A hydrolysis-resistant polyester catalyst and its preparation method and application

By preparing a combined catalyst containing titanium compounds, organic acids, and metal compounds, the problem of easy hydrolysis of titanium-based catalysts was solved, resulting in a more efficient PBT polymerization process and improved product quality.

CN114479039BActive Publication Date: 2024-11-29CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202011154924.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-26
Publication Date
2024-11-29
Estimated Expiration
2040-10-26

AI Technical Summary

Technical Problem

Existing titanium-based catalysts are prone to hydrolysis during PBT polymerization, which leads to reduced catalytic activity and affects production efficiency and equipment lifespan.

Method used

A hydrolysis-resistant polyester catalyst is prepared by using a combination of titanium-containing compounds, diols, at least two organic acids, and metal compounds through a specific process, forming a homogeneous liquid structure and improving the stability of the catalyst.

Benefits of technology

It significantly improved the catalyst's resistance to hydrolysis and the polycondensation rate, thereby enhancing the efficiency of PBT polymerization and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses a hydrolysis-resistant polyester catalyst and a preparation method and application thereof. The catalyst comprises the reaction product of the following substances: (1) a titanium-containing compound, (2) a diol, (3) at least two organic acids, and (4) a metal compound. The organic acids are selected from at least two aliphatic organic acids, preferably at least two selected from lactic acid, citric acid, malic acid, tartaric acid and oxalic acid. Compared with tetrabutyl titanate, the polyester catalyst obtained by the method of the present invention has more obvious hydrolysis resistance and better polycondensation speed when preparing polyester, and achieves better technical effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalysts, and in particular relates to a polyester catalyst, and in particular, to a hydrolysis-resistant polyester catalyst and a preparation method and application thereof. Background Art

[0002] Polybutylene terephthalate (PBT) is a crystalline linear saturated polyester and a thermoplastic material. Due to its easy processing and excellent electrical, mechanical and heat resistance properties, it is widely used in electronic and electrical components, automobiles, mechanical equipment, optical cables and optical fibers. It is also gradually being widely used in films, sheets, fibers and other fields.

[0003] The main synthesis processes of PBT are ester exchange and direct esterification. In actual production, direct esterification is often used, with tetrabutyl titanate (TBT) as a catalyst. This catalyst is easily hydrolyzed, which will lead to reduced catalytic activity, easy clogging of pipelines during production, reducing the service life of the melt filter, and affecting the long-term operation of the device. In addition, in the direct esterification method, tetrahydrofuran will be produced as a by-product in the early stage of esterification, leading to problems such as reduced reaction efficiency, consumption of raw materials and decreased product performance. Tetraisopropyl titanate (TPT) has a better catalytic effect, but it also has problems of easy hydrolysis, scaling and clogging. Other titanium salts such as the hydrolysis products of titanium oxalate, titanium tetrachloride, and titanium sulfate have poor solubility in butanediol and are not suitable for the production of PBT.

[0004] Patent CN101824143A discloses a method for preparing highly crystalline thermoplastic polybutylene terephthalate, wherein tetrabutyl titanate and nano titanium dioxide solution are used as catalysts, and talcum powder and cobalt acetate are added to react to obtain the product. PBT crystallizes quickly, but the catalyst is still prone to hydrolysis.

[0005] Patent CN102174175A discloses a polybutylene terephthalate and a method for producing the same, wherein tetrabutyl titanate and magnesium acetate are used as catalysts to obtain a polyester resin, and the hydrolysis resistance of the catalyst and the color of the product are improved to a certain extent. However, the patent does not report the polymerization speed.

[0006] Patent CN102924698A discloses a method for preparing a titanium catalyst for the synthesis of polybutylene terephthalate and its application. The invention uses titanium compounds, glycerol, alkaline substances, phosphorus compounds and metal acetates to react under certain conditions to obtain a liquid catalyst. The synthesized PBT slices have excellent properties such as color and thermal stability. However, the introduction of glycerol will affect the polymerization system.

[0007] Patent CN101253217A discloses a catalyst for preparing PBT using a titanium compound and a compound of an element from Group 1 and Group 2 of the periodic table, but the titanium compound is not resistant to hydrolysis and is easily deactivated. Summary of the invention

[0008] The present invention aims to solve the technical problems that titanium-based catalysts are easy to hydrolyze in the previous PBT polymerization process, and the easy hydrolysis leads to insufficient catalyst reaction activity in the later stage, and provides a method for preparing a hydrolysis-resistant polyester catalyst.

[0009] One of the objects of the present invention is to provide a hydrolysis-resistant polyester catalyst, which comprises the reaction product of: (1) a titanium-containing compound, (2) a diol, (3) at least two organic acids and (4) a metal compound.

[0010] In a preferred embodiment, the titanium-containing compound is selected from titanates, with Ti(OR) 4 Indicates, wherein R is selected from C 1 ~C 10 A straight chain or branched hydrocarbon group.

[0011] In a further preferred embodiment, the titanium-containing compound is Ti(OR) 4 , wherein R is selected from C 1 ~C 8 A straight chain or branched hydrocarbon group.

[0012] In a further preferred embodiment, the titanium-containing compound is at least one selected from tetramethyl titanate, tetraethyl titanate, tetraethylhexyl titanate, tetra-n-propyl titanate, tetraisopropyl titanate, tetra-n-butyl titanate, and tetraisooctyl titanate.

[0013] In a preferred embodiment, the diol is selected from C 2 ~C 10 An organic alcohol having two hydroxyl groups.

[0014] In a further preferred embodiment, the diol is selected from C 2 ~C 5 An organic alcohol having two hydroxyl groups.

[0015] In a further preferred embodiment, the diol is at least one selected from 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, pentanediol, ethylene glycol, 1,6-hexanediol, 1,4-cyclohexanedimethanol and diethylene glycol.

[0016] In a preferred embodiment, the molar ratio of the diol to the titanium-containing compound is (1-8):1.

[0017] In a further preferred embodiment, the molar ratio of the diol to the titanium-containing compound is (1-4):1.

[0018] Among them, it is preferred to determine the choice of diol when preparing the catalyst based on the diol raw material of the later condensation reaction. For example, when the catalyst is used for the condensation of terephthalic acid and butanediol, butanediol is preferably used as the diol when preparing the catalyst. In this way, titanium is well dispersed in the diol to obtain a homogeneous liquid titanium-based polyester catalyst. When used in the condensation of terephthalic acid and butanediol, the homogeneous liquid titanium-based polyester catalyst can achieve very good miscibility with the butanediol raw material.

[0019] In a preferred embodiment, the organic acid is selected from at least two aliphatic organic acids.

[0020] In a further preferred embodiment, the organic acid is selected from at least two of lactic acid, citric acid, malic acid, tartaric acid and oxalic acid.

[0021] For example, the organic acid is selected from a combination of lactic acid and citric acid.

[0022] Among them, the chelating effect of aliphatic organic acids can form a stable chelating structure with titanate, thereby effectively resisting the attack of hydroxyl groups, and the synergistic effect of two or more organic acids will make this structure more stable and more resistant to hydrolysis.

[0023] In a further preferred embodiment, the molar ratio of the organic acid to the titanium-containing compound is (0.1-18):1, preferably (0.1-12):1.

[0024] In a preferred embodiment, the metal compound is selected from at least one of metal compounds of Group IIA, Group IB, Group IIB, Group VIIB and Group VIII in the periodic table.

[0025] In a further preferred embodiment, the metal compound is at least one selected from metal compounds of zinc, manganese, magnesium, calcium and cobalt.

[0026] The organic acid can be added at any time during the reaction of the titanium compound and the diol.

[0027] In a further preferred embodiment, the molar ratio of the metal compound to the titanium-containing compound is (0.01-2):1, preferably (0.01-0.8):1.

[0028] Among them, the diol is a raw material that can react with titanate, which can remove the alkoxy groups that are easily attacked. At the same time, it serves as a good solvent for the overall reaction. Any substance added in the reaction can be well miscible with the diol.

[0029] In a preferred embodiment, the polyester catalyst is prepared at 10-180° C. within 2-6 hours.

[0030] In a preferred embodiment, the polyester catalyst is prepared at 30-140°C.

[0031] The titanium-containing compound, diol, at least two organic acids and a metal compound are reacted to obtain a homogeneous liquid titanium-based polyester catalyst.

[0032] The second object of the present invention is to provide a method for preparing the hydrolysis-resistant polyester catalyst described in the first object of the present invention, comprising the following steps:

[0033] Step 1, mixing diol, organic acid A and titanium-containing compound, and treating to obtain pre-reaction liquid A;

[0034] Step 2, adding organic acid B and diol to pre-reaction liquid A, and obtaining pre-reaction liquid B through treatment;

[0035] Step 3: adding a metal compound to the pre-reaction liquid B to obtain the hydrolysis-resistant polyester catalyst through reaction.

[0036] In a preferred embodiment, the titanium-containing compound is Ti(OR) 4 , wherein R is selected from C 1 ~C 10 A straight chain or branched hydrocarbon group, preferably, R is selected from C 1 ~C 8 A straight chain or branched hydrocarbon group, more preferably, the titanium-containing compound is selected from at least one of tetramethyl titanate, tetraethyl titanate, tetraethylhexyl titanate, tetra-n-propyl titanate, tetraisopropyl titanate, tetra-n-butyl titanate and tetra-isooctyl titanate.

[0037] In a preferred embodiment, the diol is selected from C 2 ~C 10 An organic alcohol having two hydroxyl groups, preferably selected from C 2 ~C 5 The organic alcohol having two hydroxyl groups is more preferably at least one selected from 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, pentanediol, ethylene glycol, 1,6-hexanediol, 1,4-cyclohexanedimethanol and diethylene glycol.

[0038] In a preferred embodiment, the ratio of the total molar amount of the diol in step 1 and step 2 to the molar amount of the titanium-containing compound in step 1 is (1-8):1, preferably (1-4):1.

[0039] In a preferred embodiment, in step 1, diol and organic acid A are first mixed, and then the titanium-containing compound is slowly dripped therein.

[0040] Among them, if added directly, it will cause too fast reaction, thus causing agglomeration and precipitation.

[0041] In a further preferred embodiment, in step 1, the treatment is performed as follows: stirring at 30-100° C. for 0.2-5 h, preferably, stirring at 50-90° C. for 0.5-3 h.

[0042] In a preferred embodiment, in step 2, the organic acid B and the diol are first mixed to obtain the diol containing the organic acid B, and then the diol is added to the pre-reaction solution A.

[0043] In a further preferred embodiment, in step 2, the treatment is performed as follows: stirring at 50-120° C. for 0.5-6 h, preferably, stirring at 60-110° C. for 1-5 h.

[0044] In a preferred embodiment, the organic acid A and the organic acid B as a whole contain at least two of the aliphatic organic acids, preferably contain at least two of the lactic acid, citric acid, malic acid, tartaric acid and oxalic acid.

[0045] It can also be expressed as:

[0046] Organic acid A and organic acid B are independently selected from one of aliphatic organic acids, and organic acid A and organic acid B are different, preferably one of lactic acid, citric acid, malic acid, tartaric acid or oxalic acid, and organic acid A and organic acid B are different;

[0047] Alternatively, one of the organic acid A and the organic acid B is selected from at least two of aliphatic organic acids, and the other is selected from at least one of aliphatic organic acids; preferably, one of the organic acid A and the organic acid B is selected from at least two of lactic acid, citric acid, malic acid, tartaric acid and oxalic acid, and the other is selected from at least one of lactic acid, citric acid, malic acid, tartaric acid and oxalic acid.

[0048] It is sufficient to ensure that at least two organic acids exist in the entire reaction system.

[0049] In a preferred embodiment, the ratio of the total molar amount of the organic acid A and the organic acid B to the molar amount of the titanium-containing compound is (0.1-18):1, preferably (0.1-12):1.

[0050] In a further preferred embodiment, the molar ratio of organic acid A to organic acid B is (0.1-9):1, preferably (0.1-7):1.

[0051] The total amount of acid needs to be controlled overall, but if you need to focus on improving the hue, the ratio can be controlled to be less than 1; if you need to focus on improving the activity and stability, the ratio can be controlled to be greater than 1.

[0052] In a preferred embodiment, the metal compound is selected from at least one of metal compounds of Groups IIA, IB, IIB, VIIB and VIII in the periodic table, preferably at least one of metal compounds of zinc, manganese, magnesium, calcium and cobalt.

[0053] In a further preferred embodiment, the molar ratio of the metal compound to the titanium-containing compound is (0.01-2):1, preferably (0.01-0.8):1.

[0054] In a preferred embodiment, in step 3, the reaction is carried out as follows: reacting at 60-140° C. for 0.5-5 h.

[0055] In a further preferred embodiment, in step 3, the reaction is carried out as follows: reacting at 80-120° C. for 1-3 hours.

[0056] The third object of the present invention is to provide a hydrolysis-resistant polyester catalyst obtained by the preparation method described in the second object of the present invention.

[0057] A fourth object of the present invention is to provide a method for preparing polyester, which is carried out in the presence of the hydrolysis-resistant polyester catalyst described in one of the objects of the present invention or the hydrolysis-resistant polyester catalyst obtained by the preparation method described in the second object of the present invention.

[0058] In a preferred embodiment, the weight of titanium atoms in the polyester catalyst used is 10 to 160 ppmw based on the theoretical weight of the polyester product.

[0059] In a further preferred embodiment, the weight of titanium atoms in the polyester catalyst is 10 to 100 ppmw based on the theoretical weight of the polyester product.

[0060] The theoretical weight of the polyester refers to the theoretical weight of the polyester calculated based on the raw materials before the reaction, which is obtained as follows: a dibasic acid and a diol are reacted in a 1:1 ratio, and the weight of the removed water is removed.

[0061] In a preferred embodiment, the preparation method comprises: firstly subjecting the dibasic acid and the diol to an esterification reaction at 200-230°C and normal pressure, and then polycondensing at 230-250°C and less than 150 Pa to obtain the polyester. After the reaction, the polyester is pelletized and stored.

[0062] In a further preferred embodiment, the dibasic acid is terephthalic acid, and the diol is butanediol.

[0063] Wherein, the polyester catalyst is added into the reaction system before the esterification reaction starts.

[0064] The fifth object of the present invention is to provide polyester obtained by the preparation method described in the fourth object of the present invention.

[0065] The endpoints and any values ​​of the range disclosed in the present invention are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be regarded as specifically disclosed in this article.

[0066] Compared with the prior art, the present invention has the following beneficial effects: the inventors surprisingly found that, compared with tetrabutyl titanate, the polyester catalyst obtained by the method of the present invention has more obvious hydrolysis resistance and better condensation rate when preparing polyester, thus achieving better technical effects. DETAILED DESCRIPTION

[0067] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0068] It should also be noted that the various specific technical features described in the following specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0069] In addition, the various embodiments of the present invention may be arbitrarily combined as long as they do not violate the concept of the present invention. The technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0070] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0071] In the present invention, the intrinsic viscosity, hue, etc. of polyester are tested by the following methods:

[0072] (1) Intrinsic viscosity: Phenol-tetrachloroethane mixture was used as solvent and measured with an Ubbelohde viscometer at 25°C.

[0073] (2) Hue: After the pellets were treated at 135°C for 1 hour, the Hunter L value (brightness), a value (red-green hue) and b value (yellow-blue hue) were measured using a BYK Gardner color-view automatic colorimeter. The higher the L value, the greater the brightness; the higher the b value, the yellower the polyester chips. For the present invention, it is desirable to pursue a high L value and a low b value.

[0074] (3) Hydrolysis test: Take 10 mL of the catalyst in a volumetric flask, add 20 mL of water, reflux at 90 °C for 10 h, and use a refractometer to measure the change in the value before and after reflux.

[0075] [Example 1]

[0076] Preparation of Catalyst A

[0077] Step 1: Add 157.5 g (0.75 mol) of citric acid monohydrate and 540 g (6 mol) of butanediol to a reactor equipped with an agitator, a condenser and a thermometer. After stirring evenly, slowly drop 170 g (0.5 mol) of tetrabutyl titanate into the reactor. The solution is first slightly mixed and then clarified. Stir the reaction at 70°C for 2 hours to obtain a basic solution.

[0078] Step 2: 22.5 g (0.25 mol) of lactic acid and 270 g (3 mol) of butanediol were added dropwise to the base solution, and the mixture was stirred at 90° C. for 3 hours.

[0079] Step 3: Add 21.4 g (0.1 mol) of solid powdered magnesium acetate and continue the reaction at 100° C. for 2 hours to obtain a nearly colorless homogeneous liquid, which is catalyst A.

[0080] Preparation of polyester

[0081] 600 g of terephthalic acid, 520 g of 1,4-butanediol and catalyst A (based on the amount of polyester produced, the weight of titanium atoms is 80 ppmw) are mixed into a slurry and added into a polymerization kettle for esterification reaction. The esterification temperature is 200-225°C and the pressure is normal pressure. The water and tetrahydrofuran generated by the reaction are discharged through a distillation device. After the esterification is completed, the system pressure is reduced to less than 100 Pa by vacuum pumping. At the same time, the reaction temperature is gradually increased to 250°C. When the stirring power reaches the requirement, the reaction is stopped. After that, the reaction product is continuously extruded in strips from the bottom of the polymerization kettle, cooled and pelletized.

[0082] The test results are shown in Table 1.

[0083] [Example 2]

[0084] The process of Example 1 was repeated, except that 157.5 g (0.75 mol) of citric acid monohydrate in step 1 was changed to 210 g (1 mol) of citric acid monohydrate, and other conditions remained unchanged.

[0085] The test results are shown in Table 1.

[0086] [Example 3]

[0087] The process of Example 1 was repeated, except that the amount of magnesium acetate (21.4 g (0.1 mol)) in step 3 was changed to 42.8 g (0.2 mol) of magnesium acetate, and other conditions remained unchanged.

[0088] The test results are shown in Table 1.

[0089] [Example 4]

[0090] The process of Example 1 was repeated, except that the amount of magnesium acetate (21.4 g (0.1 mol)) in step 3 was changed to 64.3 g (0.3 mol) of magnesium acetate, and other conditions remained unchanged.

[0091] The test results are shown in Table 1.

[0092] [Example 5]

[0093] Preparation of Catalyst B

[0094] Step 1: Add 540 g (6 mol) of butanediol containing 67.5 g (0.75 mol) of lactic acid into a reactor equipped with an agitator, a condenser and a thermometer, and slowly drop 170 g (0.5 mol) of tetrabutyl titanate into the reactor. The solution is first slightly mixed and then clarified. Stir the reaction at 70°C for 2 hours to obtain a basic solution.

[0095] Step 2: 52.5 g (0.25 mol) of citric acid monohydrate and 270 g (3 mol) of butanediol were added dropwise to the base solution, and the mixture was stirred at 90° C. for 3 hours.

[0096] Step 3: Add 21.4 g (0.1 mol) of solid powdered magnesium acetate and continue the reaction at 100° C. for 2 hours to obtain a nearly colorless homogeneous liquid, which is catalyst B.

[0097] The same method as in Example 1 was used to prepare polyester.

[0098] The test results are shown in Table 1.

[0099] [Example 6]

[0100] The process of Example 5 was repeated, except that the lactic acid in step 1 (67.5 g (0.75 mol)) was changed to lactic acid (90 g (1 mol), and other conditions remained unchanged.

[0101] The test results are shown in Table 1.

[0102] [Example 7]

[0103] Preparation of Catalyst C

[0104] Step 1: Add 45 g (0.5 mol) of lactic acid, 52.5 g (0.25 mol) of citric acid monohydrate, and 540 g (6 mol) of butanediol to a reactor equipped with an agitator, a condenser, and a thermometer. After stirring evenly, slowly drop 170 g (0.5 mol) of tetrabutyl titanate into the reactor. The solution is first slightly mixed and then clarified. Stir the reaction at 70°C for 2 hours to obtain a basic solution.

[0105] Step 2: 52.5 g (0.25 mol) of citric acid monohydrate and 270 g (3 mol) of butanediol were added dropwise to the base solution, and the mixture was stirred at 90° C. for 3 hours.

[0106] Step 3: Add 21.4 g (0.1 mol) of solid powdered magnesium acetate and continue the reaction at 100° C. for 2 hours to obtain a nearly colorless homogeneous liquid, which is catalyst C.

[0107] The same method as in Example 1 was used to prepare polyester.

[0108] The test results are shown in Table 1.

[0109] [Example 8]

[0110] Preparation of Catalyst D

[0111] Step 1: Add 105 g (0.5 mol) of citric acid monohydrate and 540 g (6 mol) of butanediol to a reactor equipped with an agitator, a condenser and a thermometer. After stirring evenly, slowly drop 170 g (0.5 mol) of tetrabutyl titanate into the reactor. The solution is first slightly mixed and then clarified. Stir the reaction at 70°C for 2 hours to obtain a basic solution.

[0112] Step 2: 22.5 g (0.25 mol) of lactic acid, 52.5 g (0.25 mol) of citric acid monohydrate and 270 g (3 mol) of butanediol were added dropwise to the base solution, and the mixture was stirred at 90° C. for 3 hours.

[0113] Step 3: Add 21.4 g (0.1 mol) of solid powdered magnesium acetate and continue the reaction at 100° C. for 2 hours to obtain a nearly colorless homogeneous liquid, which is catalyst D.

[0114] The same method as in Example 1 was used to prepare polyester.

[0115] The test results are shown in Table 1.

[0116] [Comparative Example 1]

[0117] Preparation of polyester

[0118] 600 g of terephthalic acid, 520 g of 1,4-butanediol and tetrabutyl titanate (based on the amount of polyester generated, the weight of titanium atoms is 120 ppmw) are mixed into a slurry and added into a polymerization kettle for esterification reaction. The esterification temperature is 200-225°C and the pressure is normal pressure. The water and tetrahydrofuran generated by the reaction are discharged through a distillation device. After the esterification is completed, the system pressure is reduced to less than 100 Pa by vacuum, and the reaction temperature is gradually increased to 250°C. When the stirring power reaches the requirement, the reaction is stopped, and then the reaction product is continuously extruded in strips from the bottom of the polymerization kettle, cooled, and pelletized.

[0119] The test results are shown in Table 1.

[0120] [Comparative Example 2]

[0121] Preparation of Catalyst E

[0122] Step 1: Add 210 g (1.0 mol) of citric acid monohydrate and 540 g (6 mol) of butanediol to a reactor equipped with an agitator, a condenser and a thermometer. After stirring evenly, slowly drop 170 g (0.5 mol) of tetrabutyl titanate into the reactor. The solution is first slightly mixed and then clarified. Stir the reaction at 70°C for 2 hours to obtain a basic solution.

[0123] Step 2: Add 270 g (3 mol) of butanediol to the base solution, stir and react at 90°C for 3 hours, then add 21.4 g (0.1 mol) of solid powdered magnesium acetate, and continue to react at 100°C for 2 hours to obtain a nearly colorless homogeneous liquid, which is catalyst E.

[0124] The same method as in Example 1 was used to prepare polyester.

[0125] The test results are shown in Table 1.

[0126] [Comparative Example 3]

[0127] Preparation of Catalyst F

[0128] Step 1: Add 90 g (1.0 mol) of lactic acid and 540 g (6 mol) of butanediol to a reactor equipped with an agitator, a condenser and a thermometer. After stirring evenly, slowly drop 170 g (0.5 mol) of tetrabutyl titanate into the reactor. The solution is first slightly mixed and then clarified. Stir the reaction at 70°C for 2 hours to obtain a basic solution.

[0129] Step 2: Add 270 g (3 mol) of butanediol to the base solution, stir and react at 90°C for 3 hours, then add 21.4 g (0.1 mol) of solid powdered magnesium acetate, and continue to react at 100°C for 2 hours to obtain a nearly colorless homogeneous liquid, which is catalyst F.

[0130] The same method as in Example 1 was used to prepare polyester.

[0131] The test results are shown in Table 1.

[0132] [Comparative Example 4]

[0133] Preparation of Catalyst G

[0134] Step 1: Add 157.5 g (0.75 mol) of citric acid monohydrate and 540 g (6 mol) of butanediol to a reactor equipped with an agitator, a condenser and a thermometer. After stirring evenly, slowly drop 170 g (0.5 mol) of tetrabutyl titanate into the reactor. The solution is first slightly mixed and then clarified. Stir the reaction at 70°C for 2 hours to obtain a basic solution.

[0135] Step 2: 52.5 g (0.25 mol) of citric acid monohydrate and 270 g (3 mol) of butanediol were added dropwise to the base solution. After stirring at 90° C. for 3 hours, 21.4 g (0.1 mol) of solid powdered magnesium acetate was added and the reaction was continued at 100° C. for 2 hours to obtain a nearly colorless homogeneous liquid, which is catalyst G.

[0136] Preparation of polyester

[0137] 600 g of terephthalic acid, 520 g of 1,4-butanediol and catalyst G (based on the amount of polyester produced, the weight of titanium atoms is 80 ppmw) are mixed into a slurry and added into a polymerization kettle for esterification reaction. The esterification temperature is 200-225°C and the pressure is normal pressure. The water and tetrahydrofuran generated by the reaction are discharged through a rectification device. After the esterification is completed, the system pressure is reduced to less than 100 Pa by vacuum pumping. At the same time, the reaction temperature is gradually increased to 250°C. When the stirring power reaches the requirement, the reaction is stopped. After that, the reaction product is continuously extruded in strips from the bottom of the polymerization kettle, cooled, and pelletized.

[0138] The test results are shown in Table 1.

[0139] [Comparative Example 5]

[0140] Preparation of Catalyst H

[0141] Step 1: Add 157.5 g (0.75 mol) of citric acid monohydrate, 22.5 g (0.25 mol) of lactic acid, and 540 g (6 mol) of butanediol to a reactor equipped with an agitator, a condenser, and a thermometer. After stirring evenly, slowly drop 170 g (0.5 mol) of tetrabutyl titanate into the reactor. The solution is first slightly mixed and then clarified. Stir and react at 70°C for 2 hours to obtain a basic solution.

[0142] Step 2: 270 g (3 mol) of butanediol was added dropwise to the base solution. After stirring at 90°C for 3 hours, 21.4 g (0.1 mol) of solid powdered magnesium acetate was added and the reaction was continued at 100°C for 2 hours to obtain a nearly colorless homogeneous liquid, which is catalyst H.

[0143] Preparation of polyester

[0144] 600 g of terephthalic acid, 520 g of 1,4-butanediol and catalyst H (based on the amount of polyester produced, the weight of titanium atoms is 80 ppmw) are mixed into a slurry and added into a polymerization kettle for esterification reaction. The esterification temperature is 200-225°C and the pressure is normal pressure. The water and tetrahydrofuran generated by the reaction are discharged through a rectification device. After the esterification is completed, the system pressure is reduced to less than 100 Pa by vacuum pumping. At the same time, the reaction temperature is gradually increased to 250°C. When the stirring power reaches the requirement, the reaction is stopped. After that, the reaction product is continuously extruded in strips from the bottom of the polymerization kettle, cooled and pelletized.

[0145] The test results are shown in Table 1.

[0146] Table 1:

[0147]

[0148] The present invention is described in detail above in conjunction with specific implementation methods and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, various equivalent substitutions, modifications or improvements can be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The protection scope of the present invention shall be subject to the attached claims.

Claims

1. A hydrolysis-resistant polyester catalyst, comprising the reaction product of: (1) a titanium-containing compound, (2) a diol, (3) at least two organic acids, and (4) a metal compound; a method for preparing the hydrolysis-resistant polyester catalyst comprising: Step 1, mixing diol, organic acid A and titanium-containing compound, and treating to obtain pre-reaction liquid A; Step 2, adding organic acid B and diol to pre-reaction liquid A, and obtaining pre-reaction liquid B through treatment; Step 3, adding metal compound to the pre-reaction liquid B, and obtaining the hydrolysis-resistant polyester catalyst through reaction; the organic acid A and organic acid B as a whole contain at least two of the aliphatic organic acids.

2. The hydrolysis-resistant polyester catalyst according to claim 1, characterized in that: The titanium-containing compound is selected from titanate esters, represented by Ti(OR)4, wherein R is selected from C1 to C 10 A straight chain or branched hydrocarbon group.

3. The hydrolysis-resistant polyester catalyst according to claim 1, characterized in that: The titanium-containing compound is selected from titanate esters, represented by Ti(OR)4, wherein R is a straight chain or branched hydrocarbon group selected from C1 to C8.

4. The hydrolysis-resistant polyester catalyst according to claim 1, characterized in that: The titanium-containing compound is at least one selected from tetramethyl titanate, tetraethyl titanate, tetraethylhexyl titanate, tetra-n-propyl titanate, tetraisopropyl titanate, tetra-n-butyl titanate, and tetraisooctyl titanate.

5. The hydrolysis-resistant polyester catalyst according to claim 1, characterized in that: The diol is selected from C2 to C 10 An organic alcohol having two hydroxyl groups.

6. The hydrolysis-resistant polyester catalyst according to claim 1, characterized in that: The diol is selected from organic alcohols having two hydroxy groups of C2 to C5.

7. The hydrolysis-resistant polyester catalyst according to claim 1, characterized in that: The diol is at least one selected from 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, pentanediol, ethylene glycol, 1,6-hexanediol, 1,4-cyclohexanedimethanol and diethylene glycol.

8. The hydrolysis-resistant polyester catalyst according to claim 1, characterized in that: The organic acid is selected from at least two of lactic acid, citric acid, malic acid, tartaric acid and oxalic acid.

9. The hydrolysis-resistant polyester catalyst according to claim 1, characterized in that: The metal compound is selected from at least one of metal compounds of Group IIA, Group IB, Group IIB, Group VIIB and Group VIII in the periodic table.

10. The hydrolysis-resistant polyester catalyst according to claim 1, characterized in that: The metal compound is at least one selected from metal compounds of zinc, manganese, magnesium, calcium and cobalt.

11. The hydrolysis-resistant polyester catalyst according to any one of claims 1 to 10, characterized in that: The molar ratio of the diol to the titanium-containing compound is (1-8):1; and / or The molar ratio of the organic acid to the titanium-containing compound is (0.1-18):1; and / or The molar ratio of the metal compound to the titanium-containing compound is (0.01-2):

1.

12. The hydrolysis-resistant polyester catalyst according to claim 11, characterized in that: The molar ratio of the diol to the titanium-containing compound is (1-4):1; and / or The molar ratio of the organic acid to the titanium-containing compound is (0.1-12):1; and / or The molar ratio of the metal compound to the titanium-containing compound is (0.01-0.8):

1.

13. A method for preparing the hydrolysis-resistant catalyst according to any one of claims 1 to 12, comprising the following steps: Step 1, mixing diol, organic acid A and titanium-containing compound, and treating to obtain pre-reaction liquid A; Step 2, adding organic acid B and diol to pre-reaction liquid A, and obtaining pre-reaction liquid B through treatment; Step 3, adding a metal compound to the pre-reaction liquid B to obtain the hydrolysis-resistant polyester catalyst through reaction; The organic acid A and the organic acid B as a whole contain at least two kinds of aliphatic organic acids.

14. The preparation method according to claim 13, characterized in that: The ratio of the total molar amount of the diol in step 1 and step 2 to the molar amount of the titanium-containing compound in step 1 is (1-8):

1.

15. The preparation method according to claim 13, characterized in that: The ratio of the total molar amount of the diol in step 1 and step 2 to the molar amount of the titanium-containing compound in step 1 is (1-4):

1.

16. The preparation method according to claim 13, characterized in that: The organic acid A and the organic acid B as a whole contain at least two of lactic acid, citric acid, malic acid, tartaric acid and oxalic acid.

17. The preparation method according to claim 13, characterized in that: The ratio of the total molar amount of the organic acid A and the organic acid B to the molar amount of the titanium-containing compound is (0.1-18):

1.

18. The preparation method according to claim 13, characterized in that: The ratio of the total molar amount of the organic acid A and the organic acid B to the molar amount of the titanium-containing compound is (0.1-12):

1.

19. The preparation method according to claim 13, characterized in that: The molar ratio of organic acid A to organic acid B is (0.1-9):

1.

20. The preparation method according to claim 13, characterized in that: The molar ratio of organic acid A to organic acid B is (0.1-7):

1.

21. The preparation method according to claim 13, characterized in that: In step 1, diol and organic acid A are first mixed, and then the titanium-containing compound is slowly dropped thereinto.

22. The preparation method according to claim 21, characterized in that: In step 1, the treatment is performed as follows: stirring at 30-100° C. for 0.2-5 h.

23. The preparation method according to claim 21, characterized in that: In step 1, the treatment is performed as follows: stirring at 50-90° C. for 0.5-3 h.

24. The preparation method according to claim 13, characterized in that: In step 2, the organic acid B and the diol are first mixed to obtain the diol containing the organic acid B, and then the diol is added into the pre-reaction liquid A.

25. The preparation method according to claim 24, characterized in that: In step 2, the treatment is performed as follows: stirring at 50-120° C. for 0.5-6 h.

26. The preparation method according to claim 24, characterized in that: In step 2, the treatment is performed as follows: stirring at 60-110° C. for 1-5 h.

27. The preparation method according to any one of claims 13 to 26, characterized in that: In step 3, the reaction is carried out as follows: reacting at 60-140° C. for 0.5-5 h.

28. The preparation method according to claim 27, characterized in that: In step 3, the reaction is carried out as follows: reacting at 80-120° C. for 1-3 h.

29. A hydrolysis-resistant polyester catalyst obtained by the preparation method according to any one of claims 13 to 28.

30. A method for preparing polyester, which is carried out in the presence of the hydrolysis-resistant polyester catalyst according to any one of claims 1 to 12 or the hydrolysis-resistant polyester catalyst obtained by the preparation method according to any one of claims 13 to 28.

31. The preparation method according to claim 30, characterized in that: The weight of titanium atoms in the polyester catalyst used is 10 to 160 ppmw based on the theoretical weight of the polyester product.

32. The preparation method according to claim 30, characterized in that: The preparation method comprises: firstly subjecting a dibasic acid and a diol to an esterification reaction at 200-230° C. and normal pressure, and then subjecting the dibasic acid and the diol to polycondensation at 230-250° C. and less than 150 Pa to obtain the polyester.

33. The preparation method according to claim 32, characterized in that: The dibasic acid is terephthalic acid, and the diol is butanediol.

34. The polyester obtained by the preparation method according to any one of claims 30 to 33.

Citation Information

Patent Citations

  • Polybutylene terephthalate and process for production thereof

    CN101253217A

  • Preparation method of high crystallization thermoplastics type polybutylene terephthalate slice

    CN101824143A

  • Polybutylene terephthalate and process for production thereof

    CN102174175A

  • Preparation method and use of titanium catalyst for synthesis of polybutylene terephthalate

    CN102924698A

  • Preparation method of low terminal carboxyl PBT resin

    CN111087583A

Cited By

  • Titanium composite catalyst as well as preparation method and application thereof

    CN121949771A