conjugated diene monomers, and the diene monomers different from the conjugated diene monomers can be, for example, 1,2-butadiene. If the modified conjugated diene polymer is a copolymer further comprising a diene monomer, the modified conjugated diene polymer can include greater than 0 wt % to 1 wt %, greater than 0 wt % to 0.1 wt %, greater than 0 wt % to 0.01 wt %, or greater than 0 wt % to 0.001 wt % of repeating units derived from diene monomers, and within this range, the effect of preventing gel formation can be achieved.
[0055] The number average molecular weight (Mn) of the modified conjugated diene polymer of one embodiment of the present invention can be 1,000 g / mol to 2,000,000 g / mol, 10,000 g / mol to 1,000,000 g / mol or 100,000 g / mol to 1,000,000 g / mol, preferably 200,000 g / mol to 1,000,000 g / mol or 300,000 g / mol to 700,000 g / mol. Within this range, excellent rolling resistance and anti-slip properties can be achieved. In another embodiment, the molecular weight distribution (PDI; MWD; Mw / Mn) of the modified conjugated diene polymer can be 1.00 or more and less than 1.70, or 1.10 or more and less than 1.70, within this range, excellent effects such as balance between stretchability, viscoelasticity and physical properties can be achieved. Meanwhile, the gel permeation chromatography (GPC) molecular weight distribution curve of the modified conjugated diene polymer has a unimodal shape, which is the molecular weight distribution shown by the polymer obtained by continuous polymerization, and can mean that the modified conjugated diene polymer has a uniform property. That is, the modified conjugated diene polymer of an embodiment of the present invention is prepared by continuous polymerization, and has a unimodal molecular weight distribution curve and a molecular weight distribution of more than 1.00 and less than 1.70. By satisfying the above-mentioned physical properties at the same time, excellent processability and excellent level of viscoelasticity, such as rolling resistance and road resistance, can be obtained.
[0056] In addition, the Si content of the modified conjugated diene polymer can be 100ppm or more, 100ppm to 10000ppm, 100ppm to 5000ppm, 100ppm to 1000ppm or 100ppm to 500ppm based on weight, within which the rubber composition comprising the modified conjugated diene polymer can have excellent physical property effects, including stretchability and viscoelasticity. The Si content can refer to the content of Si atoms present in the modified conjugated diene polymer. At the same time, the Si atom can come from a functional group derived from a modifier.
[0057] The Si content can be measured by, for example, ICP analysis, and the ICP analysis can be performed using inductively coupled plasma optical emission spectroscopy (ICP-OES; Optima 7300DV). If inductively coupled plasma optical emission spectroscopy is used, the measurement is performed in the following manner: about 0.7 g of the sample is added to a platinum (Pt) crucible, about 1 mL of concentrated sulfuric acid (98 wt %, electronic grade) is added thereto, heated at 300° C. for 3 hours, and the sample is incinerated in an electric furnace (Thermo Scientific, Lindberg Blue M) according to the procedure of steps 1 to 3 below:
[0058] 1) Step 1: initial temperature 0°C, rate (temperature / hour): 180°C / hour, temperature (holding time): 180°C (1 hour);
[0059] 2) Step 2: initial temperature 180°C, rate (temperature / hour): 85°C / hour, temperature (holding time): 370°C (2 hours); and
[0060] 3) Step 3: initial temperature 370°C, rate (temperature / hour): 47°C / hour, temperature (holding time): 510°C (3 hours),
[0061] Add 1 mL of concentrated nitric acid (48 wt%) and 20 μl of concentrated hydrofluoric acid (50 wt%) to the residue, seal the platinum crucible, and shake for more than 30 minutes. Add 1 mL of boric acid to the sample, store at 0°C for more than 2 hours, dilute with 30 ml of ultrapure water, and incinerate.
[0062] In this case, the sample is a modified conjugated diene-based polymer from which the solvent has been removed by placing in hot water heated with steam, and from which the residual monomer, the residual modifier and the oil are removed.
[0063] In addition, the cold flow of the modified conjugated diene polymer of one embodiment of the present invention can be less than 1.00, less than 0.90, less than 0.85 or less than 0.80. In addition, although the lower limit is not particularly limited, considering the prevention of deterioration of other viscoelasticity and mechanical properties, it can be preferably more than 0.10, more than 0.30, more than 0.50 or more than 0.60. In particular, the modified conjugated diene polymer can simultaneously meet the above-mentioned molecular weight distribution curve, molecular weight, molecular weight distribution and Si content and the cold flow within the above-mentioned range. Cold flow can be an index of storage stability and molding stability of the modified conjugated diene polymer. In particular, if the cold flow value is reduced, the storage stability and molding stability of the rubber composition containing the polymer can be improved. If the cold flow of the polymer is greater than 1.00, the storage stability and molding stability may be significantly deteriorated, and if the polymer is mixed into a rubber composition and stored, it will have an adverse effect on the quality.
[0064] Usually, in order to improve the compatibility with filler, if a modified polymer, particularly a terminal modified polymer, is formed that uses a specific modifier that helps to improve compatibility, the polymer chain mainly has a linear structure. However, if the ratio of the polymer chain with a linear structure is high, cold flow increases, and fluidity increases. Therefore, storage stability and molding stability are adversely affected, and if mixed, stored and used rubber composition, its quality may be adversely affected. In order to improve these defects, the modifier that can form a branched structure is used for modification, so that the deterioration of cold flow can be partially prevented, but side chains can be increased, and the defect causing the rolling resistance to be significantly reduced may occur when mixing rubber composition.
[0065] The present invention is characterized in that a modified conjugated diene-based polymer having a low cold flow value while maintaining an excellent level of rolling resistance during compounding of a rubber composition is provided by forming a polymer product mainly having a linear structure polymer chain and partially having a branched structure.
[0066] By mixing two types of modifiers having different numbers of reactive functional groups that can react with the active polymer as the modifier, a modified conjugated diene-based polymer having a low cold flow value and excellent rolling resistance when compounding a rubber composition can be obtained. In particular, as described below, by mixing a modifier having five or less reactive functional groups with a modifier having more than five reactive functional groups, the above physical properties can be achieved.
[0067] In addition, the glass transition temperature (Tg) of the modified conjugated diene polymer of one embodiment of the present invention can be -100°C to -50°C, preferably -90°C to -60°C. In particular, the modified conjugated diene polymer can simultaneously satisfy the above molecular weight distribution curve, molecular weight, molecular weight distribution, Si content and cold flow and the glass transition temperature within the above range. The glass transition temperature can be an index of wear resistance of the rubber composition comprising the modified conjugated diene polymer, and specifically, if the glass transition temperature is reduced, the wear resistance will increase when mixed into the rubber composition.
[0068] Also, according to one embodiment of the present invention, if the glass transition temperature of the modified conjugated diene-based polymer satisfies -100°C to -50°C, stretchability and viscoelasticity may be excellent, while the effect of significantly improving wear resistance may be achieved.
[0069] In addition, the N content of the modified conjugated diene polymer may be 50 ppm or more, 100 ppm or more, 100 ppm to 10,000 ppm, or 100 ppm to 5,000 ppm based on the total weight, within which the rubber composition including the modified conjugated diene polymer may exhibit excellent mechanical properties such as tensile strength and viscoelasticity. The N content may refer to the content of N atoms present in the modified conjugated diene polymer, in which case the N atoms may be derived from a functional group derived from a modifier.
[0070] In addition, the N content can be measured by the NSX analysis method, and the NSX measurement method can use a trace nitrogen quantitative analyzer (NSX-2100H).
[0071] For example, when using a trace nitrogen quantitative analyzer, turn on the trace nitrogen quantitative analyzer (autosampler, horizontal furnace, PMT & nitrogen detector), set the carrier gas flow rate to Ar 250ml / min, O 2 350ml / min, ozone generator 300ml / min, the heater is set to 800℃, and the analyzer is left to stand for about 3 hours to stabilize it. After the analyzer is stabilized, a calibration curve of 5ppm, 10ppm, 50ppm, 100ppm and 500ppm calibration curve range is made using a nitrogen standard (AccuStandard S-22750-01-5ml), and the area corresponding to each concentration is obtained. Then, a straight line is drawn using the ratio of concentration to area. Afterwards, a ceramic boat containing 20mg of the sample is placed in the automatic sampler of the analyzer and measured to obtain the area. Using the area and calibration curve of the sample thus obtained, the N content is calculated.
[0072] In this case, the sample is a modified conjugated diene polymer, the solvent of which has been thermally removed by placing the sample in hot water heated by steam and stirred, and may be a sample from which residual monomers, residual modifiers, and oil have been removed. In addition, if oil is added to the sample, the sample may be obtained after extracting (removing) the oil.
[0073] In addition, the modified conjugated diene-based polymer may have a Mooney viscosity at 100° C. of 30 or more, 40 to 150, or 40 to 140, and within this range, processability and productivity may be excellent.
[0074] In addition, the modified conjugated diene polymer of the embodiment of the present invention may preferably satisfy: based on the total weight of the polymer, the 1,2-vinyl bond content is 30.0 wt% or less. The vinyl content may refer to the weight % of the conjugated diene monomer that is not 1,4-added but 1,2-added relative to the conjugated diene copolymer composed of the monomer having a vinyl group and the aromatic vinyl monomer, and may be affected by the polymerization reaction end point, the reaction environment at the polymerization reaction end point during the polymerization process, and the like.
[0075] In particular, the 1,2-vinyl bond content may be 5 to 30% by weight, preferably 5 to 15% by weight, and depending on the 1,2-vinyl bond content, wear resistance and rolling resistance performance may be affected. If the 1,2-vinyl bond content is 30% by weight or less, better wear resistance can be ensured. Therefore, it is preferred that the 1,2-vinyl bond content satisfies the above range when preparing the modified conjugated diene polymer.
[0076] As described above, if the modified conjugated diene polymer of the present invention satisfies the above conditions at the same time, a high modification rate can be obtained, and by being applied to a rubber composition, the viscoelasticity, wear resistance, storage stability and molding stability of the rubber composition can be improved to excellent levels.
[0077] In addition, by controlling the polymerization temperature, polymerization time, and the amount of reactants, the modified conjugated diene polymer of the present invention can be prepared to meet the above-mentioned unimodal molecular weight distribution curve shape, molecular weight, molecular weight distribution, glass transition temperature, cold flow, and Si content.
[0078] According to one embodiment of the present invention, the present invention provides a method for preparing a modified conjugated diene polymer, which comprises: polymerizing a conjugated diene monomer in a hydrocarbon solvent in the presence of a polymerization initiator to prepare a living polymer (S1); reacting the living polymer prepared in step (S1) with a modifier (S2), wherein the polymerization reaction (S1) and the modification reaction (S2) are carried out continuously, and step (S1) is carried out in two or more polymerization reactors, and the polymerization conversion rate in the first polymerization reactor of these polymerization reactors is less than 50%, and the modifier comprises at least two modifiers having different numbers of reactive functional groups. In particular, the modifier comprises a first modifier and a second modifier, the first modifier is a modifier having more than five reactive functional groups capable of reacting with the living polymer, and the second modifier is a modifier having less than five reactive functional groups capable of reacting with the living polymer.
[0079] In addition, the modified conjugated diene polymer may be a polymer obtained by the preparation method.
[0080] Meanwhile, the modifier that modifies the modified conjugated diene-based polymer in the present invention may be a modifier having affinity for silica, and the modified conjugated diene-based polymer may include a unit derived from the modifier at at least one chain end thereof.
[0081] In particular, the modifier may be a modifier containing a functional group having affinity with silica in the compound used as the modifier. Such a functional group having affinity with silica may refer to a functional group having excellent affinity with a filler, particularly a silica-based filler, and capable of generating an interaction between the silica-based filler and the functional group derived from the modifier.
[0082] The modifier can be, for example, an alkoxysilane modifier, particularly an alkoxysilane modifier comprising one or more heteroatoms, wherein the heteroatoms include nitrogen atoms, oxygen atoms or sulfur atoms. If an alkoxysilane modifier is used, the end of the active polymer can be modified or coupled to a bonding state with a silyl group by a substitution reaction between the anionic active part at one end of the active polymer and the alkoxy group of the alkoxysilane modifier. As described above, according to one embodiment of the present invention, in the modifier, the reactive functional group capable of reacting with the active polymer can particularly include an alkoxy group, and particularly, the alkoxy group can be combined with a silicon (Si) atom.
[0083] According to one embodiment of the present invention, the modifier may include at least two modifiers, namely a first modifier and a second modifier, specifically, the first modifier is a modifier having more than five reactive functional groups capable of reacting with an active polymer, and the second modifier is a modifier having less than five reactive functional groups capable of reacting with an active polymer.
[0084] In particular, the first modifier may include a compound represented by Formula 1 below, and the second modifier may include at least one or more compounds represented by Formula 2 and Formula 3 below.
[0085] [Formula 1]
[0086]
[0087] In formula 1, R a1 and R a4 may be independently a single bond or an alkylene group of 1 to 10 carbon atoms, R a2 and R a3 may be independently an alkyl group of 1 to 10 carbon atoms, R a5may be a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, a divalent, trivalent or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms, or a five-membered heterocyclic group having 2 to 4 carbon atoms, which includes one or more heteroatoms selected from N, O and S, wherein the heterocyclic group may be unsubstituted or substituted with an alkyl group having 1 to 10 carbon atoms or a (trialkoxysilyl)alkyl group, and the alkyl group in the (trialkoxysilyl)alkyl group may be an alkyl group having 1 to 10 carbon atoms, and the alkoxy group may be an alkoxy group having 1 to 10 carbon atoms; m 1 It can be an integer from 1 to 3, m 2 It can be an integer from 0 to 2, where -(OR a2 )The total number of groups can be greater than five.
[0088] In another embodiment, the compound represented by Formula 1 may be a compound represented by the following Formula 1-1.
[0089] [Formula 1-1]
[0090]
[0091] In formula 1-1, R d1 It can be hydrogen or an alkyl group of 1 to 10 carbon atoms, R d2 To R d4 may be independently an alkylene group having 1 to 10 carbon atoms, R d5 To R d8 can be independently an alkyl group of 1 to 10 carbon atoms, A 3 Can be Where R d9 To R d12 may be each independently hydrogen or an alkyl group of 1 to 10 carbon atoms, and t 1 and t 2 Can be 3 independently.
[0092] In particular, in Formula 1, R a1 and R a4 may be independently a single bond or an alkylene group of 1 to 5 carbon atoms, R a2 and R a3 can be independently an alkyl group of 1 to 5 carbon atoms, R a5It may be a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a tetravalent alkylsilyl group substituted with an alkyl group having 1 to 5 carbon atoms, a five-membered heterocyclic group having 2-4 carbon atoms, which includes one or more heteroatoms selected from N, O and S, wherein the heterocyclic group may be unsubstituted or substituted with an alkyl group having 1 to 5 carbon atoms or a (trialkoxysilyl)alkyl group, and the alkyl group in the (trialkoxysilyl)alkyl group may be an alkyl group having 1 to 5 carbon atoms, and the alkoxy group may be an alkoxy group having 1 to 5 carbon atoms. In addition, the five-membered heterocyclic group may be a five-membered heterocyclic group containing N in particular.
[0093] In addition, the compound represented by Formula 1 according to another embodiment of the present invention may specifically be a compound represented by Formula 1-1, and in Formula 1-1, R d1 It can be hydrogen or an alkyl group of 1 to 5 carbon atoms, R d2 To R d4 may be independently an alkylene group having 1 to 5 carbon atoms, R d5 To R d8 can be independently an alkyl group of 1 to 5 carbon atoms, A 3 Can be Where R d9 To R d12 Each independently may be hydrogen or an alkyl group of 1 to 5 carbon atoms.
[0094] More specifically, the compound represented by Formula 1 may be one or more selected from the following groups: N,N-bis(3-(trimethoxysilyl)propyl)-methyl-1-amine, N,N-bis(3-(triethoxysilyl)propyl)-methyl-1-amine, tris(trimethoxysilyl)amine, tris(3-(trimethoxysilyl)propyl)amine, N-(3-(1H-imidazol-1-yl)propyl)-3-(triethoxysilyl)-N-(3-(triethoxysilyl)propyl)propan-1-amine, 3-(4,5-dihydro-1H-imidazol-1-yl)-N,N-bis(3-(triethoxysilyl)propyl) propyl)-1H-(3-(trimethoxysilyl)propyl)-1H-((trimethoxysilyl)propyl)propan-1-amine, N-(3-(1H-1,2,4-triazol-1-yl)propyl)-3-(trimethoxysilyl)-N-((trimethoxysilyl)propyl)propan-1-amine, and 3-(trimethoxysilyl)-N-(3-(trimethoxysilyl)propyl)-N-(3-(1-(3-(trimethoxysilyl)propyl)-1H-1,2,4-triazol-3-yl)propyl)propan-1-amine.
[0095] [Formula 2]
[0096]
[0097] In formula 2, R b1 It can be a single bond or an alkylene group of 1 to 10 carbon atoms, R b2 and R b3 may be independently an alkyl group of 1 to 10 carbon atoms or -[R b6 O] n3 -R b7 , R b4 It may be a single bond, an alkylene group of 1 to 10 carbon atoms, or -[R b6 O] n3 , R b5 It may be a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a divalent, trivalent or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms, R b6 It can be an alkylene group having 1 to 10 carbon atoms, R b7 It can be an alkyl group of 1 to 10 carbon atoms, n 1 Can be an integer from 1 to 3, n 2 Can be an integer from 0 to 2, n 3 Can be an integer from 1 to 30, where –(OR b2 ) groups may be 5 or less. In another embodiment, in Formula 2, R b2 To R b4 At least one of the following may include -[R b6 O] n3 unit.
[0098] In particular, in Formula 2, R b1 It can be a single bond or an alkylene group of 1 to 5 carbon atoms, R b2 and R b3 may be independently an alkyl group of 1 to 5 carbon atoms or -[R b6 O] n3 -R b7 , R b4 It can be a single bond, an alkylene group of 1 to 5 carbon atoms, or -[R b6 O] n3 , R b5 It may be a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a tetravalent alkylsilyl group substituted with an alkyl group having 1 to 5 carbon atoms, R b6 It can be an alkylene group having 1 to 5 carbon atoms, R b7 It can be an alkyl group with 1 to 5 carbon atoms, n 1 Can be an integer of 2 or 3, n 2 Can be an integer from 0 to 2, n 3 Can be an integer from 1 to 10.
[0099] More specifically, the compound represented by Formula 2 may be one or more selected from the following groups: N,N-bis(3-(dimethoxy(methyl)silyl)propyl)-methyl-1-amine, N,N-bis(3-(diethoxy(methyl)silyl)propyl)-methyl-1-amine, N,N-diethyl-3-(trimethoxysilyl)propan-1-amine, N,N-diethyl-3-(triethoxysilyl)propan-1-amine, N,N-bis(3-(diethoxy(methyl)silyl)propyl)-methyl-1-amine, The compounds include N-(2,5,8,11,14-pentaoxahexadecan-16-yl)-N-(3-(triethoxysilyl)propyl)-2,5,8,11,14-pentaoxahexadecan-16-yl)-N-(3-(triethoxysilyl)propyl)-3,6,9,12-tetraoxahexadecan-1-yl)-N-(3-(triethoxysilyl)propyl)-3,6,9,12-tetraoxahexadecan-1-yl)-N-(3-(triethoxysilyl)propyl)-1,1,1-trimethylsilylamine.
[0100] [Formula 3]
[0101]
[0102] In formula 3, A 1 and A 2 may be independently an alkylene group having 1 to 20 carbon atoms, R c1 To R c4 may be independently an alkyl group having 1 to 20 carbon atoms, L 1 To L 4 Each may independently be an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or a divalent, trivalent or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms.
[0103] In particular, in Formula 3, A 1 and A 2 may be independently an alkylene group having 1 to 10 carbon atoms, R c1 To R c4 may be independently an alkyl group having 1 to 10 carbon atoms, L 1 To L 4 Each may independently be an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, or a tetravalent alkylsilyl group substituted with an alkyl group having 1 to 5 carbon atoms.
[0104] More specifically, the compound represented by Formula 3 may be one or more selected from the following group: 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropane-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropane-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dimethylpropane-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropane-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropane-1-amine), 1-Amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dipropylpropan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-diethylmethan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-diethylmethan-1-amine), 3-Tetraethoxydisiloxane-1,3-diyl)bis(N,N-diethylmethan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-diethylmethan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dimethylmethan-1-amine), 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-dipropylmethan-1-amine), 3,3'-(1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(N,N-dimethylmethan-1-amine), N,N-dipropylmethan-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dimethylmethan-1-amine), 3,3'-(1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(N,N-dipropylmethan-1-amine), N,N'-((1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(propane-3,1-diyl))bis(1,1,1-trimethyl-N-(trimethylsilyl)silaneamine, N,N'-((1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(propane-3,1-diyl))bis(1,1,1-trimethyl-N-(trimethylsilyl)silaneamine), N,N'-((1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(propane-3,1-diyl))bis(1,1,1-trimethyl-N-(trimethylsilyl)silaneamine), N,N'-((1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(propane-3,1-diyl))bis(1,1,1-trimethyl-N-phenylsilane amine), N,N'-((1,1,3,3-tetraethoxydisiloxane-1,3-diyl)bis(propane-3,1-diyl))bis(1,1,1-trimethyl-N-phenylsilylamine and N,N'-((1,1,3,3-tetrapropoxydisiloxane-1,3-diyl)bis(propane-3,1-diyl))bis(1,1,1-trimethyl-N-phenylsilylamine).
[0105] The modified conjugated diene polymer of one embodiment of the present invention may be: a polymer including a unit derived from a modifier represented by Formula 1 and a unit derived from a modifier represented by Formula 2, a polymer including a unit derived from a modifier represented by Formula 1 and a unit derived from a modifier represented by Formula 3, or a mixture thereof.
[0106] In addition, according to one embodiment of the present invention, the modifier may include a first modifier and a second modifier in an equivalent ratio of 1:9 to 5:5, preferably 1:9 to 4:6, more preferably 1:9 to 3:7. If the modifier content ratio is met, rolling resistance and cold flow can be further improved.
[0107] Hereinafter, the characteristics of the modified conjugated diene-based polymer thus prepared and the modifier used in the reaction overlap with the above description, and the description thereof will be omitted.
[0108] The hydrocarbon solvent is not particularly limited, and may be, for example, one or more selected from n-pentane, n-hexane, n-heptane, isooctane, cyclohexane, toluene, benzene, and xylene.
[0109] According to one embodiment of the present invention, the modified initiator can include an organometallic compound, and based on a total of 100 grams of monomers, the amount of the organometallic compound can be 0.01mmol to 10mmol, 0.05mmol to 5mmol, 0.1mmol to 2mmol, 0.1mmol to 1mmol or 0.15 to 0.8mmol. In addition, the organometallic compound can be, for example, selected from the group consisting of methyl lithium, ethyl lithium, propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, hexyl lithium, n-decyl lithium, tert-octyl lithium, phenyl lithium, 1-naphthyl lithium, n-eicosyl lithium, 4-butylphenyl lithium, 4-tolyl lithium, cyclohexyl lithium, 3,5-di-n-heptyl cyclohexyl lithium, 4-cyclopentyl lithium, sodium naphthyl, potassium naphthyl, lithium alcoholate, sodium alcoholate, potassium alcoholate, lithium sulfonate, sodium sulfonate, potassium sulfonate, lithium amide, sodium amide, potassium amide and isopropyl lithium amide.
[0110] The polymerization step (S1) can be, for example, anionic polymerization, in particular living anionic polymerization, in which anionic active parts are formed at the polymerization ends by the growth reaction of anions. In addition, the polymerization step (S1) can be heating polymerization, isothermal polymerization or constant temperature polymerization (adiabatic polymerization). Here, constant temperature polymerization refers to a polymerization method including a step of polymerization without optional heating after adding an organometallic compound but utilizing self-generated reaction heat, heating polymerization refers to a polymerization method including a polymerization method of increasing the temperature by optional heating after injecting an organometallic compound, and isothermal polymerization refers to a polymerization method of increasing heat by heating or heat release after adding an organometallic compound to keep the polymer temperature constant.
[0111] In addition, according to one embodiment of the present invention, the polymerization step (S1) can be carried out by further adding a diene compound having 1 to 10 carbon atoms in addition to the conjugated diene monomer, in which case the effect of preventing the formation of gel on the reactor wall during long-term operation can be achieved. The diene compound may include, for example, 1,2-butadiene.
[0112] The polymerization step (S1) can be carried out at a temperature range of 100° C. or less, 50° C. to 100° C., or 50° C. to 80° C. Within this range, the conversion rate of the polymerization reaction can be increased, and the Mooney viscosity, number average molecular weight, molecular weight distribution, cold flow and glass transition temperature of the polymer can be satisfied while controlling the molecular weight distribution of the polymer. Therefore, an excellent physical property improvement effect can be obtained.
[0113] The living polymer prepared by step (S1) may refer to a polymer in which a polymer anion and an organic metal cation are coupled.
[0114] In addition, according to one embodiment of the present invention, the method for preparing modified conjugated diene polymer can be carried out by continuous polymerization in multiple reactors including two or more polymerization reactors and modification reactor. In a specific embodiment, step (S1) can be carried out continuously in two or more polymerization reactors including the first reactor, and the number of polymerization reactors can be flexibly determined according to reaction conditions and environment. Continuous polymerization can refer to the reaction process in which reactants are continuously supplied to the reactor and the reaction product produced thereby is continuously discharged. By continuous polymerization, productivity and processability can be excellent, and the excellent effect of the uniformity of the polymer prepared in this way can be obtained.
[0115] In addition, according to one embodiment of the present invention, in the case of continuously preparing an active polymer in a polymerization reactor, the polymerization conversion rate in the first reactor can be 50% or less, 10% to 50%, or 20% to 50%, within which range, the side reaction generated when the polymer is formed after the polymerization reaction is initiated can be suppressed, and a polymer having a branched structure can be induced during the polymerization process. Therefore, the Mooney viscosity, number average molecular weight, molecular weight distribution, cold flow and glass transition temperature within the above range can be satisfied, and an excellent physical property improvement effect can be obtained.
[0116] In this case, the polymerization conversion rate can be controlled according to the reaction temperature, residence time, etc. in the reactor.
[0117] The polymerization conversion rate can be determined, for example, by measuring the solid concentration in the polymer solution phase containing the polymer during the polymerization of the polymer. In a specific embodiment, in order to ensure the polymer solution, a cylindrical container is installed at the outlet of each polymerization reactor, and a certain amount of polymer solution is filled in the cylindrical container. Then, the cylindrical container is separated from the reactor, the weight (A) of the cylinder filled with the polymer solution is measured, the polymer solution filled in the cylindrical container is transported to an aluminum container (such as an aluminum pan), the weight (B) of the cylindrical container after the polymer solution is removed is measured, the aluminum container containing the polymer solution is dried in an oven at 140°C for 30 minutes, the weight (C) of the dried polymer is measured, and calculated according to the following mathematical formula 1:
[0118] [Mathematical formula 1]
[0119]
[0120] At the same time, the polymer polymerized in the first reactor can be sequentially transported to the polymerization reactor before the modification reactor, and polymerization can be performed until the final polymerization conversion becomes 95% or more. After polymerization in the first reactor, the polymerization conversion in the second reactor or in each reactor from the second reactor to the polymerization reactor before the modification reactor can be appropriately controlled to control the molecular weight distribution.
[0121] At the same time, in step (S1), during the preparation of the active polymer, the residence time of the polymer in the first reactor can be 1 minute to 40 minutes, 1 minute to 30 minutes, or 5 minutes to 30 minutes. Within this range, the polymerization conversion rate is easy to control, so the Mooney viscosity, number average molecular weight, molecular weight distribution, cold flow and glass transition temperature within the above range can be met, and excellent physical property improvement effects can be obtained.
[0122] The term "polymer" in the present invention may refer to an intermediate of the polymer type being polymerized in each reactor during the step (S1), or may refer to a polymer being polymerized in a reactor with a polymerization conversion rate of less than 90% after completing step (S1) or step (S2) and before obtaining a living polymer or a modified conjugated diene polymer.
[0123] At the same time, the polymerization step (S1) can be carried out by including a polar additive, and the polar additive can be added in a ratio of 0.001g to 50g, or 0.002g to 0.1g based on a total of 100g of monomer. In another embodiment, based on a total of 100g of organometallic compound, the polar additive can be added in a ratio of greater than 0g to 1g, 0.01g to 1g, or 0.1g to 0.9g. In the case of injecting a polar additive within the above range, the glass transition temperature, Mooney viscosity and 1,2-vinyl bond content within the above range can be met.
[0124] Polar additive can be for example selected from the group consisting of tetrahydrofuran, ditetrahydrofuranyl propane, ether, cyclopentyl ether, dipropyl ether, vinyl methyl ether, vinyl dimethyl ether, diethylene glycol, dimethyl ether, tert-butoxyethoxyethane, bis(3-dimethylaminoethyl) ether, (dimethylaminoethyl) ethyl ether, trimethylamine, triethylamine, tripropylamine and tetramethylethylenediamine, one or more, preferably triethylamine or tetramethylethylenediamine. If polar additive is included, and if conjugated diene monomer or conjugated diene monomer and aromatic vinyl monomer are copolymerized, their reaction rate differences can be compensated, and the effect of easily forming random copolymer can be achieved.
[0125] According to one embodiment of the present invention, in the reaction of step (S2), based on 100g total monomer amount, modifier can be used in an amount of 0.01mmol to 10mmol. In another embodiment, based on the organometallic compound of the modified initiator in 1mol step (S1), modifier can be used in a mol ratio of 1:0.1 to 10, 1:0.1 to 5 or 1:0.1 to 1:3. The mol ratio of modifier to organometallic compound, modifier relative to the injection amount of monomer can significantly affect the glass transition temperature of the prepared polymer, and if possible, it is preferably possible to select and use a suitable ratio within the above range.
[0126] In addition, according to one embodiment of the present invention, the modifier may include at least two types of modifiers. For example, the modifier may include a modifier that can form a polymer chain into a linear structure and a modifier that can form a polymer chain into a branched structure after modification. When using two or more modifiers with the above characteristics, a linear polymer chain and a branched polymer chain can be mixed in the polymer, and therefore, the cold flow of the polymer can be reduced. Therefore, a polymer that satisfies all physical properties of the above-mentioned modified conjugated diene polymer can be prepared.
[0127] According to the present invention, there is provided a rubber composition comprising a modified conjugated diene-based polymer.
[0128] The rubber composition may contain 10 wt % or more, 10 wt % to 100 wt %, or 20 wt % to 90 wt % of the modified conjugated diene polymer, within which range mechanical properties such as tensile strength and wear resistance are excellent, and an excellent balance between physical properties can be achieved.
[0129] In addition, in addition to the modified conjugated diene polymer, the rubber composition may further include other rubber components as required, in which case the content of the rubber component may be 90% by weight or less of the total weight of the rubber composition. In a specific embodiment, based on 100 parts by weight of the modified conjugated diene polymer, the content of the other rubber components may be 1 part by weight to 900 parts by weight.
[0130] The rubber component may be, for example, a natural rubber or a synthetic rubber, specifically, natural rubber (NR), including cis-1,4-polyisoprene; modified natural rubber obtained by modifying or purifying common natural rubber, such as epoxidized natural rubber (ENR), deproteinized natural rubber (DPNR), hydrogenated natural rubber; and synthetic rubber, such as styrene-butadiene copolymer (SBR), polybutadiene (BR), polyisoprene (IR), butyl rubber (IIR), ethylene-propylene copolymer, copolymerized isobutylene-isoprene, chloroprene rubber, copolymer (ethylene-propylene), copolymer (styrene-butadiene), copolymer (styrene-isoprene), copolymer (styrene-isoprene-butadiene), copolymer (isoprene-butadiene), copolymer (ethylene-propylene-diene), polysulfide rubber, acrylic rubber, polyurethane rubber, silicone rubber, epichlorohydrin rubber and halogenated butyl rubber, and any one of them or a mixture of two or more thereof may be used.
[0131] Based on 100 weight portions of the modified conjugated diene polymer of the present invention, the rubber composition can include 0.1 weight portion to 200 weight portions or 10 weight portions to 120 weight portions of filler. The filler can be, for example, a silicon dioxide filler, particularly wet silicon dioxide (hydrated silicate), dry silicon dioxide (anhydrous silicate), calcium silicate, aluminum silicate or colloidal silicon dioxide. Preferably, the filler can be wet silicon dioxide, which has the most significant effect of improving the compatibility of damage characteristics and wet grip. In addition, as required, the rubber composition can also include a carbon black filler.
[0132] In another embodiment, if silica is used as a filler, a silane coupling agent for improving strengthening and low heat release properties may be used together. Specific examples of the silane coupling agent may include bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyltetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyltetrasulfide, The invention can be any one of the following: 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropylbenzothiazolyl tetrasulfide, 3-triethoxysilylpropylbenzoyl tetrasulfide, 3-triethoxysilylpropylmethacrylate monosulfide, 3-trimethoxysilylpropylmethacrylate monosulfide, bis(3-diethoxymethylsilylpropyl)tetrasulfide, 3-mercaptopropyldimethoxymethylsilane, dimethoxymethylsilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide or dimethoxymethylsilylpropylbenzothiazolyl tetrasulfide, and any one of them or a mixture of two or more thereof can be used. Preferably, bis(3-triethoxysilylpropyl)polysulfide or 3-trimethoxysilylpropylbenzothiazolyl tetrasulfide may be used in view of the improvement effect of the reinforcing property.
[0133] In addition, in the rubber composition of one embodiment of the present invention, since a modified conjugated diene polymer having a functional group with high affinity to silica is introduced in the active part as the rubber component, the compounding amount of the silane coupling agent can be less than that of the general case. Therefore, based on 100 parts by weight of silica, the amount of the silane coupling agent can be 1 to 20 parts by weight, or 5 to 15 parts by weight. Within the above amount range, the effect as a coupling agent can be fully exerted, and the effect of preventing the gelation of the rubber component can be achieved.
[0134] The rubber composition of the embodiment of the present invention can be sulfur crosslinkable, and can further include a vulcanizing agent. The vulcanizing agent can be sulfur powder in particular, and based on 100 parts by weight of the rubber component, its content can be 0.1 parts by weight to 10 parts by weight. Within this range, the elasticity and strength required for the vulcanized rubber composition can be ensured, while excellent low fuel consumption can be achieved.
[0135] The rubber composition of the embodiment of the present invention may include various additives used in the general rubber industry in addition to the above components, particularly vulcanization accelerators, processing oils, plasticizers, anti-aging agents, anti-scorch agents, zinc white, stearic acid, thermosetting resins or thermoplastic resins.
[0136] The vulcanization accelerator may include, for example, thiazole compounds such as 2-mercaptobenzothiazole (M), dibenzothiazolyl disulfide (DM) and N-cyclohexyl-2-benzothiazolyl sulfenamide (CZ), or guanidine compounds such as diphenylguanidine (DPG); the content thereof is 0.1 to 5 parts by weight based on 100 parts by weight of the rubber component.
[0137] Processing oil is used as softening agent in rubber composition, and can comprise for example paraffin, cycloalkane or aromatic compound.In view of tensile strength and wear resistance, aromatic processing oil can be used, in view of hysteresis loss and low temperature performance, cycloalkane or paraffin processing oil can be used.Based on the rubber component of 100 weight parts, the content of processing oil can be below 100 weight parts.Within the above range, the tensile strength of vulcanized rubber and the deterioration of low heat release performance (low fuel consumption rate) can be prevented.
[0138] Anti-aging agents may include, for example, N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline or a condensate of diphenylamine and acetone at high temperature; based on 100 parts by weight of the rubber component, its content is 0.1 parts by weight to 6 parts by weight.
[0139] The rubber composition of the embodiment of the present invention can be obtained by grinding according to the mixing formula using grinding equipment (such as Banbury mixer, roller and internal mixer). The rubber composition with low exothermicity and good wear resistance can be obtained by the vulcanization process after the molding process.
[0140] Therefore, the rubber composition can be used to manufacture various components of a tire, such as a tire tread, an undertread, a sidewall, a carcass coating rubber, a belt coating rubber, a bead filler, a chafer and a bead coating rubber, or to manufacture rubber products in various industries, such as anti-vibration rubber, a belt conveyor and a hose.
[0141] Furthermore, the present invention provides a tire produced using the rubber composition.
[0142] A tire may be a tire or include a tire tread.
[0143] Example
[0144] Hereinafter, the present invention will be explained in more detail with reference to embodiments. However, embodiments of the present invention may be modified to various other types, and the scope of the present invention should not be limited to the embodiments described below. Embodiments of the present invention are provided to fully explain the present invention to those of ordinary skill in the art.
[0145] Example 1
[0146] Into the first reactor of the continuous reactor of the three series reactors, a 1,3-butadiene solution (wherein 60 wt% of 1,3-butadiene is dissolved in n-hexane) is injected at a rate of 14.2 kg / h, n-hexane is injected at a rate of 49.11 kg / h, a 1,2-butadiene solution (wherein 2.0 wt% of 1,2-butadiene is dissolved in n-hexane) is injected at a rate of 40 g / h, a solution as a polar additive (wherein 10 wt% of tetramethylethylenediamine is dissolved in n-hexane) is injected at a rate of 10.0 g / h, and an initiator solution (wherein 10 wt% of n-butyllithium is dissolved in n-hexane) is injected at a rate of 59.0 g / h. At this time, the temperature of the first reactor is controlled to be maintained at 65° C. At the moment when the polymerization conversion rate reaches 48%, the polymer thus obtained is transported from the first reactor to the second reactor through a transport pipe.
[0147] Then, a 1,3-butadiene solution (in which 60 wt% of 1,3-butadiene was dissolved in n-hexane) was injected into the second reactor at a rate of 0.74 kg / h, and the temperature of the second reactor was maintained at 65° C. to continue polymerization. When the polymerization conversion rate reached more than 95%, the polymer was transported from the second reactor to the third reactor through a transport pipe.
[0148] A mixed solution of a solution as a first modifier (wherein 20 wt % of N-(3-(1H-imidazole-1-yl)propyl)-3-(triethoxysilyl)-N-(3-(triethoxysilyl))propyl)propan-1-amine dissolved in n-hexane) and a solution as a second modifier (wherein 20 wt % of N,N-bis(3-(dimethoxy(methyl)silyl)propyl)-methyl-1-amine dissolved in n-hexane) was continuously supplied to the third reactor in an equivalent ratio of 0.3:0.7 to carry out a modification reaction (molar ratio of n-butyllithium:total modifier=1:1). The temperature of the third reactor was maintained at 65°C.
[0149] Then, into the polymerization solution discharged from the third reactor, a solution as an antioxidant (in which 30 wt % of IR1520 (BASF Co.) was dissolved in n-hexane) was injected at a rate of 167 g / h and stirred. The polymer thus obtained was placed in hot water heated with steam and stirred to remove the solvent, thereby obtaining a modified conjugated diene polymer.
[0150] Example 2
[0151] A modified conjugated diene polymer was prepared in the same manner as in Example 1, except that in Example 1, the modification reaction was carried out as follows: a mixed solution of a solution as a first modifier (in which 20 wt % of N-(3-(1H-imidazole-1-yl)propyl)-3-(triethoxysilyl)-N-(3-(triethoxysilyl)propyl)propan-1-amine was dissolved in n-hexane) and a solution as a second modifier (in which 20 wt % of 3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropan-1-amine) was dissolved in n-hexane) was continuously supplied to the third reactor at an equivalent ratio of 0.3:0.7.
[0152] Example 3
[0153] A modified conjugated diene polymer was prepared in the same manner as in Example 1, except that in Example 1, the modification reaction was carried out as follows: a mixed solution of a solution as a first modifier (in which 20 wt % of N-(3-(1H-imidazol-1-yl)propyl)-3-(triethoxysilyl)-N-(3-(triethoxysilyl)propyl)propan-1-amine was dissolved in n-hexane) and a solution as a second modifier (in which 20 wt % of N-(3,6,9,12-tetraoxahexadecanyl)-N-(3-(triethoxysilyl)propyl)-3,6,9,12-tetraoxahexadecan-1-amine was dissolved in n-hexane) at an equivalent ratio of 0.3:0.7 was continuously supplied to the third reactor.
[0154] Example 4
[0155] A modified conjugated diene polymer was prepared in the same manner as in Example 1, except that in Example 1, the modification reaction was carried out as follows: a mixed solution of a solution as a first modifier (in which 20 wt % of tris(3-(trimethoxysilyl)propyl)amine was dissolved in n-hexane) and a solution as a second modifier (in which 20 wt % of N,N-bis(3-(dimethoxy(methyl)silyl)propyl)methan-1-amine was dissolved in n-hexane) at an equivalent ratio of 0.3:0.7 was continuously supplied to a third reactor.
[0156] Example 5
[0157] A modified conjugated diene polymer was prepared in the same manner as in Example 1, except that in Example 1, the polymer was transported to the second reactor when the conversion rate in the first reactor reached 47%, and the modification reaction was carried out as follows: a mixed solution of a solution as a first modifier (in which 20 wt % of tris(3-(trimethoxysilyl)propyl)amine was dissolved in n-hexane) and a solution as a second modifier (in which 20 wt % of N-(3,6,9,12-tetraoxahexadecanyl)-N-(3-(triethoxysilyl)propyl)-3,6,9,12-tetraoxahexadecan-1-amine was dissolved in n-hexane) at an equivalent ratio of 0.3:0.7 was continuously supplied to the third reactor.
[0158] Comparative Example 1
[0159] The modified conjugated diene polymer was prepared in the same manner as in Example 1, except that in Example 1, when the conversion rate in the first reactor reached 46% and the temperature was 55° C., the polymer was transported to the second reactor, and a solution as a coupling agent (including 2.0 wt.% tetrachlorosilane (SiCl 4 ) dissolved in n-hexane) replaces the first and second modifiers.
[0160] Comparative Example 2
[0161] Unmodified butadiene rubber CB24 from LANXESS was purchased, and its physical properties were measured.
[0162] Comparative Example 3
[0163] A modified conjugated diene polymer was prepared in the same manner as in Example 1, except that in Example 1, the polymer was transported to the second reactor when the conversion rate in the first reactor reached 48%, and the modification reaction was carried out as follows: a solution (in which 20 wt % of N,N-bis(3-(dimethoxy(methyl)silyl)propyl)methan-1-amine was dissolved in n-hexane) as a modifier was continuously supplied to the third reactor (the molar ratio of n-butyllithium:modifier = 1:1).
[0164] Comparative Example 4
[0165] A modified conjugated diene polymer was prepared in the same manner as in Example 1, except that in Example 1, the modification reaction was carried out as follows: a solution as a modifier (in which 20 wt % of N-(3,6,9,12-tetraoxahexadecanyl)-N-(3-(triethoxysilyl)propyl)-3,6,9,12-tetraoxahexadecan-1-amine was dissolved in n-hexane) was continuously supplied (the molar ratio of n-butyllithium:modifier = 1:1).
[0166] Comparative Example 5
[0167] A modified conjugated diene polymer was prepared in the same manner as in Example 1, except that in Example 1, the polymer was transported to the second reactor when the conversion rate in the first reactor reached 47%, and the modification reaction was carried out as follows: a solution (in which 20 wt % of tris(3-(trimethoxysilyl)propylamine was dissolved in n-hexane) as a modifier was continuously supplied (the molar ratio of n-butyllithium:modifier = 1:1).
[0168] Comparative Example 6
[0169] A modified conjugated diene polymer was prepared in the same manner as in Example 1, except that in Example 1, 2.5 times the injection amount of TMEDA was added, the temperature of the first reactor was changed to 80°C, the polymer was transported to the second reactor when the conversion rate in the first reactor reached 85%, and the modification reaction was carried out as follows: a mixed solution of a solution as a first modifier (in which 20 wt% of N-(3-(1H-imidazole-1-yl)propyl)-3-(triethoxysilyl)-N-(3-(triethoxysilyl)propyl)propan-1-amine was dissolved in n-hexane) and a solution as a second modifier (in which 20 wt% of N-(3,6,9,12-tetraoxahexadecanyl)-N-(3-(triethoxysilyl)propyl)-3,6,9,12-tetraoxahexadecan-1-amine was dissolved in n-hexane) was continuously supplied to the third reactor at an equivalent ratio of 0.3:0.7.
[0170] Experimental Example 1
[0171] For each unmodified or modified conjugated diene polymer prepared in the examples and comparative examples, the 1,2-vinyl bond content, number average molecular weight (Mn, x10 3 g / mol), weight average molecular weight (Mw, x10 3 g / mol), molecular weight distribution (PDI, MWD), Mooney viscosity (MV), Si content, glass transition temperature (Tg, °C) and cold flow (mg / min). The results are shown in Tables 1 and 2 below.
[0172] 1) 1,2-vinyl bond content
[0173] The vinyl content in each polymer was measured and analyzed using a Varian VNMRS 500 MHz N MR.
[0174] In measuring NMR, 1,1,2,2-tetrachloroethane was used as a solvent, the solvent peak was calculated to be 5.97 ppm, and the 1,2-vinyl bond content (weight %) was calculated by regarding 6.9-6.2 ppm as a block styrene peak, 5.8-5.1 ppm as a 1,4-vinyl peak, and 5.1-4.5 ppm as a 1,2-vinyl peak.
[0175] 2) Weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (MWD; PDI)
[0176] The number average molecular weight (Mw), peak top molecular weight (Mp) and weight average molecular weight (Mw) were measured by gel permeation chromatography (GPC) (PL GPC220, Agilent Technologies) under the following conditions, and the molecular weight distribution was calculated by dividing the weight average molecular weight by the number average molecular weight.
[0177] – Chromatographic columns: A combination of two PLgel Olexis (Polymer Laboratories Co.) columns and one PLgel mixed-C (Polymer Laboratories Co.) column was used.
[0178] -Solvent: A mixture of tetrahydrofuran and 2 wt % of an amine compound was used.
[0179] – Flow rate: 1mL / min
[0180] – Sample concentration: 1-2 mg / mL (diluted in THF)
[0181] – Injection volume: 100μL
[0182] – Column temperature: 40℃
[0183] – Detector: Refractive index
[0184] – Standard sample: polystyrene (calibrated using cubic function)
[0185] 3) Mooney viscosity (MV)
[0186] Mooney viscosity (MV, (ML1+4, @100°C MU)) was measured using MV-2000 (ALPHA Technologies Co.) with a large rotor at 100°C at a rotor speed of 2±0.02 rpm. In this case, the sample used was left to stand at room temperature (23±3°C) for more than 30 minutes, 27±3 g of the sample was collected and placed in the mold cavity, and then the platen was operated and the measurement was performed for 4 minutes.
[0187] 4) Glass transition temperature (Tg, °C)
[0188] The modified conjugated diene polymer was used as a sample and measured using a differential scanning calorimeter (trade name "DSC3200S", manufactured by MacScience Inc.) according to ISO 22768:2006. Specifically, under the condition of circulating helium at a rate of 50 ml / min, the temperature was raised from -100°C at a rate of 10°C / min, and the DSC curve was recorded, and the peak top (inflection point) of the DSC differential curve represents the glass transition temperature.
[0189] 5) Si content
[0190] Inductively coupled plasma optical emission spectroscopy (ICP-OES; Optima 7300DV) was used as an ICP analysis method for measurement. Specifically, the measurement was performed in the following manner: about 0.7 g of the sample was added to a platinum (Pt) crucible, about 1 mL of concentrated sulfuric acid (98 wt %, electronic grade) was added thereto, heated at 300° C. for 3 hours, and the sample was incinerated in an electric furnace (Thermo Scientific, LindbergBlue M) according to the procedures of steps 1 to 3 below:
[0191] 1) Step 1: initial temperature 0°C, rate (temperature / hour): 180°C / hour, temperature (holding time): 180°C (1 hour);
[0192] 2) Step 2: initial temperature 180°C, rate (temperature / hour): 85°C / hour, temperature (holding time): 370°C (2 hours); and
[0193] 3) Step 3: initial temperature 370°C, rate (temperature / hour): 47°C / hour, temperature (holding time): 510°C (3 hours),
[0194] Add 1 mL of concentrated nitric acid (48 wt%) and 20 μl of concentrated hydrofluoric acid (50 wt%) to the residue, seal the platinum crucible, shake for more than 30 minutes, add 1 mL of boric acid to the sample, store at 0°C for more than 2 hours, dilute with 30 ml of ultrapure water, and incinerate.
[0195] 6) Cold flow (mg / min)
[0196] A modified conjugated diene polymer was used as a sample, and a dynamic temperature equilibrium between the sample and the oven was achieved in an oven at 50°C. After standing for 10 minutes, the protruding polymer sample was taken out and placed in a static state. Then, the polymer sample was extruded through a 1.4-inch orifice at a pressure of 34.6 kPa, and the extrusion amount of the polymer sample flowing out through the orifice was measured at intervals of 30 minutes for 90 minutes. The extrusion amount was calculated in grams per minute (mg / min) and displayed as cold flow. The smaller the value, the better the molding stability (storage stability).
[0197] [Table 1]
[0198]
[0199] [Table 2]
[0200]
[0201] A: N-(3-(1H-imidazol-1-yl)propyl)-3-(triethoxysilyl)-N-(3-(triethoxysilyl)propyl)propan-1-amine
[0202] B: Tris(3-(trimethoxysilyl)propyl)amine
[0203] C: N,N-Bis(3-(dimethoxy(methyl)silyl)propyl)methan-1-amine
[0204] D:3,3'-(1,1,3,3-tetramethoxydisiloxane-1,3-diyl)bis(N,N-diethylpropane-1-amine)
[0205] E: N-(3,6,9,12-tetraoxahexadecanyl)-N-(3-(triethoxysilyl)propyl)-3,6,9,12-tetraoxahexadecan-1-amine
[0206] H:Tetrachlorosilane, SiCl 4
[0207] As shown in Tables 1 and 2 above, it can be confirmed that Examples 1 to 5 of the present invention all show a molecular weight distribution (PDI) of less than 1.70 and cold flow. Figure 1 As shown, it can be confirmed that the gel permeation chromatography (GPC) molecular weight distribution curve of Example 1 of the present invention has a unimodal shape. The difference is that Comparative Examples 1 and 2, which are unmodified polymers, meet the cold flow value of less than 1.00, but the molecular weight distribution value is more than 1.70 and deviates from the scope of the present invention. In addition, Comparative Examples 3 to 6 modified with a modifier but using only one modifier meet the molecular weight distribution value of less than 1.70, but the cold flow value is more than 1.00 and deviates from the scope of the present invention. In the case where the cold flow value meets less than 1.00, the molecular weight distribution value is greater than 1.70 and deviates from the scope of the present invention.
[0208] Experimental Example 2
[0209] In order to compare and analyze the physical properties of the rubber compositions comprising the modified or unmodified conjugated diene-based copolymers prepared in Examples and Comparative Examples, and the molded articles produced therefrom, viscoelasticity and wear resistance were measured, respectively, and the results are shown in Table 4 below.
[0210] 1) Preparation of rubber samples
[0211] The modified or unmodified conjugated diene polymers of Examples and Comparative Examples were used as raw material rubbers and compounded under the compounding conditions shown in the following Table 3. The raw materials in Table 3 are expressed in parts by weight based on 100 parts by weight of the raw material rubber.
[0212] [Table 3]
[0213]
[0214] Specifically, the rubber sample was milled by first-stage milling and second-stage milling. In the first-stage milling, the raw rubber, silica (filler), organic silane coupling agent (X50S, Evonik), processing oil (TDAE oil), zinc oxide (ZnO), stearic acid, antioxidant (TMQ (RD)) (2,2,4-trimethyl-1,2-dihydroquinoline polymer), anti-aging agent (6PPD ((dimethylbutyl)-N-phenyl-phenylenediamine) and wax (microcrystalline wax) were milled using a closed mixer equipped with a temperature control device. In this case, the initial temperature of the milling device was controlled. After the compounding was completed at 70°C, the first compounded mixture was obtained at a discharge temperature of 145-155°C. In the second stage of milling, the first compounded mixture was cooled to room temperature, and the first compounded mixture, sulfur, rubber accelerator (DPD (diphenylguanidine)) and vulcanization accelerator (CZ (N-cyclohexyl-2-benzothiazolylsulfenamide)) were added to the milling device and mixed at a temperature below 100°C to obtain a second compounded mixture. Then, a rubber sample was formed through a curing process at 160°C for 20 minutes.
[0215] 2) Viscoelasticity
[0216] The viscoelasticity was examined by measuring the viscoelastic behavior to thermodynamic deformation at each measurement temperature (-60°C to 60°C) using a dynamic mechanical analyzer (GABO Co.) in the film tension mode at a frequency of 10 Hz and obtaining the tan δ value. Among the measured values, if the tan δ value at 60°C decreases, the hysteresis loss decreases, and the lower the running resistance (fuel consumption rate), the better. In the following Table 4, the standard value (Comparative Example 1) of the viscoelasticity is specified and indexed (%), so that the higher the value, the better the result.
[0217] 3) Wear resistance
[0218] Wear resistance was obtained using a DIN wear tester. A load of 10N was applied to a rotating drum with abrasive paper attached, and then the rubber sample was moved in a direction perpendicular to the direction of rotation of the drum, and the wear loss weight was measured. The rotation speed of the drum was 40rpm, and the total movement distance after the sample completed the test was 40m. The smaller the loss weight value, the better the wear resistance, but the standard value of wear resistance (Comparative Example 1) is specified and indexed (%) in Table 4, so the higher the value, the better the result.
[0219] [Table 4]
[0220]
[0221] As shown in Table 4, in Examples 1 to 6, it can be confirmed that viscoelasticity and wear resistance are improved at the same time, and in particular, it can be confirmed that both viscoelasticity and wear resistance are significantly improved compared to Comparative Examples 1 and 2 using unmodified polymers, and it can be confirmed that viscoelasticity is improved compared to Comparative Example 5 using a modifier but in which a polymer of a branched type structure forms a main structure. In addition, it can be confirmed that Comparative Examples 3 and 4 using only one modifier exhibit a cold flow greater than 1.00 as shown in Table 1, exhibit very poor storage stability and molding stability when compared to the examples, and exhibit poor viscoelasticity and wear resistance. Although the viscoelasticity or wear resistance is comparable to that of the examples, considering the storage stability and molding stability, it can be found that the polymer exhibits poor performance compared to the examples.
[0222] In addition, in Comparative Example 6, although two types of modifiers were used, it was confirmed that the viscoelasticity was poor because the conversion rate of the first polymerization reactor was not controlled.
[0223] It can be determined that in order to prepare a polymer having excellent storage stability and molding stability as well as equally excellent viscoelasticity and wear resistance, the shape of the molecular weight distribution curve needs to be unimodal, and the molecular weight distribution, cold flow and Si content need to meet a specific range by applying a specific preparation method, which includes using two types of modifiers as in the embodiments of the present invention and controlling the conversion rate of the first polymerization reactor to below 50%.
Claims
1. A modified conjugated diene polymer, which meets the following conditions: a) the molecular weight distribution curve of gel permeation chromatography (GPC) has a single peak shape; b) molecular weight distribution (PDI; MWD) is greater than 1.00 and less than 1.70; c) a cold flow of 0.50 or more and less than 1.00; and d) based on the total weight of the modified conjugated diene polymer, the Si content is 100 ppm or more, in, The modified conjugated diene polymer includes a functional group derived from a modifier, Wherein, the modifier includes a first modifier and a second modifier, The first modifier is a modifier having more than five reactive functional groups capable of reacting with the living polymer, and The second modifier is a modifier having five or less reactive functional groups capable of reacting with the living polymer, Wherein, the first modifier includes a compound represented by the following formula 1, and The second modifier includes at least one compound represented by the following Formula 2 and Formula 3: [Formula 1] In formula 1, R a1 and R a4 are each independently a single bond or an alkylene group of 1 to 10 carbon atoms, R a2 and R a3 are each independently an alkyl group having 1 to 10 carbon atoms, R a5 is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, a divalent, trivalent or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms, or a five-membered heterocyclic group having 2 to 4 carbon atoms and including one or more heteroatoms selected from N, O and S, wherein the heterocyclic group is unsubstituted or substituted with an alkyl group having 1 to 10 carbon atoms or a (trialkoxysilyl)alkyl group, and the alkyl group in the (trialkoxysilyl)alkyl group is an alkyl group having 1 to 10 carbon atoms, and the alkoxy group is an alkoxy group having 1 to 10 carbon atoms; m1 is an integer from 1 to 3, m2 is an integer from 0 to 2, wherein -(OR a2 ) The total number of groups is greater than five, [Formula 2] In formula 2, R b1 is a single bond or an alkylene group of 1 to 10 carbon atoms, R b2 and R b3 Each independently is an alkyl group having 1 to 10 carbon atoms or -[R b6 O] n3 -R b7 , R b4 is a single bond, an alkylene group of 1 to 10 carbon atoms, or -[R b6 O] n3 , R b5 is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a divalent, trivalent or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms, R b6 is an alkylene group of 1 to 10 carbon atoms, R b7 is an alkyl group of 1 to 10 carbon atoms, n1 is an integer from 1 to 3, n2 is an integer from 0 to 2, and n3 is an integer from 1 to 30, wherein –(OR b2 ) The total number of groups is less than 5, [Formula 3] In formula 3, A1 and A2 are each independently an alkylene group having 1 to 20 carbon atoms, R c1 To R c4 are each independently an alkyl group having 1 to 20 carbon atoms, L1 to L4 are each independently an alkyl group of 1 to 20 carbon atoms, an aryl group of 6 to 20 carbon atoms, or a divalent, trivalent or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms.
2. The modified conjugated diene polymer according to claim 1, wherein The glass transition temperature of the modified conjugated diene polymer is -100°C to -50°C.
3. The modified conjugated diene polymer according to claim 1, wherein The number average molecular weight of the modified conjugated diene-based polymer is 200,000 g / mol to 1,000,000 g / mol.
4. The modified conjugated diene polymer according to claim 1, wherein The modified conjugated diene-based polymer does not include a repeating unit derived from an aromatic vinyl-based monomer.
5. The modified conjugated diene polymer according to claim 1, wherein The 1,2-vinyl bond content in the modified conjugated diene polymer is 5 wt % to 30 wt %.
6. The modified conjugated diene polymer according to claim 1, wherein The modified conjugated diene-based polymer contains N atoms, and the content of the N atoms is greater than or equal to 50 ppm based on the total weight of the polymer.
7. A method for preparing a modified conjugated diene polymer, the method comprising: In the presence of a polymerization initiator, polymerizing a conjugated diene monomer in a hydrocarbon solvent to prepare a living polymer (S1); and reacting the active polymer prepared in step (S1) with a modifier (S2), The polymerization reaction (S1) and the modification reaction (S2) are carried out continuously. Step (S1) is carried out in two or more polymerization reactors, The polymerization conversion rate in the first polymerization reactor in the polymerization reactor is 50% or less, The modifier includes a first modifier and a second modifier, The first modifying agent is a modifying agent having more than five reactive functional groups capable of reacting with the living polymer, and The second modifier is a modifier having five or less reactive functional groups capable of reacting with the living polymer, Wherein, the first modifier includes a compound represented by the following formula 1, and The second modifier includes at least one compound represented by the following Formula 2 and Formula 3: [Formula 1] In formula 1, R a1 and R a4 are each independently a single bond or an alkylene group of 1 to 10 carbon atoms, R a2 and R a3 are each independently an alkyl group having 1 to 10 carbon atoms, R a5 is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, a divalent, trivalent or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms, or a five-membered heterocyclic group having 2 to 4 carbon atoms and including one or more heteroatoms selected from N, O and S, wherein the heterocyclic group is unsubstituted or substituted with an alkyl group having 1 to 10 carbon atoms or a (trialkoxysilyl)alkyl group, and the alkyl group in the (trialkoxysilyl)alkyl group is an alkyl group having 1 to 10 carbon atoms, and the alkoxy group is an alkoxy group having 1 to 10 carbon atoms; m1 is an integer from 1 to 3, m2 is an integer from 0 to 2, wherein -(OR a2 ) The total number of groups is greater than five, [Formula 2] In formula 2, R b1 is a single bond or an alkylene group of 1 to 10 carbon atoms, R b2 and R b3 Each independently is an alkyl group having 1 to 10 carbon atoms or -[R b6 O] n3 -R b7 , R b4 is a single bond, an alkylene group of 1 to 10 carbon atoms, or -[R b6 O] n3 , R b5 is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a divalent, trivalent or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms, R b6 is an alkylene group of 1 to 10 carbon atoms, R b7 is an alkyl group of 1 to 10 carbon atoms, n1 is an integer from 1 to 3, n2 is an integer from 0 to 2, and n3 is an integer from 1 to 30, wherein –(OR b2 ) The total number of groups is less than 5, [Formula 3] In formula 3, A1 and A2 are each independently an alkylene group having 1 to 20 carbon atoms, R c1 To R c4 are each independently an alkyl group having 1 to 20 carbon atoms, L1 to L4 are each independently an alkyl group of 1 to 20 carbon atoms, an aryl group of 6 to 20 carbon atoms, or a divalent, trivalent or tetravalent alkylsilyl group substituted with an alkyl group having 1 to 10 carbon atoms.
8. The method for preparing a modified conjugated diene polymer according to claim 7, wherein: The reactive functional group capable of reacting with the living polymer is an alkoxy group.
9. The method for preparing a modified conjugated diene polymer according to claim 7, wherein: The equivalent ratio of the first modifier to the second modifier is 1:9 to 5:
5. 10 . A rubber composition comprising the modified conjugated diene polymer according to claim 1 and a filler. 11 . The rubber composition according to claim 10 , comprising 0.1 to 200 parts by weight of the filler relative to 100 parts by weight of the modified conjugated diene-based polymer.
12. The rubber composition according to claim 11, wherein The filler is a silica filler or a carbon black filler.