based on 63 Heterojunction high-efficiency nuclear battery with NiO carrier transport layer and preparation method

By using a heterojunction structure based on 63NiO carrier transport layer in a beta radiation voltaic effect nuclear battery, the problem of low energy conversion efficiency caused by the self-absorption effect is solved, and more efficient power conversion is achieved, using the advantages of wide bandgap semiconductors. Advantages, improving the performance of nuclear batteries.

CN114496333BActive Publication Date: 2024-10-22JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210069812.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-21
Publication Date
2024-10-22
Estimated Expiration
2042-01-21

AI Technical Summary

Technical Problem

Existing beta radiation volt effect nuclear batteries have low energy conversion efficiency due to self-absorption effect and cannot meet the technical specifications of nuclear batteries.

Method used

It adopts a heterojunction structure based on 63NiO carrier transport layer, including sapphire substrate, undoped GaN buffer layer, P-type GaN hole collection layer, P-type 63NiO carrier transport layer and N-type ZnO electron collection layer. Hole and electron pairs are generated through the radiation ionization effect, and are collected under the action of the built-in electric field to form current, forming a PPN-type gradient component heterojunction.

Benefits of technology

It effectively reduces the impact of the self-absorption effect, improves the energy conversion efficiency of nuclear batteries, and uses the radiation resistance and carrier mobility of wide-bandgap semiconductors to improve battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114496333B_ABST
    Figure CN114496333B_ABST
Patent Text Reader

Abstract

based on 63 The heterojunction high-efficiency nuclear battery with NiO carrier transport layer belongs to the field of nuclear energy technology application, which solves the adverse effects of the self-absorption effect of the β-radiation voltaic effect nuclear battery and the low energy conversion efficiency of the nuclear battery. The nuclear battery includes: sapphire substrate, non-doped GaN buffer layer, P-type GaN hole collection layer, P-type 63 NiO carrier transport layer and N-type ZnO electron collection layer; 63 The beta particles emitted by the NiO carrier transport layer generate hole-electron pairs through the radiation ionization effect. Under the action of the built-in electric field, the electrons move to the N-type ZnO electron collection layer and are collected by the N-type ZnO electron collection layer, and the holes move to the P-type GaN hole collection layer and are collected by the P-type GaN hole collection layer to form a current. The present invention has the advantages of good radiation resistance, high carrier mobility, and its own gradient component energy level structure, which is conducive to the transport of carriers, reduces the reverse saturation current, and improves the energy conversion efficiency of the nuclear battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of nuclear energy technology application, and specifically relates to 63 Heterojunction high-efficiency nuclear battery with NiO carrier transport layer and preparation method. Background Art

[0002] Nuclear batteries are devices that use radioactive isotope decay to emit energetic particles and convert their energy into electrical energy. In recent years, with the development of micro-electromechanical systems, beta-radiation voltaic effect nuclear batteries have received extensive attention.

[0003] In beta radiation voltaic effect nuclear batteries, the commonly used radiation sources are mainly 3 H. 63 You, 147 Pm, 85 Kr, 90 Sr / 90 Y et al. 3 H sources have attracted widespread attention because the β particles they emit are relatively mild and will not cause displacement damage to semiconductor devices such as Si and Ge. 3 The power density of the H source is low. Due to the influence of self-absorption efficiency, the energy conversion efficiency and power of the nuclear battery are relatively low. 147 Pm source and 85 The application of Kr source achieved higher efficiency in early β-nuclear batteries, but its relatively short half-life and gaseous form that is not conducive to storage have affected the application field of nuclear batteries. 90 Sr / 90 The power density of the gamma radiation source is quite high. 90 Sr is a very abundant component in spent nuclear fuel and radioactive waste; therefore, 90 The price of Sr is relatively low. However, on the one hand, 90 Sr / 90 Y high-energy β particles can cause serious displacement damage to semiconductors; on the other hand, such high-energy β particles are difficult to be effectively absorbed in transducers. Even by combining the photovoltaic mechanism and using the scintillator as the intermediate layer between the radiation source and the transducer, the energy conversion efficiency of nuclear batteries will become lower. 63 Ni has a half-life of about 100 years and a power density of almost 3 H, and the emitted β particles are not enough to cause displacement damage in wide bandgap semiconductor materials. 63 Ni has great application prospects in the field of β-nuclear batteries.

[0004] Wide-bandgap semiconductors have the advantages of good radiation resistance and high carrier mobility. They have been applied in beta-radiation voltaic effect nuclear batteries and have achieved excellent results. The third-generation semiconductor materials are represented by GaN, ZnO, and 4H-SiC, and their bandgap widths are 3.4eV, 3.37eV, and 3.26eV, respectively. According to the Shockley-Queisser limit theory, when GaN and ZnO are used as transducers, the theoretical limit conversion efficiency is higher than that of 4H-SiC. Based on the existing semiconductor preparation process, it is difficult to achieve high-concentration P-type doping of ZnO. However, since GaN and ZnO have similar crystal structures and electronic properties, and Mg-doped P-type GaN can be prepared. Therefore, in beta-radiation voltaic effect nuclear batteries, the simultaneous use of P-type GaN and N-type ZnO is a good direction.

[0005] 63 Ni is a long-half-life low-energy β-radionuclide. 63 The Ni source is electroplated. 3 Ni is deposited on the source substrate in the form of metal. 63 The Ni source irradiates the semiconductor transducer device externally. 63 The existence of Ni-derived absorption effect leads to low energy conversion efficiency of nuclear battery devices and failure to meet the technical requirements of nuclear batteries. Summary of the invention

[0006] In order to solve the problems existing in the prior art, the present invention provides a 63 The heterojunction high-efficiency nuclear battery and preparation method of the NiO carrier transport layer fundamentally solve the adverse effects of the beta radiation voltaic effect nuclear battery due to the self-absorption effect, and at the same time solve the problem of low energy conversion efficiency of the nuclear battery.

[0007] The technical solution adopted by the present invention to solve the technical problem is as follows:

[0008] based on 63 The heterojunction high-efficiency nuclear battery of NiO carrier transport layer includes: sapphire substrate, non-doped GaN buffer layer, P-type GaN hole collection layer, P-type 63 NiO carrier transport layer and N-type ZnO electron collection layer; the P-type 63 The beta particles emitted by the NiO carrier transport layer generate hole-electron pairs through the radiation ionization effect. Under the action of the built-in electric field, the electrons move toward the N-type ZnO electron collection layer and are collected by the N-type ZnO electron collection layer, and the holes move toward the P-type GaN hole collection layer and are collected by the P-type GaN hole collection layer, thereby forming a current.

[0009] Preferably, the P-type GaN hole collection layer, 63 The NiO carrier transport layer and the N-type ZnO electron collection layer form a PPN type gradient composition heterojunction.

[0010] Preferably, Ni / Au electrodes are provided on the P-type GaN hole collection layer and the N-type ZnO electron collection layer, respectively, and a resistor is provided between the Ni / Au electrodes.

[0011] Preferably, the Ni / Au metal electrode evaporated on the P-type GaN hole collection layer has a thickness of Ni and Au of 20 nm and 20 nm respectively.

[0012] Preferably, the Ti / Au metal electrode evaporated on the N-type ZnO electron collection layer has a thickness of Ti and Au of 30 nm and 50 nm respectively.

[0013] Preferably, the P-type GaN hole collection layer is a Mg-doped thin film with a thickness of 4 μm to 12 μm.

[0014] Preferably, the P type 63 The NiO carrier transport layer is a Cu-doped thin film with a thickness of 300nm to 350nm.

[0015] Preferably, the N-type ZnO electron collection layer is an Al-doped thin film with a thickness of 4.5 to 9 μm.

[0016] Preferably, the sapphire substrate is a (001) oriented hexagonal Al2O3 layer.

[0017] A kind of 63 A method for preparing a heterojunction high-efficiency nuclear battery with a NiO carrier transport layer, the method comprising the following steps:

[0018] Step 1: Clean the (001) oriented sapphire substrate in a mixture of hot concentrated sulfuric acid and concentrated phosphoric acid in a volume ratio of 3:1 for at least 5 minutes;

[0019] Step 2: Using metal organic chemical vapor deposition, first grow a non-doped GaN buffer layer at 500°C to 600°C with a thickness of 1 to 2 μm; then adjust the temperature to 1000°C to grow a Mg-doped P-type GaN hole collection layer with a thickness of 4 to 12 μm;

[0020] Step 3: Deposition of Cu-doped P-type using sol-gel method 63 NiO carrier transport layer, containing radionuclides 63 Ni-NiAcetate Tetrahydrate 63Ni(CH3COO)2·4H2O was used as a precursor, ethylene glycol methyl ether CH3OCH2CH2OH was used as a solvent, and ethanolamine C2H7NO was used as a stabilizer. Stirring was performed at room temperature. 63 The Ni(CH3COO)2·4H2O powder was completely dissolved; copper acetate pentahydrate Cu(CH3COO)2·5H2O powder was added to the precursor mixed solution, heated in a water bath at a constant temperature of 60°C and stirred for 2 hours; after aging for 24 hours, it was filtered to obtain a colorless, transparent, homogeneous sol; the position of the Ni / Au electrode was reserved, and the prepared sol was evenly spin-coated on the P-type GaN hole collection layer, and heat-treated at 600°C, and repeated several times to obtain a Cu-doped sol with a thickness of 300 to 350 nm. 63 NiO thin film.

[0021] Step 4: Using metal organic chemical vapor deposition 63 An Al-doped N-type ZnO electron collection layer is grown on the NiO carrier transport layer, with a thickness of 4.5 to 9 μm;

[0022] Step 5: Use photolithography to evaporate Ni / Au electrodes on the Mg-doped P-type GaN hole collection layer; first, apply adhesive to the P-type GaN hole collection layer, then apply photoresist, bake at 90°C for 2 minutes, and photolithograph the required electrode pattern; then bake at 90°C for 2 minutes, and develop the sample; finally, use a vacuum thermal electron beam evaporation system to evaporate Ni / Au metal electrodes, with the thickness of Ni and Au being 20nm and 20nm respectively;

[0023] Step 6: Strip off the remaining photoresist and anneal at 550°C for 10 min in an air atmosphere to alloy the Ni / Au double-layer metal electrode;

[0024] Step 7: using photolithography to evaporate Ti / Au electrode 9 on the Al-doped N-type ZnO electron collection layer; the process flow is the same as that of step 5, and the thickness of Ti and Au are 30nm and 50nm respectively;

[0025] Step 8: Strip off the remaining photoresist and anneal at 300° C. for 1 min in a nitrogen atmosphere to alloy the Ti / Au double-layer metal electrode.

[0026] The beneficial effects of the present invention are: the present invention provides a 63 NiO carrier transport layer heterojunction high efficiency nuclear battery, 63 The NiO carrier transport layer, as part of both the energy carrier unit and the energy conversion unit, fundamentally solves the drawbacks of the self-absorption effect of nuclear batteries. 63The gradient component heterojunction composed of NiO layer and N-type ZnO layer utilizes the advantages of wide bandgap semiconductors such as good radiation resistance and high carrier mobility as well as its own gradient component energy level structure, which is beneficial to the transport of carriers, reduces the reverse saturation current, and improves the energy conversion efficiency of nuclear batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention is based on 63 Schematic diagram of the heterojunction high-efficiency nuclear battery structure with NiO carrier transport layer.

[0028] Figure 2 Schematic diagram of the energy conversion mechanism of the PPN type heterojunction β-radiation voltaic effect nuclear battery of the present invention.

[0029] Figure 3 Energy band distribution diagram of the PPN type gradient component heterogeneous nodule battery of the present invention.

[0030] In the figure: 1. Sapphire substrate, 2. Undoped GaN buffer layer, 3. P-type GaN hole collection layer, 4. Ni / Au electrode, 5. P-type 63 NiO carrier transport layer, 6, first wire, 7, N-type ZnO electron collection layer, 8, load resistor, 9, Ti / Au electrode, 10, second wire, 16, electron, 17, hole, zone I, N-type ZnO electron collection zone, zone II, P-type 63 NiO carrier transport region, region III, and P-type GaN hole collection region. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below with reference to the accompanying drawings and embodiments.

[0032] The present invention provides a 63 NiO carrier transport layer heterojunction high efficiency nuclear battery. Figure 1 The PPN heterojunction cell is stacked from bottom to top in sequence as follows: a sapphire substrate 1, a non-doped GaN buffer layer 2, a P-type GaN hole collection layer 3, a P-type 63 NiO carrier transport layer 5 and N-type ZnO electron collection layer 7; the Ni / Au electrode 4 is evaporated on the upper surface of the P-type GaN hole collection layer 3; the Ti / Au electrode 9 is evaporated on the upper surface of the N-type ZnO electron collection layer 7; the Ni / Au electrode and the Ti / Au electrode 9 are connected by a first wire 6, a load resistor 8 and a second wire 10. The P-type 63The β particles emitted by the NiO carrier transport layer 5 generate hole-electron pairs through the radiation ionization effect. Under the action of the built-in electric field, the electrons move to the N-type ZnO electron collection layer 7 and are collected by the N-type ZnO electron collection layer 7, and the holes move to the P-type GaN hole collection layer 3 and are collected by the P-type GaN hole collection layer 3. A first Ni / Au electrode 4 and a second Ti / Au electrode 9 are respectively provided on the P-type GaN hole collection layer 3 and the N-type ZnO electron collection layer 7. A load resistor 8 is provided between the Ni / Au electrode 4 and the Ti / Au electrode 9 to form a current. The P-type GaN hole collection layer 3 and the P-type GaN hole collection layer 3 are provided with a first Ni / Au electrode 4 and a second Ti / Au electrode 9. 63 The NiO carrier transport layer 5 and the N-type ZnO electron collection layer 7 form a PPN type gradient composition heterojunction.

[0033] In this embodiment, in the Ni / Au electrode 4, the thicknesses of Ni and Au are 20 nm and 20 nm respectively; in the Ti / Au electrode 9, the thicknesses of Ti and Au are 30 nm and 50 nm respectively. The P-type GaN hole collection layer 3 is a Mg-doped thin film with a thickness of 12 μm. 63 The NiO carrier transport layer 5 is a Cu-doped film with a thickness of 300 nm. The N-type ZnO electron collection layer 7 is an Al-doped film with a thickness of 9 μm. The sapphire substrate 1 is a (001) oriented hexagonal Al2O3 layer. Since the lattice mismatch between GaN and sapphire is too large, a two-step growth process is required: first, an undoped GaN buffer layer 2 with the same size as the substrate is epitaxially grown, and then a P-type GaN hole collection layer 3 is grown.

[0034] The bottom areas of the sapphire substrate 1, the non-doped GaN buffer layer 2 and the P-type GaN hole collection layer 3 are the same. 63 The bottom areas of the NiO carrier transport layer 5 and the N-type ZnO electron collection layer 7 are the same. The bottom area of ​​the P-type GaN hole collection layer 3 is larger than the bottom area of ​​the N-type ZnO electron collection layer 7 .

[0035] based on 63 The preparation method of a heterojunction high-efficiency nuclear battery with a NiO carrier transport layer comprises the following steps:

[0036] Step 1: Clean the (001) oriented sapphire substrate 1 in a mixture of hot concentrated sulfuric acid and concentrated phosphoric acid in a volume ratio of 3:1 for at least 5 minutes. In this embodiment, the cleaning time is 6 minutes.

[0037] Step 2: Using metal organic chemical vapor deposition, first grow a very thin non-doped GaN buffer layer 2 at a relatively low temperature (550°C) with a growth thickness of about 1.5μm. Then adjust the temperature to 1000°C to grow a Mg-doped P-type GaN hole collection layer 3 with a growth thickness of about 12μm to ensure complete energy deposition.

[0038] Step 3: Deposition of Cu-doped P-type using sol-gel method 63 NiO carrier transport layer, containing radionuclides 63 Ni-NiAcetate Tetrahydrate 63 Ni(CH3COO)2·4H2O was used as a precursor, ethylene glycol methyl ether CH3OCH2CH2OH was used as a solvent, and ethanolamine C2H7NO was used as a stabilizer. Stirring was performed at room temperature. 63 The Ni(CH3COO)2·4H2O powder was completely dissolved; copper acetate pentahydrate Cu(CH3COO)2·5H2O powder was added to the precursor mixed solution, heated in a water bath at a constant temperature of 60°C and stirred for 2 hours; after aging for 24 hours, it was filtered to obtain a colorless, transparent, homogeneous sol; the position of the Ni / Au electrode was reserved, and the prepared sol was evenly spin-coated on the P-type GaN hole collection layer, and heat-treated at 600°C, and repeated several times to obtain a Cu-doped layer with a thickness of 300nm. 63 NiO thin film.

[0039] Step 4: Using metal organic chemical vapor deposition 63 An Al-doped N-type ZnO electron collection layer 7 is grown on the NiO carrier transport layer 5 with a growth thickness of about 9 μm to ensure complete energy deposition.

[0040] Step 5: Prepare Ni / Au electrode 4, and evaporate Ni / Au electrode 4 on Mg-doped P-type GaN hole collection layer 3 by photolithography. First, apply adhesive to the clean P-type GaN hole collection layer 3, then apply photoresist, bake at 90°C for 2 minutes, and photolithograph the required electrode pattern. Then bake at 90°C for 2 minutes, and use developer to develop the sample. Finally, use vacuum thermal electron beam evaporation system to evaporate Ni / Au electrode 4, with the thickness of Ni and Au being 20nm and 20nm respectively.

[0041] Step 6: Strip off the remaining photoresist and anneal at 550° C. for 10 min in an air atmosphere to alloy the Ni / Au electrode 4 to form a good ohmic contact electrode.

[0042] Step 7: Prepare Ti / Au electrode 9, and use photolithography to evaporate Ti / Au electrode 9 on Al-doped N-type ZnO electron collection layer 7. The same process as step 5, after the process of coating, pre-baking, photolithography, baking, and developing, use a vacuum thermal electron beam evaporation system to evaporate Ti / Au electrode 9, the thickness of Ti and Au are 30nm and 50nm respectively.

[0043] Step 8: Strip off the remaining photoresist and anneal at 300°C for 1 min in a nitrogen atmosphere to alloy the Ti / Au double-layer metal electrode to form a good ohmic contact electrode.

[0044] NiO is a typical P-type semiconductor with a bandgap of 3.6 to 4.0 eV at room temperature. NiO can form high-quality heterojunctions with GaN and ZnO. The heterojunction structure of n-ZnO / NiO / p-GaN is usually used as ultraviolet light-emitting diodes. It is worth noting that the NiO in ultraviolet light-emitting diodes is intrinsic. Due to the influence of its bandgap and electron affinity, the intrinsic NiO acts as an electron blocking layer, effectively promoting the recombination of hole-electron pairs in the light-emitting diode and stimulating photons. However, NiO semiconductors can adjust the bandgap and electron affinity by doping to adapt them to different needs. Doping Cu in NiO can adjust the bandgap of NiO-based films in the range of 3.0 to 4.0 eV, and at the same time, it can also increase the electron affinity of the film. At this time, according to the affinity energy rule of semiconductor heterojunction, n-ZnO / p-NiO / p-GaN can achieve a gradient component energy level structure. p-NiO no longer acts as an electron blocking layer, but serves as the main area of ​​the depletion layer of the wide bandgap semiconductor heterojunction, separating hole-electron pairs and transmitting carriers.

[0045] In summary, the embodiments of the present invention describe in detail a method based on 63 It should be noted that the above is only a specific embodiment of the present invention, and it is not intended to limit the design and preparation of the nuclear battery of the present invention. In the present invention specification, in order to simply and clearly explain the structure and principle, the attached Figure 1 , 2 , 3 are only for explanation of general structure and principle, and are not drawn strictly according to structural proportions.

Claims

1. Based on 63 NiO carrier transport layer for heterojunction high-efficiency nuclear batteries, It is characterized in that The nuclear battery includes: a sapphire substrate, a non-doped GaN buffer layer, a P-type GaN hole collection layer, a P-type 63 NiO carrier transport layer and N-type ZnO electron collection layer; 63 The beta particles emitted by the NiO carrier transport layer generate hole-electron pairs through the radiation ionization effect. Under the action of the built-in electric field, the electrons move toward the N-type ZnO electron collection layer and are collected by the N-type ZnO electron collection layer, and the holes move toward the P-type GaN hole collection layer and are collected by the P-type GaN hole collection layer, thereby forming a current.

2. According to claim 1, based on 63 NiO carrier transport layer for heterojunction high-efficiency nuclear batteries, It is characterized in that The P-type GaN hole collection layer, the P-type 63 The NiO carrier transport layer and the N-type ZnO electron collection layer form a PPN type gradient composition heterojunction.

3. The method according to claim 1 or 2 63 NiO carrier transport layer for heterojunction high-efficiency nuclear batteries, It is characterized in that Ni / Au electrodes are respectively arranged on the P-type GaN hole collection layer and the N-type ZnO electron collection layer, and a resistor is arranged between the Ni / Au electrodes.

4. The method according to claim 3 63 NiO carrier transport layer for heterojunction high-efficiency nuclear batteries, It is characterized in that The Ni / Au metal electrode evaporated on the P-type GaN hole collection layer has a thickness of 20 nm and Au of 20 nm respectively.

5. The method according to claim 3 63 NiO carrier transport layer for heterojunction high-efficiency nuclear batteries, It is characterized in that The Ti / Au metal electrode evaporated on the N-type ZnO electron collection layer has a thickness of 30 nm and Au of 50 nm respectively.

6. The method according to claim 1 63 NiO carrier transport layer for heterojunction high-efficiency nuclear batteries, It is characterized in that The P-type GaN hole collection layer is a Mg-doped thin film with a thickness of 4 μm to 12 μm.

7. The method according to claim 1 63 NiO carrier transport layer for heterojunction high-efficiency nuclear batteries, It is characterized in that The P-type 63 The NiO carrier transport layer is a Cu-doped thin film with a thickness of 300nm to 350nm.

8. The method according to claim 1 63 NiO carrier transport layer for heterojunction high-efficiency nuclear batteries, It is characterized in that The N-type ZnO electron collection layer is an Al-doped thin film with a thickness of 4.5 to 9 μm.

9. The method according to claim 1 63 NiO carrier transport layer for heterojunction high-efficiency nuclear batteries, It is characterized in that The sapphire substrate is a (001) oriented hexagonal Al 2 O 3 layer.

10. Based on any one of claims 1 to 9 63 Preparation method of heterojunction high-efficiency nuclear battery with NiO carrier transport layer, It is characterized in that The method comprises the following steps: Step 1: Clean the (001) oriented sapphire substrate in a mixture of hot concentrated sulfuric acid and concentrated phosphoric acid in a volume ratio of 3:1 for at least 5 minutes; Step 2: Using metal organic chemical vapor deposition, first grow a non-doped GaN buffer layer at 500°C to 600°C with a thickness of 1 to 2 μm; then adjust the temperature to 1000°C to grow a Mg-doped P-type GaN hole collection layer with a thickness of 4 to 12 μm; Step 3: Deposition of Cu-doped P-type using sol-gel method 63 NiO carrier transport layer, containing radionuclides 63 Ni-NiAcetate Tetrahydrate 63 Ni(CH 3 COO 2 ·4H 2 O as a precursor, ethylene glycol methyl ether CH 3 OCH 2 CH 2 OH as solvent, ethanolamine C 2 H 7 NO is used as a stabilizer and stirred at room temperature. 63 Ni(CH 3 COO 2 ·4H 2 O powder was completely dissolved; copper acetate pentahydrate Cu(CH 3 COO 2 ·5H 2 O powder, heated, stirred and filtered to obtain a colorless, transparent, homogeneous sol; leaving a position for the Ni / Au electrode, the prepared sol is evenly spin-coated on the P-type GaN hole collection layer, and heat-treated at 600°C, repeated several times, to obtain a Cu-doped sol with a thickness of 300-350nm. 63 NiO thin film; Step 4: Using metal organic chemical vapor deposition 63 An Al-doped N-type ZnO electron collection layer is grown on the NiO carrier transport layer, with a thickness of 4.5 to 9 μm; Step 5: Use photolithography to evaporate Ni / Au electrodes on the Mg-doped P-type GaN hole collection layer; first, apply adhesive to the P-type GaN hole collection layer, then apply photoresist, bake at 90°C for 2 minutes, and photolithograph the required electrode pattern; then bake at 90°C for 2 minutes, and develop the sample; finally, use a vacuum thermal electron beam evaporation system to evaporate Ni / Au metal electrodes, with the thickness of Ni and Au being 20nm and 20nm respectively; Step 6: Strip off the remaining photoresist and anneal at 550°C for 10 min in an air atmosphere to alloy the Ni / Au double-layer metal electrode; Step 7: using photolithography to deposit a Ti / Au electrode (9) on the Al-doped N-type ZnO electron collection layer; the process is the same as that of step 5, and the thicknesses of Ti and Au are 30 nm and 50 nm respectively; Step 8: Strip off the remaining photoresist and anneal at 300° C. for 1 min in a nitrogen atmosphere to alloy the Ti / Au double-layer metal electrode.