Preparation method of porous aromatic framework (PAFs) loaded lithium iron phosphate positive electrode material
By introducing porous aromatic skeletons into the lithium iron phosphate positive electrode material, the stable composite material LiFePO4@PAFs is solved, and the thermal runaway problem of lithium iron phosphate material in high temperature and overcharging is improved, and the safety and cycle life of the battery are improved. And meets the needs of high energy density.
Patent Information
- Application Number
- CN202410863766.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-06-29
AI Technical Summary
Existing lithium iron phosphate positive electrode materials are prone to thermal runaway reactions under high temperature, overcharging or short circuit, resulting in the risk of battery explosion and a short cycle life, which cannot meet the high energy density needs of electric vehicles.
Using porous aromatic skeletons (PAFs) as base carrier, the lithium iron phosphate precursor after gel loading is sintered under an inert atmosphere to prepare a stable composite lithium iron phosphate positive electrode material LiFePO4@PAFs to form a three-dimensional structure to improve Li+ Transmission rate and material uniformity.
A composite material with high electrochemical capacity, excellent rate performance and uniform particle dispersion is achieved, reducing the risk of battery explosion, extending battery life, and improving energy density.
Smart Images

Figure CN118929604A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a phosphate-based positive electrode material, and in particular to a method for preparing a porous aromatic framework (PAFs)-loaded lithium iron phosphate positive electrode material. Background Art
[0002] Lithium iron phosphate material is a compound of lithium-ion battery positive electrode material, composed of elements such as lithium (Li), iron (Fe), phosphorus (P) and oxygen (O). Compared with traditional lithium cobalt oxide (LiCoO2) and lithium manganese oxide (LiMn2O4), lithium iron phosphate has good safety performance. Due to its high crystal structure stability, the material is not prone to thermal runaway reaction even under abnormal conditions such as high temperature, overcharge or short circuit, thereby reducing the risk of battery explosion. Secondly, lithium iron phosphate has a long cycle life. Compared with other positive electrode materials, lithium iron phosphate has a lower capacity decay rate during the cycle charge and discharge process, can maintain relatively stable battery performance, and extend the battery life. In addition, lithium iron phosphate has a high theoretical capacity of 170 mAh / g, which enables lithium iron phosphate batteries to provide higher energy density and specific capacity, meeting the requirements of battery energy density in different application scenarios. Due to the above advantages, lithium iron phosphate materials are widely used in electric vehicles, energy storage systems, portable electronic devices and other fields. Especially in the field of electric vehicles, lithium iron phosphate batteries have been favored by consumers and industries because of their safety, stability and long life.
[0003] Porous organic polymers are a class of materials that have both porous and polymer properties. They are mainly composed of carbon, hydrogen, oxygen and other elements. They can be modified to produce microstructures of different morphologies while maintaining the surface activity of the material while ensuring the existing pore structure. Porous aromatic framework polymers (PAFs) have a rigid framework and an unusually high surface area. The aromatic building skeleton unit structure is connected by CC bonds. Its typical characteristics include high specific surface area and excellent chemical stability. A method for preparing a porous aromatic framework (PAFs) loaded lithium iron phosphate cathode material. The method uses PAFs as a base material, loads a pre-treated lithium iron phosphate precursor through a gel, and sinters it in an inert atmosphere to form a stable composite lithium iron phosphate cathode material LiFePO4@PAFs. The material has a three-dimensional structure, and certain pores can effectively increase the Li + The transmission rate between the main body and the interface of the lithium iron phosphate material is increased, thereby obtaining a composite material with high electrochemical capacity, excellent rate performance and uniform particle dispersion. Summary of the invention
[0004] To achieve the above object, the present invention provides the following technical solutions: A method for preparing a porous aromatic framework (PAFs)-loaded lithium iron phosphate positive electrode material comprises the following steps: S1. Synthesize porous aromatic framework polymers (PAFs). Weigh a certain amount of benzene and aldehyde substances in proportion, add them to an organic solvent, and add a certain amount of catalyst to form a mixed solution. The mixed solution is placed in a stirrer and stirred for a certain period of time, and then transferred to a high-pressure reactor for reaction. After the reaction is completed, the PAFs-based material is taken out, washed, and dried to obtain.
[0005] S2, preparing lithium iron phosphate precursor material. Take iron source, lithium source, phosphorus source, and doping source, add them into deionized water and disperse them evenly, transfer them into a sand mill for grinding to obtain lithium iron phosphate slurry, spray dry the lithium iron phosphate slurry to obtain yellow material powder, and pre-sinter in an inert atmosphere to obtain a lithium iron phosphate precursor.
[0006] S3, prepare gel-dispersed PAFs-loaded precursor. Take starch as a carbon source and add it to deionized water, add a small amount of activation component, stir and pre-gelatinize, add a cross-linking agent to form a starch gel, then add the PAFs-based carrier in S1 and the lithium iron phosphate precursor in S2, and continue stirring to form a gel-loaded precursor.
[0007] S4, preparing LiFePO4@PAFs material. The gel-loaded precursor formed in S3 is transferred into a graphite sagger and sintered again under an inert atmosphere to obtain a composite lithium iron phosphate positive electrode material LiFePO4@PAFs.
[0008] In the step S1, the benzene substance is one of phenol, hydroquinone and triphenylamine.
[0009] In the step S1, the aldehyde substance is formaldehyde; and the organic solvent is ethanol and chloroform.
[0010] In the step S1, the catalyst is one of hydrogen chloride, sodium chloride, potassium chloride and aluminum chloride.
[0011] In the step S1, the stirring time of the stirrer is 1-3 hours; the reaction conditions in the high-pressure reactor are: reaction temperature 80-120°C, time 12-24 hours; the washing adopts methanol or ethanol or deionized water to repeatedly filter and wash to wash away unreacted raw materials and catalysts; the drying method is drying in a vacuum drying oven at 80°C for 24 hours.
[0012] In the S2 step, the iron source is one of ferric nitrate, ferric phosphate, ferrous oxalate, and ferric oxide; the lithium source is one of lithium carbonate, lithium dihydrogen phosphate, and lithium hydroxide; the phosphorus source is one of phosphoric acid and ammonium dihydrogen phosphate; and the doping source is one of titanium dioxide, ammonium metavanadate, magnesium acetate, and boric acid.
[0013] In the step S2, the molar ratio of the iron source, lithium source and phosphorus source is 1:(1-1.1):(1-1.6); the doping source is measured as 500-3600 ppm of metal elements; the amount of deionized water added is calculated based on the total mass of all solid substances so that its solid content is 30%-50%.
[0014] In the step S2, the slurry is sand-milled to a particle size of 230-580 nm; the pre-sintering is carried out in a nitrogen atmosphere, the sintering temperature is 350-480° C., the heating rate is 1-2.5° C. / min, and the holding time is 6-10 h.
[0015] In the step S3, starch is added to hot water at 30-55° C. and stirred continuously for 10-60 minutes; the activation component is one of chitosan and cellulose, and the amount used is 1.5%-6.5%.
[0016] In the step S3, the crosslinking agent is one of sodium tripolyphosphate, sodium trimetaphosphate and sodium hexametaphosphate, and the amount is 0.8%-2.6%. The PAFs-based carrier and lithium iron phosphate precursor are added under stirring, and stirring is continued for 10-30 minutes.
[0017] In the step S4, the sintering atmosphere is a nitrogen atmosphere, the sintering temperature is set to 600-900°C, the heating rate is 1-6°C / min, preferably 2-5°C / min, and the insulation time is 5-12h to obtain a composite lithium iron phosphate positive electrode material LiFePO4@PAFs.
[0018] Compared with the prior art, the present invention has the following beneficial effects: (1) The porous aromatic skeleton material has a stable CC covalent bond, which ensures the stability of its skeleton. After high-temperature sintering, it can still maintain some basic properties of three-dimensional porous materials. The starch gel loaded lithium iron phosphate material prepared by it can evenly disperse lithium iron phosphate in the carbon material to prepare a carbon grid with uniform surface coating and close connection between particles, effectively increasing Li + Diffusion rate.
[0019] (2) Using starch gel to disperse PAFs to load lithium iron phosphate precursor can effectively form a uniformly distributed PAFs-based carrier on the surface of lithium iron phosphate particles. The two substances can be fully contacted through the gel, which is beneficial to ensure the uniformity and stability of the material. (3) The present invention prepares a composite lithium iron phosphate positive electrode material LiFePO4@PAFs by calcining the spray yellow material at a relatively low temperature and then using starch gel as a carbon source through a high-temperature secondary sintering. The positive electrode material obtained by the present invention has a moderate particle size, high electrochemical capacity, high product compaction density, and excellent comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the embodiment process.
[0021] Figure 2 This is the SEM photo of LiFePO4@PAFs prepared in Example 1.
[0022] Figure 3 This is the SEM photo of LiFePO4@PAFs prepared in Example 2. DETAILED DESCRIPTION
[0023] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0024] Example 1 (1) Synthesis of PAFs: Weigh 32 g of phenol and 100 ml of formaldehyde, add them to 300 ml of ethanol solvent, then add 30 ml of hydrochloric acid as a catalyst, stir for 2.5 h, then transfer to a high-pressure reactor, react at 100 °C for 16 h, cool to room temperature, take out, wash repeatedly with ethanol and deionized water, filter and dry in an oven at 80 °C.
[0025] (2) Preparation of LFP precursor: Iron phosphate and lithium carbonate were weighed at a Fe:Li molar ratio of 1:1.025. Titanium dioxide and magnesium acetate were used as doping sources, and 1000 pmm and 240 ppm were added respectively. Deionized water was then added to keep the solid content at 42%. The slurry was transferred to a sand mill and ground to a particle size of 430 nm. Lithium iron phosphate powder was obtained by spray drying. In a nitrogen atmosphere, the temperature was raised to 360°C at 1.8°C / min and kept at this temperature for 7.5 hours to obtain a lithium iron phosphate precursor.
[0026] (3) Preparation of gel-dispersed PAFs-loaded precursor. Starch was weighed at a Fe:C molar ratio of 1:0.36 and added to 45°C deionized water. The mixture was stirred continuously for 30 min. 3.5% chitosan was added as an activating component. 0.8% sodium tripolyphosphate was added as a cross-linking agent under continuous stirring. The PAFs prepared in (1) and the LFP precursor prepared in (2) were added. The mixture was stirred continuously for 30 min to obtain a gel-dispersed PAFs-loaded precursor.
[0027] (4) Preparation of LiFePO4@PAFs material. The product obtained in (3) was transferred into a graphite crucible and sintered again under a nitrogen atmosphere. The temperature was raised to 690°C at a rate of 3°C / min and kept at this temperature for 8 h. The product was then crushed to obtain LiFePO4@PAFs material.
[0028] Example 2 (1) Synthesis of PAFs: Weigh 37.4 g of hydroquinone and 10 ml of formaldehyde solution, add them to 200 ml of ethanol solvent, then add 100 ml of saturated sodium chloride solution as a catalyst, stir for 0.5 h, then transfer to a high-pressure reactor, react at 80 °C for 24 h, cool to room temperature, take out, wash repeatedly with ethanol and deionized water, filter and dry in an oven at 80 °C.
[0029] (2) The same as step (2) in Example 1, to obtain a lithium iron phosphate precursor.
[0030] (3) Preparation of gel-dispersed PAFs-loaded precursor. Starch was weighed at a Fe:C molar ratio of 1:0.29 and added to 55°C deionized water. The mixture was stirred continuously for 20 min. 5% cellulose was added as an activating component. 1.2% sodium trimetaphosphate was added as a cross-linking agent under continuous stirring. The PAFs prepared in (1) and the LFP precursor prepared in (2) were added. The mixture was stirred continuously for 30 min to obtain a gel-dispersed PAFs-loaded precursor.
[0031] (4) The same as step (4) in Example 1, to obtain LiFePO4@PAFs material.
[0032] Example 3 (1) Synthesis of PAFs: Weigh 8.856 g of triphenylamine and 80 ml of formaldehyde, add them to 200 ml of chloroform solvent, then add 60 ml of hydrochloric acid as a catalyst, stir for 1 h, then transfer to a high-pressure reactor, react at 100 °C for 18 h, cool to room temperature, take out, wash repeatedly with methanol and deionized water, filter and dry in an oven at 80 °C.
[0033] (2) Preparation of LFP precursor: Iron phosphate and lithium carbonate were weighed at a Fe:Li molar ratio of 1:1.025. Boric acid and magnesium acetate were used as doping sources, and 800 pmm and 240 ppm were added respectively. Deionized water was then added to keep the solid content at 38%. The slurry was transferred to a sand mill and ground to a particle size of 360 nm. Lithium iron phosphate powder was obtained by spray drying. In a nitrogen atmosphere, the temperature was raised to 330°C at 2°C / min and kept at this temperature for 6.5 hours to obtain a lithium iron phosphate precursor.
[0034] (3) The same as step (3) in Example 1, to obtain a gel-dispersed PAFs-loaded precursor.
[0035] (4) Preparation of LiFePO4@PAFs material. The product obtained in (3) was transferred into a graphite crucible and sintered again under a nitrogen atmosphere. The temperature was raised to 680°C at a rate of 3.5°C / min and kept at this temperature for 7.5 h. The product was then crushed to obtain LiFePO4@PAFs material.
[0036] Example 4 (1) The same as step (1) in Example 1, PAFs were synthesized.
[0037] (2) The same as step (2) in Example 1, to obtain a lithium iron phosphate precursor.
[0038] (3) Preparation of gel-dispersed PAFs-loaded precursor. Starch was weighed at a Fe:C molar ratio of 1:0.48 and added to 50°C deionized water. The mixture was stirred for 25 min. 2.5% chitosan was added as an activating component. 0.6% sodium hexametaphosphate was added as a cross-linking agent under stirring. The PAFs prepared in (1) and the LFP precursor prepared in (2) were added. The mixture was stirred for 30 min to obtain a gel-dispersed PAFs-loaded precursor.
[0039] (4) Preparation of LiFePO4@PAFs material. The product obtained in (3) was transferred into a graphite crucible and sintered again in a nitrogen atmosphere. The temperature was raised to 7000°C at .°C / min and kept at this temperature for 7.5h. The product was then crushed to obtain LiFePO4@PAFs material.
[0040] Comparative Example 1 As comparative example 1, a gel-dispersed precursor was directly prepared without adding PAFs. That is, compared with Example 1, step (1) was not performed. In step (3), starch was weighed at a Fe:C molar ratio of 1:0.36 and added to 45°C deionized water, and stirred continuously for 30 minutes. 3.5% chitosan was added as an activation component, and 0.8% sodium tripolyphosphate was added as a cross-linking agent under continuous stirring. Only the LFP precursor prepared in (2) was added, and stirring was continued for 30 minutes to obtain a gel-dispersed PAFs-loaded precursor. The remaining steps or preparation process were consistent with Example 1.
[0041] Comparative Example 2 As comparative example 2, PAFs and LFP precursors were prepared without starch gel dispersion, and only dry mixing was performed. That is, compared with Example 1, an equal amount of starch was added as a carbon source in step (2), and step (3) was changed to taking the same amount of PAFs synthesized in step (1) and the precursor prepared in step (2) as in the example, and dry ball milling was performed to mix the two components. The remaining steps or preparation process were consistent with Example 1.
[0042] Performance Test: The products prepared in the examples and comparative examples, PVDF, and Super-p were mixed in a ratio of 90:5:5, and the solid content was 30% with N-methylpyrrolidone, and then homogenized and assembled into button cells for testing. The button cells were charged and discharged in the voltage range of 2.0-3.6V.
[0043] Test results: serial number 0.1 C discharge capacity (mAh / g) 0.5 C discharge capacity (mAh / g) 1 C discharge capacity (mAh / g) <![CDATA[Specific surface area (m 2 / g)]]> Powder resistivity (Ω.cm) <![CDATA[Powder Compaction Density (g / cm 3 )]]> Example 1 160.92 158.68 155.51 20.23 8.278 2.63 Example 2 159.21 157.36 155.38 19.36 10.658 2.60 Example 3 160.92 158.64 155.70 21.06 3.159 2.61 Example 4 161.06 158.07 156.01 20.55 5.691 2.69 Comparative Example 1 150.26 141.44 127.58 9.35 73.589 2.35 Comparative Example 2 148.50 141.09 139.5 8.99 102.359 2.31 It can be seen from the examples and comparative data that the lithium iron phosphate material prepared using the scheme of the present invention has higher discharge capacity at 0.1C, 0.5C, and 1C, larger overall specific surface area, lower resistivity, higher powder compaction density, and excellent comprehensive performance.
Claims
1. A method for preparing a porous aromatic framework PAFs-loaded lithium iron phosphate positive electrode material, characterized in that: The following steps are involved: (1) Synthesizing a porous aromatic skeleton polymer, weighing a certain amount of benzene and aldehyde in proportion, adding them to an organic solvent, and adding a certain amount of catalyst to form a mixed solution, placing the mixed solution in a stirrer and stirring for a certain period of time, then transferring it to a high-pressure reactor for reaction, and taking it out after the reaction is completed, washing it, and drying it to obtain a PAFs-based support; (2) preparing a lithium iron phosphate precursor material, taking an iron source, a lithium source, a phosphorus source, and a doping source, adding them to deionized water and dispersing them evenly, transferring them to a sand mill for grinding to obtain a lithium iron phosphate slurry, spray drying the lithium iron phosphate slurry to obtain a yellow material powder, and pre-sintering them in an inert atmosphere to obtain a lithium iron phosphate precursor; (3) Preparation of gel-dispersed PAFs-loaded precursor: starch is taken as a carbon source and added to water, and a small amount of activation component is added. After stirring for pre-gelatinization, a cross-linking agent is added to form a starch gel. Subsequently, the PAFs-based carrier in S1 and the lithium iron phosphate precursor in S2 are added, and the gel-loaded precursor is formed continuously by stirring; (4) Preparation of LiFePO4@PAFs material: The gel-loaded precursor formed in S3 is transferred into a graphite crucible and sintered again under an inert atmosphere to obtain a composite lithium iron phosphate positive electrode material LiFePO4@PAFs.
2. The method for preparing a porous aromatic framework (PAFs)-loaded lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the step (1), the benzene substance is one of phenol, hydroquinone and triphenylamine; the aldehyde substance is formaldehyde; the organic solvent is ethanol or chloroform; and the catalyst is one of hydrogen chloride, potassium chloride, sodium chloride and aluminum chloride.
3. The method for preparing a porous aromatic framework (PAFs)-loaded lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the step (1), the stirring time of the stirrer is 1-3 hours; the reaction conditions in the high-pressure reactor are: reaction temperature 80-120°C, time 12-24 hours; the washing is repeated filtration and cleaning with methanol or ethanol or deionized water to wash away unreacted raw materials and catalysts; the drying method is drying in a vacuum drying oven at 80°C for 24 hours.
4. The method for preparing a porous aromatic framework (PAFs)-loaded lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the step (2), the iron source is one of ferric nitrate, ferric phosphate, ferrous oxalate, and ferric oxide; the lithium source is one of lithium carbonate, lithium dihydrogen phosphate, and lithium hydroxide; the phosphorus source is one of phosphoric acid and ammonium dihydrogen phosphate; and the doping source is one of titanium dioxide, ammonium metavanadate, magnesium acetate, and boric acid.
5. The method for preparing a porous aromatic framework (PAFs)-loaded lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the step (2), the molar ratio of the iron source, the lithium source and the phosphorus source is 1:(1-1.1):(1-1.6); the doping source is measured as 500-3600 ppm of metal elements; and the amount of deionized water added is calculated based on the total mass of all solid substances so that the solid content is 30%-50%.
6. The method for preparing a porous aromatic framework (PAFs)-loaded lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the step (2), the slurry is sand-milled to a particle size of 230-580 nm; the pre-sintering is carried out in a nitrogen atmosphere, the sintering temperature is 350-480° C., the heating rate is 1-2.5° C. / min, and the holding time is 6-10 h.
7. The method for preparing a porous aromatic framework (PAFs)-loaded lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the step (3), starch is added to hot water at 30-55° C. and stirred continuously for 10-60 minutes; the activation component is one of chitosan and cellulose, and the amount used is 1.5%-6.5%.
8. The method for preparing a porous aromatic framework (PAFs)-loaded lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the step (3), the cross-linking agent is one of sodium tripolyphosphate, sodium trimetaphosphate, and sodium hexametaphosphate, and the amount used is 0.8%-2.6%; the PAFs-based carrier and the lithium iron phosphate precursor are continuously added under stirring, and stirring is continued for 10-30 minutes.
9. The method for preparing a porous aromatic framework (PAFs)-loaded lithium iron phosphate positive electrode material according to claim 1, characterized in that: In the step (4), the sintering atmosphere is a nitrogen atmosphere, the sintering temperature is set to 600-900°C, the heating rate is 1-6°C / min, preferably 2-5°C / min, and the insulation time is 5-12h to obtain a composite lithium iron phosphate positive electrode material LiFePO4@PAFs.
Citation Information
Patent Citations
High power iron phosphate ion battery material and preparation method thereof
CN102760880A
Method for preparing lithium phosphate / carbon-coated lithium iron phosphate composite material
CN103730657A
Composite-coated lithium iron phosphate, preparation method of composite-coated lithium iron phosphate, and lithium ion battery
CN104716320A
Lithium ion battery applied to portable mobile power supply and preparation method
CN117174831A
Preparation method of high-compaction high-capacity lithium iron phosphate positive electrode material
CN118239455A
Cited By
Application of soluble cyclotrimetaphosphate in lithium ion battery positive electrode material, polycrystalline ternary positive electrode material and preparation method of polycrystalline ternary positive electrode material
CN119994063A
Method for synthesizing ruthenium-based catalyst by utilizing ruthenium nitrosyl nitrate
CN122377486A
A method for synthesizing a ruthenium-based catalyst using ruthenium nitrosyl nitrate
CN122377486B