A high-thickness and high-strength light-cured silicon nitride ceramic and a preparation method thereof
By using the low-temperature pore-forming agent PEG in the silicon nitride ceramic paste to form holes and the cracking process, the problems of uneven density and cracking deformation in the molding of silicon nitride ceramics are solved, and the preparation of high-thickness and high-strength ceramics is achieved with maximum degreasing Thickness and strength are significantly improved.
Patent Information
- Application Number
- CN202011272964.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-11-13
AI Technical Summary
Existing silicon nitride ceramic molding methods have problems such as uneven density, difficulty in forming complex shapes, poor dimensional accuracy of finished products, high preparation costs, and high reliance on molds. In particular, cracking, deformation, and deformation are prone to occur during the degreasing and sintering process of high-thickness ceramic green bodies. Thermal expansion.
The low-temperature pore-forming agent PEG is used to form spherical holes in the ceramic paste, and the internal stress is gradually released through the cracking and carbon removal process to improve the degreasing thickness and efficiency. The uniform mixing of the powder and resin is ensured by multiple additions of powder and resin. Full wetting and uniformity to avoid heat curing and cracking.
Achieving high thickness and high strength of light-cured silicon nitride ceramics, the maximum degreasing thickness is increased to 8mm, the degreasing rate reaches 99%, and the high strength is maintained at 1400°C. The maximum three-point bending strength at room temperature is 480MPa, and the maximum compressive strength is 540MPa. .
Smart Images

Figure CN114478049B_ABST
Abstract
Description
[Technical field]
[0001] The invention belongs to the technical field of additive manufacturing and relates to a high-thickness and high-strength photocured silicon nitride ceramic and a preparation method thereof. [Background technology]
[0002] Silicon nitride ceramic components are widely used in the fields of machinery, chemical industry and automobile, such as silicon nitride ceramic gears, turbine rotors, cutting tools and bearings. At present, the forming methods of silicon nitride ceramic components include cold isostatic pressing, dry pressing, slip injection and hot die casting. Among them, although the dry pressing method is more efficient, the formed products have density differences and uneven microstructures, and it is not easy to form complex shapes and special-shaped products; the cold isostatic pressing method can obtain high-density and high-uniformity formed blanks, but it is still difficult to form ceramic parts with complex shapes, and the forming efficiency is low and there are many manual operations; although slip injection molding can form special-shaped products to achieve near-net size, the formed blanks are prone to uneven density and component segregation, as well as low forming dimensional accuracy and reduced product reliability. In addition, the molding method requires manual operation and the blank drying efficiency is low; in the prior art, the silicon nitride ceramic blanks mainly have the following technical defects: uneven finished products, poor dimensional accuracy of products after sintering, high preparation cost and high dependence on the forming mold, which limits the preparation of special-shaped silicon nitride ceramic structural parts.
[0003] Silicon nitride ceramics formed by photocuring have high precision and do not require molds, which can easily achieve personalized customization of the structure. However, since the photocuring green body contains a certain volume fraction of cured photosensitive resin, it needs to be thermally degreased due to its large internal stress, that is, the binder component is volatilized or decomposed by heating the green body to remove it from the green body. During thermal degreasing, the binder component is softened by heat, and the green body is prone to viscous flow deformation under the action of gravity and thermal stress, so the degreasing rate is too slow and time-consuming. The control of furnace temperature in the thermal degreasing process is also very strict, and it must be consistent with the volatilization and pyrolysis of the components. At the same time, thermal degreasing has size and thickness restrictions, which is suitable for relatively small precision ceramic parts. Thermal expansion is prone to occur during the thermal degreasing process, causing cracking and deformation of the green body, and limiting the degreasing and sintering of high-thickness ceramic green bodies.
[0004] As attached Figure 1 The photocured silicon nitride sample shown is a common sample in the prior art, with a size of 80 mm×20 mm (end)×2.5 mm, a green body degreased thickness of only 2.5 mm, and a maximum bending strength of only about 333 MPa. [Summary of the invention]
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a high-thickness and high-strength photocured silicon nitride ceramic and a preparation method thereof, so as to overcome the problems existing in the process of preparing photocured silicon nitride ceramics by degreasing and sintering method in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing high-thickness and high-strength light-cured silicon nitride ceramics comprises the following steps:
[0008] Step 1, mixing Si3N4 powder, Y2O3 powder, Al2O3 powder and SiO2 powder to form mixed powder A; adding stearic acid to the mixed powder A and performing dry grinding modification to obtain mixed powder B; adding dispersant 9063 and silane coupling agent KH560 to the mixed powder B, performing wet grinding modification to obtain slurry C, drying the slurry C and sieving it to obtain a premixed powder;
[0009] Step 2, mixing polyurethane, bisphenol A, IBOMA, HDDA, TPGDA, TMPTA, DPHA and fluorenyl acrylic acid and their composite glue, stirring to obtain a mixed resin D, adding TPO to the mixed resin D, and then adding the premixed powder several times until the premixed powder is completely wetted by the mixed resin D, then adding polyethylene glycol 400, and then mixing through three stages of mixing to obtain a ceramic paste;
[0010] Step 3, adding the ceramic paste to the printer after vacuum degassing, and generating a ceramic green body after printing;
[0011] Step 4, cracking, decarbonizing and sintering the ceramic green body to obtain silicon nitride ceramics.
[0012] A further improvement of the present invention is:
[0013] Preferably, in step 1, the mass fraction of Si3N4 powder in the mixed powder A is 67%, the mass fraction of Y2O3 powder is 5%, the mass fraction of Al2O3 powder is 3%, and the mass fraction of SiO2 powder is 25%.
[0014] Preferably, in step 1, the amount of stearic acid added is 3% of the mass of the mixed powder A, the amount of dispersant 9063 added is 3% of the mass of the mixed powder B, and the amount of silane coupling agent KH560 added is 8% of the mass of the mixed powder B.
[0015] Preferably, in step 1, the dry grinding time is 20 h, the wet grinding time is 20 h, and the drying temperature of slurry C is 75°C.
[0016] Preferably, in step 2, in the mixed resin D, the mass fraction of polyurethane is 3.7%, the mass fraction of bisphenol A is 8.65%, the mass fraction of IBOMA is 3.7%, the mass fraction of HDDA is 6.71%, the mass fraction of TPGDA is 5.05%, the mass fraction of TMPTA is 22.34%, the mass fraction of DPHA is 22.61%, and the mass fraction of fluorenyl acrylic acid and its composite glue is 27.24%;
[0017] The amount of TPO added is 5% of the mass of the mixed resin D, and the mixing mass ratio of the premixed powder to the mixed resin D is 3:1; after the addition of polyethylene glycol 400, the viscosity of the ceramic paste is ≥500 Pa·s.
[0018] Preferably, in step 2, the mixing process parameters of the three stages are as follows: the rotation speed of the first stage is 1000-1500 rpm, the time of the first stage is 10-15s, the rotation speed of the second stage is 1800-2200 rpm, the time of the second stage is 15-25s, the rotation speed of the third stage is 2200-2800 rpm, and the time of the third stage is 25-35s.
[0019] Preferably, the heating parameters of the cracking process are: maintaining at 200°C for 180 min, maintaining at 200°C for 60 min, maintaining at 300°C for 200 min, maintaining at 300°C for 120 min, maintaining at 350°C for 100 min, maintaining at 350°C for 180 min, maintaining at 410°C for 200 min, maintaining at 410°C for 240 min, maintaining at 450°C for 200 min, maintaining at 450°C for 240 min, maintaining at 500°C for 100 min, maintaining at 500°C for 240 min, maintaining at 550°C for 100 min, maintaining at 550°C for 180 min, maintaining at 600°C for 50 min, maintaining at 600°C for 100 min, maintaining at 800°C for 200 min, and maintaining at 800°C for 60 min.
[0020] Preferably, the heating parameters of the decarburization process are: raising the temperature of the green body to 600°C within 300 minutes, then maintaining it at 600°C for 200 minutes, then raising the temperature of the green body to 800°C within 100 minutes, maintaining the green body at 800°C for 100 minutes, and then slowly cooling it to room temperature.
[0021] Preferably, the sintering process is as follows: the temperature is raised from room temperature to 1200°C at 5°C / min, the temperature is raised to 1750°C at 4°C / min, and the temperature is kept at 1750°C for 2 hours and then cooled with the furnace.
[0022] A photocured silicon nitride ceramic prepared by the above preparation method, characterized in that the photocured ceramic has a maximum three-point bending strength of 480MPa and a maximum compressive strength of 540MPa at room temperature; the three-point bending strength of the photocured silicon nitride ceramic at 1400°C is 110MPa.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention discloses a method for preparing high-thickness and high-strength photocured silicon nitride ceramics. During the preparation process, a low-temperature pore-forming agent PEG is added to the ceramic paste, so that in the later degreasing process, the maximum degreasing thickness of the silicon nitride ceramic is increased to 8 mm, and the degreasing time is only 60 hours, and the degreasing rate can reach more than 99%. The present invention first performs polymer cracking and low-temperature pore-forming agent removal under an argon atmosphere by taking advantage of the characteristics that PEG volatilizes at 200-300°C and leaves spherical holes, wherein the latter can be almost completely removed at 300°C, providing a channel for the subsequent escape of small molecules. This process leaves a channel in the green body in advance during the degreasing process of the ceramic green body, which is beneficial to the subsequent high-temperature removal of the photosensitive resin (avoiding cracking and deformation, and increasing the limit degreasing thickness). The photosensitive resin generally used for ceramic paste solidifies by cross-linking reaction under the action of laser and photoinitiator. In this process, a large amount of internal stress accumulates inside the green body. Degreasing is to remove the above resin under the premise of releasing this stress. If degreasing is performed directly, the cured photosensitive resin will crack and oxidize rapidly, and the ceramic green body will crack and deform. Therefore, the two-step degreasing method of first cracking and then oxidation is adopted. In addition, in the cracking process, since any decomposition product of PEG is volatile, no hard shell or straw mud sediment will be generated, and it can be completely volatilized at 300℃, it is very suitable as a low-temperature pore-forming agent to leave a channel in the ceramic green body in advance, which is convenient for the removal of the cured photosensitive resin without deformation and cracking. In the preparation process of the ceramic paste, in order to improve the uniformity of the powder and the resin, the method of adding ceramic powder to the resin solution one by one is adopted, which can also avoid the partial thermal curing of the paste due to the difficulty in discharging the heat generated during the rotation process due to the addition of too much powder at a single time. By adding the premixed powder several times, the premixed powder can be fully wetted.
[0025] Furthermore, the mixing process is divided into multiple times to make the mixing more uniform. In addition, the number of times the ceramic powder is added to the mixed resin ranges from 4 to 6 times.
[0026] The present invention also discloses a high-thickness and high-strength photocured silicon nitride ceramic prepared by the above-mentioned preparation method. The photocured ceramic has a maximum three-point bending strength of 480 MPa and a maximum compression strength of 540 MPa at room temperature; the three-point bending strength of the photocured silicon nitride ceramic at 1400°C is 110 MPa.
Brief Description of the Drawings
[0027] Figure 1 This is a diagram of a silicon nitride sample prepared in the prior art;
[0028] Among them, (a) is a real picture; (b) is a size sample picture;
[0029] Figure 2 This is a diagram showing the working principle of the low-temperature pore-forming agent PEG of the present invention;
[0030] Figure 3 Figure 1 is a diagram of the degreasing process; (a) is a diagram of the cracking process; (b) is a diagram of the carbon removal process;
[0031] Figure 4 This is a process diagram of silicon nitride sintering process;
[0032] Figure 5 This is a physical picture of the prepared silicon nitride ceramic;
[0033] Among them, (a) is the printed green body; (b) is the sintered body; (c) is the sintered body with a thickness of 8 mm;
[0034] Figure 6 TG-DSC curve of silicon nitride SLA printed green body under argon. [Specific implementation method]
[0035] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0036] In the description of the present invention, it should be noted that the orientations or positional relationships indicated by the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. are based on the orientations or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention; the terms "first", "second", and "third" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance; in addition, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection or a detachable connection; it can be directly connected or indirectly connected through an intermediate medium, and it can be the internal communication of two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0037] The present invention discloses a high-thickness and high-strength light-cured silicon nitride ceramic and a preparation method thereof, which specifically comprises the following steps:
[0038] Step 1: Two-step powder modification.
[0039] Si3N4 powder, Y2O3 powder, Al2O3 powder and SiO2 powder are mixed to form mixed powder A, wherein the mass fraction of Si3N4 powder is 67%, the mass fraction of Y2O3 powder is 5%, the mass fraction of Al2O3 powder is 3%, and the mass fraction of SiO2 powder is 25%; Si3N4 powder is formed by mixing Si3N4 powders of two particle sizes of 0.7 μm and 2 μm in a volume ratio of 1:1.
[0040] 3 wt% of stearic acid (the particle size of stearic acid is greater than 100 mesh) is added to the mixed powder A for dry grinding modification. During the dry grinding process, the ball-to-material ratio is 1.5 times, the rotation speed is 320 rpm, and the dry grinding time is 20 hours. The dry-milled powder is sieved through 80 mesh to obtain a mixed powder B. The ball milling medium-alcohol is added for dry grinding. The purpose of dry grinding is to break the agglomeration of ceramic particles and mix the silicon nitride powder with the sintering aid powder evenly and coat the stearic acid. Then, 3 wt% dispersant 9063 and 8 wt% silane coupling agent KH560 were added to the mixed powder B to carry out wet grinding modification. The purpose of wet grinding is to couple the ceramic powder and improve its compatibility with the resin. The ball-to-material ratio during wet grinding is 1.5 times, the rotation speed is 320 rpm, and the time is 20 h to obtain slurry C. The slurry C was dried in an oven at 75°C for 4 h, and then sieved through 80 mesh to obtain a premixed powder.
[0041] Step 2, preparation of premix and ceramic paste:
[0042] 1) Add different types of resins into the homogenizer according to different mass fractions, including 3.7wt% polyurethane, 8.65wt% bisphenol A, 3.7wt% IBOMA, 6.71wt% HDDA, and 1.3wt% TPGDA. 5.05wt%, TMPTA 22.34wt%, DPHA- 22.61wt%, fluorene acrylic acid and its composite glue 27.24wt%, after being stirred evenly with a stainless steel rod to obtain a mixed resin D, 5wt% of TPO by weight is added to the mixed resin D, and the premixed powder is added in batches after stirring. The mixing mass ratio of the premixed powder to the mixed resin D is 3:1. Because the silicon nitride powder in the premixed powder is not easy to disperse, it is necessary to add it to the mixed resin D one by one. The number of times the premixed powder is added to the mixed resin D is 4-6 times until it is completely wetted by the resin. After weighing, the mass counterweight of the homogenizer is adjusted to the same as the former. In the last step, polyethylene glycol 400 (PEG) is added. The amount of PEG added is 4.8wt% of the ceramic paste. PEG is a wetting agent. The more PEG is added, the lower the viscosity of the ceramic paste. The judgment standard is that the viscosity after addition cannot be lower than 500Pa·s (the ceramic printer platform is open, and the paste viscosity is too low and will flow out of the printing plane during printing). After the ceramic powder and resin are fully mixed, the required mixing program is selected and the equipment is started. In the program, the speed range of the first step is 1000-1500rpm, the time is 10-15s, the speed range of the second step is 1800-2200rpm, the time is 15-25s, and the speed range of the third step is 2200-2800rpm, the time is 25-35s.
[0043] The above-mentioned fluorene-based acrylic acid and its composite glue are commercially available products, and the product name is A-BPEF glue-40. The product appearance is colorless or light yellow transparent viscous liquid, its viscosity is ≤20000 (mPa·s, 30°C), its refractive index at 20°C is 1.6010-1.6030, and its acid value is ≤0.5mgKOH / g.
[0044] Step 3, printing process:
[0045] 1) Place the prepared ceramic paste in a vacuum degassing machine, draw the vacuum degree to -0.1MPa, and the degassing time is 30min;
[0046] 2) Stick the printed sticker to the magnetic paper, then glue the magnetic paper to the stainless steel plate of the printing platform, add the ceramic paste into the hopper, and adjust the gap between the scraper and the platform (leveling);
[0047] 3) Import the print model (stl format) into the computer that comes with the printer, set the parameters and start printing. Laser wavelength: 355nm; laser power: 91mW; scanning speed: 1600mm / s; scanning path: chess (this path is the printing scanning strategy that comes with the ceramic printer CERAMAKER system), and generate ceramic green body after printing
[0048] Step 4: Debinding and sintering
[0049] The ceramic printed green body is degreased and sintered. The degreasing process is as follows: Figure 3 As shown; the degreasing of the present invention comprises two steps, the first step is a cracking process, using a tube furnace cracking method, see Figure 3 (a) is a specific step of the cracking process, the cracking process, according to Figure 6 The specific process parameters of the cracking process are as follows: 20℃→180min-200℃→60min-200℃→200min-300℃→120min-300℃→100min-350℃→180min-350℃→200min-410℃→240min-410℃→200min-450℃→240min-450℃→100min-500℃→240min-500℃→100min-550 ℃→180min-550℃→50min-600℃→100min-600℃→200min-800℃→60min-800℃, the argon flow rate of the cracking process is 3L / min, here the cracking refers to the thermal cracking of the solidified resin in the ceramic printing green body under an inert atmosphere (argon). It can be seen from the process steps that the cracking process heats up slowly, and the slow cracking process causes the long-chain molecules to break and release small molecules, and some glassy carbon remains. At 300℃, PEG is completely removed, leaving mesoporous holes. At 800℃, the solidified resin is evenly removed along the above holes, accompanied by volume shrinkage and a small amount of glassy carbon.
[0050] After cracking, carbon removal is performed. Figure 3 (b) is a specific decarbonization process for decarbonization in a muffle furnace, and its specific process is to raise the temperature of the green body to 600°C within 300 minutes, then maintain it at 600°C for 200 minutes, then raise the temperature of the green body to 800°C within 100 minutes, keep the green body at 800°C for 100 minutes, and then slowly cool it to room temperature. The decarbonization process is to oxidize and remove the residual glassy carbon in the green body after the high-temperature cracking in the air atmosphere. After the decarbonization process, the volume of the green body does not change significantly, and the glassy carbon is completely removed.
[0051] Figure 4The figure shows the sintering process of silicon nitride, where the nitrogen pressure is 3MPa, and the specific process parameters of the sintering process are: 5℃ / min room temperature rises to 1200℃, 4℃ / min temperature rises to 1750℃, 1750℃ is kept for 2h, and cooled with the furnace. The silicon nitride ceramic sintered body is obtained. The silicon nitride green body that has completed the degreasing process is subjected to gas pressure sintering. During the sintering process, the phase transformation from α-Si3N4 to β-Si3N4 occurs, and the body undergoes a 20% linear shrinkage, that is, the densification process of the ceramic is completed.
[0052] The common degreasing process is to place the green body directly in air or oxygen atmosphere for degreasing, and the resin is cracked and the residual carbon is oxidized at the same time. In order to prevent the green body from cracking during the degreasing process, the present invention divides the above process into two steps, so a decarbonization process is required. The cracking principle of the post-treatment process of the present invention is as follows Figure 2 As shown in the figure, the ceramic printing green body is composed of ceramic particles, curing resin and PEG, the ceramic particles are in the network structure of the curing resin, and PEG is evenly dispersed in the above system; after the low-temperature degreasing of 200-300°C in the cracking process, the ceramic green body shrinks a little in volume, PEG is removed and mesoporous holes are left, accompanied by the cracking of a small amount of curing resin, and after high-temperature degreasing at 800°C, a certain density of ceramic particle accumulation and a small amount of residual carbon (glassy carbon) left by the resin remain in the system; therefore, after cracking, a green body with mesoporous holes is formed, and finally after subsequent decarburization (800°C air atmosphere, Figure 3 (b)) process, the degreasing process is completed.
[0053] The ultimate degreasing thickness of silicon nitride SLA printed green body is 8mm. The maximum three-point bending strength of silicon nitride sintered body at room temperature is 480MPa, the maximum compression strength is 540MPa, and the high temperature (1400℃) three-point bending strength is 110MPa.
[0054] Embodiment 1:
[0055] Step 1: Two-step powder modification.
[0056] Si3N4 powder, Y2O3 powder, Al2O3 powder and SiO2 powder are mixed to form mixed powder A, wherein the mass fraction of Si3N4 powder is 67%, the mass fraction of Y2O3 powder is 5%, the mass fraction of Al2O3 powder is 3%, and the mass fraction of SiO2 powder is 25%; Si3N4 powder is formed by mixing Si3N4 powders of two particle sizes of 0.7 μm and 2 μm in a volume ratio of 1:1.
[0057] 3 wt% of stearic acid (the particle size of stearic acid is greater than 100 mesh) was added to the mixed powder A, and dry grinding modification was performed. During the dry grinding process, the ball-to-material ratio was 1.5 times, the rotation speed was 320 rpm, and the dry grinding time was 20 h. The dry-milled powder was sieved through 80 mesh to obtain a mixed powder B. Then, 3 wt% of the mass of the mixed powder B dispersant 9063 and 8 wt% of the mass of the mixed powder B silane coupling agent KH560 were added to the mixed powder B, and wet grinding modification was performed. During the wet grinding process, the ball-to-material ratio was 1.5 times, the rotation speed was 320 rpm, and the time was 20 h to obtain slurry C. The slurry C was dried in an oven at 75° C. for 4 h, and then sieved through 80 mesh to obtain a premixed powder.
[0058] Step 2, preparation of premix and ceramic paste:
[0059] Different types of resins are added to the homogenizer tank according to different mass fractions, including 3.7wt% polyurethane, 8.65wt% bisphenol A, 3.7wt% IBOMA-monofunctional group, 6.71wt% HDDA-bifunctional group, 5.05wt% TPGDA-bifunctional group, 22.34wt% TMPTA-trifunctional group, 22.61wt% DPHA-hexafunctional group, 27.24wt% fluorene acrylic acid and its composite glue, and stirred evenly with a stainless steel rod to obtain a mixed resin D, 5wt% TPO is added to the mixed resin D, and ceramic powder is added after stirring until it is completely wetted by the resin, and the mass counterweight of the homogenizer is adjusted to the same as the former after weighing, and polyethylene glycol 400 (PEG) is added in the last step, and the specific amount can be added according to the required amount. After the above ceramic powder is fully mixed with the resin, the required mixing program is selected and the equipment is started. In the program, the first step speed is 1300rpm, the time is 13s, the second step speed range is 2000rpm, the time is 20s, and the third step speed range is 2500rpm, the time is 30s.
[0060] Step 3, Printing process
[0061] Place the prepared ceramic paste in a vacuum degassing machine, and draw the vacuum degree to -0.1MPa. The degassing time is 30min. Glue the printed sticker to the magnetic paper, and then glue the magnetic paper to the stainless steel plate of the printing platform. Add the ceramic paste into the hopper, adjust the gap between the scraper and the platform (leveling); import the printing model (stl format) into the computer that comes with the printer, set the parameters and start printing. Laser wavelength: 355nm; laser power: 91mW; scanning speed: 1600mm / s; scanning path: chess. Print the green blank.
[0062] Step 4: Debinding and sintering
[0063] The printed silicon nitride green body is degreased and sintered. The degreasing process is as follows: Figure 3 As shown, Figure 3 (a) is a cracking process, which adopts a tube furnace cracking method, wherein the argon gas flow rate is 3L / min, Figure 3 (b) is the carbon removal process. Figure 4 Shown is the silicon nitride sintering process, where the nitrogen pressure is 3 MPa.
[0064] After degreasing in an argon atmosphere, the glassy carbon left by the cracking of the resin in the ceramic green body is removed by an air furnace. Using the above degreasing method, the maximum degreasing thickness of the silicon nitride ceramic printing green body can be increased to 8mm. Figure 5 The silicon nitride sintered body with a size of 50mm*8mm*8mm did not show any cracking or deformation, and had good compactness. According to the three-point bending test and compression test, the three-point bending strength and compression strength of the silicon nitride sintered body were 480MPa and 540MPa, respectively.
[0065] Example 2
[0066] In the mixing procedure in step 2, the first step speed is 1000 rpm, the time is 15 s, the second step speed interval is 1800 rpm, the time is 25 s, and the third step speed interval is 2200 rpm, the time is 35 s. The rest of the parts not involved are the same as those in Example 1.
[0067] Example 3
[0068] In the mixing procedure in step 2, the third step speed is 1500 rpm, the time is 10 s, the second step speed interval is 2200 rpm, the time is 15 s, and the third step speed interval is 2800 rpm, the time is 255 s. The rest of the parts not involved are the same as those in Example 1.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing high-thickness and high-strength light-cured silicon nitride ceramics, characterized in that: The following steps are involved: Step 1, mixing Si3N4 powder, Y2O3 powder, Al2O3 powder and SiO2 powder to form mixed powder A; adding stearic acid to the mixed powder A and performing dry grinding modification to obtain mixed powder B; adding dispersant 9063 and silane coupling agent KH560 to the mixed powder B, performing wet grinding modification to obtain slurry C, drying the slurry C and sieving it to obtain a premixed powder; In step 1, the dry grinding time is 20 h, the wet grinding time is 20 h, and the drying temperature of slurry C is 75 ° C; Step 2, mixing polyurethane, bisphenol A, IBOMA, HDDA, TPGDA, TMPTA, DPHA and fluorenyl acrylic acid and its composite glue, stirring to obtain a mixed resin D, adding TPO to the mixed resin D, and then adding the premixed powder several times until the premixed powder is completely wetted by the mixed resin D, then adding polyethylene glycol 400, and then mixing through three stages of mixing to obtain a ceramic paste; in the mixed resin D, the mass fraction of polyurethane is 3.7%, the mass fraction of bisphenol A is 8.65%, the mass fraction of IBOMA is 3.7%, the mass fraction of HDDA is 6.71%, the mass fraction of TPGDA is 5.05%, the mass fraction of TMPTA is 22.34%, the mass fraction of DPHA is 22.61%, and the mass fraction of fluorenyl acrylic acid and its composite glue is 27.24%; In step 2, the mixing process parameters of the three stages are as follows: the speed of the first stage is 1000-1500 rpm, the time of the first stage is 10-15 s, the speed of the second stage is 1800-2200 rpm, the time of the second stage is 15-25 s, the speed of the third stage is 2200-2800 rpm, and the time of the third stage is 25-35 s; The amount of TPO added is 5% of the mass of the mixed resin D, and the mass ratio of the premixed powder to the mixed resin D is 3:1; the amount of polyethylene glycol 400 added is 4.8 wt% of the ceramic paste, and the viscosity of the ceramic paste after addition is ≥500 Pa•s; Step 3, adding the ceramic paste to the printer after vacuum degassing, and generating a ceramic green body after printing; Step 4, cracking, decarbonizing and sintering the ceramic green body to obtain silicon nitride ceramics; The heating parameters of the cracking process are: maintaining at 200°C for 180min, maintaining at 200°C for 60min, maintaining at 300°C for 200min, maintaining at 300°C for 120min, maintaining at 350°C for 100min, maintaining at 350°C for 180min, maintaining at 410°C for 200min, maintaining at 410°C for 240min, maintaining at 450°C for 200min, maintaining at 450°C for 240min, maintaining at 500°C for 100min, maintaining at 500°C for 240min, maintaining at 550°C for 100min, maintaining at 550°C for 180min, maintaining at 600°C for 50min, maintaining at 600°C for 100min, maintaining at 800°C for 200min, and maintaining at 800°C for 60min; The heating parameters of the decarburization process are: the temperature of the green body is raised to 600°C within 300 min, then maintained at 600°C for 200 min, then the temperature of the green body is raised to 800°C within 100 min, the green body is maintained at 800°C for 100 min, and then slowly cooled to room temperature; The sintering process is as follows: the room temperature is raised to 1200°C at 5°C / min, the temperature is raised to 1750°C at 4°C / min, and the temperature is kept at 1750°C for 2h before cooling with the furnace.
2. The method for preparing a high-thickness and high-strength light-cured silicon nitride ceramic according to claim 1, characterized in that: In step 1, the mass fraction of Si3N4 powder in the mixed powder A is 67%, the mass fraction of Y2O3 powder is 5%, the mass fraction of Al2O3 powder is 3%, and the mass fraction of SiO2 powder is 25%.
3. The method for preparing a high-thickness and high-strength light-cured silicon nitride ceramic according to claim 1, characterized in that: In step 1, the amount of stearic acid added is 3% of the mass of the mixed powder A, the amount of dispersant 9063 added is 3% of the mass of the mixed powder B, and the amount of silane coupling agent KH560 added is 8% of the mass of the mixed powder B.
4. A light-cured silicon nitride ceramic prepared by the preparation method according to any one of claims 1 to 3, characterized in that: The maximum three-point bending strength of the light-cured silicon nitride ceramic at room temperature is 480 MPa, and the maximum compression strength is 540 MPa; the three-point bending strength of the light-cured silicon nitride ceramic at 1400° C. is 110 MPa.