Protection method, protective composite mixture and coating for cathode blocks of aluminum electrolysis cells with baked anodes

By using a composite coating of titanium diboride powder and binder on the cathode block of the aluminum electrolytic cell, combined with graphite powder anti-oxidation treatment, the problem of insufficient mechanical strength and wear resistance of the coating at high temperatures is solved, and the electrolysis time is prolonged. groove service life and optimized bottom wear protection.

CN114450437BActive Publication Date: 2024-10-01OBSHCHESTVO S OGRANICHENNOY OTVETSTVENNOSTYU OBEDINENNAYA KOMPANIYA RUSAL INZHENERNO TEKHNOLOGICHESKIY TSENTR
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080067702.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-24
Filing Date
2020-08-25
Publication Date
2024-10-01
Estimated Expiration
2040-08-25

AI Technical Summary

Technical Problem

When the existing technology protects the cathode block of an aluminum electrolytic cell, the coating lacks high-temperature mechanical strength and wear resistance, and fails to effectively reduce bottom wear, affecting the service life of the electrolytic cell.

Method used

Using a composite mixture containing titanium diboride powder and adhesive, the TiB2-C protective composite coating is formed by spraying or roller coating, combined with graphite powder anti-oxidation treatment to ensure that the coating maintains adhesion and resistance at high temperatures. Abrasive and localized protection for bottom wear areas.

Benefits of technology

The high-temperature mechanical strength and wear resistance of the cathode block are significantly improved, extending the service life of the electrolytic cell. By controlling the binder content and particle size distribution, the shrinkage and cracking of the coating are reduced, and the overall performance is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention proposes a method for protecting the cathode block of an aluminum electrolytic cell with a baked anode, comprising preparing a mixture of a heat-resistant material and a binder, applying the mixture as a coating on the surface of the cathode block according to the wear of the bottom, and drying the coating. At the same time, titanium diboride powder or a bimodal or multimodal mixture of titanium diboride powder is used as a heat-resistant material, and the characteristics of its particle size composition conform to the bimodal or multimodal particle size distribution, which helps to improve the process performance during the preparation of the suspension, and improve the physical and mechanical properties of the protective coating, that is, reduce shrinkage and eliminate cracking. A sulfonated product of the reaction of naphthalene and formaldehyde is used as a binder, and the binder has a coke residue of at least 30wt.%, and after drying, a layer of graphite powder is applied to the surface of the coating to prevent it from being oxidized during the startup process, and the startup process is accompanied by the formation of a TiB2-C protective composite coating wetted by aluminum when the bottom is heated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of nonferrous metallurgy, namely, the electrolytic deposition of aluminum, and can be used to protect cathode blocks of aluminum electrolytic cells with baked anodes (BA) to reduce the wear of the cathode blocks and extend their service life. Background Art

[0002] The modern aluminum industry needs to increase the power of the electrolytic cell, which requires the bottom block to have stronger corrosion resistance to the electrolyte, high thermal conductivity and electrical conductivity. In order to meet the above requirements, electrode manufacturers are turning to the production of graphitized products and graphite bottom blocks, the use of which can increase the service life of the electrolytic cell. However, in the electrolyte used by traditional industry, aluminum does not wet the bottom material, which causes a layer of molten metal to form on the surface of the cathode material. This significantly increases the distance between the two electrodes and the current consumption. In addition, the degree of wetting depends on the impregnation intensity of the electrolyte that penetrates under the metal layer and impregnates the bottom during startup. The penetration of electrolyte and metallic aluminum into the cracks and macropores of the positive electrode block is one of the reasons for the low strength and low wear resistance of the surface layer of the positive electrode block. This problem is mainly related to graphite blocks, which have poor mechanical wear resistance compared to the carbon graphite blocks used in the early days. Wetted aluminum cathodes have significant advantages in overcoming these shortcomings.

[0003] A method for protecting cathode blocks by coating a heat-resistant coating made of a heat-resistant material is known (patent US20010046605). The method comprises preparing an aqueous suspension of powdered titanium diboride dispersed in an oxalate complex, applying the suspension coating on the surface and drying to form a hard, heat-resistant surface. The coating is applied to the cathode of a high-temperature cryolite bath. During the electrolysis process, the oxalate complex in the coating is destroyed to form aluminum oxide and 20-30% hydrated Al 2 O 3 Meanwhile, aluminum oxalate complex is a complex of oxalic acid and powder, containing aluminum oxide (70-80% anhydrous Al 2 O 3 ). The oxalate complex is prepared 4 hours before mixing with powdered titanium diboride. The suspension contains 30-90 wt.% titanium diboride (5-30 μm particles), a powdered heat-resistant material dispersed in the aluminum oxalate complex. The thickness of the coating is between 1-15 mm.

[0004] The closest in terms of technical essence and the results achieved is the method for forming a protective coating on carbonaceous parts of electrolytic cells in the production of aluminum (patents RU 2257425, C25C3 / 08, C25C7 / 02, B05D1 / 00, B05D7 / 24 or patent US 6475358). This method for treating the carbonaceous elements of the electrolytic cell (cathode) provides for the preparation of a liquid suspension of a refractory material, for example, for the cathode, preferably titanium diboride (TiB2) dispersed in a mixture of a lignin sulfonate binder (50% solution) and a phenolic resin. 2 ), and the suspension is applied as a coating on the surface of the carbonaceous component. The content of the components in the suspension can vary within the following ranges, wt. %:

[0005] - 20-70 wt.% titanium diboride;

[0006] - 5-40 wt.% phenolic polymer (binder);

[0007] - 5-40 wt. % lignin sulfonate solution (50%).

[0008] Some compounds may also contain up to 5 wt.% anthracite.

[0009] The authors of the present invention have obtained a suspension in the form of a viscous dispersed system which has sufficient fluidity to apply a coating with a thickness of 1-3 mm on the cathode block, preferably by spraying with a sprayer. The resulting suspension can also be applied to the surface in multiple layers continuously with a brush or a roller. The coating is dried in the open air at room temperature for 10 hours. Then, a layer of coke (10 cm) is covered on the surface of the coating, and the cathode is then preheated according to the conventional start-up mode. Electrolysis tests carried out at 900° C. for 100 hours show that the entire surface of the treated cathode sample is wetted by aluminum and shows no signs of corrosion.

[0010] The disadvantages of this paradigm are:

[0011] - When a mixture of lignin sulfonate binder and phenolic resin is used, the amount of coke remaining is low and the protective coating formed has neither high temperature mechanical strength nor wear resistance;

[0012] - The coating is applied to the entire surface of the bottom without considering the wear condition of the bottom, which also reduces the economic benefits;

[0013] - No procedures are provided to adjust for shrinkage and cracking of protective coatings. Summary of the invention

[0014] The object of the present invention is to develop a method for protecting cathode blocks of aluminum electrolysis cells with baked anodes, as well as a composite mixture and a coating which can reduce wear and extend the service life of cathode blocks of aluminum electrolysis cells with baked anodes.

[0015] The technical result is the solution of the problem and the extension of the service life of the electrolyzer.

[0016] The problem has been solved and the technical result achieved is due to the fact that the cathode blocks of aluminum electrolysis cells with baked anodes are to be protected to extend their service life. According to the proposed invention, the novelty of the preparation method includes a composite mixture of a refractory material and a binder, the mixture is applied to the surface of the cathode block and the resulting coating is dried, including the binder is used in the form of a sulfonated product of the reaction of naphthalene and formaldehyde, the binder has a coke residue of at least 30% by weight, the refractory material is used in the form of titanium diboride powder or a bimodal or multimodal mixture of titanium diboride powders, the particle size composition of which is characterized by a bimodal or multimodal particle size distribution, and after drying, a layer of graphite powder is applied to the surface of the coating to prevent the coating from being oxidized during the startup process, which is accompanied by the formation of aluminum-wet TiB during heating. 2 -C Protective composite coating.

[0017] Other significant features of the present invention contribute to achieving the technical effect. Therefore, a mixture with a binder content of 35-50wt.% and a titanium diboride content of 65-50wt.% is prepared and applied in layers on the surface of the cathode block by roller leveling or spraying after pouring. Taking into account the wear condition of the bottom, the mixture is applied at least to the area of ​​the bottom with the greatest wear, and the mixture is locally applied along the side of the electrolytic cell in the form of a strip 500-1,200mm wide to obtain a protective coating with a thickness of 0.8-1mm. After applying the mixture to the cathode block of the electrolytic cell, the coating is dried for at least 8 hours at room temperature at the production site. Graphite powder is applied to the surface of the coating with a thickness of 15-30mm. The bottom is heated to 950°C for 48-72 hours to form TiB 2 -C Protective composite coating. TiB 2 -C protective composite coating contains 15-40wt.% carbon. The mixture is continuously mixed until smooth to prevent TiB 2 Sedimentation of particles and separation of mixtures.

[0018] The relevant composite mixture for protecting the cathode block of the aluminum electrolysis cell with baked anodes contains 65-50 wt.% of binder and 65-50 wt.% of titanium diboride. After drying, a layer of graphite powder is applied on the surface of the coating to protect it from oxidation during the startup process, which is accompanied by the formation of aluminum-wet TiB during heating. 2 -C Protective composite coating.

[0019] The invention also discloses a composite mixture for obtaining TiB of a cathode block of an aluminum electrolysis cell having a baked anode. 2 -C protective composite coating, in which TiB 2 The content of titanium diboride is 65-50wt.%, which is used in the form of titanium diboride powder or a bimodal or multimodal mixture of titanium diboride powder, and the characteristics of its particle size composition conform to the bimodal or multimodal particle size distribution, and the amount of binder is 35-50wt.%, the binder is used in the form of a sulfonated product of the reaction of naphthalene and formaldehyde, and the binder has at least 30wt.% coke residue.

[0020] TiB of the cathode block of the aluminum electrolysis cell with baked anode obtained by the above method 2 -C protective composite coatings have also been claimed. The coating should preferably contain 15-40 wt.% carbon.

[0021] Mode for carrying out the invention

[0022] The method involves initially determining the maximum wear area of ​​the bottom by known methods (by mapping the bottom wear condition) and obtaining the Al-wetted TiB 2 -C Protective composite coating.

[0023] By mixing the binder with titanium diboride (TiB 2 ) Mixed to get TiB 2 -C protective composite coating, the particle size composition of which is characterized by a bimodal or multimodal particle size distribution until a smooth slurry with the following proportions is obtained: 35-50 wt.% binder, 65-50 wt.% TiB 2 A sulfonated product of naphthalene and formaldehyde is used as a binder, the binder having a coke residue of at least 30 wt.%. 2 , using titanium diboride powder or a bimodal or multimodal mixture of titanium diboride powders, the particle size composition of which is characterized by a bimodal or multimodal particle size distribution, which helps to improve the processing performance during suspension preparation, as well as improve the physical and mechanical properties of the protective coating, namely reducing shrinkage and eliminating cracking.

[0024] During further operation, the compound is continuously mixed until smooth to prevent TiB 2Sedimentation of particles and segregation of the mixture. Next, the prepared mixture is applied to the bottom of the electrolytic cell by pouring and then leveling with a roller or by spraying. In this case, the mixture is applied locally along the sides of the electrolytic cell in the form of strips with a width of 500-1,200 mm on the areas with the greatest wear on the bottom. The protective coating thickness layer is 0.8-1 mm. The coating is dried at room temperature at the production site for at least 8 hours. Then, a layer of graphite powder with a thickness of 15-30 mm is applied to the surface of the coating to protect it from oxidation during startup.

[0025] During the start-up of the electrolytic cell, the bottom is heated to 950°C over 48-72 hours, forming a TiB with a carbon concentration of about 15-40wt.% and aluminum wetted. 2 -C composite coating.

[0026] TiB 2 -C protective composite coating has high adhesion to cathode block material, wear resistance, crack resistance, and it is wetted by liquid aluminum, which leads to reduced contact resistance and Al-TiB 2 - Increased chemical resistance at the C boundary.

[0027] Increasing the binder content in the composite mixture beyond 50 wt.% results in a loss of the desired physical and mechanical properties (i.e. the properties mentioned above), as well as a decrease in apparent density, compressive strength values, and an increase in open porosity and resistivity. Reducing the binder content below 35 wt.% results in a loss of processing properties of the composite mixture.

[0028] The authors of the present invention tested the proposed method, composite mixture and coating on an industrial electrolytic cell with baked anodes. The quality of the protective coating on the industrial electrolytic cell with baked anodes was determined by controlling the mass percentage of impurities in the crude aluminum, the cathode voltage drop value and the current distribution on the steel strip.

[0029] The results of the electrolyzer operation after start-up confirmed that there was no degradation of the bottom wetting coating and, therefore, the effectiveness of the proposed protection method and the corresponding composite mixture and coating were also confirmed.

[0030] Example of Embodiment of the Invention

[0031] Example 1

[0032] 1 kg of titanium diboride powder with a particle size of 1-80 μm was charged into a mixer. Then, 50 wt.% of TiB 2 In the adhesive, mix the adhesive until smooth. During further operation, the compound is continuously mixed until smooth to prevent TiB 2 Sedimentation of particles and separation of mixtures.

[0033] The prepared mixture was placed in a 100x100 mm 2 The size of the protective coating is 0.6±0.1mm, 1mm and 10mm based on the type of physical and mechanical property test.

[0034] The coating is allowed to dry at room temperature for no longer than 48 hours.

[0035] The coating is then covered with a layer of coke powder and placed in an oven, where it is heated to 950°C over 48 hours and then kept at this temperature for 5 hours, thereby forming a TiB 2 -C composite coating.

[0036] The carbon content in the composite coating is 20%.

[0037] TiB 2 -C protective coating material has the following characteristics: apparent density is 1.98±0.12g / cm 3 ; Compressive strength 32±3MPa; Open porosity 30±2%; Resistivity at room temperature 70±5 micro-ohm·m; Thermal expansion coefficient 5.7±0.5x10 -6 K -1 ; The bonding strength to the cathode block material is 2±0.5MPa; the wetting angle is <90 degrees.

[0038] Example 2

[0039] 1kg has a bimodal particle size distribution (d av 1 =2.5μm and d av 2 =53 μm) or a titanium diboride powder mixture with a multimodal particle size distribution (containing large, medium and small particles of 1 to 100 μm) is charged into a mixer. Then, a binder in a proportion of 35 wt.% is added to the 65 wt.% TiB 2 In the process, the adhesive was mixed for 15 minutes until smooth. During the further operation, the compound was continuously mixed until smooth to prevent TiB 2 Sedimentation of particles and separation of mixtures.

[0040] The prepared mixture was placed in a 100x100 mm 2 The size of the protective coating is 0.6±0.1mm, 1mm and 10mm based on the type of physical and mechanical property test.

[0041] The coating is allowed to dry at room temperature for no longer than 48 hours.

[0042] The coating is then covered with a layer of coke powder and placed in an oven, where it is heated to 950°C over 48 hours and then kept at this temperature for 5 hours, thereby forming TiB 2 -C composite coating.

[0043] The carbon content in the composite coating is 15 wt.%.

[0044] TiB 2 -C protective coating material has the following characteristics: apparent density is 2.2±0.1g / cm 3 , compressive strength 46±2МPa; porosity 9±2%; resistivity at room temperature 52±5 micro-ohm·m; thermal expansion coefficient 5.3±0.5x10 -6 K -1 ; The adhesion strength to the cathode block material is 4±0.5МPa; the wetting angle is <90 degrees.

[0045] Example 3

[0046] 40 kg of titanium diboride powder with a particle size of 1-80 μm was charged into a mixer. Then, a binder in a ratio of 50 wt.% was added to the 50 wt.% TiB 2 , mix the adhesive until smooth. In the following operation, continue to mix the compound until smooth to prevent TiB 2 Sedimentation of particles and separation of mixtures.

[0047] The prepared mixture was then applied to the bottom of an electrolytic cell with baked anodes. In this case, the coating was applied in strips with a width of 900 mm along the sides of the electrolytic cell in the areas of greatest wear on the bottom.

[0048] The prepared mixture was applied to the bottom of a high current electrolytic cell by spraying with a spray gun. The layer thickness was 0.8-1 mm.

[0049] Under the conditions of the production site, the coating was dried at room temperature for 8 hours.

[0050] The coating surface is covered with a 30mm thick layer of graphite powder to protect it from oxidation during startup.

[0051] During the start-up of the electrolytic cell, the bottom is heated to 950°C over 48-72 hours to form an aluminum-wet composite coating TiB 2 -C.

[0052] The carbon content in the composite coating is 20%. The wear rate of the coating is 2.8±0.5 mm / year.

[0053] Example 4

[0054] 40 kg of titanium diboride powder mixture (dav 1 =2.5μm and d av 2 =53 μm) or having a multimodal particle size distribution (containing large, medium and small particles from 1 to 100 μm) is loaded into the mixer. Then, a binder in a proportion of 35 wt.% is added to 65 wt.% of TiB 2 and mix the adhesive for 15 minutes until smooth. During further operation, the compound is continuously mixed until smooth to prevent TiB 2 Sedimentation of particles and separation of mixtures.

[0055] The prepared mixture was applied to the bottom of a high current electrolytic cell by pouring and then leveled with a roller.

[0056] The coating is applied in strips with a width of 900 mm along the sides of the electrolytic cell in the area of ​​the bottom where the wear is greatest. The layer thickness is 0.8-1 mm.

[0057] Allow the coating to dry at room temperature for at least 8 hours under production site conditions.

[0058] The coating surface is covered with a layer of graphite powder with a thickness of 15-30mm to protect it from oxidation during the startup process. During the start-up of the electrolytic cell, the bottom is heated to 950℃ for 48-72 hours, resulting in the formation of an aluminum-wetted composite coating TiB 2 -C.

[0059] The carbon content in the composite coating is 15wt.%. The wear rate of the coating is 2.8±0.5mm / year.

[0060] The present disclosure relates to non-limiting embodiments defined in the following terms:

[0061] Item 1. A method for preparing a TiB cathode block for an aluminum electrolysis cell having a baked anode 2 -C protective composite coating method, comprising preparing a composite mixture of a heat-resistant material and a binder, applying the mixture to the surface of the cathode block and drying the coating, wherein the binder is used in the form of a sulfonated product of the reaction of naphthalene and formaldehyde, the binder has a coke residue of at least 30 wt.%, the heat-resistant material is used in the form of titanium diboride powder or a bimodal or multimodal mixture of titanium diboride powders, the particle size composition of which is characterized by a bimodal or multimodal particle size distribution, and after drying, a layer of graphite powder is applied to the surface of the coating to prevent it from being oxidized during the startup process, which is accompanied by the formation of aluminum-wet TiB when the bottom is heated. 2 -C Protective composite coating.

[0062] Clause 2. The method according to clause 1, wherein the binder content of the prepared mixture is 35-50 wt.%, and the titanium diboride content is 65-50 wt.%.

[0063] Clause 3. The method according to clause 1, wherein the mixture is applied in layers to the surface of the cathode block by pouring and then leveling with a roller or by spraying.

[0064] Clause 4. The method according to clause 1, wherein the mixture is applied to at least the area of ​​the bottom that is most worn, taking into account the wear condition of the bottom.

[0065] Clause 5. The method of clause 1, wherein the mixture is locally applied along the sides of the electrolytic cell in the form of a strip 500-1,200 mm wide.

[0066] Clause 6. The method according to clause 1, wherein the mixture is applied to obtain a protective coating having a thickness of 0.8-1 mm.

[0067] Clause 7. The method according to clause 1, wherein after applying the mixture to the cathode block of the electrolytic cell, the coating is dried at room temperature for at least 8 hours under production site conditions.

[0068] Clause 8. The method according to clause 1, wherein the graphite powder is applied to the coating surface in a thickness of 15-30 mm.

[0069] Item 9. The method according to Item 1, wherein the bottom is heated to 950°C for 48-72 hours to form TiB 2 -C Protective composite coating.

[0070] Clause 10. The method of clause 1, wherein the TiB 2 -C The protective composite coating contains 15-40 wt.% carbon.

[0071] Item 11. The method according to Item 1, wherein the mixture is continuously mixed until smooth to prevent TiB 2 Sedimentation of particles and separation of mixtures.

[0072] Item 12. A method for preparing a TiB cathode block for an aluminum electrolysis cell having a baked anode 2-C protective composite coating method, comprising preparing a composite mixture of a refractory material and a binder, applying the mixture to the surface of a cathode block and drying to obtain a coating, wherein the binder is used in the form of a sulfonated product of a reaction of naphthalene with formaldehyde, the binder having a coke residue of at least 30 wt.%, the refractory material is used in the form of a titanium diboride powder or a bimodal or multimodal mixture of titanium diboride powders, the particle size composition of which is characterized by a bimodal or multimodal particle size distribution, in which case the binder content of the prepared mixture is 35-50 wt.% and 65-50 wt.% of titanium diboride, after drying, a layer of graphite powder is applied to the surface of the coating to protect it from oxidation during the startup process, which is accompanied by the formation of TiB wetted with aluminum during bottom heating 2 -C Protective composite coating.

[0073] Item 13. A TiB for obtaining cathode blocks for aluminum electrolysis cells with baked anodes 2 -C composite mixture of protective composite coating, which contains 65-50wt.% TiB 2 , used in the form of titanium diboride powder or a bimodal or multimodal mixture of titanium diboride powders, the particle size composition of which is characterized by a bimodal or multimodal particle size distribution, and a binder in an amount of 35-50wt.%, which is used in the form of a sulfonated product of the reaction of naphthalene with formaldehyde and has a coke residue of at least 30wt.%.

[0074] Item 14. TiB of a cathode block for an aluminum electrolysis cell having a baked anode 2 - C protective composite coating, characterized in that it is obtained by a method according to any one of clauses 1 to 10 and contains carbon in an amount of 15 to 40 wt.%.

[0075] Item 15. A TiB cathode block for an aluminum electrolytic cell having a baked anode 2 -C protective composite coating, characterized in that it is obtained by the process according to clause 12 and contains 15-40 wt.% carbon.

Claims

1. A method for preparing a TiB2-C protective composite coating for a cathode block of an aluminum electrolytic cell having a baked anode, comprising preparing a composite mixture of a heat-resistant material and a binder, coating the mixture on the surface of the cathode block and drying the coating, wherein the binder is used in the form of a sulfonated product of a reaction between naphthalene and formaldehyde, the binder having a coke residue of at least 30 wt.%, and the heat-resistant material is used in the form of a titanium diboride powder or a bimodal or multimodal mixture of titanium diboride powders, the particle size composition of which is characterized by a bimodal or multimodal particle size distribution, and after drying, coating the surface of the coating with a layer of graphite powder to prevent it from being oxidized during the startup process, which is accompanied by the formation of an aluminum-wet TiB2-C protective composite coating when the bottom is heated.

2. The method according to claim 1, wherein: The mixture is applied in layers to the surface of the cathode block by pouring and then leveling with a roller or by spraying.

3. The method according to claim 1, wherein: Taking into account the wear condition of the bottom, the mixture is applied at least to the areas of the bottom that are most worn.

4. The method according to claim 1, wherein: The mixture was locally applied along the sides of the electrolytic cell in the form of a strip 500-1,200 mm wide.

5. The method according to claim 1, wherein: The mixture was applied to obtain a protective coating with a thickness of 0.8-1 mm.

6. The method according to claim 1, wherein: After applying the mixture to the cathode blocks of the electrolytic cell, the coating was dried at room temperature for at least 8 hours under production site conditions.

7. The method according to claim 1, wherein: Apply graphite powder on the coating surface with a thickness of 15-30mm.

8. The method according to claim 1, wherein: The bottom is heated to 950°C for 48-72 hours to form a TiB2-C protective composite coating.

9. The method according to claim 1, wherein: The TiB2-C protective composite coating contains 15-40 wt.% carbon.

10. The method according to claim 1, wherein: The mixture was continuously mixed until smooth to prevent settling of the TiB2 particles and segregation of the mixture.

11. A method for preparing a TiB2-C protective composite coating for a cathode block of an aluminum electrolytic cell having a baked anode, comprising preparing a composite mixture of a heat-resistant material and a binder, applying the mixture to the surface of the cathode block and drying to obtain a coating, wherein the binder is used in the form of a sulfonated product of a reaction between naphthalene and formaldehyde, the binder having a coke residue of at least 30 wt.%, wherein: The heat-resistant material is used in the form of titanium diboride powder or a bimodal or multimodal mixture of titanium diboride powder, the particle size composition of which is characterized by a bimodal or multimodal particle size distribution. In this case, the prepared mixture has a binder content of 35-50wt.% and a titanium diboride content of 65-50wt.%. After drying, a layer of graphite powder is applied to the surface of the coating to protect it from oxidation during the startup process, which is accompanied by the formation of a TiB2-C protective composite coating wetted with aluminum during bottom heating.

12. A composite mixture for obtaining a TiB2-C protective composite coating for cathode blocks of aluminum electrolysis cells with baked anodes, comprising TiB2 in an amount of 65-50 wt.%, used in the form of titanium diboride powder or a bimodal or multimodal mixture of titanium diboride powders, the particle size composition of which is characterized by a bimodal or multimodal particle size distribution, and a binder in an amount of 35-50 wt.%, used in the form of a sulfonation product of the reaction of naphthalene with formaldehyde, the binder having a coke residue of at least 30 wt.%.

13. A TiB2-C protective composite coating for cathode blocks of an aluminum electrolysis cell having baked anodes, characterized in that: It is obtained by a process according to any one of claims 1 to 9 and has a carbon content of 15 to 40 wt.%.

14. A TiB2-C protective composite coating for cathode blocks of aluminum electrolytic cells having baked anodes, characterized in that: It is obtained by a process according to claim 11 and has a carbon content of 15-40 wt.%.