An oxygen barrier layer and a self-flattened dot digital flexible resin plate with a raised surface grained thereon
By using an oxygen barrier layer formed by the reaction of amine-containing water-soluble resin and water-based carboxyl-containing flexible resin in digital flexographic plates, the problems of insufficient photopolymerization and film defects under the influence of oxygen are solved, and higher printing transfer capabilities are achieved. and color reproduction effects, simplifying the plate making process and reducing equipment costs.
Patent Information
- Application Number
- CN202210110288.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-01-29
AI Technical Summary
The influence of oxygen during the main exposure period of existing digital flexographic plates leads to insufficient polymerization of the photopolymerized layer, resulting in fine dots and low edges. The coating method also has problems with dust interlayers and high equipment costs.
The amine-containing water-soluble resin and the water-based carboxyl-containing flexible resin are reacted in water to form a granular oxygen barrier layer, which is directly coated on the photosensitive elastomer to form raised surface roughness to improve the printing transfer ability and color restoration effect.
It achieves the flat-top shape of dots, improves the amount of printing transfer ink and color reproduction, simplifies the plate making process, and reduces equipment costs.
Smart Images

Figure CN114474959B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a digitally imageable flexographic printing plate, and in particular to an oxygen barrier layer and a self-flattened dot digital flexible resin plate with a raised surface graining comprising the oxygen barrier layer. This application belongs to the green printing material of the sub-direction 3.19 Ecological Environment Materials under the key direction of 3.1 New Functional Materials Industry in the catalog of strategic emerging industries. Background Art
[0002] Digitally imageable flexographic printing plates are generally known. They comprise at least one dimensionally stable support film, a photopolymerizable elastomer layer and a digitally imageable layer. Examples of digitally imageable layers include laser-ablatable layers, layers that can be written using an inkjet printer or thermal imaging layers, wherein laser-ablatable layers are currently popular in the digital flexographic market.
[0003] The laser ablatable layer, also called the LAMS (laser ablatable mask) layer, is opaque to ultraviolet light, visible light, and infrared light, and typically contains a binder and at least one IR absorber, such as carbon black. An IR laser is used to write an image into the laser ablatable layer by ablation—that is, in the portion of the LAMS layer hit by the laser beam, the film layer is ablated and decomposed to reveal the photopolymerizable layer. The laser ablatable mask layer can be placed directly on the photopolymerizable layer, or other layers, such as an oxygen barrier layer, can be provided between the photopolymerizable layer and the laser ablatable mask layer. Examples of making a printable flexographic plate from an unprocessed flexographic plate by IR ablation of the LAMS layer are described in US 5, 262,275, EP1,069,475, and CN 107969149 A.
[0004] The digital flexographic platemaking process is as follows: After the computer-controlled laser ablates the ablation mask layer to form an image, the plate is exposed to UVA radiation through the mask. The photopolymerizable layer is photopolymerized in the non-masked areas of the mask, while in the masked areas, there is no polymerization. After exposure, the remaining parts of the mask are removed together with the unpolymerized parts of the photopolymerizable layer. This removal can be carried out using one or more solvents or heat. If organic solvents are used, a drying step is added, and the resulting flexographic printing plate is also usually post-processed by exposure to UVA and / or UVC light. When the digital flexographic plate is exposed, it is usually carried out in air (in the presence of oxygen).
[0005] During the main exposure, the presence of oxygen has a considerable impact on fine dots, such as dots greater than 133lpi and less than 5%. For ordinary digital flexographic plates, 3% is usually difficult to develop, and 5% dots are far from the theoretical reduction area. As we all know, molecular oxygen can combine with free radicals. Due to the presence of molecular oxygen during the free radical polymerization initiated by UV light, oxygen can react with free radicals on the surface of the photopolymer layer. As a result, the photopolymerizable components of the flexographic plate are difficult to fully polymerize with each other due to the lack of free radicals. The lower area of the photopolymer layer surface is less affected because oxygen is not easy to reach. In the plate making and washing process after photopolymerization, the incompletely polymerized layer is removed, and the flexographic plate dots are therefore smaller than the area they should theoretically reach. From the perspective of a dot, the closer the area is to the edge, the fewer free radicals there are, and the easier it is to be consumed by oxygen, so the less fully polymerized, the easier it is to be washed away, and the result is that the dot is bullet-shaped, with a very sharp top, and the dot is high in the middle and low at the edge, that is, the dot is not flat-topped, but has an oblique angle. This effect is described, for example, in EP 2128 702 A1, page 15 Figure 1 middle.
[0006] If the destructive effect of oxygen on cross-linking polymerization is fundamentally eliminated, full polymerization of the photosensitive elastomer becomes possible, and the light-exposed parts from the inside of the plate to the surface can be effectively polymerized, so that finer details can be formed on the printing plate. In addition, the small dots with a flatter surface stand more stably and carry more ink. Therefore, it is best to shield the plate from oxygen during the main exposure so that the photopolymerization can be more complete.
[0007] A few years ago, DuPont invented exposure under inert gas (see US 8 241 835) or in a vacuum environment. Flint Group used high-power UVA light to expose flexographic plates (see EP 2 596 404). In this way, a large number of free radicals are formed in a short time, and the yield is sufficient to offset the effect of oxygen. These two methods require the addition of corresponding equipment to overcome the effect of oxygen. These methods are effective, but increase the cost of the platemaking center.
[0008] MacDermid, after the laser ablation film has been engraved and ablated, applies an oxygen-blocking film to the flexographic photosensitive elastomer to prevent the effect of oxygen on crosslinking polymerization during the main exposure, see US 2012 / 0164584. The patent describes applying a barrier layer by lamination after laser imaging and before UVA main exposure. The method of applying the coating is also mentioned.
[0009] Kodak, separately produces mask films, very similar to conventional films. The ablated imaged mask film is used as an original image to be laminated on a photosensitive elastomer for exposure and plate making. WO 2005 / 101130 Al discloses a multilayer mask for producing flexographic printing plates. The mask is imaged with a laser and then laminated to a flexographic photosensitive elastomer. The carrier of the mask acts as an oxygen barrier during subsequent exposure to UVA radiation.
[0010] However, lamination methods, such as MacDermid's method, where the digital flexo plate is ablated and then laminated. Kodak's method, where the imaged film is laminated to the flexo plate, have some drawbacks that are not easy to overcome. Lamination can cause defects, such as dust particles or air being trapped between the two during the lamination process. As we know, the slightest defect can make the flexographic printing plate useless. In addition, these lamination operations are performed by the platemaking center, so from the user's point of view, they are extremely unsatisfactory.
[0011] From the user's perspective, it is necessary to integrate an oxygen-blocking structural layer onto the plate. For this purpose, plate manufacturers have developed relevant technologies.
[0012] US 5, 262, 275 discloses a plate manufacturing technology containing an oxygen barrier layer, which sequentially comprises a carrier, a photopolymerizable layer, a barrier layer and a laser-ablative mask layer. The barrier layer can prevent the components of different layers from being mixed, such as the monomers migrating from the photopolymerizable layer to the laser-ablative layer, and protect the photopolymerizable layer during the exposure of the flexographic plate to prevent the quenching of free radicals by oxygen. The material of the barrier layer is polyamide, polyvinyl alcohol, hydroxyalkyl cellulose, ethylene-vinyl acetate copolymer, amphoteric copolymer and a combination thereof. The thickness of the barrier layer is 0.25µm to 76µm, preferably 0.38-64µm.
[0013] WO2012 / 145111Al has a similar structure to the flexographic plate. The material of the barrier layer recommended therein is polyamide, polyvinyl alcohol, hydroxyalkyl cellulose, polyvinyl pyrrolidone, ethylene-vinyl acetate copolymer, amphoteric copolymer, cellulose acetate butyrate, alkyl cellulose, butyral, cyclized rubber or a combination thereof. In addition, the barrier layer should have a thickness of less than 6.9×10 -9 m 2 / s oxygen diffusion coefficient and at least 50%, preferably at least 75% light transmittance. The barrier layer has a layer thickness of 1-100µm, preferably 1-20µm.
[0014] US8,492,074B2 describes a digitally imageable flexographic structure with a barrier layer comprising at least two different resins. The barrier layer is laminated after imaging, or it may already be present in the flexographic printing plate as an integrated component. The resin of the barrier layer is preferably selected from polyvinyl pyrrolidone, purple lacquer, polyvinyl butyral, polyvinylidene chloride or vinyl chloride copolymers.
[0015] In addition, other digitally imageable flexographic printing plates with integrated barrier layers are described in patents related to water-washable plates, which need to have a photopolymerizable layer that can be washed off in water or aqueous solutions. Therefore, the printing plate preferably contains a water-soluble or at least water-developable polymer as a binder for the barrier layer and the laser-ablatable mask layer:
[0016] EP 2284612 describes barrier layers comprising water-soluble polyamides, polyvinyl alcohol, polyacrylic acid, polyethylene oxide, cellulose and cellulose derivatives.
[0017] EP 1156368 describes a barrier layer comprising an alkali-soluble cellulose derivative with a plasticizer to make the layer flexible. However, water-washable flexographic printing plates have only limited use for high-quality flexographic printing because such plates swell in polar ink solvents, resulting in inconsistent print quality.
[0018] WO 2015 / 040094 describes a flexographic printing plate having a photopolymerizable layer soluble in an organic solvent, a water-soluble laser-ablatable mask layer and a water-soluble barrier layer. The preferred material for the oxygen barrier layer is a partially hydrolyzed polyvinyl acetate copolymer. However, the flexographic printing plate must be washed in two stages, first with water to remove the mask layer and the barrier layer, and then with a solvent to remove the unpolymerized photopolymerized layer. This requires a different plate washing device than usual, and therefore requires a higher cost.
[0019] CN107969149A solves the gradient adhesion required between the layers of the multi-layer flexographic printing plate. On the one hand, it ensures that the outer film is anchored on the laser-ablative mask layer, and on the other hand, before laser imaging, the outer film is removed without damaging the mask. When the outer film is removed, the laser-ablative mask layer and the oxygen barrier layer remain intact on the plate. In order to increase the ink carrying capacity of the plate, 2-6μm SiO2 and silicate fillers are added to the oxygen barrier layer, so that sand grains are formed on the surface of the raised part of the printing plate surface. Summary of the invention
[0020] In order to solve the above problems, the present invention provides an oxygen barrier layer and a self-flattened dot digital flexible resin plate with a grained surface of a raised portion thereof. The particles in the oxygen barrier layer are formed by reacting an amine-containing water-soluble resin with a carboxyl-containing polymer resin in water, that is, they are directly formed in the oxygen barrier layer coating liquid, eliminating the process of dispersing solid particles, so that the oxygen barrier layer contains particles. The oxygen barrier layer coating liquid is coated on a photosensitive elastomer, that is, a UV-polymerized relief-forming layer. The grained surface has a higher ability to transfer printing ink, and the ink layer of the printed matter is thicker and the color reproduction is more realistic.
[0021] The object of the present invention is achieved in the following manner: an oxygen barrier layer, the oxygen barrier layer contains particles of 0.01-10μm in size; the oxygen barrier layer is formed by coating and drying an oxygen barrier layer coating liquid, the raw materials of the oxygen barrier layer coating liquid are a flexible adhesive with oxygen barrier effect, an amine-containing water-soluble resin and an aqueous carboxyl-containing flexible resin, and in an aqueous solution containing a flexible adhesive with oxygen barrier effect, the amine-containing water-soluble resin and the aqueous carboxyl-containing flexible resin react to obtain particles of 0.01-10μm in size.
[0022] The present application utilizes an amine-containing water-soluble resin and an aqueous carboxyl-containing flexible resin to react in water to form particles, thereby eliminating the process of dispersing solid particles and achieving the inclusion of particles in the oxygen barrier layer. The size of the particles is controlled by filtering or the concentration of the dispersed material and the feeding speed and stirring speed of the two reaction components. The turbid liquid after the reaction is applied as a coating liquid, such as coating on a photosensitive elastomer, i.e., a UV-polymerized relief-forming layer. After drying, the particle shape is printed on the surface of the flexographic plate during the platemaking process, thereby increasing the roughness of the raised portion of the plate material and improving the ability of the plate material to transfer printing ink.
[0023] The oxygen permeability of the flexible adhesive with oxygen barrier effect is less than 500 (cm 3 ×100μm) / (m 2 ×d×bar).
[0024] The flexible adhesive having oxygen barrier effect is polyvinyl pyrrolidone.
[0025] Preferably, the polyvinyl pyrrolidone comprises two polyvinyl pyrrolidone with different K values, one with a K value less than or equal to 5000, and one with a K value greater than or equal to 10,000. The polyvinyl pyrrolidone with a small K value has a good oxygen barrier effect, and the polyvinyl pyrrolidone with a large K value has better film-forming properties.
[0026] Amine-containing water-soluble resins are also excellent adhesives, bonding elastomers and laser ablation masks together. However, the bonding force of amine-containing water-soluble resins is deeply affected by carbon dioxide, and the bonding ability of amine-containing water-soluble resin molecules that absorb carbon dioxide decays. In order to control the decay of bonding force within a certain period of time, more amine-containing water-soluble resin molecules are required. Therefore, the smaller the molecular weight of the amine-containing water-soluble resin, the more molecules of the same mass of amine-containing water-soluble resin, and the more carbon dioxide is absorbed. The penetration rate of carbon dioxide into the plate is limited. If there are enough amine-containing water-soluble resin molecules, there will be more amine-containing water-soluble resins that do not absorb carbon dioxide and maintain the original bonding force. Therefore, we prefer small molecular weight amine-containing water-soluble resins, which can ensure that a certain bonding force is maintained within a certain period of time. Preferably, the molecular weight of the amine-containing water-soluble resin is 1000-70,000. More preferably, the amine-containing water-soluble resin is preferably a low molecular weight polyethyleneamine or polyethyleneimine of 1000-5000.
[0027] The water-based carboxyl-containing flexible resin may be a carboxyl acrylic resin.
[0028] The oxygen barrier layer coating liquid also includes a leveling agent. The weight of polyvinyl pyrrolidone in the oxygen barrier layer is 50%-80%, the weight of water-based carboxyl-containing flexible resin in the oxygen barrier layer is 10%-30%, the weight of amine-containing water-soluble resin in the oxygen barrier layer is 5%-12.5%, and the weight of the leveling agent in the oxygen barrier layer is 5%-7.5%.
[0029] The preparation method of the oxygen barrier layer coating liquid comprises the following steps: dissolving a flexible adhesive having an oxygen barrier effect and an amine-containing water-soluble resin in water, slowly adding an aqueous solution of an aqueous carboxyl-containing flexible resin under stirring, and finally adding a leveling agent and stirring to obtain the oxygen barrier layer coating liquid; or dissolving a flexible adhesive having an oxygen barrier effect and an aqueous carboxyl-containing flexible resin in water, slowly adding an aqueous solution of an amine-containing water-soluble resin under stirring, and finally adding a leveling agent and stirring to obtain the oxygen barrier layer coating liquid.
[0030] Application of the oxygen barrier layer.
[0031] A self-flattened dot digital flexible resin plate with grained raised surface comprises the following from bottom to top: a structural layer, a support, a relief-forming layer capable of ultraviolet polymerization, an oxygen barrier layer, a laser-ablative mask layer and a removable protective film; the oxygen barrier layer is the oxygen barrier layer described above.
[0032] The thickness of the ultraviolet-polymerizable relief-forming layer is 0.6-7 mm, the thickness of the oxygen-barrier layer is 0.5-5 μm, and the thickness of the laser-ablative mask layer is 0.5-5 μm.
[0033] The thickness of the oxygen barrier layer is particularly preferably 1 μm to 2 μm.
[0034] Compared with the prior art, the particles in the oxygen barrier layer of the present application are formed by reacting an amine-containing water-soluble resin with a carboxyl-containing polymer resin in water, that is, they are directly formed in the oxygen barrier layer coating liquid, eliminating the process of dispersing solid particles, so that the particles are contained in the oxygen barrier layer. The oxygen barrier layer coating liquid is coated on a photosensitive elastomer, i.e., a UV-polymerized relief-forming layer. After drying, the particle shape is printed on the surface of the flexographic plate during the platemaking process, thereby increasing the roughness of the raised part of the plate and improving the ability of the plate to transfer printing ink. Moreover, by using the oxygen barrier layer of the present application, the cracks on the large solid and large dots of the flexible resin plate disappear. Instead, there are sand grains (fine pits) on the dots and solid. The sand grain surface has a higher ability to transfer ink, and the ink layer of the printed matter is thicker and the color reproduction is more realistic.
[0035] According to the common flexographic plate-making procedure, the printing plate is made, the dot form is a flat-top dot, the surface of the raised part of the plate image forms a grain, and the amount of transferred ink is increased during the printing of the plate. The plate comprises a support film; an organic solvent-soluble photopolymerizable layer; an organic solvent-soluble and dispersible oxygen barrier layer, a laser-ablable mask layer and a protective film. The characteristics of the flexographic printing plate of the present invention are that the raised part of the image has its own grain, and when the printing plate is processed, the processing method is simple and reliable, the made plate has a higher dot restoration quality, and the printed product has a higher restoration level. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the plate test result of Example 1. At 150lpi, without adding a correction curve, 2% dots can be restored to 0.5%.
[0037] Figure 2 This is the plate of Example 1, and a picture of the solid part under a 500x microscope. Some small micro-pits can be observed in the solid part under a 500x microscope.
[0038] Figure 3 This is the plate test result of Example 2, 1% dot profile at 150lpi without adding a correction curve.
[0039] Figure 4 This is a picture of the solid part of the plate of Example 2 under a 500x microscope. Some small micro-pits can be observed in the solid part under a 500x microscope. DETAILED DESCRIPTION
[0040] A self-flattened dot digital flexible resin plate with grained raised surface, comprising the following structural layers from bottom to top, a support (A), a photopolymerizable relief-forming layer (B), an oxygen barrier layer (C), a laser-ablative mask layer (D) and a removable protective film (E).
[0041] The following is a detailed description of each structural layer.
[0042] Support (A)
[0043] The flexographic plate of the present invention comprises a dimensionally stable carrier-support. A dimensionally stable carrier with a thickness of 50-300 μm is generally used, and its material includes steel, aluminum, alloy or plastic, such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate or polycarbonate. A PET film with a thickness of 100-200 μm is particularly suitable. In ordinary flexographic plates, a PET film with a thickness of 175 μm is used for plates with a thickness of 1.14 mm or less, and a PET film with a thickness of 125 μm is used for flexographic plates of other thicknesses.
[0044] The dimensionally stable carrier may be subjected to conventional adhesion treatment, such as corona treatment, chemical corrosion treatment, physical bonding, etc.
[0045] Photopolymerizable relief-forming layer (B)
[0046] The flexographic plate comprises at least a photopolymerizable relief-forming layer (B). Between the support and the relief-forming layer, there may be other layers, such as an adhesive layer or a layer for enhancing elasticity. The photopolymerizable relief-forming layer may also be a UV-polymerizable relief-forming layer.
[0047] The photopolymerizable projection-forming layer is of conventional structure, for example comprising at least an elastomeric binder, an ethylenically unsaturated compound, a photoinitiator or a photoinitiator system, and one or more other components, such as a plasticizer, a dye, a UV absorber, and the like.
[0048] Elastomeric binders are well known to those skilled in the art, such as styrene-diene block copolymers, natural rubber, polybutadiene, polyisoprene, styrene-butadiene rubber, nitrile rubber, butyl rubber, styrene-isoprene rubber, styrene-butadiene-isoprene rubber, polynorbornene rubber or ethylene-propylene-diene rubber. Preferably, the binder is soluble in non-polar hydrocarbon solvents and alcohols with medium polarity.
[0049] The elastomer preferably comprises a thermoplastic elastomer block copolymer of an alkenyl aromatic compound and a 1,3-diene, and the preferred elastomeric binder is a triblock copolymer of the A-B-A type or a radial block copolymer of the (AB)n type, wherein A is styrene and B is a diene, as well as statistical copolymers and random copolymers of styrene and diene. The total amount of the elastomeric binder is preferably 45-75% by weight; olefinically unsaturated double bond and polymerizable monomers, generally 3-15% by weight; at least one photoinitiator or photoinitiator system, preferably 3-6% by weight; plasticizers, modified and unmodified natural oils and natural resins, preferably 0-40% by weight. In addition, the relief-forming layer may contain surface-active substances, such as hydrophobic waxes or siliconized or perfluorinated compounds, as described in US 8,114,566. During the drying of the flexographic printing plate, these substances migrate from the relief layer to the surface, repel the printing ink, and reduce the accumulation of fine dots during printing, thereby reducing the frequency of having to clean the printing plate.
[0050] The thickness of the relief-forming layer is usually 0.1 to 7 mm, preferably 0.5 to 4 mm, more preferably 0.7 to 2.5 mm.
[0051] Oxygen barrier layer (C)
[0052] The oxygen barrier layer is arranged between the relief forming layer and the laser ablatable mask layer (D) that is ablated to form an image. The laser ablatable mask layer is a laser ablatable mask / laser ablatable black film. The oxygen barrier layer can bond the photosensitive elastomer layer (i.e., the relief forming layer) and the laser ablatable mask layer together. When the protective film (E) is removed, the laser ablatable mask / laser ablatable black film can be perfectly separated from the protective film and completely covered on the surface of the photosensitive elastomer. At the same time, when the laser ablatable mask / laser ablatable black film is laser ablated for imaging, the laser ablation does not damage the oxygen barrier layer. After the black film is ablated, the oxygen barrier layer still remains intact on the photosensitive elastomer.
[0053] The oxygen permeability of the oxygen barrier layer is usually less than 1000, preferably less than 500 (cm 3 ×100μm) / (m 2 × d × bar). For the barrier layer (C), in principle any flexible elastic adhesive can be used whose oxygen permeability is below an agreed maximum value and which meets other requirements, such as transparency to UVA light and solubility or dispersibility in commercially available flexographic processing media.
[0054] Flexible adhesives with oxygen barrier effect, such as polyvinyl pyrrolidone, are used in this patent. The K value of polyvinyl pyrrolidone is related to the viscosity of its aqueous solution. For the convenience of coating, it is necessary to select polyvinyl pyrrolidone with a suitable K value (the K value range is 1,000-70,000). Although its oxygen barrier performance is sufficient, it is difficult for pure polyvinyl pyrrolidone to perfectly bond the laser ablation black film and the photosensitive elastomer.
[0055] For this purpose, a basic adhesive component for increasing adhesion is also needed, which is an oligomeric or polymeric basic adhesive component - an amine-containing water-soluble resin.
[0056] The oxygen barrier layer contains polyvinyl pyrrolidone and amine-containing water-soluble resin, which can bond the laser ablation black film and the photosensitive elastomer well. However, it is strange that although the dots on the plate after plate making and washing are flat-top dots, there are crack-like shapes on the solid part of the plate or on the large dots. It is estimated that the oxygen barrier layer has cracks on a large area, that is, there is a problem with the flexibility of polyvinyl pyrrolidone.
[0057] To this end, this patent specifically introduces a flexible resin, a water-based carboxyl-containing resin, which is a carboxyl-containing flexible resin that itself has considerable softness. What is particularly surprising is that this substance can react with an amine-containing water-soluble resin to form fine particles. When the oxygen barrier layer acts as an adhesive to bond the laser ablation black film and the photosensitive elastomer together, these tiny particles form fine pits on the surface of the elastomer. After the plate is washed, a grainy surface is formed in the dots and solid parts. The ink transfer ability of the plate prepared according to this patent is significantly improved.
[0058] Incredibly, after adding the carboxyl-containing flexible resin, the cracks on the large solid and large dots disappeared. Instead, the grains (small pits) on the dots and solid appeared. The grain surface has a higher ability to transfer ink, and the ink layer of the printed matter is thicker and the color reproduction is more realistic.
[0059] The preparation method of the oxygen barrier layer coating liquid can be: dissolving a flexible adhesive having an oxygen barrier effect and an amine-containing water-soluble resin in water, slowly adding an aqueous solution of an aqueous carboxyl-containing flexible resin under stirring, and finally adding a surfactant and stirring to obtain an oxygen barrier layer coating liquid; or dissolving a flexible adhesive having an oxygen barrier effect and an aqueous carboxyl-containing flexible resin in water, slowly adding an aqueous solution of an amine-containing water-soluble resin under stirring, and finally adding a surfactant and stirring to obtain an oxygen barrier layer coating liquid.
[0060] Water is used as a solvent, and when it is coated on the photoreceptor to form an oxygen barrier layer, the water is evaporated.
[0061] The surfactant here is a leveling agent, which is a commonly used leveling agent for oxygen barrier layers and is used to adjust the tension for ease of coating.
[0062] The diameter of the particles in the oxygen barrier layer can be controlled by controlling the concentration of the dispersant (such as polyvinyl pyrrolidone), the reaction feed rate and the stirring speed, and finally by filtering the oxygen barrier coating liquid. Generally, it should be controlled below 10µm, preferably below 7µm. The roughness should be such that the details cannot be observed by the eyes. The most preferred range is 0.05-1µm.
[0063] The three main and indispensable components of the oxygen barrier layer of this patent are polyvinyl pyrrolidone, amine-containing water-soluble resin and water-based carboxyl-containing flexible resin. Examples of amine-containing water-soluble resins include polyethyleneimine and polyvinylamine; examples of water-based carboxyl-containing flexible resins include carboxyl acrylic resin.
[0064] Among them, in the weight of the entire oxygen barrier layer, polyvinyl pyrrolidone accounts for 50%-80% of the dry weight of the oxygen barrier layer, the water-based carboxyl-containing flexible resin accounts for 10%-30% of the dry weight of the oxygen barrier layer, the amine-containing water-soluble resin accounts for 5%-12.5% of the dry weight of the oxygen barrier layer, and the leveling agent accounts for 5%-7.5% of the dry weight of the oxygen barrier layer.
[0065] The thickness of the oxygen barrier layer is preferably 1μm-2μm. Although a thicker oxygen barrier layer can be more conducive to the perfection of oxygen barrier, the enlargement of the dots becomes a problem of the plate material. At the same time, a thicker oxygen barrier layer is easy to break at low temperatures. A thinner oxygen barrier layer does not block enough oxygen, and the cross-linking of small dots is partially affected by oxygen and cannot be restored well. Since the oxygen barrier layer cannot dissolve and swell too much in the plate washing solution, the less the better while ensuring the effect of oxygen barrier.
[0066] Laser ablative mask layer (D)
[0067] Laser ablation black film (also called laser ablation mask)
[0068] The laser ablation mask layer is located between the oxygen barrier layer and the protective film of the plate.
[0069] The film layer can absorb infrared laser and be ablated by laser. For example, the 830nm and 1064nm laser imaging machines currently on the market can perform laser ablation imaging on it to become a mask.
[0070] On the one hand, the film layer can absorb infrared laser and burn, and on the other hand, the film layer must have sufficient blocking effect on ultraviolet rays. During the plate making process, under UVA exposure, the photosensitive elastomer covered by the black film will not undergo cross-linking and polymerization.
[0071] The film layer should also be soluble or dispersed in commercially available plate washing liquids.
[0072] The laser ablation mask layer is a conventional laser ablation mask in the prior art.
[0073] The main components of the laser ablation mask layer include:
[0074] At least one component capable of absorbing infrared rays and being ablated by infrared rays is carbon black, including various forms of carbon black, such as carbon black, graphite, carbon nanoparticles, carbon nanotubes, etc. Among them, carbon nanoparticles are most preferred.
[0075] Very suitable flexible elastic binders for the mask layer are, for example, ethylene vinyl acetate, flexible elastic polyamides, flexible elastic polyurethanes, polyvinyl pyrrolidone (PVP), nitrocellulose, polyvinyl acetals such as poly (vinyl butyral-vinyl alcohol) copolymers (Butvar®, Mowital®) or poly (vinyl butyral-vinyl acetal-vinyl alcohol) copolymers (Pioloform®). Of course, other flexible elastic materials can also be used as binders, such as partially hydrolyzed polyvinyl acetate. A preferred binder for the mask layer is the flexible elastic polyamide Technomelt® PA6900.
[0076] The amount of absorbing material is generally such that the optical density of the layer to UVA radiation is 1-5. The UVA radiation range includes light having a wavelength of 300-400 nm. The optical density is the logarithmic coefficient of the light permeability of the layer within this wavelength range. Therefore, when measuring the optical density, the value determined is not a single value of light permeability at a specific wavelength, but an average value of light permeability within a specified wavelength range. The optical density is usually measured using a commercially available densitometer (e.g. from x-rite), wherein the wavelength range is selected before the measurement. For the purposes of the present invention, all quoted optical density measurements are based on the UVA range, i.e. the range of 300-400 nm.
[0077] The preferred mask layer has an optical density of 2-5. The high optical density ensures that the areas of the photosensitive elastomer covered by the mask do not polymerize during exposure to UVA light. Suitable light-absorbing materials include in particular carbon black, graphite, carbon black nanoparticles or carbon nanotubes. These materials absorb very well in the near IR range and are therefore both laser-ablative and UV-blocking materials. The amount of such material used in the entire mask layer is in the range of 10% to 60% by weight, preferably 20% to 40%. The weight of the mask layer is 2-5 g / m 2 , preferably 2-4g / m 2 When it is within this range, the ablation energy is about 3.0-4.5J / cm 2, which can be well suited to the flexographic laser ablation imaging machine on the market and make the laser ablation imaging machine work in a normal state and with appropriate efficiency.
[0078] Protective film (E)
[0079] As the top layer of the plate material, the flexographic printing plate of the present invention comprises a removable protective film / outer film, the purpose of which is to protect the flexographic printing plate. It is removed before laser ablation imaging. The material of the removable protective film / outer film can be a PET film. The thickness is 80-150 μm, preferably 100-130 μm, and the average roughness value (Ra) is preferably 0.02-0.5 μm. This film material can be transparent or semi-opaque. Generally, the film material preferably has a certain degree of haze to facilitate the distinction between the two sides of the plate material.
[0080] The UV-polymerizable relief-forming layer, the oxygen-barrier layer, and the laser-ablative mask layer can be dissolved or dispersed in popular flexographic plate-washing liquids on the market, such as Minchen plate-washing liquid, a plate-washing liquid mixed with n-butanol and tetrachloroethylene, and the like.
[0081] Production of the flexographic printing plate of the present invention
[0082] The flexographic printing plate of the present invention is prepared in a manner known in principle by melting the components of the photopolymerizable layer in an extruder, mixing them and discharging the melt of the photopolymerizable material through a slot die into the gap of the rollers of a calender. On one calendering roller runs a support film, which is optionally coated with other layers, such as an adhesive layer, and via another calendering roller runs a prefabricated outer film comprising a laser ablation mask and an oxygen barrier layer. The outer film comprising a dimensionally stable support, a photopolymerizable layer and an oxygen barrier layer and a laser ablation mask layer is combined together by calendering.
[0083] In the production of the outer film assembly, a laser-ablatable mask layer is first applied to the outer film. The coating procedure can be carried out from a solution, a melt or by spraying. The laser-ablatable mask layer is then covered with an oxygen barrier layer. Before the application of the subsequent layers, it may be necessary to partially treat the surface of the PET substrate to be coated, for example by corona treatment, in order to achieve a greater spreading capacity. It must be noted that the effect of the corona pretreatment generally decreases with the storage time of the printing plate and does not achieve permanent satisfactory adhesion.
[0084] Alternatively, each layer may be applied to different films and then laminated together. For example, the mask layer and the oxygen barrier layer may be applied to one film each. In this case, the mask layer is applied to the outer film, and the oxygen barrier layer is applied to the temporary auxiliary film. After the coating, the two films are laminated to each other by lamination, and the temporary auxiliary film is removed.
[0085] The techniques for coating are known to the person skilled in the art. The thickness of the layer to be applied can be adjusted in a manner known in principle by diluting the coating solution or by varying coating parameters, such as the knife gap or the coating speed or the feed rate. To improve the coating quality, it may be necessary to add surface-active substances or flow control aids to the coating solution.
[0086] The coated outer film is rolled up and passed through one of the calender rolls during the subsequent extrusion and in this way firmly bonded to the photosensitive elastomer as a whole plate.
[0087] Alternatively, a layer-by-layer lamination process can be used in multiple steps. For example, the oxygen barrier layer contained on the temporary auxiliary film can be passed through a calender and combined with the photopolymerizable layer. The auxiliary film is then removed. Then, in a second lamination step, the laser-ablatable mask layer is laminated with the photosensitive elastomer laminated with the oxygen barrier layer to form a plate.
[0088] Process of processing the plate material of the present invention into a flexographic printing plate
[0089] The plate making process includes the following method steps 1-7:
[0090] 1. Back-expose the plate to form a suitable base. This step can also be performed after step 4.
[0091] 2. Remove the outer film. Simply remove the protective layer, and the laser-ablative mask layer and the underlying oxygen barrier layer will still remain intact on the UV-polymerizable relief-forming layer / photosensitive elastomer;
[0092] 3. Use IR laser to image on the laser-ablative mask layer. Such laser imaging machine is also called CDI. There are two types of machines on the market: 1064nm and 830nm.
[0093] 4. UVA light is used to expose and image the photosensitive elastomer through a mask. It can be either a common UVA lamp or the latest UV LED lamp beads;
[0094] 5. Use a flexographic plate washing liquid to remove the remaining portion of the laser-ablative mask layer, the oxygen barrier layer and the unpolymerized portion of the photosensitive elastomer. The plate washing liquid can be a well-known solution of tetrachloroethylene and n-butanol mixed in a volume ratio of 3 to 1, or various environmentally friendly plate washing liquids commonly found on the market;
[0095] 6. Fully dry the obtained flexographic printing plate;
[0096] 7. Post-exposure to UVA and de-sticking to UVC, or skip this step.
[0097] After the above plate-making process, the plate material becomes a flexographic plate that can be printed. This plate-making process is exactly the same as that of ordinary digital flexographic plates.
[0098] When using the flexographic plate of the present invention, there is no need for expensive and inconvenient exposure conditions such as nitrogen filling, expensive and inconvenient film lamination of the imaged laser ablation mask, or lamination of the imaged film onto a photosensitive elastomer through a laminating device.
[0099] Alternatively, the flexographic plate of the present invention can also be thermally developed. In this case, the flexographic plate is mounted on a drum and heated from the surface until melting occurs. A strip of fabric is then pressed against the flexographic plate to remove the unexposed areas of the photosensitive elastomer, the barrier layer, and the remnants of the laser-ablatable mask layer. This operation is repeated multiple times until the desired relief height is achieved.
[0100] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that this embodiment is only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Technical personnel skilled in the art can make some non-essential improvements and adjustments based on the above-mentioned contents of the present invention.
[0101] Example 1
[0102] This patent is realized by adding an oxygen barrier functional layer on the basis of a digital flexographic plate, and the technology involved in the digital flexographic plate is omitted.
[0103] In the preparation of the oxygen barrier coating liquid, the following ingredients have a total weight of 80 grams and are prepared from the following raw materials in terms of dry weight percentage:
[0104] Polyvinylpyrrolidone K30, commercially available, 80%;
[0105] PD-2000, a water-soluble resin containing amine groups with a molecular weight of 2000, from Lucky Chemical Company, 10%;
[0106] Carboxyl-containing flexible resin SR, from Lucky Chemicals, 5%;
[0107] Surfactant—Perfluorobutyl yellow yl fluoride, 5%.
[0108] In addition to the above ingredients,
[0109] Water, 920 g.
[0110] The preparation method of the oxygen barrier coating liquid is as follows: polyvinyl pyrrolidone and SR resin are dissolved in water, PD-2000 aqueous solution is slowly added under high-speed stirring (1000-2000 rpm), and finally a surfactant is added, and after proper stirring, the oxygen barrier coating liquid is obtained. The SR resin and PD-2000 resin can also be exchanged without affecting the properties of the oxygen barrier coating liquid.
[0111] Apply the oxygen barrier coating liquid to the Huaguang DR170LS photosensitive elastomer through a No. 20 wire rod, and then press the black film on the oxygen barrier layer; or apply it on the black film and then press it on the Huaguang DR170LS photosensitive elastomer. Stay at a temperature of 100-120℃ for five minutes. Cool to room temperature to make a plate.
[0112] Then, make the plate like a normal digital flexible resin plate. For example, after back exposure, remove the film base on the black film, laser image on ESKO's CDI, expose for 15 minutes on a Kemao exposure machine with a normal UVA lamp (LED lamp bead main exposure results are better), wash the plate on a Kemao normal inline plate washer at 160mm / min (or on a platform plate washer), use the commercially available Minchen environmentally friendly plate washing liquid (or perchloroethylene plate washing liquid, the volume ratio of perchloroethylene to n-butanol is 3:1, if the ratio of perchloroethylene is too large, there may be problems with not washing cleanly). After baking the plate, post-exposure and detackification.
[0113] Test the plate.
[0114] like Figure 1 As shown in the figure, at 150lpi, without adding a correction curve, 2% dots can be restored to 0.5%, and some small pits can be observed in the solid part under a 500x microscope, such as Figure 2 shown.
[0115] The surface tension of the solid part was tested. The same photosensitive elastomer, without oxygen barrier layer, would not form micro-cells, and the surface tension was 38mN / m. After adding oxygen barrier layer, micro-cells were formed, and the surface tension was 42mN / m.
[0116] The actual printing test shows that the ink density on the substrate is satisfactory, and all meet and exceed the national standard for three-color printing ink color requirements. The color control of three-color printing can be achieved.
[0117] Example 2
[0118] In the preparation of the oxygen barrier coating liquid, the following ingredients have a total weight of 80 grams and are prepared from the following raw materials by weight percentage:
[0119] Polyvinylpyrrolidone K90, commercially available, 50%;
[0120] PD-70000 resin, a water-soluble resin containing amino groups with a molecular weight of 70,000, from Lucky Chemicals, 30%;
[0121] Carboxyl-containing flexible resin SR, from Lucky Chemicals, 12.5%;
[0122] Surfactant—Perfluorobutyl yellow yl fluoride, 7.5%.
[0123] In addition to the above ingredients,
[0124] Water, 920 g.
[0125] The preparation method of the oxygen barrier coating liquid is as follows: dissolve polyvinyl pyrrolidone and SR water together, slowly add PD-70000 aqueous solution under high-speed stirring (1000-2000 rpm), and finally add surfactant, and after proper stirring, the oxygen barrier coating liquid is obtained. The SR resin and PD-70000 resin can also be exchanged without affecting the properties of the oxygen barrier coating liquid.
[0126] Apply the coating liquid of the oxygen barrier layer to the Huaguang DR170LS photosensitive elastomer through a No. 20 wire rod, and then press the black film (supplement the model and manufacturer of the black film) on the oxygen barrier layer; or apply it on the black film and then press it on the Huaguang DR170LS photosensitive elastomer. Stay at a temperature of 100-120℃ for five minutes. Cool to room temperature to make a plate.
[0127] Then, make the plate like a normal digital flexible resin plate. For example, after back exposure, remove the film base on the black film, laser image on ESKO's CDI, expose for 15 minutes on a normal UVA lamp tube of Kemao's exposure machine (LED lamp bead main exposure results are better), wash the plate on a normal inline plate washer of Kemao at 160mm / min (or on a platform plate washer), use the commercially available Minchen environmentally friendly plate washing liquid (or perchloroethylene plate washing liquid, the volume ratio of perchloroethylene to n-butanol is 3:1, if the ratio of perchloroethylene is too large, there may be problems with not washing cleanly). After baking, post-exposure and detackification.
[0128] Test the plate.
[0129] like Figure 3 As shown in the figure, at 150lpi, without adding a correction curve, 1% of the dots can be restored to 0.5%, and some small pits can be observed in the solid part under a 500x microscope, such as Figure 4 shown.
[0130] The surface tension of the solid part was tested. The same photosensitive elastomer, without oxygen barrier layer, would not form micro-cells, and the surface tension was 38mN / m. After adding oxygen barrier layer, micro-cells were formed, and the surface tension was 42mN / m.
[0131] The actual printing test shows that the ink density on the substrate is satisfactory, and all meet and exceed the national standard for three-color printing ink color requirements. The color control of three-color printing can be achieved.
[0132] The above description is only a preferred embodiment of the present invention, but the protection scope of the present invention is not limited thereto. It should be pointed out that for those skilled in the art and any technician familiar with the technical field, without departing from the overall concept of the present invention, the technical solution and the inventive concept of the present invention are equivalently replaced or changed, and several changes and improvements are made, which should also be regarded as the protection scope of the present invention.
Claims
1. An oxygen barrier layer, characterized in that: The oxygen barrier layer contains particles with a size of 0.01-10 μm; the oxygen barrier layer is formed by coating and drying an oxygen barrier layer coating liquid, the raw materials of which are a flexible adhesive with an oxygen barrier effect, an amine-containing water-soluble resin, a water-based carboxyl-containing flexible resin and a leveling agent, the flexible adhesive with an oxygen barrier effect is polyvinyl pyrrolidone, the amine-containing water-soluble resin is a polyethylene amine or polyethylene imine with a molecular weight of 1000-5000, and the water-based carboxyl-containing flexible resin is a carboxyl acrylic resin; The oxygen barrier layer coating liquid is prepared by any of the following two methods: The first method is prepared by the following steps: polyvinyl pyrrolidone and an amine-containing water-soluble resin are dissolved in water, and an aqueous solution of a water-based carboxyl-containing flexible resin is slowly added under stirring, and finally a leveling agent is added and stirred to obtain an oxygen barrier coating liquid; The second method is prepared by the following steps: polyvinyl pyrrolidone and water-based carboxyl-containing flexible resin are dissolved in water, and an aqueous solution of an amine-containing water-soluble resin is slowly added under stirring, and finally a leveling agent is added and stirred to obtain an oxygen barrier coating liquid; In the aqueous solution containing polyvinyl pyrrolidone, the amino-containing water-soluble resin and the aqueous carboxyl-containing flexible resin react to obtain particles with a size of 0.01-10 μm.
2. The oxygen barrier layer according to claim 1, characterized in that: The oxygen permeability of the flexible adhesive with oxygen barrier effect is less than 500 (cm 3 ×100μm) / (m 2 ×d×bar).
3. The oxygen barrier layer according to claim 1, characterized in that: The weight of polyvinyl pyrrolidone in the oxygen barrier layer is 50%-80%, the weight of water-based carboxyl-containing flexible resin in the oxygen barrier layer is 10%-30%, the weight of amine-containing water-soluble resin in the oxygen barrier layer is 5%-12.5%, and the weight of leveling agent in the oxygen barrier layer is 5%-7.5%.
4. The oxygen barrier layer according to claim 1, characterized in that: The K value of polyvinyl pyrrolidone ranges from 1,000 to 70,000.
5. The oxygen barrier layer according to claim 4, characterized in that: The polyvinyl pyrrolidone comprises two polyvinyl pyrrolidone with different K values, one with a K value less than or equal to 5000, and the other with a K value greater than or equal to 10000.
6. Use of the oxygen barrier layer according to any one of claims 1 to 5.
7. A self-flattened dot digital flexible resin plate with grained raised surface, comprising, from bottom to top, the following structural layers, a support, a UV-polymerizable relief-forming layer, an oxygen barrier layer, a laser-ablative mask layer, and a removable protective film; characterized in that: The oxygen barrier layer is the oxygen barrier layer described in any one of claims 1 to 5.
8. The self-flattened dot digital flexible resin plate with grained raised surface according to claim 7, characterized in that: The thickness of the ultraviolet-polymerizable relief-forming layer is 0.6-7 mm, the thickness of the oxygen-barrier layer is 0.5-5 μm, and the thickness of the laser-ablative mask layer is 0.5-5 μm.
9. The self-flattened dot digital flexible resin plate with grained raised surface according to claim 7, characterized in that: The thickness of the oxygen barrier layer is 1 μm-2 μm.