Film for producing optical film, method for producing optical film, and optical film
By using a silanol-modified PVA optical film manufacturing method, the problem of poor film-forming properties of high-polymerization-degree PVA films has been solved, enabling the manufacture of high-performance optical films, especially polarizing films with excellent optical performance and resistance to damp heat.
Patent Information
- Application Number
- CN202080070727.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-08
- Filing Date
- 2020-09-24
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-09-24
AI Technical Summary
In the prior art, the increased viscosity of aqueous solutions of high-polymerization-degree PVA films leads to poor film-forming properties, making it difficult to manufacture high-performance optical films in industrial production, and the films also have insufficient resistance to damp heat.
Optical films are manufactured using polyvinyl alcohol (silanol-modified PVA) containing silicon groups, with a viscosity-average polymerization degree of 1,000 to 6,000, a saponification degree of ≥98.7%, and a silicon group content of 0.01% to 1.0%, through a uniaxial stretching process to improve optical performance and resistance to damp heat.
It achieves superior optical properties and resistance to damp heat compared to unmodified PVA, while improving productivity, film-forming properties, and stretchability, making it suitable for manufacturing optical films such as polarizing films.
Smart Images

Figure DEST_PATH_IMAGE001 
Figure FDA0005022622980000011 
Figure FDA0005022622980000021
Abstract
Description
Technical Field
[0001] The present invention relates to a film for producing an optical film, a method for producing an optical film, and an optical film. Background Art
[0002] Polarizing plates with light-transmitting and light-shielding functions are the basic components of liquid crystal displays (LCDs) along with liquid crystals that change the polarization state of light. Many polarizing plates have a structure in which a protective film such as a triacetyl cellulose (TAC) film is attached to the surface of the polarizing film. As a polarizing film, a substrate (stretched film) made by uniaxially stretching a polyvinyl alcohol film (hereinafter sometimes referred to as "PVA") is adsorbed with an iodine-based dye (I3 - 、I5 - Polarizing films obtained by using dichroic pigments such as , etc.) and dichroic organic dyes have become mainstream.
[0003] LCD is used in a wide range of small instruments such as calculators and watches, smart phones, notebook personal computers, liquid crystal monitors, liquid crystal color projectors, liquid crystal televisions, vehicle-mounted navigation systems, portable phones, and metering equipment for indoor and outdoor use. In recent years, these devices have been required to improve display quality. Along with this, high performance is also required for polarizing films, specifically, polarizing films with excellent optical properties such as polarization degree and transmittance are required. In addition, durability is also important for polarizing films, for example, it is required to maintain good performance even in a high temperature and humid environment. For optical films other than polarizing films, optical performance and durability are also required.
[0004] As a polarizing film with improved optical performance and moisture and heat resistance, a polarizing film using PVA with a high degree of polymerization is known (Patent Document 1). In Patent Document 1, a PVA film-forming solution obtained by dissolving PVA with a high degree of polymerization in a solvent containing dimethyl sulfoxide as a main component is used for film formation.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent document 1: Japanese Patent Application Laid-Open No. 1-105204. Summary of the invention
[0008] Problem that the invention aims to solve
[0009] In the industrial production of PVA film, a PVA aqueous solution using water as a solvent is usually used as a film-forming solution in consideration of environmental aspects, economic efficiency, etc. However, PVA with a high degree of polymerization has poor film-forming properties due to the increased viscosity of its aqueous solution, and is not preferred in industrial production. Therefore, a method for improving the optical properties and moisture-heat resistance of an optical film other than a method for increasing the degree of polymerization of PVA is desired.
[0010] The present invention is made based on the above situation, and its purpose is to provide a film for optical film manufacturing that has good productivity and can obtain an optical film with better optical properties and moisture-heat resistance than when using unmodified PVA with the same degree of polymerization, as well as a method for manufacturing an optical film and an optical film obtained using this film for optical film manufacturing.
[0011] Means used to solve problems
[0012] The above object is achieved by providing any one of the following technical solutions.
[0013] [1] A film for producing an optical film, comprising polyvinyl alcohol having a silicon-containing group, wherein the silicon-containing group is a silanol group or a group that can be converted into a silanol group in the presence of water, the polyvinyl alcohol having a viscosity-average degree of polymerization of 1,000 to 6,000, a degree of saponification of 98.7 mol % or more, and a content of the silicon-containing group relative to all structural units of 0.01 mol % to 1.0 mol % or less;
[0014] [2] The film for producing an optical film according to [1], wherein the saponification degree is 99.5 mol % or more;
[0015] [3] The film for optical film production according to [1] or [2], wherein the product of the viscosity average degree of polymerization and the content of the silicon-containing group is 100 mol % or more and 2,000 mol % or less;
[0016] [4] The film for producing an optical film according to any one of [1] to [3], which has an average thickness of 1 μm to 75 μm;
[0017] [5] The film for producing an optical film according to any one of [1] to [4], wherein the film has a degree of swelling of 140% to 400%;
[0018] [6] The film for producing an optical film according to any one of [1] to [5], wherein the optical film is a polarizing film;
[0019] [7] The film for producing an optical film according to any one of [1] to [6], which is an unstretched film;
[0020] [8] A method for producing an optical film, comprising the step of uniaxially stretching the film for producing an optical film according to any one of [1] to [7];
[0021] [9] The method for producing an optical film according to [8], wherein the optical film is a polarizing film;
[0022]
[10] An optical film comprising polyvinyl alcohol having a silicon-containing group, wherein the silicon-containing group is a silanol group or a group that can be converted into a silanol group in the presence of water, the polyvinyl alcohol having a viscosity-average degree of polymerization of 1,000 to 6,000, a degree of saponification of 98.7 mol % or more, and a content of the silicon-containing group relative to all structural units of 0.01 mol % to 1.0 mol % or less;
[0023]
[11] The optical film according to
[10] , which is a polarizing film; and
[0024]
[12] The optical film according to
[10] or
[11] , which is a single-layer film.
[0025] Effects of the Invention
[0026] According to the present invention, there can be provided a film for optical film manufacturing which has good productivity and is capable of obtaining an optical film having better optical properties and moisture-heat resistance than when using unmodified PVA having the same degree of polymerization, as well as a method for manufacturing an optical film and an optical film obtained using such a film for optical film manufacturing. DETAILED DESCRIPTION
[0027] <Film for Optical Film Production>
[0028] The film for producing an optical film of the present invention contains polyvinyl alcohol having a silicon-containing group (hereinafter sometimes referred to as "silanol-modified PVA").
[0029] (Silanol modified PVA)
[0030] The silanol-modified PVA is a polymer having a vinyl alcohol unit (-CH2-CH(OH)-) as a structural unit and having a silicon-containing group. The silanol-modified PVA may contain a structural unit having a silicon-containing group, and may further have a vinyl ester unit such as a vinyl acetate unit, or other structural units.
[0031] The lower limit of the viscosity average polymerization degree of the silanol-modified PVA is 1,000, preferably 2,000, and more preferably 2,500. By making the viscosity average polymerization degree of the silanol-modified PVA above the above lower limit, the stretching processability of the film for optical film manufacturing of the present invention becomes excellent, and an optical film with excellent optical properties and moisture-heat resistance can be obtained. On the other hand, the upper limit of the above viscosity average polymerization degree is 6,000, preferably 5,000, and more preferably 4,000. By making the viscosity average polymerization degree of the silanol-modified PVA below the above upper limit, good water solubility is exerted, and the viscosity increase of the aqueous solution is suppressed. Therefore, by making the viscosity average polymerization degree of the silanol-modified PVA below the above upper limit, good film-forming properties are exerted, and the productivity of the film for optical film manufacturing of the present invention can be improved.
[0032] The viscosity average degree of polymerization refers to the average degree of polymerization measured in accordance with the description of JIS K6726-1994. That is, in this specification, the viscosity average degree of polymerization is obtained by measuring the residual vinyl ester groups of PVA in water at 30°C after re-saponification and purification, and then calculating the viscosity average degree of polymerization using the following formula based on the intrinsic viscosity [η] (unit: deciliter / g) obtained.
[0033] Viscosity average degree of polymerization Po = ([η] × 10 4 / 8.29) (1 / 0.62) .
[0034] The lower limit of the saponification degree of the silanol-modified PVA is 98.7 mol%, preferably 99.0 mol%, more preferably 99.5 mol%, further preferably 99.8 mol%, and particularly preferably 99.9 mol%. By making the saponification degree above the above lower limit, an optical film having excellent optical properties and resistance to moisture and heat can be obtained. On the other hand, the upper limit of the saponification degree is not particularly limited, but is preferably below 99.99 mol% from the viewpoint of the productivity of the silanol-modified PVA.
[0035] The saponification degree of PVA refers to the ratio (mol %) of the number of moles of vinyl alcohol units in PVA relative to the total number of moles of structural units (typically vinyl ester units) that can be converted into vinyl alcohol units by saponification and vinyl alcohol units. The saponification degree of PVA can be measured according to the description of JIS K6726-1994.
[0036] The silanol-modified PVA has a silicon-containing group. The silicon-containing group is a silanol group or a group that can be converted into a silanol group in the presence of water. A silanol group refers to a group having a silicon atom and at least one hydroxyl group bonded to the silicon atom. The number of hydroxyl groups possessed by the silanol group is generally any one of 1 to 3, preferably 3. The hydroxyl groups possessed by the silanol group may exist in the form of a salt (e.g., -ONa, -OK, etc.).
[0037] The group that can be converted into a silanol group in the presence of water refers to a group that can be converted into a silanol group when PVA is hydrolyzed in water under the conditions of a reaction time of 2 hours and a reaction temperature of 150° C. Examples of the group that can be converted into a silanol group in the presence of water include groups having at least one alkoxy group or acyloxy group bonded to a silicon atom, and specifically, trimethoxysilyl, triethoxysilyl, triisopropoxysilyl, dimethoxymethylsilyl, diethoxymethylsilyl, methoxydimethylsilyl, ethoxydimethylsilyl, triacetoxysilyl, and the like.
[0038] Examples of the silicon-containing group, that is, the silanol group or the group that can be converted into a silanol group in the presence of water include groups represented by any of the following formulae (1) to (3). Among these, the group represented by the following formula (1) is preferred.
[0039] [Chemistry 1]
[0040]
[0041] In formulas (1) to (3), R 1 Each is independently a hydrogen atom, a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or a substituted or unsubstituted acyl group having 1 to 20 carbon atoms. 2 Each is independently a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms.
[0042] As R 1 and R 2 The hydrocarbon group having 1 to 20 carbon atoms as shown in the formula (R) may be an aliphatic hydrocarbon group, an alicyclic hydrocarbon group (cyclohexyl group, etc.), an aromatic hydrocarbon group (phenyl group, etc.), etc., preferably an aliphatic hydrocarbon group. Examples of the aliphatic hydrocarbon group include alkyl groups such as methyl, ethyl, and propyl groups; alkenyl groups such as vinyl groups; alkynyl groups such as ethynyl groups, etc., preferably alkyl groups. 1 and R 2 The number of carbon atoms of the hydrocarbon group represented by is preferably 1 to 6, more preferably 1 to 3. 1 and R 2 At least a part of hydrogen atoms in the hydrocarbon group shown may be substituted with a halogen atom, a carboxyl group, an alkoxy group (methoxy group, ethoxy group, etc.) or the like.
[0043] As R 1 The acyl group having 1 to 20 carbon atoms as shown in , can be a group in which a carbonyl group (-CO-) is bonded to the above hydrocarbon group having 1 to 20 carbon atoms. Specifically, acetyl, propionyl, benzoyl, etc. can be mentioned. 1 The number of carbon atoms of the acyl group represented by is preferably 1 to 6, more preferably 1 to 3. 1 At least a part of hydrogen atoms in the acyl group may be substituted with a halogen atom, a carboxyl group, an alkoxy group (such as a methoxy group), or the like.
[0044] In the group represented by any one of the above formulae (1) to (3), at least one R 1 When it is a hydrogen atom, the group is a silanol group. 1 When all of R are not hydrogen atoms, the group is a group that can be converted into a silanol group in the presence of water. 1 , preferably a hydrogen atom, or a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms.
[0045] From the viewpoint of the optical properties of the obtained optical film, etc., it is preferred that the silicon-containing group is directly bonded to a carbon atom in the polymer main chain via a silicon-carbon bond.
[0046] The content of silicon-containing groups in the silanol-modified PVA relative to all structural units is 0.01 mol% or more and 1.0 mol% or less. In this way, by using a silanol-modified PVA having a specified amount of silicon-containing groups, the optical properties and moisture and heat resistance of the obtained optical film are significantly improved compared with the existing optical film obtained by using unmodified PVA with the same degree of polymerization. It should be noted that the unmodified PVA is a PVA obtained by saponifying a homopolymer of vinyl ester. On the other hand, if compared with a PVA with a high degree of polymerization having the same optical properties as the obtained optical film, the viscosity of the aqueous solution of the above-mentioned silanol-modified PVA at high temperature (e.g., 80°C) is low. Therefore, by using a silanol-modified PVA, the optical film manufacturing film can improve the optical properties and moisture and heat resistance of the obtained optical film while having good productivity (film forming properties). Alternatively, by using a silanol-modified PVA, the obtained optical film can exert excellent optical properties and moisture and heat resistance, and can improve the productivity (film forming properties) of the optical film manufacturing film.
[0047] The silicon-containing group of silanol-modified PVA is 0.01 mol of content lower limit relative to total structural units, preferably 0.05 mol, more preferably 0.1 mol, further preferably 0.25 mol%. By making the content of silicon-containing group more than the above-mentioned lower limit, it is possible to give full play to the above-mentioned effect brought by silanol modification. On the other hand, the silicon-containing group of silanol-modified PVA is 1.0 mol of content upper limit relative to total structural units, preferably 0.8 mol, more preferably 0.6 mol%. By making the content of silicon-containing group below the above-mentioned upper limit, the water solubility of silanol-modified PVA and the viscosity stability of the aqueous solution become good, it is possible to improve film productivity (film making) etc.
[0048] In the silanol-modified PVA, the content (mol %) of the silicon-containing group is obtained, for example, by proton NMR of the vinyl ester polymer before saponification. Here, when measuring the proton NMR of the vinyl ester polymer before saponification, the vinyl ester polymer is reprecipitated and purified with hexane-acetone to completely remove unreacted monomers from the polymer, then dried under reduced pressure at 90° C. for 2 days, dissolved in CDCl3 solvent and subjected to analysis.
[0049] The lower limit of the product of the viscosity average degree of polymerization of the silanol-modified PVA and the content of the silicon-containing group is preferably 100 mol%, more preferably 300 mol%, further preferably 500 mol, and particularly preferably 700 mol%. By making the above product above the above lower limit, the optical properties and moisture-heat resistance of the obtained optical film become more excellent. On the other hand, the upper limit of the above product is preferably 2,000 mol%, more preferably 1,500, and further preferably 1,200. By making the above product below the above upper limit, the water solubility of the silanol-modified PVA can be further improved, and the productivity of the film for manufacturing the optical film can be further improved.
[0050] The silanol-modified PVA preferably contains a structural unit having a silicon-containing group. Examples of the structural unit having a silicon-containing group include a structural unit represented by the following formula (4).
[0051] [Chemistry 2]
[0052]
[0053] In formula (4), R 3 is a hydrogen atom or a methyl group. 4 is a single bond or a divalent linking group. 5 A silicon-containing group.
[0054] As R 3 , preferably a hydrogen atom.
[0055] As R 4 The divalent linking group shown in the figure may be -(CH2) n -(n is an integer from 1 to 5) or -CONR 6 -R 7 -(R 6 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. 7 For the above-(CH2) n -, or a group represented by a divalent hydrocarbon group containing at least one of an oxygen atom and a nitrogen atom).
[0056] Examples of the divalent hydrocarbon group containing at least one of an oxygen atom and a nitrogen atom include -CH2CH2NHCH2CH2CH2-, -CH2CH2NHCH2CH2-, -CH2CH2NHCH2-, -CH2CH2N(CH3)CH2CH2-, -CH2CH2N(CH3)CH2-, -CH2CH2OCH2CH2CH2-, -CH2CH2OCH2CH2-, -CH2CH2OCH2CH2-, etc. The number of carbon atoms in the divalent hydrocarbon group containing at least one of an oxygen atom and a nitrogen atom can be, for example, 2 or more and 6 or less.
[0057] R4 Preferred is a single bond.
[0058] As R 5 As a specific example of the silicon-containing group represented by the formula (1), a group represented by any one of the formulas (1) to (3) is mentioned as described above, and a group represented by the formula (1) is preferred.
[0059] The number of silicon-containing groups contained in the structural unit having a silicon-containing group is not particularly limited and may be 1. The content range of the structural unit having a silicon-containing group relative to all structural units of the silanol-modified PVA may be the content range of the above-mentioned silicon-containing group relative to all structural units. In addition, the range of the product of the viscosity-average degree of polymerization of the silanol-modified PVA and the content of the structural unit having a silicon-containing group may be the range of the product of the above-mentioned viscosity-average degree of polymerization and the content of the silicon-containing group.
[0060] The silanol-modified PVA may have other structural units except the vinyl alcohol unit, the vinyl ester unit and the structural unit having the silicon-containing group. Wherein, the content of the above-mentioned other structural units of the silanol-modified PVA relative to the total structural units is sometimes preferably 15 mol % or less, more preferably 5 mol % or less, further preferably 1 mol % or less, and further preferably 0.1 mol % or less. The silanol-modified PVA is substantially composed of the vinyl alcohol unit, the vinyl ester unit and the structural unit having the silicon-containing group, thereby sometimes more fully exerting the effect of the present invention.
[0061] The film for producing an optical film may contain one type of silanol-modified PVA alone, or may contain two or more types of silanol-modified PVAs that are different in degree of polymerization, degree of saponification, content of silicon-containing groups, etc.
[0062] The lower limit of the content of the silanol-modified PVA in the optical film manufacturing film is not particularly limited, preferably 50% by mass, more preferably 80% by mass, and further preferably 85% by mass. By setting the content of the silanol-modified PVA to above the above lower limit, the effect of the present invention can be further improved. On the other hand, the upper limit of the content is not particularly limited, and can be 100% by mass, preferably 99% by mass, and more preferably 95% by mass.
[0063] (Method for producing silanol-modified PVA)
[0064] The method for producing the silanol-modified PVA is not particularly limited, and the silanol-modified PVA can be produced, for example, by copolymerizing a vinyl ester monomer and a monomer having a silicon-containing group, and saponifying the obtained vinyl ester polymer.
[0065] Examples of the vinyl ester monomer include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl pivalate, vinyl versatate, etc. Among these, vinyl acetate is preferred.
[0066] Examples of the monomer having a silicon-containing group include vinyl trimethoxysilane, vinyl methyl dimethoxysilane, vinyl dimethyl methoxysilane, vinyl triethoxysilane, vinyl methyl diethoxysilane, vinyl dimethyl ethoxysilane, allyl trimethoxysilane, allyl methyl dimethoxysilane, allyl dimethyl methoxysilane, allyl triethoxysilane, allyl methyl diethoxysilane, allyl dimethyl ethoxysilane, vinyl tri (β-methoxyethoxy) silane, vinyl isobutyl dimethoxysilane, vinyl ethyl dimethoxysilane, vinyl methoxy dibutyloxysilane, vinyl dimethoxy 1-Butoxysilane, vinyl tributoxysilane, vinyl methoxydihexyloxysilane, vinyl dimethoxyhexyloxysilane, vinyl trihexyloxysilane, vinyl methoxydioctyloxysilane, vinyl dimethoxyoctyloxysilane, vinyl trioctyloxysilane, vinyl methoxydilauryloxysilane, vinyl dimethoxylauryloxysilane, vinyl methoxydioleoxysilane, vinyl dimethoxyoleoxysilane, 3-(meth)acrylamide-propyltrimethoxysilane, 3-(meth)acrylamide-propyltriethoxysilane, 3-(meth)acrylamide-propyltri(β-methoxyethoxy)silane, 2-( 1-(Meth)acrylamide-ethyltrimethoxysilane, 1-(Meth)acrylamide-methyltrimethoxysilane, 2-(Meth)acrylamide-2-methylpropyltrimethoxysilane, 2-(Meth)acrylamide-isopropyltrimethoxysilane, N-(2-(Meth)acrylamide-ethyl)-aminopropyltrimethoxysilane, (3-(Meth)acrylamide-propyl)-oxypropyltrimethoxysilane, 3-(Meth)acrylamide-propyltriacetoxysilane, 2-(Meth)acrylamide-ethyltriacetoxysilane, 4-(Meth)acrylamide-butyltriacetoxysilane, 3-(Meth)acrylamide-propyltriacetoxysilane, triacetoxysilane, 2-(methyl)acrylamide-2-methylpropyl triacetoxysilane, N-(2-(methyl)acrylamide-ethyl)-aminopropyl triacetoxysilane, 3-(methyl)acrylamide-propyl isobutyl dimethoxysilane, 2-(methyl)acrylamide-ethyl dimethylmethoxysilane, 3-(methyl)acrylamide-propyl methyl diacetoxysilane, 2-(methyl)acrylamide-2-methylpropyl hydrogenated dimethoxysilane, 3-(N-methyl-(methyl)acrylamide)-propyl trimethoxysilane, 2-(N-ethyl-(methyl)acrylamide)-ethyl triacetoxysilane, etc.
[0067] The method for copolymerizing the vinyl ester monomer and the monomer having a silicon-containing group is not particularly limited, and examples thereof include known methods such as bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization. Among these methods, bulk polymerization under solvent-free conditions and solution polymerization using a solvent such as alcohol are preferred. Examples of solvents used as solvents in solution polymerization include esters such as methyl acetate and ethyl acetate; aromatic hydrocarbons such as benzene and toluene; and lower alcohols such as methanol and ethanol.
[0068] As the initiator used in the copolymerization reaction, a conventionally known azo initiator, peroxide initiator, redox initiator, etc. can be appropriately selected. Examples of azo initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), etc. Examples of peroxide initiators include percarbonate compounds such as di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, and di(ethoxyethyl) peroxydicarbonate; perester compounds such as tert-butyl peroxyneodecanoate, α-isopropyl peroxyneodecanoate, and tert-butyl peroxyneodecanoate; acetylcyclohexylsulfonyl peroxide, diisobutyryl peroxide; phenoxyacetic acid 2,4,4-trimethylpentyl-2-peroxyester, etc. Furthermore, the above-mentioned peroxide-based initiators can be combined with potassium persulfate, ammonium persulfate, hydrogen peroxide, etc. to prepare an initiator. As redox-based initiators, there can be cited initiators obtained by combining the above-mentioned peroxides with reducing agents such as sodium bisulfite, sodium bicarbonate, tartaric acid, L-ascorbic acid, and Rongalite.
[0069] The polymerization temperature during the copolymerization reaction is not particularly limited, but is preferably 0°C to 180°C, more preferably 20°C to 160°C, and further preferably 30°C to 150°C.
[0070] When the vinyl ester monomer is copolymerized with the monomer having a silicon-containing group, other copolymerizable monomers may be copolymerized as needed as long as the effect of the present invention is not impaired. Examples of the other monomers include ethylene; olefins having 3 to 30 carbon atoms such as propylene, 1-butene, and isobutylene; acrylic acid or its salts; acrylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, and octadecyl acrylate; methacrylic acid or its salts; methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, and octadecyl methacrylate; acrylamide, N-methylacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, diacetoneacrylamide, acrylamidopropanesulfonic acid or its salts, acrylamidopropyldimethylamine or its salts, N acrylamide derivatives such as -hydroxymethyl acrylamide or its derivatives; methacrylamide derivatives such as methacrylamide, N-methyl methacrylamide, N-ethyl methacrylamide, methacrylamide propanesulfonic acid or its salts, methacrylamide propyl dimethylamine or its salts, N-hydroxymethyl methacrylamide or its derivatives; N-vinylamides such as N-vinyl formamide, N-vinylacetamide, N-vinyl pyrrolidone; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, dodecyl vinyl ether, stearyl vinyl ether; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; maleic acid or its salts, esters or anhydrides; itaconic acid or its salts, esters or anhydrides; isopropenyl acetate, etc. The vinyl ester polymer may have a structural unit derived from one or more of the above-mentioned other monomers.
[0071] The proportion of the structural units derived from the above-mentioned other monomers (monomers other than the vinyl ester monomer and the monomer having a silicon-containing group) in the vinyl ester polymer is not limited unless the effect of the present invention is impaired. Depending on the number of moles of all structural units constituting the vinyl ester polymer, it is sometimes preferably 15 mol% or less, more preferably 5 mol% or less, further preferably 1 mol% or less, and further preferably 0.1 mol% or less.
[0072] The vinyl ester polymer is then saponified in a solvent according to a known method and directed to a silanol-modified PVA. As a solvent used in the saponification reaction, an alcohol is preferably used. As an alcohol, lower alcohols such as methanol and ethanol can be listed, and methanol is particularly suitable. In addition to alcohol, the solvent used in the saponification reaction may further contain esters such as acetone, methyl acetate, ethyl acetate, and organic solvents such as toluene. As a catalyst used in the saponification reaction, hydroxides of alkali metals such as potassium hydroxide and sodium hydroxide; base catalysts such as sodium methoxide; acid catalysts such as inorganic acids, etc. can be listed. As the temperature of the saponification reaction, it can be set to, for example, above 20°C and below 60°C. When a gel-like product gradually precipitates as the saponification reaction proceeds, the product is crushed and washed at this time, and then dried to obtain a silanol-modified PVA.
[0073] (Plasticizer)
[0074] The film for optical film manufacturing of the present invention preferably contains a plasticizer. By making the film for optical film manufacturing contain a plasticizer, stretchability and the like can be improved. As the plasticizer, polyols are preferred. As polyols, ethylene glycol, glycerol, propylene glycol, diethylene glycol, diglycerol, triethylene glycol, tetraethylene glycol, trimethylolpropane, etc. can be listed. Among these, glycerol is preferred from the viewpoint of the effect of improving stretchability. One or more plasticizers can be used.
[0075] As the lower limit of the content of the plasticizer in the film for optical film manufacturing of the present invention, relative to 100 parts by mass of silanol-modified PVA, it is preferably 1 part by mass, more preferably 3 parts by mass, and further preferably 5 parts by mass. By making the content of the plasticizer above the above lower limit, the stretchability of the film is improved, and the optical properties of the obtained optical film can be further improved. On the other hand, as the upper limit of the content of the plasticizer, relative to 100 parts by mass of silanol-modified PVA, it is preferably 20 parts by mass, more preferably 17 parts by mass, and further preferably 15 parts by mass. By making the content of the plasticizer below the above upper limit, it is possible to suppress the film from becoming too soft and causing a decrease in handling properties.
[0076] (Surfactant)
[0077] The optical film production film preferably contains a surfactant. By using a film-forming stock solution containing a surfactant for film production, the film-forming property is improved, the film thickness unevenness is suppressed, and the film is easily peeled off from the metal roll or belt used for film production. When the optical film production film is produced from a film-forming stock solution containing a surfactant, the obtained film may contain a surfactant.
[0078] The type of surfactant is not particularly limited, but anionic surfactants and nonionic surfactants are preferred from the viewpoint of peelability from a metal roll or a belt.
[0079] Examples of the anionic surfactant include carboxylic acid-type surfactants such as potassium laurate; sulfate-ester-type surfactants such as polyoxyethylene lauryl ether sulfate and octyl sulfate; and sulfonic acid-type surfactants such as dodecylbenzenesulfonate.
[0080] Examples of the nonionic surfactant include alkyl ether types such as polyoxyethylene oleyl ether; alkyl phenyl ether types such as polyoxyethylene octylphenyl ether; alkyl ester types such as polyoxyethylene laurate; alkyl amine types such as polyoxyethylene lauryl amino ether; alkyl amide types such as polyoxyethylene lauric acid amide; polypropylene glycol ether types such as polyoxyethylene polyoxypropylene ether; alkanolamide types such as lauric acid diethanolamide and oleic acid diethanolamide; allyl phenyl ether types such as polyoxyalkylene allyl phenyl ether, and the like.
[0081] The surfactant may be used alone or in combination of two or more.
[0082] When the optical film manufacturing film includes a surfactant, the lower limit of its content is preferably 0.01 mass parts relative to 100 mass parts of silanol-modified PVA, more preferably 0.02 mass parts, and more preferably 0.05 mass parts. By setting the content of the surfactant to more than the above lower limit, the film-making property and the peeling property are further improved. On the other hand, the upper limit of the content is preferably 0.5 mass parts relative to 100 mass parts of silanol-modified PVA, more preferably 0.3 mass parts, and more preferably 0.1 mass parts. By setting the content of the surfactant to below the above upper limit, it is possible to suppress the surfactant from oozing out to the surface of the film and causing adhesion, and it is possible to suppress the reduction of the handling property.
[0083] (Other additives, etc.)
[0084] The film for producing an optical film of the present invention may further contain fillers, processing stabilizers such as copper compounds, weathering stabilizers, colorants, ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, flame retardants, other thermoplastic resins, lubricants, fragrances, defoamers, deodorants, extenders, peeling agents, mold release agents, reinforcing agents, crosslinking agents, mildew inhibitors, preservatives, crystallization rate retarders and other additives as needed.
[0085] The film for optical film manufacturing of the present invention may contain PVA other than the above-mentioned silanol-modified PVA. The total proportion of all PVA, plasticizer and surfactant including silanol-modified PVA in the film for optical film manufacturing of the present invention is sometimes preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and further preferably 99% by mass or more. The film for optical film manufacturing of the present invention is substantially composed of PVA, plasticizer and surfactant, so that the effect of the present invention can be more fully exerted.
[0086] The content ratio of the silanol-modified PVA in the total PVA contained in the film for producing an optical film of the present invention is preferably 50% by mass or more, more preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and further preferably 99% by mass or more. In the film for producing an optical film of the present invention, by mainly using silanol-modified PVA as PVA, the effect of the present invention can be more fully exerted.
[0087] The total ratio of the silanol-modified PVA, the plasticizer, and the surfactant in the film for producing an optical film of the present invention is sometimes preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and further preferably 99% by mass or more. The film for producing an optical film of the present invention is substantially composed of the silanol-modified PVA, the plasticizer, and the surfactant, so that the effect of the present invention can be more fully exerted.
[0088] (Shape / physical properties, etc.)
[0089] The film for producing an optical film of the present invention is a so-called raw material film used as a material of an optical film. However, the film for producing an optical film of the present invention is not limited to the one in a roll shape.
[0090] The average thickness of the film for optical film manufacturing of the present invention is not particularly limited, and as a lower limit, it is preferably 1 μm, more preferably 5 μm, and further preferably 10 μm. By making the average thickness above the above lower limit, it is possible to suppress breakage during uniaxial stretching treatment when manufacturing the optical film. In addition, as the upper limit of the average thickness, it is preferably 75 μm, more preferably 60 μm, further preferably 45 μm, and further preferably 35 μm. By making the average thickness below the above upper limit, it is possible to suppress stretching unevenness during uniaxial stretching treatment. It should be noted that the "average thickness" refers to the average value of the thickness measured at any 5 points (hereinafter, the same for the average thickness).
[0091] The film for optical film manufacturing of the present invention may be a single-layer film composed of one PVA layer (a layer containing silanol-modified PVA), or a multilayer film containing one PVA layer. Among them, when used for manufacturing a polarizing film, etc., a single-layer film is preferred. As the lower limit of the average thickness of the PVA layer possessed by the film for optical film manufacturing of the present invention, it is preferably 1 μm, more preferably 5 μm, and further preferably 10 μm. By making the average thickness above the above lower limit, it is possible to suppress breakage during uniaxial stretching treatment when manufacturing the optical film. In addition, as the upper limit of the average thickness, it is preferably 75 μm, more preferably 60 μm, further preferably 45 μm, and further preferably 35 μm. By making the average thickness below the above upper limit, it is possible to suppress stretching unevenness during uniaxial stretching treatment.
[0092] The specific composition and suitable composition of the PVA layer in the film for producing an optical film can be referred to the description of the specific composition and suitable composition of the film for producing an optical film itself.
[0093] When the optical film manufacturing film of the present invention is a single-layer film, in order to ensure operability, the average thickness is preferably 20 μm or more, more preferably 30 μm or more. On the other hand, when the optical film manufacturing film of the present invention is a multilayer film, the average thickness of the PVA layer can be set to 20 μm or less, or 15 μm or less.
[0094] A multilayer film refers to a film having more than two layers. The number of layers of the multilayer film may be 5 or less layers, or 3 or less layers. As a multilayer film, a film for optical film manufacturing having a laminated structure of a substrate resin layer and a PVA layer may be cited. The average thickness of the substrate resin layer is, for example, 20 μm or more and 500 μm or less. The substrate resin layer in the multilayer film is preferably capable of uniaxial stretching together with the PVA layer. As the resin constituting the substrate resin layer, polyester, polyolefin, etc. may be used. Among them, an amorphous polyester resin is preferably used, and polyethylene terephthalate and an amorphous polyester resin obtained by copolymerizing polyethylene terephthalate with copolymer components such as isophthalic acid and 1,4-cyclohexanedimethanol are suitable. An adhesive layer may be provided between the substrate resin layer and the PVA layer.
[0095] The width of the optical film manufacturing film of the present invention is not particularly limited and can be determined according to its use, etc. For example, the lower limit of the width of the optical film manufacturing film is preferably 3m. In recent years, from the viewpoint of the gradual enlargement of the screen of liquid crystal televisions and liquid crystal monitors, if the width of the optical film manufacturing film is set to 3m or more in advance, it is suitable for the use of them as final products. On the other hand, the upper limit of the width of the optical film manufacturing film is preferably 7m. By setting the width to 7m or less, when the optical film is manufactured using a practical device, a uniaxial stretching treatment can be effectively performed.
[0096] From the viewpoints of productivity and optical properties of the optical film, the degree of swelling of the film for manufacturing the optical film of the present invention is preferably in the range of 140% to 400%. The lower limit of the degree of swelling is more preferably 180%, and more preferably 190%. In addition, the upper limit of the degree of swelling is more preferably 220%, and more preferably 210%. The degree of swelling of the film can be adjusted to a smaller value by, for example, strengthening the heat treatment conditions.
[0097] Here, "the degree of swelling of the membrane" refers to a value obtained by the following formula.
[0098] Swelling degree (%) = 100 × N / M
[0099] In the formula, N represents the mass (g) of the sample collected from the film after immersing it in distilled water at 30°C for 30 minutes and removing the surface water. M represents the mass (g) of the sample after drying it in a dryer at 105°C for 16 hours.
[0100] The film for optical film manufacturing of the present invention is usually a substantially unstretched film (unstretched film, non-stretched film). The in-plane phase difference of the original film for optical film manufacturing is preferably 100 nm or less, and more preferably 50 nm or less. Generally, the optical film can be obtained by stretching the film for optical film manufacturing of the present invention (uniaxial stretching treatment or biaxial stretching treatment).
[0101] The film for optical film manufacturing according to the present invention can have good productivity, and can obtain an optical film having better optical properties and moisture and heat resistance than the case of using unmodified PVA with the same degree of polymerization. It should be noted that the optical properties include light transmittance, polarization, etc. As optical films that can be manufactured using the film for optical film manufacturing, polarizing films, phase difference films, viewing angle improvement films, brightness enhancement films, etc. can be listed, preferably polarizing films.
[0102] <Method for producing film for optical film production>
[0103] The method for producing the film for producing an optical film of the present invention is not particularly limited, and a method that allows the film thickness and width to be more uniform after film production can be preferably used. For example, the film production solution can be prepared by dissolving silanol-modified PVA and, if necessary, one or more of a plasticizer, a surfactant, and other additives in a liquid medium. When the film production solution contains at least one of a plasticizer, a surfactant, and other additives, these components are preferably uniformly mixed.
[0104] As the liquid medium for preparing the film-making stock solution, for example, water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylene glycol, glycerol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, trimethylolpropane, ethylenediamine, diethylenetriamine, etc. can be listed, and one or more of these can be used. Among these, water is preferably used from the viewpoint of the burden on the environment and recyclability. In addition, the water solubility of the above-mentioned silanol-modified PVA is also good, and the viscosity increase when it is made into an aqueous solution at a higher temperature (for example, 80°C) is also suppressed. From this point of view, water can also be suitably used as the liquid medium.
[0105] The volatility of the film-forming stock solution (the proportion of volatile components such as liquid medium removed by volatilization and evaporation during film-forming) is preferably 50% by mass or more and 95% by mass or less, more preferably 55% by mass or more and 90% by mass or less, and further preferably 60% by mass or more and 85% by mass or less. By making the volatility of the film-forming stock solution 50% or more, the viscosity of the film-forming stock solution will not become too high, and the filtration and degassing when preparing the film-forming stock solution will be smoothly carried out, and it is easy to manufacture a film with few foreign matter and defects. On the other hand, by making the volatility of the film-forming stock solution 95% or less, the concentration of the film-forming stock solution will not become too low, and it is easy to manufacture the film industrially.
[0106] The temperature of the film-forming stock solution during film formation can be, for example, 70° C. to 90° C. By using silanol-modified PVA and forming the film at such a high temperature, the viscosity of the film-forming stock solution can be suppressed low, and film forming properties can be improved.
[0107] As the film-making method when using the film-making stock solution to make a film, for example, a cast film-making method, an extrusion film-making method, a wet film-making method, a gel film-making method, etc. can be listed. These film-making methods can only adopt one kind, and two or more kinds can also be combined. Among these film-making methods, the cast film-making method and the extrusion film-making method can obtain a film with uniform thickness and width and good physical properties, so it is preferred. The manufactured film can be dried, heat-treated as required.
[0108] As examples of specific methods for manufacturing the film for optical film manufacturing of the present invention, the following examples can be cited. Using a T-slit die, a hopper plate, an I-die, a lip coater die, etc., the film-making stock solution is uniformly sprayed or cast on the circumferential surface of the rotating and heated first roller (or belt) located on the most upstream side. The volatile components are evaporated from one surface of the film sprayed or cast on the circumferential surface of the first roller (or belt) to be dried. Then, it is further dried on the circumferential surface of one or more rotating and heated rollers arranged on its downstream side, or it is further dried by passing it through a hot air drying device. Thereafter, the film is wound up using a winding device. Drying based on a heated roller and drying based on a hot air drying device can be implemented in appropriate combination.
[0109] It should be noted that when the film for optical film manufacturing of the present invention is a multilayer film, the multilayer film can be manufactured by, for example, coating a film-making stock solution on a substrate resin film (substrate resin layer). In this case, in order to improve the adhesion between the PVA layer and the substrate resin layer, the surface of the substrate resin film can be modified or an adhesive can be coated on the surface of the substrate resin film.
[0110] <Method for producing optical film>
[0111] The method for producing an optical film of the present invention comprises the step of uniaxially stretching the film for producing an optical film. Hereinafter, as an example of the method for producing an optical film, a method for producing a polarizing film will be specifically described.
[0112] As a method for manufacturing a polarizing film, there can be cited a method that includes a dyeing step for dyeing a film for manufacturing an optical film (hereinafter also referred to as a "PVA film"), a stretching step for uniaxial stretching, a swelling step for further swelling the film as needed, a crosslinking step for crosslinking the film, a fixing step for fixing the film, a cleaning step for cleaning the film, a drying step for drying the film, a heat treatment step for heat treatment, etc. In this case, the order of the steps is not particularly limited, and the steps can be performed in the order of, for example, a swelling step, a dyeing step, a crosslinking step, a stretching step, a fixing step, etc. In addition, one or more steps can be performed simultaneously, and each step can be performed two or more times.
[0113] The swelling process can be performed by immersing the PVA film in water. The water temperature when immersed in water is preferably above 20°C and below 55°C, more preferably above 22°C and below 50°C, and further preferably above 25°C and below 45°C. In addition, the time of immersion in water is preferably, for example, above 0.1 minute and below 5 minutes, and more preferably above 0.5 minute and below 3 minutes. It should be noted that the water when immersed in water is not limited to pure water, and can be an aqueous solution in which various components are dissolved, or a mixture of water and an aqueous medium.
[0114] The dyeing process can be carried out by contacting the PVA film with a dichroic pigment. As a dichroic pigment, an iodine-based pigment is generally used. As the timing of dyeing, it can be any stage before uniaxial stretching, during uniaxial stretching, and after uniaxial stretching. It is suitable to adopt a method of dyeing by immersing the PVA film in a solution (especially an aqueous solution) containing iodine-potassium iodide as a dyeing bath. The iodine concentration in the dyeing bath is preferably 0.01 mass % or more and 0.5 mass % or less, and the concentration of potassium iodide is preferably 0.01 mass % or more and 10 mass % or less. In addition, the temperature of the dyeing bath is preferably set to 20°C or more and 50°C or less, and particularly preferably set to 25°C or more and 40°C or less. Suitable dyeing time is 0.2 minutes or more and 5 minutes or less.
[0115] By carrying out a cross-linking process in which the silanol-modified PVA in the PVA film is cross-linked, it is possible to effectively suppress the dissolution of the silanol-modified PVA into water during wet stretching at high temperature. From this point of view, the cross-linking process is preferably carried out after the dyeing process and before the stretching process. The cross-linking process can be carried out by immersing the PVA film in an aqueous solution containing a cross-linking agent. As a cross-linking agent, one or more boron compounds such as borate such as boric acid and borax can be used. The concentration of the cross-linking agent in the aqueous solution containing the cross-linking agent is preferably 1% by mass or more and 15% by mass or less, more preferably 1.5% by mass or more and 7% by mass or less, and further preferably 2% by mass or more and 6% by mass or less. By making the concentration of the cross-linking agent within the above range, sufficient stretchability can be maintained. The aqueous solution containing the cross-linking agent may contain potassium iodide and the like. The temperature of the aqueous solution containing the cross-linking agent is preferably set to be above 20°C and below 60°C, and particularly preferably set to be above 25°C and below 55°C. By setting the temperature within the above range, efficient cross-linking can be achieved.
[0116] The stretching process of uniaxially stretching the PVA film can be carried out by either a wet stretching method or a dry stretching method. In the case of the wet stretching method, it can be carried out in an aqueous solution containing boric acid, or in the above-mentioned dyeing bath or in the fixing treatment bath described later. In addition, in the case of the dry stretching method, stretching can be carried out directly at room temperature, or it can be stretched while heating, or it can be carried out in the air using the PVA film after absorbing water. Among these, from the aspect of being able to stretch along the width direction with high uniformity, the wet stretching method is preferably used, and uniaxial stretching is more preferably carried out in an aqueous solution containing boric acid. The boric acid concentration in the boric acid aqueous solution is preferably 0.5 mass % or more and 6.0 mass % or less, more preferably 1.0 mass % or more and 5.0 mass % or less, and particularly preferably 1.5 mass % or more and 4.0 mass % or less. In addition, the boric acid aqueous solution may contain potassium iodide, and the concentration of potassium iodide is preferably 0.01 mass % or more and 10 mass % or less. The stretching temperature in the uniaxial stretching is preferably 30° C. or higher and 90° C. or lower, more preferably 40° C. or higher and 80° C. or lower, particularly preferably 50° C. or higher and 75° C. or lower.
[0117] From the perspective of polarization performance of the obtained polarizing film, the stretching ratio in uniaxial stretching (total stretching ratio compared to the unstretched PVA film) is preferably 5 times or more, more preferably 5.5 times or more. The upper limit of the stretching ratio is not particularly limited, and the stretching ratio is preferably 8 times or less.
[0118] The uniaxial stretching direction when the long PVA film is uniaxially stretched is not particularly limited, and uniaxial stretching in the length direction and uniaxial stretching in the transverse direction can be adopted. From the aspect of being able to obtain a polarizing film with excellent polarization performance, uniaxial stretching in the length direction is preferred. The uniaxial stretching in the length direction can be performed by using a stretching device having a plurality of rollers parallel to each other and changing the circumferential speed between the rollers. On the other hand, the transverse uniaxial stretching can be performed using a tenter-type stretching machine.
[0119] When manufacturing a polarizing film, in order to make the dichroic pigment (iodine-based pigment, etc.) firmly adsorbed on the PVA film, a fixing treatment process can be performed after the stretching process. As a fixing treatment bath used in the fixing treatment, an aqueous solution containing one or more boron compounds such as boric acid and borax can be used. In addition, iodine compounds and metal compounds can be added to the fixing treatment bath as needed. The concentration of the boron compound in the fixing treatment bath is preferably 2% by mass or more and 15% by mass or less, particularly preferably 3% by mass or more and 10% by mass or less. By setting the concentration of the boron compound to within the above range, the adsorption of the dichroic pigment can be made more firmly. The temperature of the fixing treatment bath is preferably 15°C or more and 60°C or less, particularly preferably 25°C or more and 40°C or less.
[0120] The cleaning process is generally performed by immersing the film in distilled water, pure water, an aqueous solution, etc. At this time, from the viewpoint of improving polarization performance, it is preferred to use an aqueous solution containing an iodide such as potassium iodide as an auxiliary agent, and the concentration of the iodide is preferably set to 0.5 mass % or more and 10 mass % or less. In addition, the temperature of the aqueous solution in the cleaning process is usually 5°C or more and 50°C or less, preferably 10°C or more and 45°C or less, and more preferably 15°C or more and 40°C or less. By setting the temperature of the aqueous solution to the above range, the polarization performance can be further improved.
[0121] The drying conditions are not particularly limited, but the PVA film is preferably dried at a temperature of 30° C. to 150° C., particularly preferably 50° C. to 130° C. Drying at a temperature within the above range makes it easier to obtain a polarizing film having excellent dimensional stability.
[0122] It should be noted that optical films other than polarizing films such as retardation films can also be produced by a method including the step of uniaxially stretching the film for producing an optical film of the present invention. The specific production method can employ conventionally known methods except for using the film for producing an optical film of the present invention.
[0123] <Optical Film>
[0124] The optical film of the present invention is an optical film comprising PVA having a silicon-containing group (silanol-modified PVA), wherein the silicon-containing group is a silanol group or a group that can be converted into a silanol group in the presence of water, the viscosity-average degree of polymerization of the silanol-modified PVA is greater than 1,000 and less than 6,000, the degree of saponification is greater than 98.7 mol %, and the content of the silicon-containing group relative to all structural units is greater than 0.01 mol % and less than 1.0 mol %.
[0125] The optical film of the present invention may be an optical film obtained by the above-mentioned manufacturing method using the film for manufacturing the optical film of the present invention. The specific structure, content and other details of the silanol-modified PVA contained in the optical film of the present invention are the same as those of the silanol-modified PVA contained in the film for manufacturing the optical film of the present invention. In addition, the optical film of the present invention may contain other components that are the same as those of the film for manufacturing the optical film of the present invention.
[0126] The optical film of the present invention may be a polarizing film, a phase difference film, a viewing angle improving film, a brightness enhancing film, etc., preferably a polarizing film. In this case, the polarizing film generally contains a dichroic dye, and the silanol-modified PVA may be cross-linked.
[0127] The optical film of the present invention is preferably a stretched film, more preferably a uniaxially stretched film. In addition, the optical film of the present invention can be a single-layer film or a multi-layer film, preferably a single-layer film. In the case of such a film, the optical film of the present invention is more suitable for use as a polarizing film, etc.
[0128] When the optical film of the present invention is a polarizing film, the dichroic ratio (R) of the polarizing film is preferably 100 or more. By including the above-mentioned silanol-modified PVA, a polarizing film having such a high dichroic ratio (R) can be manufactured with good productivity. The dichroic ratio (R) is more preferably 150 or more, and further preferably 190 or more. The upper limit of the dichroic ratio (R) is, for example, 350, and can be 300.
[0129] The calculation method of the dichroic ratio (R) of the polarizing film is as follows. First, the relationship between the transmittance (T') after excluding surface reflection and the single transmittance (T) is shown in formula (a). At this time, the refractive index of the polarizing film is set to 1.5, and the surface reflectivity is set to 4%. The relationship between the transmittance (T'), the degree of polarization (V) and the dichroic ratio (R) is shown in formula (b). Therefore, based on the measurement of the single transmittance (T) and the degree of polarization (V), the dichroic ratio (R) of the polarizing film can be calculated by using these values to solve formulas (a) and (b).
[0130] T'=T / (1-0.04) 2 …(a)
[0131] R={-ln[T'(1-V)]} / {-ln[T'(1+V)]}...(b).
[0132] Polarizing film is usually used by laminating an optically transparent and mechanically strong protective film on both sides or one side thereof to form a polarizing plate. As the protective film, triacetyl cellulose (TAC) film, cycloolefin polymer (COP) film, cellulose acetate-butyrate (CAB) film, acrylic film, polyester film, etc. can be used. In addition, as adhesives for laminating, PVA adhesives, urethane adhesives, acrylate ultraviolet curing adhesives, etc. can be listed. That is, the polarizing plate has a polarizing film and a protective film directly laminated or laminated on one side or both sides of the polarizing film with the aid of an adhesive layer.
[0133] The polarizing plate can be used as a component of an LCD by, for example, applying an acrylic adhesive and then bonding it to a glass substrate. It should be noted that the polarizing plate may be further bonded with a phase difference film, a viewing angle improvement film, a brightness enhancement film, and the like. Example
[0134] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples. The methods of each measurement and evaluation are as follows.
[0135] [Polymerization degree of PVA (viscosity average polymerization degree)]
[0136] The viscosity average degree of polymerization of PVA synthesized in the following synthesis examples was measured in accordance with the description of JIS K6726-1994.
[0137] [Saponification degree of PVA]
[0138] The saponification degree of PVA synthesized in the following synthesis examples was measured in accordance with the description of JIS K6726-1994.
[0139] [Content of silicon-containing groups in PVA]
[0140] For the PVA synthesized in the following synthesis example, the content of silicon-containing groups relative to all structural units was measured based on the proton NMR of the vinyl ester polymer before saponification. When measuring the proton NMR of the vinyl ester polymer before saponification, the vinyl ester polymer was reprecipitated and purified using hexane-acetone to completely remove unreacted monomers from the polymer, then dried under reduced pressure at 90°C for 2 days, dissolved in CDCl3 solvent and subjected to analysis.
[0141] [Viscosity of 10 mass % PVA aqueous solution]
[0142] 10 g of PVA synthesized in the following synthesis example was weighed into a sample bottle, and pure water was added so as to make a total of 100 g. After being dissolved in a 95°C water bath for 4 hours while being stirred with a stirrer, it was left to stand overnight in a dryer at 80°C for degassing. The viscosity of the resulting 10% by mass PVA aqueous solution at 80°C was measured using a B-type viscometer.
[0143] [Swelling degree of membrane]
[0144] The films (films for optical film production) obtained in the following examples and comparative examples were cut into pieces of 1.5 g and immersed in 1000 g of distilled water at 30°C for 30 minutes. After immersion for 30 minutes, the film was taken out, and the surface water was absorbed with filter paper, and its mass (N) was measured. Then, the film was dried in a dryer at 105°C for 16 hours, and the mass (M) after drying was measured. The swelling degree of the film was calculated from the obtained mass (N) and mass (M) using the following formula.
[0145] Swelling degree (%) = 100 × N / M
[0146] [Dichroic ratio of polarizing film (optical performance)]
[0147] A rectangular sample of the polarizing film having a length of 4 cm was taken from the center of the width direction of the polarizing film obtained in the following examples and comparative examples. The sample was subjected to visibility correction in the visible light region of 2° field of view with C light source using a spectrophotometer ("V7100" manufactured by JASCO Corporation) with an integrating sphere in accordance with JIS Z8722 (method for measuring object color) and then measured for single transmittance (T) and polarization degree (V).
[0148] The dichroic ratio (R) of the polarizing film was calculated by solving the following equations (a) and (b) from the obtained single transmittance (T) and polarization degree (V). Here, the refractive index of the polarizing film was set to 1.5 and the surface reflectance was set to 4%.
[0149] T'=T / (1-0.04) 2 …(a)
[0150] R={-ln[T'(1-V)]} / {-ln[T'(1+V)]}...(b).
[0151] [Moisture and heat resistance of polarizing film]
[0152] The polarizing films obtained in the following examples and comparative examples were fixed to a metal frame, and a spectrophotometer with an integrating sphere ("V7100" manufactured by JASCO Corporation) was used to perform visibility correction in the visible light region of 2° field of view with C light source according to JIS Z8722 (method for measuring object color), and the single transmittance (T0) and polarization degree (V0) were measured on this basis. Furthermore, the polarizing film fixed to the metal frame was subjected to a wet heat treatment at 60°C and 90%RH for 12 hours, and the transmittance (T0) after 12 hours was measured by the spectrophotometer in the same manner. 12 ) and polarization degree (V 12 The increase in transmittance after wet heat treatment (T 12 -T0:%) and the reduction in polarization degree (V0-V 12 :%) as an indicator of moisture and heat resistance.
[0153] [Synthesis Example 1] Synthesis of PVA-1
[0154] 2590 g of vinyl acetate, 410 g of methanol and 5.3 g of vinyl trimethoxysilane were added to a 6L reaction tank equipped with a stirrer, a nitrogen inlet, an additive inlet and an initiator addition port. After the temperature was raised to 60°C, the system was purged with nitrogen by bubbling with nitrogen for 30 minutes. The temperature in the reaction tank was adjusted to 60°C, 0.32 g of 2,2'-azobis(isobutyronitrile) was added, and polymerization was started. From the moment of starting the polymerization, 135 g of methanol containing 2.5% by mass of vinyl methoxysilane was added to the system while performing a polymerization reaction for 3 hours, and the polymerization was stopped at this moment. The polymerization rate at the moment of stopping the polymerization reaction was 26.8%. It should be noted that the polymerization temperature was maintained at 60°C during the polymerization. Next, unreacted vinyl acetate was removed under reduced pressure to obtain a methanol solution of polyvinyl acetate (hereinafter sometimes abbreviated as PVAc).
[0155] The concentration of the obtained PVAc methanol solution was adjusted to 23.5%, and a NaOH methanol solution (10% concentration) was added to achieve an alkali molar ratio (number of moles of NaOH / number of moles of vinyl ester units in PVAc) of 0.04 for saponification. The obtained polyvinyl alcohol was washed with methanol.
[0156] The PVA-1 obtained by the above operation had a polymerization degree (viscosity average polymerization degree) of 2,400, a saponification degree of 99.9 mol %, a silicon-containing group content of 0.2 mol %, and a viscosity of 920 mPa·s in a 10 mass % aqueous solution at 80°C.
[0157] [Synthesis Examples 2~11] Synthesis of PVA-2~PVA-11
[0158] According to Synthesis Example 1, and by appropriately adjusting the ratio of the monomers used, the polymerization conditions and the saponification conditions, PVA-2~PVA-11 having the degree of polymerization (viscosity average degree of polymerization), saponification degree and SiOH group content (content of silicon-containing groups) recorded in Tables 1~3 were obtained.
[0159] [Example 1]
[0160] An aqueous solution containing 100 parts by mass of PVA-1, 10 parts by mass of glycerol as a plasticizer, and 0.1 parts by mass of sodium polyoxyethylene lauryl ether sulfate as a surfactant, and having a PVA content of 9.5% by mass, was prepared as a film-forming stock solution. The film-forming stock solution was dried on a metal roll at 80° C., and the obtained film was heat-treated at 120° C. for 10 minutes in a hot air dryer to adjust the swelling degree to 200%, thereby preparing a PVA film (film for optical film production) with an average thickness of 30 μm.
[0161] A sample of 5 cm in width × 9 cm in length was cut from the central part of the width direction of the obtained PVA film in a manner that a uniaxial stretching can be performed in a range of 5 cm in width × 5 cm in length. The sample was immersed in pure water at 30°C for 60 seconds, and uniaxially stretched to 2.0 times in the length direction for swelling treatment. Next, it was immersed in an aqueous solution containing 0.05% by mass of iodine and 5.0% by mass of potassium iodide (dyeing treatment bath: temperature 32°C) for 120 seconds, and uniaxially stretched to 1.2 times (2.4 times as a whole) in the length direction, so that iodine was adsorbed. Next, it was immersed in an aqueous solution containing 2.6% by mass of boric acid (boric acid cross-linking treatment bath: temperature 32°C) for 120 seconds, and uniaxially stretched to 1.25 times (3.0 times as a whole) in the length direction. Furthermore, the film was immersed in a 58°C aqueous solution (uniaxial stretching treatment bath) containing 2.8% by mass of boric acid and 5% by mass of potassium iodide, and uniaxially stretched in the longitudinal direction to 6.0 times as a whole. Thereafter, the film was washed by immersing in a 22°C potassium iodide aqueous solution (washing bath) containing 1.5% by mass of boric acid and 3.5% by mass of potassium iodide at a temperature of 22°C for 5 seconds. Finally, the film was dried at 80°C for 4 minutes to obtain a polarizing film.
[0162] The obtained polarizing film was used to measure the single transmittance (T) and polarization degree (V) by the above method to obtain the dichroic ratio (R). In addition, the wet heat resistance of the polarizing film was evaluated by the above method. The results are shown in Table 1.
[0163] [Examples 2 to 5 and Comparative Examples 1 to 4]
[0164] The PVA (PVA-2 to PVA-9) listed in Tables 1 to 3 was used, and the PVA content of the film-forming stock solution and the heat treatment temperature were adjusted so that the average thickness of the PVA film was 30 μm and the swelling degree was 200%. The same operation as in Example 1 was performed to produce and evaluate the PVA film. The obtained PVA film was used to produce and evaluate the polarizing film in the same manner as in Example 1. The results are shown in Tables 1 to 3.
[0165] [Comparative Example 5]
[0166] A PVA film was produced in the same manner as in Example 1 except that PVA-10 was used as PVA and the PVA content in the film-forming stock solution and the heat treatment temperature were adjusted so that the average thickness of the PVA film was 30 μm and the swelling degree was 200%. However, the film was broken in the uniaxial stretching treatment bath, and no polarizing film could be obtained.
[0167] [Comparative Example 6]
[0168] An attempt was made to prepare a film-forming stock solution and a 10 mass % PVA aqueous solution using PVA-11 as PVA, but PVA did not dissolve and the film-forming stock solution could not be prepared.
[0169] [Table 1]
[0170] .
[0171] [Table 2]
[0172] .
[0173] [Table 3]
[0174] .
[0175] As shown in Tables 1 to 3, PVA1 to PVA-5 used in Examples 1 to 5 are sufficient in water solubility to prepare film-making stock solutions, and the resulting PVA films (films for optical film manufacturing) can be fully stretched to obtain polarizing films. As such, it can be seen that the productivity of the PVA films of Examples 1 to 5 is good. In addition, compared with the polarizing films obtained using unmodified PVA having the same degree of polymerization, the polarizing films obtained from the PVA films of Examples 1 to 5 have excellent optical properties (dichroic ratio) and moisture and heat resistance. Specifically, as shown in Table 1, compared with the polarizing film of Comparative Example 1 obtained using unmodified PVA having a degree of polymerization of 2,400, the polarizing films of Examples 1 to 3 obtained using silanol-modified PVA having a degree of polymerization of 2,400 have a high dichroic ratio and a small reduction in polarization degree. Compared with the polarizing film of Comparative Example 2 obtained using unmodified PVA having a polymerization degree of 3,300, the polarizing film of Example 4 obtained using silanol-modified PVA having a polymerization degree of 3,300 has a high dichroic ratio, a small increase in transmittance, and a small decrease in polarization degree. Compared with the polarizing films of Comparative Examples 3 and 4 obtained using unmodified PVA having a polymerization degree of 1,700, the polarizing film of Example 5 obtained using silanol-modified PVA having a polymerization degree of 1,700 has a high dichroic ratio, a small increase in transmittance, and a small decrease in polarization degree.
[0176] In addition, if Comparative Example 2 is compared with Example 1, for example, using Comparative Example 1 obtained by using unmodified PVA with a polymerization degree of 2,400 as a reference, the following conclusions can be obtained. Comparative Example 2 uses PVA with a large polymerization degree relative to Comparative Example 1. Example 1 uses PVA modified with silanol relative to Comparative Example 1. The dichroic ratio of Comparative Example 2 is 201, and the dichroic ratio of Example 1 is 208, and the dichroic ratios are improved to the same extent compared with Comparative Example 1 with a dichroic ratio of 162. However, if the viscosity of the aqueous solution of PVA is compared, the viscosity of the PVA of Comparative Example 1 is 910 mPa・s, while the viscosity of the PVA of Comparative Example 2 is greatly increased to 2,740 mPa・s. On the other hand, the viscosity of the PVA of Example 1 is 920 mPa・s, and the increase in viscosity is suppressed. That is, it can be said that the silanol-modified PVA of the example can maintain good film forming properties (productivity) and improve the optical performance and moisture-heat resistance of the optical film.
[0177] Industrial Applicability
[0178] The film for producing an optical film of the present invention can be suitably used as a constituent material of LCD, that is, a material such as a polarizing film.
Claims
1. A film for optical film production, comprising polyvinyl alcohol having a silicon-containing group, The silicon-containing group is a silanol group or a group that can be converted into a silanol group in the presence of water, The polyvinyl alcohol has a viscosity average degree of polymerization of 1,000 or more and 6,000 or less, a saponification degree of 98.7 mol % or more, and a content of the silicon-containing group relative to all structural units of 0.01 mol % or more and 1.0 mol % or less, The polyvinyl alcohol has a structural unit represented by the following formula (4): The film for producing an optical film has a swelling degree of 140% or more and 400% or less, In formula (4), R 3 is a hydrogen atom or a methyl group; R 4 is a single bond or -(CH2) n -or-CONR 6 -R 7 - shown group, wherein, n is an integer from 1 to 5, R 6 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 7 For the above-(CH2) n -, or a divalent hydrocarbon group containing at least one of an oxygen atom and a nitrogen atom; R 5 A silicon-containing group.
2. The film for producing an optical film according to claim 1, wherein The saponification degree is 99.5 mol % or more.
3. The film for producing an optical film according to claim 1 or 2, wherein The product of the viscosity average degree of polymerization and the content of the silicon-containing group is 100 mol % or more and 2,000 mol % or less. The film for producing an optical film according to claim 1 or 2, which has an average thickness of 1 μm to 75 μm.
5. The film for producing an optical film according to claim 1 or 2, wherein The optical film is a polarizing film. The film for producing an optical film according to claim 1 or 2, which is an unstretched film. 7 . A method for producing an optical film, comprising the step of uniaxially stretching the film for producing an optical film according to claim 1 .
8. The method for producing an optical film according to claim 7, wherein: The optical film is a polarizing film.
9. An optical film comprising polyvinyl alcohol having a silicon-containing group, The silicon-containing group is a silanol group or a group that can be converted into a silanol group in the presence of water, The polyvinyl alcohol has a viscosity average degree of polymerization of 1,000 or more and 6,000 or less, a saponification degree of 98.7 mol % or more, and a content of the silicon-containing group relative to all structural units of 0.01 mol % or more and 1.0 mol % or less, The polyvinyl alcohol has a structural unit represented by the following formula (4): The film for producing an optical film has a swelling degree of 140% or more and 400% or less, In formula (4), R 3 is a hydrogen atom or a methyl group; R 4 is a single bond or -(CH2) n -or-CONR 6 -R 7 -, n is an integer from 1 to 5, R 6 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 7 For the above-(CH2) n -, or a divalent hydrocarbon group containing at least one of an oxygen atom and a nitrogen atom; R 5 A silicon-containing group. 10 . The optical film according to claim 9 , which is a polarizing film. The optical film according to claim 9 or 10, which is a single-layer film.