Coated high-voltage lithium-rich manganese-based positive electrode material as well as preparation method and application thereof

By using LiAlO2, Li3PO4 and LiAlP2O7 coatings, the corrosion and pollution of lithium-rich manganese-based positive electrode materials at high voltages are solved, the cycle stability and Li+ diffusion performance of the material are improved, and zero emissions and cost savings are achieved. , suitable for lithium-ion batteries.

CN119092668APending Publication Date: 2024-12-06BEIJING CHUANGNENG HUITONG TECH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411196291.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the cycle of lithium-rich manganese-based positive electrode materials under high voltage, there is corrosion and oxygen loss of the material by the electrolyte, resulting in structural collapse and capacity attenuation. The existing coating methods have problems of uneven coating and sewage pollution.

Method used

LiAlO2, Li3PO4 and LiAlP2O7 are used as coatings to prepare a coated high-voltage lithium-rich manganese-based positive electrode material through reaction and heat treatment with the positive electrode material matrix to avoid electrolyte corrosion and HF side reactions, and improve Li+ diffusion performance.

Benefits of technology

The surface coating uniformity and cycle stability of the positive electrode material are improved, and the wastewater generation and material costs are reduced. It is suitable for lithium-ion batteries in the 3C, new energy vehicles and large-scale energy storage fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092668A_ABST
    Figure CN119092668A_ABST
Patent Text Reader

Abstract

The invention discloses a coated high-voltage lithium-rich manganese-based positive electrode material as well as a preparation method and application thereof, and belongs to the technical field of lithium ion battery materials. The positive electrode material comprises a positive electrode material matrix and a coating on the surface of the positive electrode material matrix; the component of the cathode material matrix is xLi2MnO3. (1-x) LiMO2, x is more than or equal to 0.1 and less than or equal to 0.5, and M is selected from at least one of Ni element, Mn element and Co element; and the coating material is prepared from the following components: LiAlO2, Li3PO4 and LiAlP2O7. The surface coating is uniform, and the Li < + > diffusion performance of a material interface is effectively improved through the synergistic effect of multiple Li-containing compounds, so that the cycling stability and the rate capability of the material under high voltage are improved. The preparation method has the advantages of zero emission, material saving and preparation cost reduction. The prepared positive electrode material can be widely applied to the 3C field, the new energy automobile field and the large energy storage field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium-ion battery materials, and in particular to a coated high-voltage lithium-rich manganese-based positive electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are widely used in 3C, new energy vehicles and large-scale energy storage fields due to their high output voltage, high energy density and environmental friendliness. As a member of the lithium-ion battery cathode material family, lithium-rich manganese-based materials are expected to become a new type of commercial lithium-ion battery cathode material that replaces ternary cathode materials due to their high specific capacity. However, during the circulation of lithium-rich manganese-based materials under high voltage, the electrolyte material seriously corrodes the cathode material, which in turn causes irreversible oxygen loss and transition metal dissolution, resulting in structural collapse and capacity decay of the material under high voltage conditions.

[0003] At present, most of the methods for improving the cycle performance of lithium-rich manganese-based cathode materials use dry or wet coating of oxides (Al2O3, ZrO2, TiO2, etc.) to improve the serious corrosion of the electrolyte during the cycle. The consequence is that the oxide coating is uneven and it is impossible to ensure that all the coatings generate Li-containing compounds, which will directly affect the conductivity and electrical properties of lithium-rich manganese-based cathode materials. In addition, the conventional wet coating process will produce sewage, which contains chemical reagents and heavy metal elements and must be treated to meet the standards before it can be discharged; while polluting the environment, it will inevitably increase the material manufacturing cost.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a coated high-voltage lithium-rich manganese-based positive electrode material and a preparation method and application thereof to solve the above-mentioned technical problems.

[0006] The present invention is achieved in that:

[0007] In a first aspect, an embodiment of the present invention provides a coated high-voltage lithium-rich manganese-based positive electrode material, the positive electrode material comprising a positive electrode material substrate and a coating on the surface of the positive electrode material substrate;

[0008] The composition of the positive electrode material matrix is ​​xLi2MnO3·(1-x)LiMO2, 0.1≤x≤0.5, and M is selected from at least one of Ni, Mn and Co;

[0009] The components of the coating include LiAlO2, Li3PO4 and LiAlP2O7.

[0010] In a second aspect, an embodiment of the present invention provides a method for preparing a positive electrode material as described above, comprising:

[0011] The positive electrode material matrix, phosphate and aluminum salt, auxiliary agent and water are reacted in proportion to obtain an initial coating;

[0012] The initial coating is heat treated to obtain a positive electrode material.

[0013] In a third aspect, an embodiment of the present invention provides a lithium-ion battery, which includes the positive electrode material as described above or the positive electrode material prepared by the preparation method as described above.

[0014] In a fourth aspect, an embodiment of the present invention provides a use of the positive electrode material as described above or the positive electrode material prepared by the preparation method as described above in the preparation of a lithium-ion battery.

[0015] The present invention has the following beneficial effects:

[0016] The coated high-voltage lithium-rich manganese-based positive electrode material provided in the embodiment of the present invention has a uniform surface coating, and the coating components on the surface of the positive electrode material substrate include LiAlO2, Li3PO4 and LiAlP2O7; it not only avoids the corrosion of the coated substrate by the electrolyte, but also reduces the side reaction between HF and the positive electrode material; in addition, the surface coating is a variety of Li-containing compounds, and the synergistic effect between them effectively improves the Li + The diffusion performance is improved, thereby improving the cycle stability and rate performance of the material under high voltage. The preparation method provided by the present invention does not produce wastewater, is pollution-free, can achieve zero emission, and saves materials and reduces preparation costs. The coated high-voltage lithium-rich manganese-based positive electrode material prepared by the present invention can be used to prepare lithium-ion batteries and is widely used in the 3C field, new energy vehicle field and large-scale energy storage field. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0018] Figure 1 A schematic diagram of the stability results of the coated high-voltage lithium-rich manganese-based positive electrode materials prepared in Examples 1-3 and Comparative Example 1 after 12 cycles;

[0019] Figure 2 A schematic diagram of the stability results of the coated high-voltage lithium-rich manganese-based positive electrode materials prepared in Examples 1-3 and Comparative Example 1 after 80 cycles;

[0020] Figure 3Morphology test pictures of the coated high-voltage lithium-rich manganese-based positive electrode materials prepared in Example 1 and Comparative Example 1: (a) Example 1, (b) Comparative Example 1. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0022] In a first aspect, an embodiment of the present invention provides a coated high-voltage lithium-rich manganese-based positive electrode material, the positive electrode material comprising a positive electrode material substrate and a coating on the surface of the positive electrode material substrate;

[0023] The composition of the positive electrode material matrix is ​​xLi2MnO3·(1-x)LiMO2, 0.1≤x≤0.5, and M is selected from at least one of Ni, Mn and Co;

[0024] The components of the coating include LiAlO2, Li3PO4 and LiAlP2O7.

[0025] It should be noted that the coating provided in the embodiment of the present invention is a composite material, which can improve the distribution uniformity and dynamic balance ability of the electrolyte; in addition, the composite material adheres to the surface of the electrode active material and the conductive agent, etc., prevents the particles of the electrode material from peeling off and agglomerating, and improves the structural stability of the electrode.

[0026] The surface of the coating provided by the embodiment of the present invention is uniform, which not only avoids the corrosion of the electrolyte on the positive electrode material matrix, but also reduces the side reaction between HF and the positive electrode material; in addition, the surface coating is a variety of Li-containing compounds, and the synergistic effect between them effectively improves the Li + Diffusion properties, thereby improving the cycle stability and rate performance of the material at high voltage.

[0027] In a second aspect, an embodiment of the present invention provides a method for preparing a positive electrode material as described above, comprising:

[0028] The positive electrode material matrix, phosphate and aluminum salt, auxiliary agent and water are reacted in proportion to obtain an initial coating;

[0029] The initial coating is heat treated to obtain a positive electrode material.

[0030] The preparation method provided by the embodiment of the present invention does not generate wastewater, is pollution-free, can achieve zero emissions, and at the same time saves materials and reduces preparation costs.

[0031] In an optional embodiment of the present invention, the preparation method of the positive electrode material matrix includes the following:

[0032] The lithium source and the metal precursor are mixed and sintered to obtain a positive electrode material matrix.

[0033] Furthermore, the lithium source is selected from at least one of lithium hydroxide, lithium carbonate and lithium nitrate. Specifically, the lithium source can be a single-component substance, a combination of two components, or a combination of three components.

[0034] Furthermore, the metal precursor includes at least one of nickel, manganese and cobalt. It should be noted that in the embodiment of the present invention, the metal precursor used is a metal carbonate, specifically Ni 0.3 Mn 0.6 Co 0.1 In other embodiments of the present invention, reasonable adjustments can be made according to actual needs, such as the metal precursor used is Ni 0.3 Mn 0.7 CO3.

[0035] It should be noted that nickel mainly provides high energy density and good cycle stability in lithium batteries. The presence of nickel makes the battery have a higher theoretical capacity and actual capacity. In addition, nickel is relatively easy to synthesize and has a low cost. Manganese provides high energy density and good cycle stability in lithium batteries. It is used in combination with nickel and cobalt to form a complex oxide structure, which provides the battery with high energy density and good cycle stability. In addition, the use of manganese not only improves the performance of the battery, but also reduces the cost. Cobalt in lithium batteries can improve the cycle and rate performance of the material and thus improve the cycle performance and stability of the battery, but too high a cobalt content will lead to a decrease in the actual capacity.

[0036] Furthermore, the molar ratio of the lithium source to the metal precursor is (1.1-1.5): 1. If it exceeds this range, the charge and discharge capacity, rate performance and cycle performance of the positive electrode material will decrease.

[0037] In a preferred embodiment of the present invention, the molar ratio of the lithium source to the metal precursor is (1.3-1.4):1.

[0038] In an optional embodiment of the present invention, the lithium source and the metal precursor are mixed and treated for at least 0.5 h.

[0039] Specifically, the lithium source and the metal precursor are added to a high-speed mixer in proportion, mixed for 0.5h-2.0h, and then the mixture is sintered to prepare a positive electrode material matrix. In other embodiments of the present invention, the equipment for mixing the raw materials can be replaced according to actual needs, and the specific time of the mixing treatment is reasonably adjusted according to the actual amount of raw materials processed.

[0040] In an optional embodiment of the present invention, the sintering process includes:

[0041] Raise the temperature to 300-650°C at a rate of 2°C / min-10°C / min, and keep it for 2h-10h; then raise the temperature to 800-1100°C at a rate of 1°C / min-2°C / min, and keep it for 5h-10h; then reduce the temperature to room temperature at a rate of 80°C / h-120°C / h.

[0042] Further, the temperature is increased to 500°C-650°C at a rate of 2°C / min-5°C / min, and kept at this temperature for 2h-8h; then the temperature is increased to 800°C-1000°C at a rate of 1°C / min-2°C / min, and kept at this temperature for 6h-10h; and then the temperature is decreased to room temperature at a rate of 80°C / h-100°C / h.

[0043] In a preferred embodiment of the present invention, the sintering process includes: heating to 500-650°C at a rate of 5°C / min, and keeping warm for 2h-5h; then heating to 850-1000°C at a rate of 2°C / min, and keeping warm for 8h-10h; and then cooling to room temperature at a rate of 100°C / h.

[0044] The present invention does not specifically limit the equipment for sintering. Specifically, the sintering equipment used in the embodiments of the present invention is an atmosphere box furnace. The equipment has the characteristics of accurate temperature control, safety and reliability, balanced temperature field, fast temperature rise and fall rate, flexible atmosphere control and good sealing performance. In other embodiments of the present invention, other sintering equipment can be selected according to actual needs.

[0045] It should be noted that the composition of the positive electrode material matrix obtained after sintering is xLi2MnO3·(1-x)LiMO2, 0.1≤x≤0.5, and M is selected from at least one of Ni, Mn and Co.

[0046] In an optional embodiment of the present invention, the preparation method further comprises:

[0047] After adding water to the positive electrode material matrix, phosphate and aluminum salt are added.

[0048] It should be noted that in the embodiments of the present invention, the water used is specifically deionized water. In other embodiments of the present invention, the water can be ultrapure water, distilled water or purified water according to actual needs.

[0049] Specifically, the positive electrode material matrix and deionized water are added to a stirring device in proportion and stirred. During continuous stirring, a certain proportion of phosphate and aluminum salt are added, and then the auxiliary agent solution is added. The reaction is stirred for 1h-2h, and the initial coating is obtained by dehydration through suction filtration.

[0050] In an optional embodiment of the present invention, the main component of the auxiliary agent solution is lithium hydroxide, mainly because lithium hydroxide can synthesize an aluminum hydroxide sol system with an aluminum source. Specifically, it is a solution prepared by mixing lithium hydroxide with deionized water. In the present invention, the concentration of the auxiliary agent solution is not particularly limited, and it is added in the form of a solution, mainly because the auxiliary agent is added in the form of ions to help accelerate the reaction rate and make the reaction more sufficient. In other embodiments of the present invention, an auxiliary agent in solid form can also be directly added.

[0051] It should be noted that the hydroxide ions provided by the additive and the aluminum ions in the aluminum salt help to transform the solution system into a sol system, which is conducive to setting the coating to be evenly coated on the surface of the coated particles. In addition, the additive directly affects the composition of the initial coating.

[0052] Furthermore, the mass ratio of the positive electrode material matrix and water is 1:(1-10); the molar ratio of the total amount of phosphate and aluminum salt added to the positive electrode material matrix is ​​(0.0001-0.1):1; the molar ratio of the lithium source to the total amount of phosphate and aluminum salt added is (1-13):1.

[0053] It should be noted that the mass ratio of the positive electrode material matrix and water, the molar ratio of the total amount of phosphate and aluminum salt added to the positive electrode material matrix, and the molar ratio of the lithium source to the total amount of phosphate and aluminum salt added are set within specific ranges. If they are exceeded, a stable sol system cannot be formed or the element loss is too large.

[0054] In a preferred embodiment of the present invention, the mass ratio of the positive electrode material matrix and water is 1:(3-8); the molar ratio of the total amount of phosphate and aluminum salt added to the positive electrode material matrix is ​​(0.0015-0.0300):1; the molar ratio of the lithium source to the total amount of phosphate and aluminum salt added is (3-9):1.

[0055] In an optional embodiment of the present invention, the composition of the initial coating includes Al(OH)3 and Li3PO4.

[0056] It should be noted that the formation mechanism of the initial coating 3OH - +Al 3+ →Al(OH)3,3Li+ +PO4 3- →Li3PO4.

[0057] In an optional embodiment of the present invention, the molar ratio of phosphate to aluminum salt is 1:(1-10). It should be noted that the phosphate and aluminum salt used in the present invention are both soluble salts.

[0058] Wherein, the soluble phosphate is selected from at least one of aluminum dihydrogen phosphate, ammonium dihydrogen phosphate, sodium phosphate and potassium phosphate; the soluble aluminum salt is selected from at least one of aluminum nitrate, aluminum chloride, aluminum sulfate, aluminum dihydrogen phosphate and aluminum phosphate. It should be noted that the soluble phosphate and soluble aluminum salt can be reasonably adjusted according to actual needs. Because aluminum dihydrogen phosphate and aluminum phosphate contain both phosphate and aluminum elements, in other embodiments of the present invention, one substance can be directly selected, such as any one of aluminum dihydrogen phosphate or aluminum phosphate for reaction.

[0059] In an optional embodiment of the present invention, the initial coating is heat treated at a temperature of 500° C. to 900° C. for a time of 2 h to 10 h.

[0060] Furthermore, the initial coating is heat treated at a temperature of 700°C-900°C and a time of 5h-6h.

[0061] The initial coating is heat treated to obtain the positive electrode material. It should be noted that the formation mechanism of the positive electrode material is as follows: aLi + +bM 2+ +cO 2- →xLi2MnO3·(1-x)LiMO2.

[0062] In a third aspect, an embodiment of the present invention provides a lithium-ion battery, which includes the positive electrode material as described above or the positive electrode material prepared by the preparation method as described above.

[0063] In a fourth aspect, an embodiment of the present invention provides a use of the positive electrode material as described above or the positive electrode material prepared by the preparation method as described above in the preparation of a lithium-ion battery.

[0064] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0065] Example 1

[0066] This embodiment provides a coated high-voltage lithium-rich manganese-based positive electrode material, and the preparation method thereof comprises the following steps:

[0067] (1) Lithium carbonate, a lithium source, and a metal precursor (Ni) were mixed in a molar ratio of 1.30:1. 0.3 Mn 0.6 Co 0.1CO3) was added into a high-speed mixer for mixing, and then sintered after mixing for 1 hour; the sintering process was as follows: heating to 600°C at a rate of 5°C / min and then keeping the temperature for 2 hours, then heating to 900°C at a rate of 2°C / min and then keeping the temperature for 8 hours, and finally cooling to room temperature at a rate of 100°C / h, and the sintered material was sieved to obtain a positive electrode material matrix;

[0068] The composition of the positive electrode material matrix is ​​0.3Li2MnO3·0.7LiNi 0.429 Mn 0.429 Co 0.143 O2 (also known as Li 1.3 Ni 0.3 Mn 0.6 Co 0.1 O 2.3 ).

[0069] (2) adding the cathode material matrix and deionized water into a stirring tank in a mass ratio of 1:5, and adding Al(H2PO4)3 into the stirring tank, wherein the molar ratio of Al(H2PO4)3 to the cathode material matrix is ​​0.0034:1;

[0070] The auxiliary agent lithium hydroxide is dissolved in deionized water and added to a stirring tank for stirring reaction. After the reaction is performed for 1 hour, the initial coating is obtained by filtration and dehydration. The molar ratio of lithium hydroxide to Al(H2PO4)3 is 9:1. The components of the initial coating are Al(OH)3 and Li3PO4.

[0071] (3) drying the initial coating and then heat treating it at a temperature of 850° C. for 5 h; cooling it after the heat treatment, and sieving it after cooling to obtain the positive electrode material;

[0072] The coating components on the surface of the positive electrode material are LiAlO2, Li3PO4 and LiAlP2O7.

[0073] Example 2

[0074] This embodiment provides a coated high-voltage lithium-rich manganese-based positive electrode material, and its preparation method is different from that of embodiment 1 in that:

[0075] (1) Lithium source lithium carbonate and metal precursor (Ni 0.3 Mn 0.6 Co 0.1 The molar ratio of CO3) is 1.10:1.

[0076] Example 3

[0077] This embodiment provides a coated high-voltage lithium-rich manganese-based positive electrode material, and its preparation method is different from that of embodiment 1 in that:

[0078] (1) Lithium source lithium carbonate and metal precursor (Ni 0.3 Mn 0.6 Co 0.1 The molar ratio of CO3) is 1.50:1.

[0079] Example 4

[0080] This embodiment provides a coated high-voltage lithium-rich manganese-based positive electrode material, and its preparation method is different from that of embodiment 1 in that:

[0081] (2) adding the cathode material matrix and deionized water into a stirring tank in a mass ratio of 1:3, and adding phosphate NH4H2PO4 and aluminum salt Al(NO3)3·9H2O into the stirring tank, wherein the molar ratio of the total amount of phosphate and aluminum salt added to the cathode material matrix is ​​0.0136:1; and the molar ratio of phosphate NH4H2PO4 and aluminum salt Al(NO3)3·9H2O is 1:2;

[0082] The auxiliary agent lithium hydroxide is dissolved in deionized water and then added to a stirring tank for stirring reaction. After the reaction for 1 hour, the initial coating is obtained by suction filtration and dehydration. The molar ratio of the total amount of lithium hydroxide to phosphate and aluminum salt is 3:1.

[0083] The components of the initial coating are Al(OH)3 and Li3PO4.

[0084] (3) drying the initial coating and then performing a heat treatment at a temperature of 700° C. for 6 h; cooling after the heat treatment, and sieving after cooling to obtain a positive electrode material;

[0085] The coating components on the surface of the positive electrode material are LiAlO2, Li3PO4 and LiAlP2O7.

[0086] Example 5

[0087] This embodiment provides a coated high-voltage lithium-rich manganese-based positive electrode material, and its preparation method is different from that of embodiment 1 in that:

[0088] (1) Lithium hydroxide, a lithium source, and a metal precursor (Ni) were mixed in a molar ratio of 1.35:1. 0.3 Mn 0.6 Co 0.1 CO3) was added into a high-speed mixer for mixing, and then sintered after mixing for 1 hour; the sintering process was as follows: heating to 500°C at a rate of 5°C / min and then keeping the temperature for 5 hours, then heating to 800°C at a rate of 2°C / min and then keeping the temperature for 10 hours, and finally cooling to room temperature at a rate of 100°C / h, and the sintered material was sieved to obtain a positive electrode material matrix;

[0089] The composition of the positive electrode material matrix is ​​0.3Li2MnO3·0.7LiNi 0.429 Mn 0.429 Co 0.143 O2 (also known as Li 1.3 Ni 0.3 Mn 0.6 Co 0.1 O 2.3 ).

[0090] (2) adding the cathode material matrix and deionized water into a stirring tank in a mass ratio of 1:8, and adding phosphate Na3PO4 and aluminum salt AlCl3 into the stirring tank, wherein the molar ratio of the total amount of phosphate and aluminum salt added to the cathode material matrix is ​​0.027:1; and the molar ratio of phosphate Na3PO4 and aluminum salt AlCl3 is 2:3;

[0091] The auxiliary agent lithium hydroxide is dissolved in deionized water and added into a stirring tank for stirring reaction. After the reaction for 1 hour, the initial coating is obtained by filtration and dehydration. The molar ratio of the total amount of lithium hydroxide added to the phosphate and aluminum salt is 8:1. The components of the initial coating are Al(OH)3 and Li3PO4.

[0092] (3) drying the initial coating and then heat treating it at a temperature of 850° C. for 5 h; cooling it after the heat treatment, and sieving it after cooling to obtain the positive electrode material;

[0093] The coating components on the surface of the positive electrode material are LiAlO2, Li3PO4 and LiAlP2O7.

[0094] Comparative Example 1

[0095] This comparative example provides a coated high-voltage lithium-rich manganese-based positive electrode material, and its preparation method is different from that of Example 1 in that:

[0096] (2) Adding the cathode material matrix and deionized water into a stirring tank in a mass ratio of 1:5, and adding nano-alumina powder into the stirring tank, the molar ratio of the nano-alumina powder to the cathode material matrix being 0.0017:1, stirring for 1 hour, and then filtering and dehydrating to obtain an initial coating.

[0097] (3) drying the initial coating and then heat treating it at a temperature of 850° C. for 5 h; cooling it after the heat treatment, and sieving it after cooling to obtain the positive electrode material;

[0098] The coating component on the surface of the positive electrode material is nano-aluminum oxide.

[0099] Test Example 1

[0100] In this test example, the powder resistance test of the coated high-voltage lithium-rich manganese-based positive electrode materials prepared in Examples 1-3 and Comparative Example 1 was carried out. The test instrument was a two-probe / four-probe powder material resistivity tester. The relevant parameter settings were a test temperature of 25°C and a sample cross section of 132.732 mm. 2 , holding time 10s, specific results are shown in Table 1.

[0101] Table 1

[0102]

[0103]

[0104] As can be seen from Table 1, the data of Examples 1-3 show that the powder resistance of the coated high-voltage lithium-rich manganese-based positive electrode material prepared in the examples shows a trend of first decreasing and then increasing as the molar ratio of the raw material lithium source lithium carbonate to the metal precursor increases; under different pressure conditions, the powder resistance of Example 1 is always low, and the powder resistance of Comparative Example 1 is larger than that of Example 1. Specifically, when the powder pressure is 200MPa, the coating raw material in Comparative Example 1 is changed to nano-alumina powder, and the powder resistance of the coated high-voltage lithium-rich manganese-based positive electrode material prepared therefrom is 359.9% higher than that of Example 1; when the powder pressure is 300MPa, the powder resistance of Comparative Example 1 is 459.8% higher than that of Example 1.

[0105] Test Example 2

[0106] In this test example, the high voltage lithium-rich manganese-based positive electrode materials prepared in Examples 1-3 and Comparative Example 1 were tested for rate performance and cycle stability under high voltage. The test instrument was a new well battery tester, and the relevant parameter settings were C2032 button batteries, 2-4.8V voltage range, rate test was 0.1C / 0.2C / 0.5C discharge, and cycle test was 1.0C discharge. Among them, the rate performance results are shown in Figure 1 The cyclic stability results are shown in Figure 2 .

[0107] from Figure 1 It can be seen that the data of Examples 1-3 show that with the increase of the molar ratio of the raw material lithium source lithium carbonate to the metal precursor, the rate performance of the prepared positive electrode material shows a trend of first increasing and then decreasing, and Example 1 has the best rate performance; compared with Comparative Example 1, Example 1 has better rate performance using synthetic aluminum sol than the nano alumina powder as the coated raw material, among which the 0.2C discharge capacity retention rate of Example 1 is about 2% higher than that of Comparative Example 1, and the 0.5C discharge capacity retention rate of Example 1 is about 3% higher than that of Comparative Example 1.

[0108] from Figure 2It can be seen that the data of Examples 1-3 show that with the increase of the molar ratio of the raw material lithium source lithium carbonate to the metal precursor, the cycle performance of the prepared positive electrode material shows a trend of first increasing and then decreasing. Example 1 has the best cycle performance, and the cycle capacity retention rate after 100 cycles of 1.0C discharge is 95.62%; compared with Comparative Example 1, Example 1 has better cycle stability using synthetic aluminum sol than the nano alumina powder as the coated raw material, among which the cycle capacity retention rate of Example 1 after 100 cycles of 1.0C discharge is 2.25% higher than that of Comparative Example 1.

[0109] Test Example 3

[0110] This test example tests the morphology of the coated high-voltage lithium-rich manganese-based positive electrode materials prepared in Example 1 and Comparative Example 1, using an electron microscope, the brand of which is a Hitachi scanning electron microscope. Figure 3 ,in Figure 3 (a) is the morphology test of Example 1, Figure 3 (b) is the morphology test of Example 1.

[0111] from Figure 3 It can be seen that the coating of Comparative Example 1 is point-shaped (local primary particles) coating, and the coating uniformity is poor, while Example 1 is surface coating, and the coating uniformity is good.

[0112] In summary, the coated high-voltage lithium-rich manganese-based positive electrode material provided by the embodiment of the present invention has a uniform surface coating, and the surface coating is a variety of Li-containing compounds, which have a synergistic effect on each other, effectively improving the Li + The diffusion performance is improved, thereby improving the cycle stability and rate performance of the material under high voltage. The preparation method provided by the present invention does not produce wastewater, is pollution-free, can achieve zero emission, and saves materials and reduces preparation costs. The coated high-voltage lithium-rich manganese-based positive electrode material prepared by the present invention can be used to prepare lithium-ion batteries and is widely used in the 3C field, new energy vehicle field and large-scale energy storage field.

[0113] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A coated high voltage lithium-rich manganese-based positive electrode material, characterized in that: The positive electrode material comprises a positive electrode material matrix and a coating on the surface of the positive electrode material matrix; The composition of the positive electrode material matrix is ​​xLi2MnO3·(1-x)LiMO2, 0.1≤x≤0.5, and M is selected from at least one of Ni, Mn and Co; The components of the coating include LiAlO2, Li3PO4 and LiAlP2O7.

2. A method for preparing a positive electrode material as claimed in claim 1, characterized in that: The preparation method comprises: The positive electrode material matrix, phosphate, aluminum salt, auxiliary agent and water are reacted in proportion to obtain an initial coating; The initial coating is heat treated to obtain the positive electrode material.

3. The preparation method according to claim 2, characterized in that: In the preparation method: After adding water to the positive electrode material matrix, phosphate and aluminum salt are added; Preferably, the mass ratio of the positive electrode material matrix to the water is 1:(1-10); Preferably, the molar ratio of the total amount of the phosphate and the aluminum salt added to the positive electrode material matrix is ​​(0.0001-0.1):1; Preferably, the molar ratio of the auxiliary agent to the total amount of the phosphate and the aluminum salt added is (1-13):

1.

4. The preparation method according to claim 2, characterized in that: The auxiliary agent includes lithium hydroxide; Preferably, the composition of the initial coating includes Al(OH)3 and Li3PO4.

5. The preparation method according to claim 2, characterized in that: The molar ratio of the phosphate to the aluminum salt is 1:(1-10); Preferably, the phosphate is selected from at least one of aluminum dihydrogen phosphate, ammonium dihydrogen phosphate, sodium phosphate and potassium phosphate; Preferably, the aluminum salt is selected from at least one of aluminum nitrate, aluminum chloride, aluminum sulfate, aluminum dihydrogen phosphate and aluminum phosphate.

6. The preparation method according to claim 2, characterized in that: The initial coating is heat treated at a temperature of 500°C-900°C for a time of 2h-10h; Preferably, the initial coating is heat treated at a temperature of 700° C.-900° C. for 5 h-6 h.

7. The preparation method according to claim 2, characterized in that: The preparation method of the positive electrode material matrix comprises the following steps: Mixing a lithium source and a metal precursor, and subjecting the mixture to sintering treatment to obtain the positive electrode material matrix; Preferably, the lithium source is selected from at least one of lithium hydroxide, lithium carbonate and lithium nitrate; Preferably, the metal precursor includes at least one of nickel, manganese and cobalt; Preferably, the molar ratio of the lithium source to the metal precursor is (1.10-1.50):1; Preferably, the lithium source and the metal precursor are mixed for at least 0.5 h.

8. The preparation method according to claim 7, characterized in that: The sintering process includes: heating to 300-650°C at a rate of 2°C / min-10°C / min, and keeping the temperature for 2h-10h; then heating to 800-1100°C at a rate of 1°C / min-2°C / min, and keeping the temperature for 5h-10h; and then cooling to room temperature at a rate of 80°C / h-120°C / h; Preferably, the sintering process includes: heating to 500-650°C at a rate of 5°C / min, and keeping warm for 2h-5h; then heating to 850-1000°C at a rate of 2°C / min, and keeping warm for 8h-10h; and then cooling to room temperature at a rate of 100°C / h.

9. A lithium ion battery, characterized in that: It includes the positive electrode material as claimed in claim 1 or the positive electrode material prepared by the preparation method as claimed in claims 2-8.

10. Use of the positive electrode material according to claim 1 or the positive electrode material prepared by the preparation method according to claims 2 to 8 in preparing a lithium ion battery.

Citation Information

Cited By

  • LiAlO2 coated lithium-rich manganese-based material as well as preparation method and application thereof