Flame retardant polycarbonate composition and thin-walled products made therefrom
By using homopolycarbonate, copolycarbonate, poly(carbonate-siloxane) and mineral-filled silicone flame retardant in thin-walled products, the heat resistance and low temperature resistance in thin-walled products are solved. The problem of difficulty in achieving impactability has achieved V0-level flame test and Vica softening temperature satisfaction.
Patent Information
- Application Number
- CN202080068424.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-09-30
AI Technical Summary
It is difficult to achieve heat resistance and low temperature impact resistance in thin-walled products, and existing flame retardant compositions may lead to a decrease in Vicar softening temperature and thermal deformation temperature when improving flame performance.
Using silicone flame retardant synergist containing homopolycarbonate, copolycarbonate, poly(carbonate-siloxane), mineral-filled silicone flame retardant, anti-drip agent and C1-16 alkyl sulfonate flame retardant The composition is ensured that the Vicar softening temperature and flame test grade are met by testing the molded sample under ISO-306 and UL-94 standards.
The flame retardant test grade and low-temperature impact resistance of V0 at 1.0 mm and 0.8 mm thicknesses were achieved while maintaining excellent properties of poly(carbonate-siloxane), such as impact resistance and thermal properties.
Smart Images

Figure BDA0003571041180000021 
Figure BDA0003571041180000031 
Figure BDA0003571041180000032
Abstract
Description
[0001] Related Applications
[0002] This application claims the benefit of U.S. Application No. 62 / 908,096, filed September 30, 2019, which is incorporated herein by reference in its entirety. Background Art
[0003] The present disclosure relates to flame retardant compositions, and in particular to flame retardant compositions, methods of preparation, and use thereof in thin-walled articles.
[0004] Polycarbonates can be used to make articles and assemblies for a wide range of applications, from automotive parts to electronic appliances. Due to their widespread use, especially in electronic devices, it is desirable to provide flame retardant polycarbonates with heat resistance and impact resistance. In thin-wall applications, such as applications where the thickness of the polycarbonate at any position in the article is 0.2 to 1.0 mm, or 0.2 to 0.8 mm, or 0.2 to 0.4 mm, it may be particularly difficult to achieve such properties.
[0005] Therefore, there remains a need in the art for flame retardant compositions having good heat resistance and low temperature impact resistance in thin wall articles. Summary of the invention
[0006] The above and other deficiencies in the art are met by a flame retardant composition comprising: 34-94 wt% of a homopolycarbonate, a copolycarbonate, or a combination thereof; 5-85 wt% poly(carbonate-siloxane) in an amount effective to provide 2-6 wt% dimethylsiloxane; 0.05-0.6 wt%, preferably 0.1-0.4 wt% C 1-16 an alkyl sulfonate flame retardant; 1-15 wt % of a mineral-filled silicone flame retardant synergist; 0.05-0.5 wt % of an anti-drip agent; optionally, 0.001-10 wt % of an additive composition, or 1-20 wt % of a glass fiber composition, or a combination thereof, wherein each amount is based on a total weight of the flame retardant composition totaling 100 wt %; and wherein a molded sample of the flame retardant composition has a Vicat softening temperature greater than or equal to 140° C. measured at a load of 10 N and a heating rate of 50° C. / hour according to ISO-306 standard, and a flame test rating of V0 measured at a thickness of 1.0 mm or at a thickness of 0.8 mm according to UL-94.
[0007] In another aspect, a method of preparation includes combining the above components to form a flame retardant composition.
[0008] In yet another aspect, an article comprises the flame retardant composition described above.
[0009] In yet another aspect, a method for preparing an article comprises molding, extruding, or forming the flame retardant composition described above into an article.
[0010] The above described and other features are exemplified by the following detailed description, examples, and claims. DETAILED DESCRIPTION
[0011] Poly(carbonate-siloxane) can offer advantages over standard polycarbonates, such as low temperature impact, high ductility, better flow, chemical resistance, and hydrolytic stability. However, as the demand for weight reduction and complexity in product design increases, there is a need to develop engineering thermoplastic compositions that can meet market trends and stricter regulations, including flame performance at low thicknesses.
[0012] By adding phosphorus-based additives, those skilled in the art can achieve thin wall UL94 V0 performance, however, this can undesirably result in a reduction in one or both of the Vicat softening temperature and the heat distortion temperature (HDT). Therefore, there is a need for a flame retardant composition having thin wall UL94 flame retardancy (e.g., V0 at 0.8 mm) while maintaining the favorable properties of poly(carbonate-siloxane) (e.g., impact resistance).
[0013] Surprisingly and unexpectedly, the present inventors have discovered herein that a flame retardant comprising a homopolycarbonate, a copolycarbonate or a combination thereof, a poly(carbonate-siloxane), a mineral-filled silicone flame retardant synergist, an anti-drip agent, and C 1-16 The molded samples of the composition of the alkyl sulfonate flame retardant provided a combination of flame retardant test ratings of V0 at 1.0 mm thickness and 0.8 mm thickness and low temperature impact resistance. Advantageously, the flame retardant composition maintains thermal properties, such as Vicat softening temperature.
[0014] As used herein, "polycarbonate" refers to a polymer having repeating structural carbonate units of formula (1):
[0015]
[0016] Among them, R 1 At least 60% of the total number of groups contain aromatic moieties, with the remainder being aliphatic, alicyclic or aromatic. 1 It is C 6-30 An aromatic group is a group that contains at least one aromatic moiety. 1 Can be derived from the formula HO-R 1 -OH, especially an aromatic dihydroxy compound of formula (2):
[0017] HO-A 1 -Y 1 -A 2 -OH (2)
[0018] Among them A 1 and A 2 are each a monocyclic divalent aromatic group, and Y 1 is a single bond or has A 1 With A 2 In one aspect, one atom separates A 1 With A 2 Preferably, each R 1 It can be derived from bisphenols of formula (3):
[0019]
[0020] Where R a and R b are independently halogen, C 1-12 Alkoxy or C 1-12 alkyl, p and q are each independently an integer from 0 to 4. It should be understood that when p or q is less than 4, the valence of each carbon of the ring is filled with hydrogen. a is a bridging group connecting two hydroxy-substituted aromatic groups, wherein the bridging group and the hydroxy substituent of each C6 arylene group are arranged in the ortho, meta or para position (preferably para position) to each other on the C6 arylene group. a is a single bond, -O-, -S-, -S(O)-, -S(O)2-, -C(O)-, or C 1-60 Organic groups. The organic bridging group may be cyclic or acyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogens, oxygen, nitrogen, sulfur, silicon or phosphorus. C 1-60 The organic group is such that the C6 arylene groups attached thereto are each attached to a common alkylidene carbon or to a C 1-60 In one aspect, p and q are each 1, and R a and R b Each is a C arranged meta to the hydroxyl group on each arylene group 1-3 Alkyl group, preferably methyl group.
[0021] In one aspect, X a It is C 3-18 Cycloalkylidene, formula -C(R c )(R d )-C 1-25 Alkylene, where R c and R d are independently hydrogen, C 1-12 Alkyl, C 1-12 Cycloalkyl, C 7-12 Arylalkyl, C 1-12Heteroalkyl, or cyclic C 7-12 Heteroarylalkyl, or -C(=R e )-, wherein R e It is a two-price C 1-12 Hydrocarbyl. These types of groups include methylene, cyclohexylmethylidene, ethylidene, neopentylidene, and isopropylidene, as well as 2-[2.2.1]-bicycloheptylidene, cyclohexylidene, 3,3-dimethyl-5-methylcyclohexylidene, cyclopentylidene, cyclododecylidene, and adamantylidene.
[0022] In another aspect, X a It is C 1-18 Alkylene, C 3-18 Cycloalkylene, fused C 6-18 Cycloalkylene, or formula -J 1 -GJ 2 - group, where J 1 and J 2 Is the same or different C 1-6 Alkylene, G is C 3-12 Cycloalkylidene or C 6-16 Arylene.
[0023] For example, X a It can be a substituted C of formula (4) 3-18 Cycloalkylidene
[0024]
[0025] Where R r , R p , R q and R t are independently hydrogen, halogen, oxygen, or C 1-12 Hydrocarbyl; Q is a direct bond, carbon, or divalent oxygen, sulfur, or -N(Z)-, wherein Z is hydrogen, halogen, hydroxyl, C 1-12 Alkyl, C 1-12 Alkoxy, C 6-12 Aryl or C 1-12 acyl; r is 0 to 2, t is 1 or 2, q is 0 or 1, and k is 0 to 3, provided that R r , R p , R q , and R tAt least two of the fused rings are together a fused alicyclic, aromatic or heteroaromatic ring. It should be understood that when the fused ring is aromatic, the ring shown in formula (4) will have unsaturated carbon-carbon bonds, wherein the ring is fused. When k is 1 and q is 0, the ring shown in formula (4) contains 4 carbon atoms, when k is 2, the ring shown in formula (4) contains 5 carbon atoms, and when k is 3, the ring contains 6 carbon atoms. In one aspect, two adjacent groups (e.g., R q and R t together) form an aromatic group, and in another aspect, R q and R t together form an aromatic group and R r and R p Together they form a second aromatic group. q and R t When they form an aromatic group, R p It may be a double-bonded oxygen atom, ie, a ketone, or Q may be -N(Z)-, wherein Z is phenyl.
[0026] Bisphenol, of which X a is a cycloalkylidene group of formula (4) and can be used to prepare a polycarbonate containing a phthalide carbonate unit of formula (1a)
[0027]
[0028] Where R a , R b , p and q are as in formula (3), R 3 Each independently is C 1-6 alkyl, j is 0 to 4, and R4 is hydrogen, C 1-6 Alkyl, or substituted or unsubstituted phenyl, for example with up to 5 C 1-6 For example, the phthalide carbonate unit has the formula (1b):
[0029]
[0030] Where R 5 is hydrogen, optionally substituted with up to 5 C 1-6 Alkyl or C 1-4 In the aspect of formula (1b), R 5 is hydrogen, methyl or phenyl, preferably phenyl. Carbonate unit (1b), (wherein R 5 is phenyl) may be derived from 2-phenyl-3,3'-bis(4-hydroxyphenyl)phthalimide (also known as 3,3-bis(4-hydroxyphenyl)-2-phenylisoindolin-1-one, or N-phenylphenolphthalein bisphenol ("PPPBP")).
[0031] Other bisphenol carbonate repeating units of this type are isatin carbonate units of formula (1c) and (1d)
[0032]
[0033] Where R a and R b are independently halogen, C 1-12 Alkoxy or C 1-12 alkyl, p and q are each independently 0 to 4, and R i It is C 1-12 Alkyl, optionally substituted with 1 to 5 C 1-10 Alkyl-substituted phenyl or optionally substituted with 1 to 5 C 1-10 In one aspect, R a and R b are each methyl, p and q are each independently 0 or 1, and R i It is C 1-4 Alkyl or phenyl.
[0034] Other examples of bisphenol carbonate units derived from bisphenol (3) wherein X a is substituted or unsubstituted C 3-18 Cycloalkylidene, including cyclohexylidene-bridged bisphenols of formula (1e)
[0035]
[0036] Where R a and R b Each is independently C 1-12 Alkyl, R g It is C 1-12 alkyl, p and q are each independently 0 to 4, and t is 0 to 10. In one specific aspect, each R a and R b In one aspect, at least one of R a and R b Each is independently C 1-4 Alkyl, R g It is C 1-4 alkyl, p and q are each 0 or 1, and t is 0 to 5. In another specific aspect, R a , R b and R g Each is methyl, p and q are each 0 or 1, and t is 0 or 3, preferably 0. In yet another aspect, p and q are each 0, each R g is methyl, and t is 3, such that X a It is 3,3-dimethyl-5-methylcyclohexylidene.
[0037] Examples of other bisphenol carbonate units derived from bisphenol (3) wherein X a is substituted or unsubstituted C 3-18 Cycloalkylidene groups, including adamantyl units of formula (1f) and fluorenyl units of formula (1g)
[0038]
[0039] Where R a and R b Each is independently C 1-12 alkyl, p and q are each independently 1 to 4. In one specific aspect, each R a and R b In one aspect, at least one of R a and R b Each is independently C 1-3 alkyl, and p and q are each 0 or 1; preferably, R a , R b Each is a methyl group, p and q are each 0 or 1, and when p and q are 1, the methyl group is arranged at the meta position of the cycloalkylidene bridging group. The carbonate containing units (1a) to (1g) can be used to prepare a polycarbonate having a high glass transition temperature (Tg) and a high heat deformation temperature.
[0040] Formula HO-R 1 Other useful dihydroxy compounds of -OH include aromatic dihydroxy compounds of formula (6):
[0041]
[0042] Each R h are independently a halogen atom, C 1-10 Hydrocarbon groups such as C 1-10 Alkyl, halogen substituted C 1-10 Alkyl, C 6-10 Aryl or halogen substituted C 6-10 Aryl, and n is 0 to 4. Halogen is typically bromine.
[0043] Some illustrative examples of dihydroxy compounds that can be used are described, for example, in WO 2013 / 175448 A1, US 2014 / 0295363 and WO 2014 / 072923. Specific examples of the bisphenol compound of formula (3) include 1,1-bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane (hereinafter "bisphenol A" or "BPA"), 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, 1,1-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)n-butane, 2,2-bis(4-hydroxy-2-methylphenyl)propane, 1,1-bis(4-hydroxy-tert-butylphenyl)propane, 3,3-bis(4-hydroxyphenyl)phthalimide, 2-phenyl-3,3-bis(4-hydroxyphenyl)phthalimide (PPPBP), and 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane (DMBPC). Combinations may also be used. In one specific aspect, the polycarbonate is a linear homopolymer derived from bisphenol A, wherein each A in formula (3) 1 and A 2 is p-phenylene, and Y 1 It is isopropylidene.
[0044] The polycarbonate may have an intrinsic viscosity of 0.3 to 1.5 deciliters per gram (dl / gm), preferably 0.45 to 1.0 dl / gm, as measured in chloroform at 25°C. The polycarbonate may have a weight average molecular weight (Mw) of 20,000 to 30,000 grams per mole (g / mol), preferably 20,000 to 25,000 g / mol, 25,000 g / mol to 35,000 g / mol, preferably 27,000 to 32,000 g / mol, such as by gel permeation chromatography (GPC) using a crosslinked styrene-divinylbenzene column and calibrated to a bisphenol A homopolycarbonate reference. GPC samples were prepared at a concentration of 1 mg / ml and eluted at a flow rate of 1.5 ml / min.
[0045] The homopolycarbonate, copolycarbonate, or combinations thereof can be present, for example, 34-94 wt%, 40-80 wt%, 50-80 wt%, 60-80 wt%, 70-80 wt%, or 65-75 wt%, each based on the total weight of the flame retardant composition.
[0046] "Polycarbonate" includes homopolycarbonates (wherein each R 1 are the same), in carbonates ("copolycarbonates") containing different R 1 The copolycarbonate may contain bisphenol A units and at least one other type of unit.
[0047] The flame retardant composition comprises a poly(carbonate-siloxane), also known in the art as a polycarbonate-polysiloxane copolymer. The polysiloxane block comprises repeating diorganosiloxane units as in formula (10):
[0048]
[0049] Where each R is independently C 1-13 A monovalent organic group. For example, R can be C 1-13 Alkyl, C 1-13 Alkoxy, C 2-13 Alkenyl, C 2-13 Alkenyloxy, C 3-6 Cycloalkyl, C 3-6 Cycloalkoxy, C 6-14 Aryl, C 6-10 Aryloxy, C 7-13 Arylalkylene, C 7-13 Aryl alkeneoxy, C 7-13 Alkyl arylene or C 7-13 The foregoing groups may be completely or partially halogenated with fluorine, chlorine, bromine, or iodine, or combinations thereof. In one aspect, when a transparent poly(carbonate-siloxane) is desired, R is not substituted with halogen. Combinations of the foregoing R groups may be used in the same copolymer.
[0050] The value of E in formula (10) can vary widely, depending on the type and relative amount of each component in the flame retardant composition, the desired performance of the composition, and other considerations. Typically, E has an average value of 2 to 1,000, preferably 2 to 500, 2 to 200, or 2 to 125, 5 to 80, or 10 to 70. In one aspect, E has an average value of 10 to 80 or 10 to 40, and in another aspect, E has an average value of 40 to 80, or 40 to 70. When E has a lower value, such as less than 40, it is desirable to use a relatively large amount of poly (carbonate-siloxane) copolymers. On the contrary, when E has a higher value, such as greater than 40, a relatively low amount of poly (carbonate-siloxane) copolymers can be used. A combination of the first and second (or more) poly (carbonate-siloxane) copolymers can be used, wherein the average value of E of the first copolymer is less than the average value of E of the second copolymer.
[0051] In one aspect, the polysiloxane block has formula (11)
[0052]
[0053] wherein E and R are as defined in formula (10); each R may be the same or different and is as defined above; and Ar may be the same or different and is substituted or unsubstituted C6-30 Arylene, wherein the bond is directly attached to the aromatic moiety. The Ar group in formula (11) can be derived from C 6-30 Dihydroxyarylene compounds, for example dihydroxyarylene compounds of formula (3) or (6). Dihydroxyarylene compounds are 1,1-bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, 1,1-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)n-butane, 2,2-bis(4-hydroxy-1-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl sulfide) and 1,1-bis(4-hydroxy-tert-butylphenyl)propane.
[0054] In another aspect, the polysiloxane block has formula (13)
[0055]
[0056] where R and E are as described above, and each R 5 Independently divalent C 1-30 In one specific aspect, the polysiloxane block has the formula (14):
[0057]
[0058] wherein R and E are as defined above. 6 For divalent C 2-8 Each M in formula (14) may be the same or different and may be halogen, cyano, nitro, C 1-8 Alkylthio, C 1-8 Alkyl, C 1-8 Alkoxy, C 2-8 Alkenyl, C 2-8 Alkenyloxy, C 3-8 Cycloalkyl, C 3-8 Cycloalkoxy, C 6-10 Aryl, C 6-10 Aryloxy, C 7-12 Aralkyl, C 7-12 Aralkyloxy, C 7-12 Alkyl or C 7-12 Alkaryloxy, wherein each n is independently 0, 1, 2, 3 or 4.
[0059] In one aspect, M is bromo or chloro, alkyl such as methyl, ethyl or propyl, alkoxy such as methoxy, ethoxy or propoxy, or aryl such as phenyl, chlorophenyl or tolyl; R 6is dimethylene, trimethylene or tetramethylene; and R is C 1-8 In one aspect, R is methyl, M is methoxy, n is 1, and R is 1. 6 It is a two-price C 1-3 The specific polysiloxane block has the following formula
[0060]
[0061] or a combination thereof, wherein E has an average value of 2 to 200, 2 to 125, 5 to 125, 5 to 100, 5 to 50, 20 to 80, or 5 to 20.
[0062] The blocks of formula (14) can be derived from the corresponding dihydroxy polysiloxanes, which in turn can be prepared to effect a platinum-catalyzed addition between siloxane hydrides and aliphatically unsaturated monohydric phenols such as eugenol, 2-alkylphenols, 4-allyl-2-methylphenol, 4-allyl-2-phenylphenol, 4-allyl-2-bromophenol, 4-allyl-2-tert-butoxyphenol, 4-phenyl-2-phenylphenol, 2-methyl-4-propylphenol, 2-allyl-4,6-dimethylphenol, 2-allyl-4-bromo-6-methylphenol, 2-allyl-6-methoxy-4-methylphenol, and 2-allyl-4,6-dimethylphenol. Poly(carbonate-siloxane) copolymers can then be prepared, for example, by the synthetic procedure of European Patent Application Publication No. 0 524 731 A1 to Hoover, page 5, Preparation 2.
[0063] The transparent poly(carbonate-siloxane) copolymer comprises carbonate units (1) derived from bisphenol A, and repeating siloxane units (14a), (14b), (14c), or a combination thereof (preferably Formula 14a), wherein E has an average value of 4 to 50, 4 to 15, preferably 5 to 15, more preferably 6 to 15, and still more preferably 7 to 10. The transparent copolymer can be made using one or both of the tubular reactor processes described in U.S. Patent Application 2004 / 0039145A1, or alternatively the poly(carbonate-siloxane) copolymer can be synthesized using the process described in U.S. Patent No. 6,723,864.
[0064] The poly(carbonate-siloxane) copolymer can contain 50 to 99 weight percent carbonate units and 1 to 50 weight percent siloxane units. Within this range, the poly(carbonate-siloxane) copolymer can contain 70 to 98 weight percent, more preferably 75 to 97 weight percent carbonate units and 2 to 30 weight percent, more preferably 3 to 25 weight percent siloxane units.
[0065] In one aspect, blends of the formula are used, particularly blends of bisphenol A homopolycarbonate and poly(carbonate-siloxane) block copolymers of bisphenol A blocks and eugenol-terminated polydimethylsiloxane blocks.
[0066]
[0067] wherein x is 1 to 200, preferably 5 to 85, preferably 10 to 70, preferably 15 to 65, and more preferably 40 to 60; x is 1 to 500, or 10 to 200, and z is 1 to 1000, or 10 to 800. In one aspect, x is 1 to 200, y is 1 to 90 and z is 1 to 600, and in another aspect, x is 30 to 50, y is 10 to 30 and z is 45 to 600. The polysiloxane blocks may be randomly distributed or controlled distributed in the polycarbonate blocks.
[0068] In one aspect, the poly(carbonate-siloxane) copolymer comprises 10 weight percent (wt%) or less, preferably 6 wt% or less, and more preferably 4 wt% or less of polysiloxane, based on the total weight of the poly(carbonate-siloxane) copolymer, and is generally optically transparent and is commercially available from SABIC under the name EXL-T. In another aspect, the poly(carbonate-siloxane) copolymer comprises 10 wt% or more, preferably 12 wt% or more, and more preferably 14 wt% or more of the polysiloxane copolymer, based on the total weight of the poly(carbonate-siloxane) copolymer, which is generally optically opaque and is commercially available from SABIC as EXL-P.
[0069] The flame retardant composition can include a poly(carbonate-siloxane) with 40wt% siloxane content, a poly(carbonate-siloxane) with 20wt% siloxane content, a poly(carbonate-siloxane) with 6wt% siloxane content, or a combination thereof. In some aspects, the flame retardant composition includes 5-15wt% or 5-10wt% of a poly(carbonate-siloxane) copolymer with 40wt% siloxane content. In some aspects, the flame retardant composition includes 10-25wt%, 10-20wt% or 10-15wt% of a poly(carbonate-siloxane) copolymer with 20wt% siloxane content. In some aspects, the flame retardant composition includes 35-82wt%, 45-82wt%, 55-82wt% or 65-82wt% of a poly(carbonate-siloxane) copolymer with 6wt% siloxane content.
[0070] The poly(carbonate-siloxane) can have a weight average molecular weight of 2,000 to 100,000 g / mol, preferably 5,000 to 50,000 g / mol, as measured by gel permeation chromatography using a crosslinked styrene-divinylbenzene column at a sample concentration of 1 mg / ml and as calibrated using polycarbonate standards.
[0071] The poly(carbonate-siloxane) can have a melt volume flow rate of 1 to 50 cubic centimeters per 10 minutes (cc / 10 min), preferably 2 to 30 cc / 10 min, measured at 300°C / 1.2 kg. Combinations of poly(carbonate-siloxane)s having different flow properties can be used to achieve the overall desired flow properties.
[0072] The poly(carbonate-siloxane) can be present, for example, at 5-85 wt%, 5-70 wt%, 5-50 wt%, 5-35 wt%, 10-70 wt%, 10-50 wt%, 10-35 wt%, 10-30 wt%, 15-50 wt% or 15-30 wt%, each based on the total weight of the flame retardant composition.
[0073] The flame retardant composition comprises C 1-16 Alkyl sulfonate flame retardants. Examples include potassium perfluorobutane sulfonate (Rimar salt), potassium perfluorooctane sulfonate, and tetraethylammonium perfluorohexane sulfonate. Based on the total weight of the flame retardant composition, C 1-16 The alkyl sulfonate flame retardant is present in an amount of 0.05-0.6 wt%, preferably 0.1-0.4 wt%. 1-16Alkyl sulfonate flame retardants are additional flame retardants, and may include salts of aromatic sulfonates such as sodium benzene sulfonate, sodium toluene sulfonate (NaTS), etc., aromatic sulfone sulfonates such as potassium diphenyl sulfone sulfonate (KSS), etc.; by reacting, for example, alkali metals or alkaline earth metals (e.g., lithium, sodium, potassium, magnesium, calcium, and barium salts) with inorganic acid complex salts, such as oxygen anions (e.g., alkali metal and alkaline earth metal salts of carbonate, such as Na2CO3, K2CO3, MgCO3, CaCO3, and BaCO3, or fluoride anion complexes such as Li3AlF6, BaSiF6, KBF4, K3Al F6, KAlF4, K2SiF6 or Na3AlF6 etc. are formed by reaction. Rimar salt and KSS and NaTS, alone or in combination with other flame retardants, are particularly useful. When present, inorganic flame retardant salts are generally present in an amount of 0.01-5.0 parts by weight, more preferably 0.1 to 1.0 parts by weight, based on 100 parts by weight of the flame retardant composition. Aromatic sulfonates may be present in an amount of 0.01 to 0.1 wt%, preferably 0.02 to 0.06 wt%, and more preferably 0.03 to 0.05 wt%, based on 100 parts by weight of the flame retardant composition.
[0074] In one respect, unlike C 1-16 The flame retardant of the alkyl sulfonate flame retardant is an organophosphorus flame retardant. In the organophosphorus flame retardant having at least one organic aromatic group, the aromatic group can be a substituted or unsubstituted C containing one or more monocyclic or polycyclic aromatic moieties (which can optionally contain up to three heteroatoms (N, O, P, S or Si)) and optionally also containing one or more non-aromatic moieties (e.g., alkyl, alkenyl, alkynyl or cycloalkyl). 3-30 Group. The aromatic portion of the aromatic group can be directly bonded to the organophosphorus flame retardant, or bonded via another portion (e.g., an alkylene group). The aromatic portion of the aromatic group can be directly bonded to the organophosphorus flame retardant, or bonded via another portion (e.g., an alkylene group). In one aspect, the aromatic group is the same as the aromatic group of the polycarbonate backbone, such as a bisphenol group (e.g., bisphenol A), a monoarylene group (e.g., 1,3-phenylene or 1,4-phenylene), or a combination comprising at least one of the foregoing.
[0075] The organophosphorus flame retardant may include a phosphate (P(=O)(OR)3), a phosphite (P(OR)3), a phosphonate (RP(=O)(OR)2), a phosphinate (R2P(=O)(OR)), a phosphine oxide (R3P(=O)) or a phosphine (R3P), wherein each R in the aforementioned organophosphorus flame retardant may be the same or different, provided that at least one R is an aromatic group. Combinations of different organophosphorus flame retardants may be used. The aromatic group may be directly or indirectly bonded to the phosphorus or oxygen of the organophosphorus flame retardant (i.e., the ester).
[0076] In one aspect, the organophosphorus flame retardant is a monomeric phosphate. Representative monomeric aromatic phosphates have the formula (GO) 3P = O, wherein each G is independently an alkyl, cycloalkyl, aryl, alkylarylene or arylalkylene group having up to 30 carbon atoms, provided that at least one G is an aromatic group. Two G groups can be linked together to provide a cyclic group. In some aspects, G corresponds to a monomer for forming a polycarbonate, for example, resorcinol. Exemplary phosphates include phenyl didodecyl phosphate, phenyl di(neopentyl) phosphate, phenyl di(3,5,5'-trimethylhexyl) phosphate, ethyl diphenyl phosphate, 2-ethylhexyl di(p-tolyl) phosphate, di(2-ethylhexyl) p-tolyl phosphate, tricresyl phosphate, di(2-ethylhexyl) phenyl phosphate, tri(nonylphenyl) phosphate, didodecyl p-tolyl phosphate, dibutylphenyl phosphate, 2-chloroethyl diphenyl phosphate, p-tolyl di(2,5,5'-trimethylhexyl) phosphate, 2-ethylhexyl diphenyl phosphate, etc. Specific aromatic phosphates are those in which each G is aromatic, for example, triphenyl phosphate, tricresyl phosphate, isopropylated triphenyl phosphate, etc.
[0077] Di- or polyfunctional organophosphorus flame retardants are also useful, for example, compounds of the formula:
[0078]
[0079] Each G 1 Independently for C 1-30 Hydrocarbon; each G 2 Independently for C 1-30 Hydrocarbyl or alkoxy; X a As defined in formula (3) or formula (4); each X is independently bromine or chlorine; m is 0 to 4, and n is 1 to 30. In one specific aspect, X a It is a single bond, methylene, isopropylidene or 3,3,5-trimethylcyclohexylidene.
[0080] Specific organophosphorus flame retardants include acid esters of formula (13):
[0081]
[0082] Each R 16 Independently for C 1-8 Alkyl, C 5-6 Cycloalkyl, C 6-20 Aryl or C 7-12 Arylalkylene, each optionally substituted with C 1-12 Alkyl, specifically C 1-4 alkyl substituted, and X is a mononuclear or polynuclear aromatic C 6-30 Partial or linear or branched C2-30 an aliphatic group which may be OH-substituted and may contain up to 8 ether bonds, provided that at least one R 16 or X is an aromatic group; each n is independently 0 or 1; and q is 0.5 to 30. In some aspects, each R 16 Independently for C 1-4 Alkyl, naphthyl, phenyl (C 1-4 ) alkylene, optionally C 1-4 Alkyl substituted aryl; each X is a mononuclear or polynuclear aromatic C 6-30 In some aspects, each R 16 is aromatic, such as phenyl; each X is a mononuclear or polynuclear aromatic C 6-30 moieties, including moieties derived from formula (2); n is 1; and q is 0.8 to 15. In other aspects, each R 16 is phenyl; X is tolyl, xylyl, propylphenyl or butylphenyl, one of the following divalent groups:
[0083]
[0084] or a combination comprising one or more of the foregoing; n is 1; and q is 1 to 5, or 1 to 2. In some aspects, at least one R 16 Or X corresponds to the monomer used to form the polycarbonate, such as bisphenol A, resorcinol, etc. This type of organophosphorus flame retardants include bis(diphenyl)phosphate of hydroquinone, resorcinol bis(diphenyl phosphate) (RDP), and bisphenol A bis(diphenyl)phosphate (BPADP) and their oligomeric and polymeric counterparts.
[0085] The organophosphorus flame retardant containing a phosphorus-nitrogen bond can be a phosphazene, a phosphazene chloride, a phosphorus ester amide, a phosphoric acid amide, a phosphonic acid amide, a phosphinate amide or a tri(aziridinyl)phosphine oxide. These flame retardant additives are commercially available. In one aspect, the organophosphorus flame retardant containing a phosphorus-nitrogen bond is a phosphazene or a cyclophosphazene of the formula:
[0086]
[0087] wherein w1 is 3 to 10,000; w2 is 3 to 25, or 3 to 7; and each R w Independently for C 1-12 In the aforementioned groups, at least one hydrogen atom in these groups may be substituted by a group having N, S, O or F atoms, or an amino group. For example, each R w It may be a substituted or unsubstituted phenoxy, amino or polyoxyalkylene group. wThere may further be a crosslink with another phosphazene group. Exemplary crosslinks include bisphenol groups, such as bisphenol A groups. Examples include phenoxycyclotriphosphazene, octaphenoxycyclotetraphosphazene, decaphenoxycyclopentaphosphazene, and the like. In one aspect, the phosphazene has a structure represented by the following formula:
[0088]
[0089] Commercially available phenoxyphosphazenes having the above structure are LY202 manufactured and sold by Lanyin Chemical Co., Ltd, FP-110 manufactured and sold by Fushimi Pharmaceutical Co., Ltd, and SPB-100 manufactured and sold by Otsuka Chemical Co., Ltd.
[0090] In the flame retardant composition, there is an anti-drip agent, such as a fibril-forming or non-fibril-forming fluoropolymer such as polytetrafluoroethylene (PTFE). The anti-drip agent can be encapsulated by a rigid copolymer as described above, such as a styrene-acrylonitrile copolymer (SAN). PTFE encapsulated in SAN is referred to as TSAN. Encapsulated fluoropolymers can be prepared by polymerizing the encapsulating polymer in the presence of a fluoropolymer, such as an aqueous dispersion. TSAN can provide significant advantages over PTFE because TSAN can be more easily dispersed in the composition. Based on the total weight of the encapsulated fluoropolymer, TSAN can contain 50wt% PTFE and 50wt% SAN. Based on the total weight of the copolymer, SAN can contain, for example, 75wt% styrene and 25wt% acrylonitrile. Alternatively, the fluoropolymer can be pre-blended with a second polymer such as an aromatic polycarbonate or SAN in some manner to form an aggregate material used as an anti-drip agent. Either method can be used to produce encapsulated fluoropolymers. Anti-drip agents are generally used in an amount of 0.05 to 0.5% by weight, based on 100% by weight of the flame retardant composition.
[0091] The flame retardant composition comprises a mineral-filled silicone flame retardant synergist. Minerals that can be used include carbonates, oxides, nitrides or sulfates of various elements, such as aluminum, barium, boron, calcium, magnesium, silicon and titanium. Combinations of these elements can be used. Exemplary mineral fillers include calcium carbonate, barium sulfate, magnesium silicate, calcium silicate, aluminum silicate, calcium aluminum silicate, silicon aluminum silicate, aluminum oxide, silicon dioxide, titanium dioxide (such as rutile and anatase), barium titanate, strontium titanate or a combination thereof. Combinations of different mineral fillers can be used. The mineral filler can be naturally derived, such as dolomite, bentonite, talc, corundum, phyllosilicate (mica), wollastonite or kaolin; or the mineral filler can be processed. For example, the silica can be in the form of a gas phase, a precipitate or an extract. These silicas are generally characterized by a surface area greater than about 50 m2 / gm. Fumed silica can be used, which can have up to 900 m 2 / gm, but preferably has a surface area of 50 to 400m 2 / gm surface area. The mineral filler can be optionally surface treated with a silicon-containing compound such as an organofunctional alkoxysilane coupling agent. Zirconate or titanate coupling agents can be used. Such coupling agents can improve the dispersion of the filler in the polysiloxane.
[0092] The silicone may be a polysiloxane (diorganopolysiloxane), in which the organic group may be C 1-6 Alkyl, C 6-12 The organic group may be optionally substituted with halogen (e.g., 1 to 3 chlorine, bromine, or fluorine atoms). In one aspect, the organic group may be methyl (polydimethylsiloxane). Functional groups such as hydroxyl, C 1-6 Alkoxy, hydride, or vinyl groups may be present in the mineral-filled silicone flame retardant synergist, or in the silicone used to prepare the mineral-filled silicone flame retardant synergist. The silicone may include other types of silicone units, for example, resulting from crosslinking of the silicone during the production of the mineral-filled silicone flame retardant synergist.
[0093] In one aspect, a mineral filled silicone flame retardant synergist is present in an amount of 1-99 wt%, or 1-75 wt%, or 1-50 wt%, or 1-25 wt%, or 1 to 20 wt% in combination with a mineral filler synergist present in an amount of 1-99 wt%, or 25-99 wt%, or 50-99 wt%, or 75-99 wt%, or 80-90 wt%, each based on the total weight of the combination.
[0094] In another aspect, the weight ratio of mineral to silicone in the mineral-filled silicone flame retardant synergist can be 5:95 to 95:5, or 20:80 to 80:20, or 60:40 to 40:60. The mineral-filled silicone flame retardant synergist can contain 1-20wt% silicon, or 2-18wt% silicon, or 3-15wt% silicon, or 5-12wt% silicon, or 6-10wt% silicon, or 7-8wt% silicon. Examples of mineral-filled silicone flame retardant synergists and their methods of making silicone glue are disclosed in WO 2011 / 16136A2. Exemplary mineral-filled silicone flame retardant synergists can be commercially available from Polymer Dynamix, New Jersey, USA under the trade name DynaSilTM. The mineral-filled silicone flame retardant synergist can serve as a cost-effective alternative to antimony-containing synergists. Without wishing to be bound by theory, the mineral filled silicone flame retardant synergist flows to the flame front and forms a thin glassy barrier to form a robust char upon combustion. In some aspects, the mineral filled silicone flame retardant synergist is a silicone composition comprising fumed silica, for example, polydimethylsiloxane.
[0095] The mineral filled silicone flame retardant synergist can be present in the form of, for example, 1-15 wt%, 1-12 wt%, 1-10 wt%, 1-8 wt%, 1-5 wt%, 2-15 wt%, 2-12 wt%, 2-10 wt%, 1-8 wt%, 2-5 wt%, 3-15 wt%, 3-12 wt%, 3-8 wt%, 4-15 wt%, 4-12 wt%, 4-10 wt%, 4-8 wt%, 5-15 wt%, 5-12 wt%, or 5-10 wt%, 1 to less than 7.5 wt%, or 2.5 to less than 7.5 wt%, each based on the total weight of the flame retardant composition.
[0096] The flame retardant composition can further include an additive composition, which includes various additives that are usually incorporated into this type of polymer composition, provided that the additive is selected to not significantly adversely affect the desired properties of the flame retardant composition, especially heat resistance, transparency, and flame retardancy. A combination of additives can be used. The additive composition can include an impact modifier, a flow modifier, a particle filler (e.g., particle polytetrafluoroethylene (PTFE), glass, carbon, minerals, or metals), a reinforcing filler (e.g., glass fibers such as E, A, C, ECR, R, S, D, or NE glass, etc.), an antioxidant, a heat stabilizer, a light stabilizer, an ultraviolet (UV) light stabilizer, a UV absorbing additive, a plasticizer, a lubricant, a release agent (such as a stripping agent), an antistatic agent, an antifogging agent, an antimicrobial agent, a colorant (e.g., a dye or a pigment), a surface effect additive, a radiation stabilizer, a different from C 1-16Flame retardant of alkyl sulfonate flame retardant or mineral filled silicone flame retardant synergist or combination thereof. For example, the total amount of the additive composition can be 0.001 to 10.0 wt%, or 0.01 to 5 wt%, or 0.1 to 5 wt%, each based on the total weight of the flame retardant composition.
[0097] There is considerable overlap among plasticizers, lubricants, and mold release agents, including, for example, phthalates (e.g., octyl-4,5-epoxy-hexahydrophthalate), tris-(octyloxycarbonylethyl)isocyanurate, di- or polyfunctional aromatic phosphates (e.g., resorcinol tetraphenyl diphosphate (RDP), bis(diphenyl)phosphate of hydroquinone, and bis(diphenyl)phosphate of bisphenol A); poly-α-olefins; epoxidized soybean oil; silicones, including silicone oils (e.g., poly(dimethyldiphenylsiloxane)); fatty acid esters (e.g., C 1-32 Alkyl stearyl esters, such as methyl stearate and stearyl stearate, and esters of stearic acid, such as pentaerythritol tetrastearate, glyceryl tristearate (GTS), etc.), waxes (e.g., beeswax, montan wax, paraffin wax, etc.), or a combination comprising at least one of the aforementioned plasticizers, lubricants, and release agents. These flame retardants are generally used in an amount of 0.01-5 wt % based on the total weight of the flame retardant composition totaling 100 wt %.
[0098] Antioxidant additives include organic phosphites such as tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, distearylpentaerythritol diphosphite; alkylated monophenols or polyphenols; alkylation reaction products of polyphenols with dienes, such as tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane; butylation reaction products of p-cresol or dicyclopentadiene; alkylated hydroquinones; hydroxylated thiodiphenyl ethers; alkylidene-bisphenols; benzyl compounds; β-(3,5-di-tert-butyl-4-hydroxy Esters of β-(5-tert-butyl-4-hydroxy-3-methylphenyl)-propionic acid and monohydric alcohols or polyhydric alcohols; Esters of thioalkyl or thioaryl compounds, such as distearyl thiopropionate, dilauryl thiopropionate, ditridecyl thiodipropionate, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; amides of β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid, or a combination comprising at least one of the foregoing antioxidants. The antioxidant is used in an amount of 0.01-0.2, or 0.01-0.1 parts by weight, based on the total weight of the flame retardant composition totaling 100 wt%.
[0099] The flame retardant composition is substantially free of chlorine and bromine. "Substantially free of chlorine and bromine" refers to materials produced without intentional addition of chlorine or bromine or chlorine or bromine-containing materials. However, it should be understood that in facilities for processing a variety of products, a certain amount of cross contamination may occur, resulting in a level of bromine or chlorine that is generally a few parts per million by weight. Under this understanding, it can be easily understood that "substantially free of bromine and chlorine" can be defined as having a bromine or chlorine content of less than or equal to 100 parts per million (ppm) by weight, less than or equal to 75ppm, or less than or equal to 50ppm. In some aspects, "substantially free of bromine and chlorine" refers to a total bromine and chlorine content of less than or equal to 100 parts per million by weight, or less than or equal to 75ppm, or less than or equal to 50ppm. When this definition is applied to flame retardants, it is based on the gross weight of flame retardants. When this definition is applied to flame retardant compositions, it is based on the gross weight of flame retardants.
[0100] The amounts of the various components of the flame retardant composition may vary depending on the characteristics of each component and the desired performance. The flame retardant composition may include 34-94 wt% or 65-75 wt% of a homopolycarbonate, copolycarbonate, or a combination thereof, preferably bisphenol A homopolycarbonate; 5-85 wt% or 15-50 wt% of poly(carbonate-siloxane) in an amount effective to provide 2-6 wt% of dimethylsiloxane; 0.05-0.6 wt%, preferably 0.1-0.4 wt% of C 1-16 alkyl sulfonate flame retardant; 1-15wt% or 1-10wt% of mineral-filled silicone flame retardant synergist; 0.01-0.5wt% or 0.5 to 5wt% of anti-drip agent; and optionally, 0.001-10wt% or 1 to 5wt% of additive composition, wherein each amount is based on the total weight of the flame retardant composition totaling 100wt%. In another aspect, the flame retardant composition can include 65-75wt% of bisphenol homopolycarbonate having a weight average molecular weight from 25,000 to 35,000 g / mole, preferably 27,000 to 32,000 g / mole; 15-25wt% of the poly (carbonate-siloxane); 0.2-0.6wt%, preferably 0.1-0.4wt% of potassium perfluorobutane sulfonate as C 1-16alkyl sulfonate flame retardant; 1-10 wt% of the mineral filled poly(dimethylsiloxane) flame retardant synergist; 0.05-0.5 wt% of an anti-drip agent; optionally, up to 5 wt% of an additive composition, or up to 20 wt% of a glass fiber composition, or a combination thereof, wherein each amount is based on the total weight of the flame retardant composition totaling 100 wt%. In any of these aspects, the amount of mineral filled silicone flame retardant synergist can be 1-12 wt%, 1-10 wt%, 1-8 wt%, 1-5 wt%, 2-15 wt%, 2-12 wt%, 2-10 wt%, 1-8 wt%, 2-5 wt%, 3-15 wt%, 3-12 wt%, 3-8 wt%, 4-15 wt%, 4-12 wt%, 4-10 wt%, 4-8 wt%, 5-15 wt%, 5-12 wt% or 5-10 wt%.
[0101] Flame retardant compositions can be manufactured by various methods. For example, in a HENSCHEL-Mixer high-speed mixer, powdered polycarbonate, flame retardant or other optional components are optionally first blended with any filler. Other low shear methods, such as manual mixing, can also accomplish this blending. The blend is then fed to the throat of a twin-screw extruder through a hopper. Alternatively, at least one component, such as reinforcing filler or glass fiber, can be incorporated into the composition by directly feeding the extruder through a side filler at the throat or downstream. Additives such as mineral-enhanced silicon synergists can also be mixed into a masterbatch with the desired polymer and fed to the extruder. The extruder is usually operated at a temperature higher than that necessary to cause the composition to flow. The extrudate is immediately quenched and granulated in a water bath. As required, the pellets prepared in this way can be a quarter inch long or shorter. Such pellets can be used for subsequent molding, shaping, or forming.
[0102] The molded sample of the flame retardant composition may have a Vicat softening temperature of at least 140° C. measured according to ISO-306 standard on a 4 mm thick ISO bar at a load of 10 N and a heating rate of 50° C. / hour (B50).
[0103] The molded sample of the flame retardant composition may have a flame retardant strength of greater than or equal to 35 kJ / m 2 according to ISO-180:2000 standard using a 5.5 J hammer at -30°C on a notched 4 mm thick ISO bar. 2 Notched Izod beam impact.
[0104] The molded sample of the flame retardant composition has a flame retardancy test rating of V0, measured at a thickness of 1.0 mm, preferably 0.8 mm, according to UL-94.
[0105] The flame retardant composition can be used in articles including molded articles, thermoformed articles, extruded films, extruded sheets, one or more layers of multilayer articles, substrates for coated articles, or substrates for metallized articles. Optionally, the article has no significant part deformation or discoloration when the article is subjected to secondary operations such as overmolding, lead-free soldering, wave soldering, low-temperature soldering, or coating or a combination thereof. The article can be partially or completely coated with, for example, a hard coating, a UV protective coating, an anti-refractive coating, an anti-reflective coating, a scratch-resistant coating or a combination thereof, or metallized.
[0106] Also provided are shaped, formed, or molded articles comprising the flame retardant composition. The flame retardant composition can be molded into useful shaped articles by various methods, such as injection molding, extrusion, rotational molding, blow molding, and thermoforming. Some examples of articles include computer and business machine housings such as housings for monitors, handheld electronic device housings such as housings for mobile phones, electrical connectors, and components of lighting equipment, decorative objects, household appliances, roofs, greenhouses, sunrooms, swimming pool fences, etc.
[0107] The present disclosure is further illustrated by the following examples, which are non-limiting.
[0108] Example
[0109] The materials in Table 1 were used.
[0110] Table 1
[0111]
[0112]
[0113] The samples were prepared as described below and the following test methods were used.
[0114] All powder additives were mixed together with polycarbonate powder using a paint shaker and fed to the extruder through a feeder. Extrusion of all combinations was performed on a 25 mm twin screw extruder according to the extrusion profiles in Table 2.
[0115] Table 2
[0116] parameter unit Standard value Feed ℃ 40 Zone 1 Temperature ℃ 200 Zone 2 Temperature ℃ 250 Zone 3 Temperature ℃ 270 Zone 4-9 Temperature ℃ 310 Screw speed rpm 300 Production kg / h Approx. 14 Torque % Maximum
[0117] Molding of the samples for testing was performed on an Engel 45 ton injection molding machine equipped with an insert mold from AXXICON. The temperature profiles and general molding parameters for standard and abusive conditions are reported in Table 3.
[0118] Table 3
[0119]
[0120]
[0121] The melt volume rate (MVR) was determined according to ASTM D1238-04 at 300°C using a 1.2 kg weight in 300 seconds.
[0122] ISO notched Izod impact measurements (INI) were performed according to ISO-180:2000 standard using a 5.5 J hammer at -30°C on notched 4 mm thick ISO bars.
[0123] The Vicat softening temperature (Vicat) was measured on 4 mm thick ISO bars at a load of 10 N and a heating rate of 50° C. / hour (B50) according to ISO-306 standard.
[0124] Flammability was determined by using the UL-94 standard (Table 4). Vx vertical flammability tests were performed at 1.0 mm and 0.8 mm. A V rating was obtained for each set of 5 bars. In some cases, a second set of 5 bars was tested to give an indication of the robustness of the rating.
[0125] Table 4
[0126] <![CDATA[t1 and / or t2]]> 5-stick FOT* Burning dripping V0 <10 <50 no V1 <30 <250 no V2 <30 <250 yes NR (No Grade) >30 >250
[0127] *FOT: Total extinguishing time of all 5 rods (FOT = t1 + t2)
[0128] Examples 1-13
[0129] The formulations and properties of Examples 1-13 are shown in Table 5.
[0130] Table 5
[0131]
[0132]
[0133] *Comparative Example
[0134] Comparative Example 1 shows that the absence of Si-FR and PC-Si results in a V0 UL94 rating and poor low temperature impact resistance at 1.0 mm and 0.8 mm thickness. Adding Si-FR to a flame retardant composition in which PC-Si is not present and the Rimar loading is 0.4 wt% fails to improve low temperature impact resistance and adversely affects the flame test rating in terms of improved impact resistance (compare Comparative Example 2 with Comparative Example 1). Reducing the Rimar loading from 0.4 wt% to 0.1 wt% results in poor flame test ratings and poor low temperature impact resistance at 1.0 mm and 0.8 mm thickness (compare Comparative Example 3 with Comparative Example 2). Comparative Example 4 shows the incorporation of an impact modifier (i.e., MBS) in the composition in which the absence of Si-FR and PC-Si results in an improvement in low temperature impact resistance, but a degradation of the flame test rating (compare Comparative Example 4 with Comparative Example 3). The combination of Si-FR and MBS fails to improve low temperature impact resistance (compare Comparative Example 5 with Comparative Example 4). As shown in Example 7, in a composition with 0.4 wt% Rimar salt loading, the combination of PC-Si and Si-FR resulted in a flame retardant test rating of V0 at both 1.0 mm and 0.8 mm thickness, as well as improved low temperature impact resistance (INI, -30C>60 kJ / m 2). Replacing Rimar salt with KSS resulted in an adverse effect on flame test ratings at 1.0 mm and 0.8 mm thicknesses (compare Comparative Example 8 with Example 7). A composition having a combination of PC-Si and Si-FR and excluding Rimar salt and KSS flame retardant resulted in V0 at 1.0 mm thickness and V2 at 0.8 mm thickness (see Comparative Example 9). Comparative Example 10 shows that at a lower Rimar salt loading (i.e., 0.1 wt%), the composition having PC-Si but not Si-FR failed to provide improved flame test ratings at 1.0 mm and 0.8 mm thicknesses (compare Comparative Example 10 with Comparative Example 6). However, even at a lower Rimar salt loading of 0.1 wt%, the combination of PC-Si and Si-FR resulted in a combination of a V0 flame retardant test rating at 1.0 mm and 0.8 mm thicknesses and good low temperature impact resistance (Example 11). Example 12 shows that when the loading of Si-FR is increased from 2.5wt% to 5wt%, the desired combination of V0 flame retardant test rating and good low temperature impact resistance at 1.0mm and 0.8mm thickness is obtained. Comparative Example 13 shows that in a composition having a combination of PC-Si (22wt%) and Si-FR, in which Rimar salt is present at a loading of 0.1wt%, increasing the Si-FR loading from 5wt% to 7.5wt% results in a loss of V0 flame retardant test rating at both 1.0mm and 0.8 thickness. In summary, the combination of PC-Si, Si-FR and Rimar results in a V0 flame retardant test rating and good low temperature impact resistance (i.e., greater than 35kJ / m at -30°C) at both 1.0mm and 0.8mm thickness. 2 ) is the expected combination.
[0135] The following aspects illustrate possible implementations.
[0136] Aspect 1 A flame retardant composition comprising: 34-94 wt% of a homopolycarbonate, a copolycarbonate, or a combination thereof; 5-85 wt% of a poly(carbonate-siloxane) in an amount effective to provide 2-6 wt% of dimethylsiloxane; 0.05-0.6 wt%, preferably 0.1-0.4 wt% of C 1-16an alkyl sulfonate flame retardant; 1-15 wt% of a mineral-filled silicone flame retardant synergist; 0.05-0.5 wt% of an anti-drip agent; optionally, 0.001-10 wt% of an additive composition, or 0.1-20 wt% of a glass fiber composition, or a combination thereof, wherein each amount is based on the total weight of the flame retardant composition totaling 100 wt%; and wherein a molded sample of the flame retardant composition has a Vicat softening temperature greater than or equal to 140°C measured at a load of 10 N and a heating rate of 50°C / hour according to ISO-306 standard, and a flame test rating of V0 measured at a thickness of 1.0 mm or at a thickness of 0.8 mm according to UL-94.
[0137] Aspect 2 The flame retardant composition according to claim 1, wherein a molded sample of the flame retardant composition has a flame retardant strength greater than or equal to 35 kJ / m measured at -30°C using a 5.5 joule hammer on a 4 mm specimen according to ISO-180:2000 standard. 2 a notched Izod impact strength of greater than or equal to 5 cubic centimeters per 10 minutes at 300°C using a 1.2 kg weight in accordance with ASTM D1238-04; or a combination thereof.
[0138] Aspect 3: The flame retardant composition according to any one of the preceding claims, wherein the homopolycarbonate or the copolycarbonate comprises bisphenol A repeating units.
[0139] Aspect 4 A flame retardant composition according to any of the preceding claims, wherein a homopolycarbonate is present and comprises bisphenol A homopolycarbonate having a weight average molecular weight of 20,000 to 30,000 g / mole, preferably 20,000 to 25,000 g / mole; bisphenol A homopolycarbonate having a weight average molecular weight of 25,000 to 35,000 g / mole, preferably 27,000 to 32,000 g / mole; or a combination thereof, each as measured by gel permeation chromatography using bisphenol A homopolycarbonate standards.
[0140] Aspect 5. A flame retardant composition according to any of the preceding claims, wherein the poly(carbonate-siloxane) comprises 5 to 99 weight percent of bisphenol A carbonate units and 1 to 50 weight percent of dimethylsiloxane units, each based on the weight of the polydimethylsiloxane.
[0141] Aspect 6: The flame retardant composition according to any one of the preceding claims, wherein the silicone containing the mineral silicone flame retardant synergist is a polydiorganosiloxane, preferably a polydimethylsiloxane.
[0142] Aspect 7: The flame retardant composition according to any one of the preceding claims, wherein the C1-16 The alkyl sulfonate flame retardant includes potassium perfluorobutane sulfonate, potassium perfluorooctane sulfonate, tetraethylammonium perfluorohexane sulfonate or a combination thereof, preferably potassium perfluorobutane sulfonate.
[0143] Aspect 8a A flame retardant composition according to any of the preceding claims, wherein the mineral-filled silicone flame retardant synergist is a silicone flame retardant additive present in an amount of 1-99wt%, or 1-75wt%, or 1-50wt%, or 1-25wt%, or 1wt% to 20wt% in combination with a mineral filler synergist present in an amount of 1-99wt%, or 25-99wt%, or 50-99wt%, or 75-99wt%, or 80-90wt%, each based on the total weight of the combination.
[0144] Aspect 8b. A flame retardant composition according to any of the preceding claims, wherein the mineral-filled silicone flame retardant synergist contains 1-20 wt% silicon, or 2-18 wt% silicon, or 3-15 wt% silicon, or 5-12 wt% silicon, or 6-10 wt% silicon, or 7-8 wt% silicon.
[0145] Aspect 9: The flame retardant composition according to any one of the preceding claims, wherein the anti-drip agent comprises a fluoropolymer, preferably a polymer-encapsulated fluoropolymer, more preferably a polytetrafluoroethylene-encapsulated styrene-acrylonitrile copolymer, or a combination thereof.
[0146] Aspect 10 The flame retardant composition according to any one or more of the preceding claims, comprising 65-75 wt% of a bisphenol homopolycarbonate having a weight average molecular weight of 25,000 to 35,000 g / mol, preferably 27,000 to 32,000 g / mol; 15-70 wt% of the poly(carbonate-siloxane); 0.2-0.6 wt%, preferably 0.2-0.4 wt% of potassium perfluorobutanesulfonate as C 1-16 an alkyl sulfonate flame retardant; 1-10 wt % of the mineral-filled poly(dimethylsiloxane) flame retardant synergist; 0.01-0.5 wt % of an anti-drip agent; optionally, 0.01 to 5 wt % of an additive composition, or 0.1 to 10 wt % of a glass fiber composition, or a combination thereof, wherein each amount is based on the total weight of the flame retardant composition totaling 100 wt %.
[0147] Aspect 11: A flame retardant composition according to any one of the preceding claims, wherein additives are present, the additives comprising particulate fillers, reinforcing agents (such as glass fibers), antioxidants, heat stabilizers, light stabilizers, ultraviolet light stabilizers, plasticizers, lubricants, mold release agents, antistatic agents, surface effect additives, radiation stabilizers, other than C 1-16A flame retardant of an alkyl sulfonate flame retardant and a mineral filled poly(dimethylsiloxane) flame retardant synergist or a combination thereof.
[0148] Aspect 12 An article according to any of the preceding claims, wherein the article is an extruded article, a molded article, a pultruded article, a thermoformed article, a foamed article, a layer of a multilayer article, a substrate for a coated article, or a substrate for a metallized article, preferably wherein the article is a molded article.
[0149] Aspect 13. The article of claim 12, wherein the article is a molded housing.
[0150] Aspect 14: The article of claim 12 or 13, wherein the article is a circuit housing.
[0151] Aspect 15 A method for forming an article according to any one or more of the preceding claims, comprising molding, casting or extruding the article.
[0152] Alternatively, the compositions, methods and articles may comprise, consist of or consist essentially of any suitable material, step or component disclosed herein. The compositions, methods and articles may additionally or alternatively be formulated so as to be free of or essentially free of any material (or species), step, or component that is otherwise not necessary to achieve the function or purpose of the compositions, methods, and articles.
[0153] All ranges disclosed herein include endpoints, and the endpoints can be combined independently of each other (e.g., the range of "up to 25wt%, or more specifically, 5wt% to 20wt%" includes the endpoints and all intermediate values of the range of "5wt% to 25wt%", etc.). "Combination" includes blends, mixtures, alloys, reaction products, etc. Unless otherwise indicated herein or clearly contradicted by the context, the terms "one" and "a" and "the" do not represent a limitation of quantity, but are interpreted to cover the singular and plural. Unless otherwise expressly stated, "or" means "and / or". Throughout the specification, reference to "some aspects", "one aspect", etc. means that the specific elements described in conjunction with the aspect are included in at least one aspect described herein, and may or may not be present in other aspects. In addition, it should be understood that the described elements can be combined in any suitable manner in various aspects. "Their combination" is open and includes any combination that includes at least one of the listed components or properties, optionally together with unlisted similar or equivalent components or properties.
[0154] Unless otherwise specified herein, all test standards are the most current standards in effect as of the filing date of this application or, if priority is claimed, as of the filing date of the earliest priority application in which the test standards appear.
[0155] Unless otherwise defined, technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this application belongs. All cited patents, patent applications and other references are incorporated herein by reference in their entirety. However, if a term in this application contradicts or conflicts with a term in an incorporated reference, the term in this application takes precedence over the conflicting term in the incorporated reference.
[0156] Compounds are described using standard nomenclature. For example, any position not substituted by any specified group is understood to have its valency filled by a specified bond or hydrogen atom. A dash ("-") that is not between two letters or symbols is used to indicate the point of attachment of a substituent. For example, -CHO is attached through the carbon of the carbonyl group.
[0157] The term "alkyl" refers to a branched or straight chain unsaturated aliphatic hydrocarbon group, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, sec-pentyl, and n-hexyl and sec-hexyl. "Alkenyl" refers to a straight or branched monovalent hydrocarbon group having at least one carbon-carbon double bond (e.g., vinyl (-HC=CH2)). "Alkoxy" refers to an alkyl group connected by oxygen (i.e., alkyl-O-), such as methoxy, ethoxy and sec-butoxy. "Alkylene" refers to a straight or branched saturated divalent aliphatic hydrocarbon group (e.g., methylene (-CH2-) or propylene (-(CH2)3-)). "Cycloalkylene" refers to a divalent cyclic alkylene group, -C n H 2n-x , where x is the number of hydrogens substituted by cyclization. "Cycloalkenyl" refers to a monovalent group having one or more rings and one or more carbon-carbon double bonds in the ring, wherein all ring members are carbon (e.g., cyclopentyl and cyclohexyl). "Aryl" refers to an aromatic hydrocarbon group containing a specific number of carbon atoms, such as phenyl, trocon, indanyl or naphthyl. "Arylene" refers to a divalent aryl group. "Alkylidenearylene" refers to an arylene substituted by an alkyl group. "Arylalkylene" refers to an alkylene substituted by an aryl group (e.g., benzyl). The prefix "halogen" refers to a group or compound comprising one or more fluorine, chlorine, bromine or iodine substituents. There may be a combination of different halogen groups (e.g., bromine and fluorine), or there may be only chlorine groups. The prefix "hetero" refers to a compound or group including at least one ring member that is a heteroatom (e.g., 1, 2 or 3 heteroatoms), wherein the heteroatoms are each independently N, O, S, Si or P. "Substituted" means that the compound or group is substituted with at least one (e.g., 1, 2, 3 or 4) substituents, each of which may be independently C 1-9 Alkoxy, C 1-9 Haloalkoxy, nitro (-NO2), cyano (-CN), C 1-6 Alkylsulfonyl (-S(=O)2-alkyl), C 6-12Arylsulfonyl (-S(=O)2-aryl)thiol (-SH), thiocyanato (-SCN), tosyl (CH3C6H4SO2-), C 3-12 Cycloalkyl, C 2-12 Alkenyl, C 5-12 Cycloalkenyl, C 6-12 Aryl, C 7-13 Arylalkylene, C 4-12 Heterocycloalkyl and C 3-12 A heteroaryl group replaces a hydrogen provided that the normal valence of the substituted atom is not exceeded. The number of carbon atoms specified in the group does not include any substituents. For example, -CH2CH2CN is a C2 alkyl group substituted with a nitrile.
[0158] While particular aspects have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are presently unforeseen or possibly unforeseeable may occur to the applicant or others skilled in the art. Accordingly, the appended claims as filed and as they may be amended are intended to cover all such alternatives, modifications, variations, improvements, and substantial equivalents.
Claims
1. A flame retardant composition comprising: 65-94wt% bisphenol homopolycarbonate; 5-35 wt % poly(carbonate-siloxane) in an amount effective to provide 2-6 wt % dimethylsiloxane; 0.05-0.6wt% C 1-16 Alkyl sulfonate flame retardants; 1 wt % to less than 7.5 wt % of a mineral-filled silicone flame retardant synergist comprising fumed silica; 0.05-0.5wt% of an anti-drip agent; Optionally, 0.001-10 wt% of the additive composition, or 0.1-20 wt% of the glass fiber composition, or a combination thereof wherein each amount is based on the total weight of the flame retardant composition totaling 100 wt%; and The molded sample of the flame retardant composition has a Vicat softening temperature greater than or equal to 140°C, measured according to ISO-306 at a load of 10 N and a heating rate of 50°C / hour, and Flame test rating of V0 measured in accordance with UL-94 at a thickness of 1.0 mm or at a thickness of 0.8 mm.
2. The flame retardant composition according to claim 1, wherein The molded samples of the flame retardant composition have Notched Izod impact resistance of 35 kJ / m2 or greater measured at -30°C using a 5.5 joule hammer on a 4 mm specimen according to ISO-180:2000; or A melt volume rate greater than or equal to 5 cubic centimeters per 10 minutes at 300°C using a 1.2 kg weight in accordance with ASTM D1238-04; or a combination thereof.
3. The flame retardant composition of claim 1, comprising 2.0 wt% to less than 7.5 wt% of a mineral-filled polydimethylsiloxane flame retardant synergist comprising fumed silica.
4. The flame retardant composition according to claim 1, wherein The homopolycarbonate is present, and the homopolycarbonate comprises Bisphenol A homopolycarbonate having a weight average molecular weight of 20,000 to 30,000 g / mol; or Bisphenol A homopolycarbonate having a weight average molecular weight of 25,000 to 35,000 g / mol; or a combination thereof, each measured by gel permeation chromatography using a bisphenol A homopolycarbonate standard.
5. The flame retardant composition according to claim 1, wherein The poly(carbonate-siloxane) comprises 5 to 99 weight percent bisphenol A carbonate units and 1 to 50 weight percent dimethylsiloxane units, each based on the weight of the polydimethylsiloxane.
6. The flame retardant composition according to claim 1, wherein The silicone containing mineral silicone flame retardant synergist is a polydiorganosiloxane.
7. The flame retardant composition according to claim 1, comprising 4.0 wt% to less than 7.5 wt% of a mineral-filled polydimethylsiloxane flame retardant synergist comprising fumed silica, wherein: The C 1-16 The alkyl sulfonate flame retardant comprises potassium perfluorobutane sulfonate, potassium perfluorooctane sulfonate, tetraethylammonium perfluorohexane sulfonate or a combination thereof.
8. The flame retardant composition according to claim 1, wherein The C 1-16 Alkyl sulfonate flame retardants include potassium perfluorobutane sulfonate.
9. The flame retardant composition according to claim 1, wherein The mineral-filled silicone flame retardant synergist comprises 1-20 wt % silicon; or wherein the mineral filled silicone flame retardant synergist is a combination of a silicone flame retardant additive present in an amount of 1-99 wt % and a mineral filler synergist present in an amount of 1-99 wt %, each based on the total weight of the combination.
10. The flame retardant composition according to claim 1, wherein The mineral-filled silicone flame retardant synergist comprises 2-18 wt % silicon; or wherein the mineral filled silicone flame retardant synergist is a combination of a silicone flame retardant additive present in an amount of 1-75 wt % and a mineral filler synergist present in an amount of 25-99 wt %, each based on the total weight of the combination.
11. The flame retardant composition according to claim 1, wherein The mineral-filled silicone flame retardant synergist comprises 3-15 wt % silicon; or wherein the mineral filled silicone flame retardant synergist is a combination of a silicone flame retardant additive present in an amount of 1-50 wt % and a mineral filler synergist present in an amount of 50-99 wt %, each based on the total weight of the combination.
12. The flame retardant composition according to claim 1, wherein The mineral-filled silicone flame retardant synergist comprises 5-12 wt % silicon; or wherein the mineral filled silicone flame retardant synergist is a combination of a silicone flame retardant additive present in an amount of 1-25 wt % and a mineral filler synergist present in an amount of 75-99 wt %, each based on the total weight of the combination.
13. The flame retardant composition according to claim 1, wherein The mineral-filled silicone flame retardant synergist comprises 6-10 wt % silicon; or wherein the mineral filled silicone flame retardant synergist is a combination of a silicone flame retardant additive present in an amount of 1-20 wt % and a mineral filler synergist present in an amount of 80-90 wt %, each based on the total weight of the combination.
14. The flame retardant composition according to claim 1, wherein The mineral filled silicone flame retardant synergist contains 7-8 wt % silicon.
15. The flame retardant composition according to claim 1, wherein The anti-drip agent comprises a fluoropolymer.
16. The flame retardant composition according to claim 1, comprising: 65-75 wt% of a bisphenol homopolycarbonate having a weight average molecular weight of 25,000 to 35,000 g / mole; 5-35 wt% of the poly(carbonate-siloxane); 0.05-0.6wt% as the C 1-16 Potassium perfluorobutane sulfonate of alkyl sulfonate flame retardant; 4.0 wt % to less than 7.5 wt % of a mineral-filled polydimethylsiloxane flame retardant synergist comprising fumed silica; 0.01-0.5wt% of an anti-drip agent; Optionally, 0.01-5 wt % of an additive composition, or 1-20 wt % of a glass fiber composition, or a combination thereof; Each amount is based on the total weight of the flame retardant composition which totals 100 wt%.
17. The flame retardant composition according to claim 1, wherein The additives are present, and the additives include fillers, reinforcing agents, antioxidants, heat stabilizers, light stabilizers, ultraviolet light stabilizers, plasticizers, lubricants, mold release agents, antistatic agents, surface effect additives, radiation stabilizers, different from the C 1-16 The flame retardant comprises an alkyl sulfonate flame retardant and the mineral-filled silicone flame retardant synergist comprising fumed silica or a combination thereof.
18. An article comprising the flame retardant composition according to any one of claims 1 to 17, wherein: The article is an extruded article, a molded article, a pultruded article, a thermoformed article, a foamed article, a layer of a multilayer article, a substrate for a coated article or a substrate for a metallized article.
19. The article of claim 18, wherein: The article is a molded housing.
20. The article according to claim 18 or 19, wherein The article is a circuit housing.