Method for manufacturing polarizing film, device for manufacturing polarizing film and control system
By combining the tension meter and the tension cutting roller between the processing groove and the bonding roller, the tension change problem caused by the low moisture rate of the polarizing mirror on the oven outlet side is solved, and the stable transportation of the polarizing film is achieved.
Patent Information
- Application Number
- CN202080065896.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-19
- Filing Date
- 2020-07-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-07-28
AI Technical Summary
In the existing polarizing film manufacturing method, the low moisture rate of the polarizing mirror on the outflow side of the oven leads to a large change in tension, affecting the transport stability, and prone to transport obstacles or fracture problems.
A tension gauge and a first tension cutting roller are arranged between the processing groove and the bonding roller. The circumferential speed of the tension cutting roller is adjusted by constant tension control to ensure that the tension is within a predetermined value range and reduce tension changes in the polarizing mirror.
Even if the moisture content of the polarizer on the oven is low, the transport of the polarizer is stabilized, avoiding the risk of transport obstacles and fracture.
Smart Images

Figure CN114514112B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a polarizing film, an apparatus for manufacturing a polarizing film, and a control system, wherein a roll film is uniaxially stretched while being dyed with a dichroic substance in a treatment tank, then dried in an oven to produce a polarizer, and the polarizer is laminated to a protective film by a laminating roller to produce a polarizing film. In particular, the present invention relates to a method for manufacturing a polarizing film, an apparatus for manufacturing a polarizing film, and a control system, which can stabilize the transportation of the polarizer between the treatment tank and the laminating roller even if the moisture content of the polarizer at the exit side of the oven is low. Background Art
[0002] Conventionally, polarizing films including polarizers are used as constituent materials of liquid crystal display devices, polarized sunglasses, etc. The polarizing films are composed of, for example, a polarizer dyed with a dichroic substance such as iodine and a protective film bonded to the polarizer to protect the polarizer.
[0003] As described in Patent Document 1, for example, the polarizing film is produced by a roll-to-roll method in which a series of steps from producing a long strip of polarizer to bonding a long strip of protective film to obtain a long strip of polarizing film are performed on one production line.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2004-341515 Summary of the invention
[0007] Problems to be solved by the invention
[0008] Figure 3 This is a diagram schematically showing an example of the general configuration of a manufacturing device and a control system used in a conventional roll-to-roll method for manufacturing a polarizing film. Figure 3 The arrows indicated by solid lines indicate the conveying direction of each film.
[0009] like Figure 3As shown, in the conventional method for manufacturing a polarizing film, first, a roll film F0 wound on a delivery roller 1 is drawn out, immersed in a treatment bath in a treatment tank 2 (for example, a swelling treatment tank, a dyeing treatment tank, a cross-linking treatment tank, a stretching treatment tank, and a cleaning treatment tank, in order from the upstream side of the conveying direction of the roll film F0), dyed with a dichroic substance such as iodine or a dichroic dye, and uniaxially stretched. Next, it is dried in an oven 3, thereby obtaining a polarizer F1. Next, for example, an active energy ray-curable adhesive is applied to both sides of the polarizer F1 using a coating machine 6. In addition, for example, an active energy ray-curable adhesive is applied to one side of a protective film F2 drawn out from a delivery roller (not shown) using a coating machine (not shown). Then, the protective film F2 coated with the adhesive is bonded to both sides of the polarizer F1 coated with the adhesive by a bonding roller 7. Then, although not shown in the figure, the adhesive between the polarizer F1 and the protective film F2 is irradiated with active energy rays from an active energy ray irradiation device to be cured, and then dried in an oven, and other films (surface protective film, etc.) are bonded as needed to produce a polarizing film.
[0010] like Figure 3 As shown, the conventional manufacturing apparatus comprises: a first tension cutting roller 20 disposed between the processing tank 2 and the laminating roller 7 and conveying the polarizer F1 (including the roll film F0 after being processed in the processing tank 2 and before being dried in the oven 3), and a second tension cutting roller 60 conveying the roll film F0 in the processing tank 2. Figure 3 In the example shown, three first tension cutting rollers 20a to 20c are arranged as the first tension cutting rollers 20, and five second tension cutting rollers 60a to 60e are arranged as the second tension cutting rollers 60. Figure 3 In the illustrated example, both the first tension cutting roller 20 and the second tension cutting roller 60 are nip rollers.
[0011] A conventional control system 100A includes a control device 40 and an encoder 50 .
[0012] The encoder 50 measures the rotation speed of the laminating roller 7 and outputs it to the control device 40. The control device 40 calculates the peripheral speed P0' of the laminating roller 7 based on the input rotation speed of the laminating roller 7 and the pre-stored outer diameter of the laminating roller 7. Then, the control device 40 controls the peripheral speed of the first tension cutting roller 20 in such a way that the ratio of the peripheral speed P0' of the laminating roller 7 to the peripheral speed of the first tension cutting roller 20 becomes a predetermined value (ratio constant control). Specifically, when the circumferential speed of the first tension cutting roller 20a is set to P1a, the circumferential speed of the first tension cutting roller 20b is set to P1b, and the circumferential speed of the first tension cutting roller 20c is set to P1c, the control device 40 determines the circumferential speeds P1a, P1b, and P1c in the manner of P1a / P0'=α1, P1b / P0'=α2, and P1c / P0'=α3 (α1, α2, and α3 are given constants), so that the first tension cutting rollers 20a to 20c are rotated at the respective circumferential speeds P1a to P1c, and the control signal is sent to the driving part (motor etc. not shown in the figure) of the first tension cutting rollers 20a to 20c. Generally speaking, since the laminating roller 7 rotates at a predetermined constant circumferential speed, the first tension cutting roller 20 also rotates at a constant circumferential speed.
[0013] It should be noted that in Figure 3 In the example shown, the circumferential speed P0' of the bonding roller 7 is calculated based on the result obtained by measuring the rotational speed of the bonding roller 7, and the circumferential speed of the first tension cutting roller 20 is controlled based on the calculated circumferential speed P0'. However, sometimes the circumferential speed of the bonding roller 7 is not actually measured / calculated, but the circumferential speed of the first tension cutting roller 20 is controlled based on the set value of the circumferential speed of the bonding roller 7 or the set value of the rotational speed.
[0014] The control device 40 controls the peripheral speed of the second tension cutting roller 60 so that the ratio of the peripheral speed P0' of the laminating roller 7 to the peripheral speed of the second tension cutting roller 60 becomes a predetermined value (ratio constant control). Specifically, when the circumferential speed of the second tension cutting roller 60a is set to P2a, the circumferential speed of the second tension cutting roller 60b is set to P2b, the circumferential speed of the second tension cutting roller 60c is set to P2c, the circumferential speed of the second tension cutting roller 60d is set to P2d, and the circumferential speed of the second tension cutting roller 60e is set to P2e, the control device 40 determines the circumferential speeds P2a, P2b, P2c, P2d and P2e in a manner such that P2a / P0'=β1, P2b / P0'=β2, P2c / P0'=β3, P2d / P0'=β4, P2e / P0'=β5 (β1, β2, β3, β4, β5 are given constants) so that the second tension cutting rollers 60a~60e are rotated at their respective circumferential speeds P2a~P2e, and a control signal is sent to the driving part (motor etc. not shown in the figure) of the second tension cutting rollers 60a~60e. As described above, generally, the laminating roll 7 rotates at a constant peripheral speed, and therefore, the second tension cutting roll 60 also rotates at a constant peripheral speed.
[0015] The constant ratio control of the peripheral speed of the second tension cutting roller 60 is necessary to stretch the web film F0 at a predetermined given stretch ratio.
[0016] In the method for manufacturing a polarizing film using the existing control system 100A described above, the circumferential speed of the first tension cutting roller 20 for transporting the polarizer F1 is controlled by a constant ratio control method between the processing tank 2 and the bonding roller 7, and the set tension of the polarizer F1 to be transported at each position is determined by each ratio α1 to α3. However, the tension actually generated in the polarizer F1 varies greatly depending on the state of the polarizer F1. If the tension actually generated in the polarizer F1 varies greatly, sometimes the transportation of the polarizer F1 will be hindered. In addition, if excessive tension is generated, there is a possibility that the polarizer F1 will break. Moreover, even if the polarizing film is manufactured under the same manufacturing conditions, the reproducibility of the tension actually generated in the polarizer F1 is poor. Therefore, it is necessary for the operator to manually fine-tune each ratio α1 to α3.
[0017] The method of transporting the polarizer F1 (transportation between the processing tank 2 and the bonding roller 7) in the conventional method of manufacturing a polarizing film is not likely to cause trouble when the polarizer F1 is likely to expand and contract relatively greatly. That is, if the polarizer F1 is likely to expand and contract greatly, even if the actual tension varies greatly, the influence of the tension variation can be mitigated by the expansion and contraction of the polarizer F1.
[0018] However, in recent years, the production of polarizers F1 having a low moisture content (for example, the moisture content of the polarizer F1 at the exit side of the oven 3 is 15% or less) has begun.
[0019] The polarizer F1 having a low moisture content hardly expands or contracts. Therefore, in the conventional method for producing a polarizing film, it is difficult to alleviate the influence of tension fluctuations, and there is a problem that the transportation of the polarizer F1 may be hindered or the polarizer F1 may be broken.
[0020] Therefore, an object of the present invention is to provide a method for producing a polarizing film, a polarizing film producing apparatus, and a control system that can stabilize the conveyance of the polarizer between a treatment tank and a laminating roller even if the moisture content of the polarizer at the exit side of an oven is low.
[0021] Solutions to the problem
[0022] In order to solve the above-mentioned problems, the present invention provides a method for manufacturing a polarizing film, in which a roll film is dyed with a dichroic material while being uniaxially stretched in a treatment tank, and then, it is dried in an oven to make a polarizer, and the polarizer is laminated to a protective film with a laminating roller to manufacture the polarizing film. The above-mentioned manufacturing method includes: a first tension cutting roller for transporting the above-mentioned polarizer is arranged between the above-mentioned treatment tank and the above-mentioned laminating roller, and a tension meter is provided between the above-mentioned treatment tank and the above-mentioned laminating roller and on the downstream side of the above-mentioned first tension cutting roller, and a first control step of controlling the circumferential speed of the above-mentioned first tension cutting roller in such a way that the tension measured by the tension meter becomes a predetermined value.
[0023] The "tension cutting roller" in the present invention (the first tension cutting roller and the second tension cutting roller in the preferred method described later) refers to a roller on which the film will not slip and on which the tension difference between the upstream and downstream sides of the roller can be controlled. As a tension cutting roller, for example, a clamping roller or a suction roller can be used.
[0024] In addition, the "downstream side" in the present invention means the downstream side in the conveyance direction of the polarizer or the roll film.
[0025] According to the present invention, in the first control step, the peripheral speed of the first tension cutting roller is controlled so that the tension measured by the tension meter disposed on the downstream side of the first tension cutting roller reaches a predetermined value (hereinafter, appropriately referred to as "tension constant control"). That is, the peripheral speed of the first tension cutting roller is controlled so that the actually measured tension becomes a predetermined value, so that even if the moisture content of the polarizer on the oven outlet side is low, the variation of the tension actually generated in the polarizer becomes small, and the transportation of the polarizer can be stabilized.
[0026] It is preferred that a plurality of the tension meters and the first tension cutting rollers are alternately arranged between the treatment tank and the bonding roller. In the first control step, after the circumferential speed is controlled using a combination of the tension meter and the first tension cutting roller arranged on the most downstream side, the circumferential speed is controlled sequentially toward the upstream side by a combination of the tension meter and the first tension cutting roller arranged closer to the upstream side than the combination arranged on the most downstream side.
[0027] In the above-mentioned preferred method, "upstream side" refers to the upstream side of the conveying direction of the polarizer or the roll film. In addition, in the above-mentioned preferred method, "control of the circumferential speed using the combination of the above-mentioned tension meter and the above-mentioned first tension cutting roller arranged on the most downstream side" refers to controlling the circumferential speed of the first tension cutting roller arranged on the most downstream side in such a manner that the tension measured by the tension meter arranged on the most downstream side reaches a predetermined value. In addition, in the above-mentioned preferred method, "control of the circumferential speed using the combination of the above-mentioned tension meter and the above-mentioned first tension cutting roller arranged on the most downstream side closer to the upstream side than the combination arranged on the most downstream side" refers to controlling the circumferential speed of the first tension cutting roller arranged on the upstream side and closest to the tension meter in such a manner that the tension measured by the tension meter arranged on the most downstream side reaches a predetermined value. In addition, in the above-mentioned preferred method, "execute sequentially toward the upstream side" means that the control of the circumferential speed is performed sequentially toward the upstream side from the control of the circumferential speed using the combination of the tension meter and the first tension cutting roller arranged on the most downstream side to the control of the circumferential speed using the combination of the tension meter and the first tension cutting roller arranged on the most upstream side.
[0028] For example, in the case where the first tension cutting roller and the tension meter are arranged in groups of three each (the tension meter 30a, the first tension cutting roller 20a, the tension meter 30b, the first tension cutting roller 20b, the tension meter 30c, and the first tension cutting roller 20c are arranged in sequence from the downstream side), it means that after controlling the circumferential speed of the first tension cutting roller 20a in such a way that the tension measured using the tension meter 30a becomes a predetermined value, the circumferential speed of the first tension cutting roller 20b is controlled in such a way that the tension measured using the tension meter 30b becomes a predetermined value, and then the circumferential speed of the first tension cutting roller 20c is controlled in such a way that the tension measured using the tension meter 30c becomes a predetermined value.
[0029] According to the above preferred method, when a plurality of tension meters and first tension cutting rollers are alternately arranged, after the peripheral speed is controlled by the combination of the tension meter and the first tension cutting roller arranged on the most downstream side, the peripheral speed is controlled sequentially toward the combination arranged on the upstream side, so that the control does not dissipate and stable peripheral speed control can be achieved. Therefore, when a plurality of tension meters and first tension cutting rollers are alternately arranged, the variation of the tension actually generated in the polarizer becomes small, and the transportation of the polarizer can be stabilized.
[0030] Preferably, the method includes: arranging the first tension cutting roller on the exit side of the processing tank, and arranging the second tension cutting roller for conveying the roll film in the processing tank, and after executing the first control process, measuring the circumferential speed of the first tension cutting roller arranged on the exit side of the processing tank, and controlling the circumferential speed of the second tension cutting roller in such a manner that the ratio of the circumferential speed of the first tension cutting roller obtained by the above measurement to the circumferential speed of the second tension cutting roller reaches a predetermined value.
[0031] In the present invention, the circumferential speed of the first tension cutting roller is controlled in a tension constant control manner. Therefore, the circumferential speed of the first tension cutting roller arranged on the outlet side of the processing tank is different from the conventional case of being controlled in a ratio constant control manner, and varies instead of being constant.
[0032] According to the above-mentioned preferred method, in the second control step, the circumferential speed of the second tension cutting roller is basically controlled in such a way that the ratio of the circumferential speed of the first tension cutting roller arranged on the outlet side of the processing tank to the circumferential speed of the second tension cutting roller reaches a predetermined value, that is, the ratio constant control is performed. However, the circumferential speed of the first tension cutting roller arranged on the outlet side of the processing tank, which serves as a reference for the ratio, is the actually measured circumferential speed. Therefore, as described above, even if the circumferential speed of the first tension cutting roller arranged on the outlet side of the processing tank changes, the ratio constant control can be appropriately performed, and the roll film can be stretched at a predetermined given stretch ratio.
[0033] The present invention can be suitably used when the moisture content of the polarizer at the exit side of the oven is 15% or less, that is, it can be suitably used for a polarizer that hardly expands or contracts due to its low moisture content.
[0034] It should be noted that the "moisture content of the polarizer" refers to the proportion of water contained in the polarizer after drying in the oven. Specifically, the weight of the polarizer after drying in the oven (weight of the polarizer after drying) and the weight of the polarizer after substantially removing the water from the polarizer after drying (weight of the polarizer after complete drying) are measured respectively, and each weight is substituted into the following formula to obtain the value.
[0035] Moisture content of polarizer = (weight of polarizer after drying - weight of polarizer after complete drying) / weight of polarizer after drying × 100
[0036] The present invention can be suitably used when the thickness of the polarizer at the outlet side of the oven is 20 μm or less, that is, it can be suitably used for a polarizer that is thin and easily broken due to excessive tension.
[0037] In addition, in order to solve the above-mentioned problems, the present invention also provides a manufacturing device for a polarizing film, which comprises: a treatment tank for dyeing a roll film with a dichroic material while performing uniaxial stretching, an oven for drying the roll film treated in the above-mentioned treatment tank to make a polarizer, a bonding roller for bonding the above-mentioned polarizer to a protective film, and a first tension cutting roller arranged between the above-mentioned treatment tank and the above-mentioned bonding roller and for transporting the above-mentioned polarizer, the above-mentioned manufacturing device comprises: a tension meter arranged between the above-mentioned treatment tank and the above-mentioned bonding roller and located on the downstream side of the above-mentioned first tension cutting roller, and a control device, the above-mentioned control device controls the circumferential speed of the above-mentioned first tension cutting roller in such a way that the tension measured by the tension meter becomes a predetermined value.
[0038] Furthermore, in order to solve the above-mentioned problem, the present invention further provides a control system used in the above-mentioned polarizing film manufacturing device, the control system comprising: the above-mentioned tensiometer and the above-mentioned control device.
[0039] Effects of the Invention
[0040] According to the present invention, even if the moisture content of the polarizer at the exit side of the oven is low, the conveyance of the polarizer between the treatment tank and the laminating roller can be stabilized. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is a diagram schematically showing an example of the general configuration of a polarizing film manufacturing apparatus to which a polarizing film manufacturing method according to one embodiment of the present invention is applied.
[0042] Figure 2 More specifically, Figure 1 A diagram showing a portion of a polarizing film manufacturing apparatus related to a control system.
[0043] Figure 3 This is a diagram schematically showing an example of the general configuration of a manufacturing device and a control system used in a conventional roll-to-roll method for manufacturing a polarizing film.
[0044] Explanation of symbols
[0045] F0···Roll Film
[0046] F1···Polarizer
[0047] F2···Protective film
[0048] F···Polarizing film
[0049] 2···Treatment tank
[0050] 3. Oven
[0051] 7···Laminating roller
[0052] 20, 20a, 20b, 20c... first tension cutting roller
[0053] 30, 30a, 30b, 30c...Tensiometer
[0054] 40···Control device
[0055] 60, 60a, 60b, 60c, 60d, 60e...second tension cutting roller
[0056] 70···Encoder
[0057] 100···Control System DETAILED DESCRIPTION
[0058] Hereinafter, a method for manufacturing a polarizing film, a polarizing film manufacturing apparatus, and a control system according to an embodiment of the present invention will be described with reference to the drawings.
[0059] It should be noted that, in this specification, the numerical range represented by "lower limit value X to upper limit value Y" means greater than the lower limit value X and less than the upper limit value Y. When a plurality of the above numerical ranges are respectively described, any lower limit value and any upper limit value can be selected to set "any lower limit value to any upper limit value".
[0060] In addition, each drawing is shown for reference only, and it should be noted that the size, scale, and shape of the components and the like shown in each drawing may be different from the actual ones.
[0061] In addition, in the following description, a "manufacturing method of a polarizing film" and a "manufacturing apparatus of a polarizing film" may be simply referred to as a "manufacturing method" and a "manufacturing apparatus", respectively.
[0062] Figure 1 It is a figure which shows typically the outline|summary structural example of the manufacturing apparatus of the polarizing film to which the manufacturing method of the polarizing film of this embodiment is applied. Figure 2 Yes Figure 1 FIG. 2 is a diagram of a portion of a polarizing film manufacturing apparatus related to the control system of the present embodiment. Figure 1 and Figure 2 The arrows shown indicate the transport direction of the respective films.
[0063] like Figure 1 or Figure 2 As shown, the manufacturing device of the present embodiment is a roll-to-roll manufacturing device that performs a series of processes from the manufacture of the polarizer F1 to at least bonding the protective film F2 to obtain the polarizing film F on one production line. The manufacturing device of the present embodiment comprises: a treatment tank 2 for dyeing the roll film F0 with a dichroic substance while performing uniaxial stretching, an oven 3 for drying the roll film F0 treated in the treatment tank 2 to produce the polarizer F1, a bonding roller 7 for bonding the polarizer F1 and the protective film F2, and a first tension cutting roller 20 that is arranged between the treatment tank 2 and the bonding roller 7 and transports the polarizer F1. A plurality of first tension cutting rollers 20 of the present embodiment are arranged. Specifically, as Figure 2 As shown, three first tension cutting rollers 20a to 20c are arranged in order from the downstream side (downstream side in the conveying direction of the polarizer F1) as the first tension cutting rollers 20. The first tension cutting rollers 20 of the present embodiment are all nip rollers.
[0064] However, the present invention is not limited thereto, and two or more first tension cutting rollers 20 may be provided, or only one first tension cutting roller 20 may be provided. In addition, the first tension cutting roller 20 may be a roller of other forms such as a suction roller.
[0065] In addition, the manufacturing apparatus of this embodiment is provided with a tension meter 30 disposed between the treatment tank 2 and the laminating roller 7 and located on the downstream side of the first tension cutting roller 20. In this embodiment, a plurality of tension meters 30 are disposed (the same number as the first tension cutting roller 20). Specifically, Figure 2 As shown, as the tension meter 30, three tension meters 30a to 30c are arranged in order from the downstream side. This is because three first tension cutting rollers 20 are arranged. More specifically, the three tension meters 30a to 30c are arranged alternately with the three first tension cutting rollers 20a to 20c. That is, the tension meter 30a is arranged on the downstream side of the first tension cutting roller 20a, the tension meter 30b is arranged on the downstream side of the first tension cutting roller 20b (the upstream side of the first tension cutting roller 20a), and the tension meter 30c is arranged on the downstream side of the first tension cutting roller 20c (the upstream side of the first tension cutting roller 20b).
[0066] As the tension meter 30 , for example, a micro-displacement tension detector “LX-100TD” manufactured by Mitsubishi Electric Corporation, which uses a micro-displacement method as a measurement principle, can be used.
[0067] Furthermore, the manufacturing apparatus of the present embodiment includes a control device 40. The control device 40 is constituted by a computer or a PLC (Programmable Logic Controller).
[0068] Furthermore, the manufacturing apparatus of the present embodiment includes an encoder 70 that measures the rotation speed of the first tension cutting roller 20 c disposed on the outlet side of the processing tank 2 .
[0069] The control system 100 of the present embodiment is configured to include the tension meter 30 , the control device 40 , and the encoder 70 described above.
[0070] In addition, the manufacturing apparatus of this embodiment includes a second tension cutting roller 60 for conveying the roll film F0 in the processing tank 2. A plurality of second tension cutting rollers 60 of this embodiment are arranged. Specifically, Figure 2 As shown in FIG. 1 , five second tension cutting rollers 60a to 60e are arranged in order from the upstream side (the upstream side in the conveying direction of the roll film F0). Figure 2 The structure of the treatment tank 2 in the figure is simplified and illustrated as a single tank, but in fact, the treatment tank 2 of this embodiment is composed of five tanks divided from the upstream side, namely, a swelling treatment tank, a dyeing treatment tank, a cross-linking treatment tank, a stretching treatment tank, and a cleaning treatment tank. The second tension cutting roller 60a is arranged at the entrance side of the swelling treatment tank, the second tension cutting roller 60b is arranged at the entrance side of the dyeing treatment tank, the second tension cutting roller 60c is arranged at the entrance side of the cross-linking treatment tank, the second tension cutting roller 60d is arranged at the entrance side of the stretching treatment tank, and the second tension cutting roller 60e is arranged at the entrance side of the cleaning treatment tank. The second tension cutting rollers 60 of this embodiment are all clamping rollers.
[0071] However, the present invention is not limited thereto, and two, three, four or six or more second tension cutting rollers 60 may be provided, or one second tension cutting roller 60 may be provided. In addition, the second tension cutting roller 60 may be a roller of other forms such as a suction roller.
[0072] The manufacturing apparatus of the present embodiment includes various conventionally known components that a general manufacturing apparatus of a polarizing film includes in addition to the components described above.
[0073] When the polarizing film F is manufactured using the manufacturing device of the present embodiment described above, first, the roll film F0 wound on the delivery roller 1 is unwound, immersed in the treatment bath in the treatment tank 2 (in the present embodiment, it is composed of a swelling treatment tank, a dyeing treatment tank, a cross-linking treatment tank, a stretching treatment tank, and a cleaning treatment tank in order from the upstream side of the conveying direction of the roll film F0), and uniaxially stretched while being dyed with a dichroic substance such as iodine and a dichroic dye. Next, it is dried in an oven 3 to obtain a polarizer F1. The polarizer F1 is an optical element having the property of transmitting light (polarized light) vibrating only in one specific direction and blocking light vibrating in other directions. The polarizer F1 of the present embodiment is in the form of a soft film.
[0074] The roll film F0 is in the form of a long strip. In this specification, the long strip refers to a rectangle whose length in the longitudinal direction is sufficiently greater than the length in the short side direction (direction perpendicular to the longitudinal direction). The length in the longitudinal direction of the long strip is, for example, 10 m or more, preferably 50 m or more.
[0075] As the roll film F0, there is no particular limitation. From the perspective of excellent dyeability using a dichroic substance, it is preferred to use a film comprising a hydrophilic polymer film (e.g., a polyvinyl alcohol film, etc.), and more preferably a hydrophilic polymer film. As a film comprising a hydrophilic polymer film, a film stacked with a hydrophilic polymer film and a non-hydrophilic polymer film can be cited. In this case, it is preferred that a hydrophilic polymer film is stacked on the surface and / or back of the non-hydrophilic polymer film. In this case, the hydrophilic polymer film stacked on the surface and / or back of the non-hydrophilic polymer film can be a thin film with a thickness of about several μm.
[0076] As the hydrophilic polymer film, there is no particular limitation, and existing known films can be used. Specifically, as the hydrophilic polymer film, for example: polyvinyl alcohol (PVA) films, partially formalized PVA films, polyethylene terephthalate (PET) films, ethylene-vinyl acetate copolymer films, their partially saponified films, etc. can be cited. In addition, in addition, polyene oriented films such as dehydrated products of PVA, dehydrochlorinated products of polyvinyl chloride, polyethylene films after stretching orientation, etc. can also be used. Among these, from the excellent dyeability of utilizing dichroic substances, particularly preferred PVA polymer films.
[0077] As the raw material polymer of the PVA polymer film, for example, a polymer obtained by polymerizing vinyl acetate and then saponifying it, a polymer obtained by copolymerizing vinyl acetate with a small amount of copolymerizable monomers such as unsaturated carboxylic acid and unsaturated sulfonic acid, etc. The polymerization degree of the PVA polymer is not particularly limited, but from the perspective of solubility in water, it is preferably 500 to 10000, and more preferably 1000 to 6000. In addition, the saponification degree of the PVA polymer is preferably 75 mol% or more, and more preferably 98 mol% to 100 mol%.
[0078] The thickness of the untreated film web F0 is not particularly limited, and is, for example, 15 μm to 110 μm.
[0079] As described above, the treatment tank 2 of this embodiment is composed of a swelling treatment tank, a dyeing treatment tank, a cross-linking treatment tank, a stretching treatment tank, and a cleaning treatment tank in order from the upstream side in the conveying direction of the roll film F0, and each tank has, for example, the following structure.
[0080] <Swelling treatment tank>
[0081] The swelling treatment tank is a treatment tank containing a swelling treatment liquid. The swelling treatment liquid swells the roll film F0. As the swelling treatment liquid, water, for example, can be used. In addition, an aqueous solution obtained by adding an appropriate amount of iodine compounds such as glycerol and potassium iodide to water can also be used as the swelling treatment liquid. When glycerol is added, its concentration is preferably 5% by weight or less, and when iodine compounds such as potassium iodide are added, its concentration is preferably 10% by weight or less.
[0082] <Dyeing treatment tank>
[0083] The dyeing treatment tank is a treatment tank containing a dyeing treatment liquid. The dyeing treatment liquid dyes the roll film F0. As the dyeing treatment liquid, a solution containing a dichroic substance as an effective ingredient can be listed. As the dichroic substance, iodine, organic dyes, etc. can be listed. It is preferred to use a solution obtained by dissolving iodine in a solvent as the dyeing treatment liquid. As a solvent, water is usually used, but an organic solvent that is compatible with water can also be further added. As the concentration of iodine in the dyeing treatment liquid, it is not particularly limited, preferably in the range of 0.01% by weight to 10% by weight, more preferably in the range of 0.02% by weight to 7% by weight, and further preferably in the range of 0.025% by weight to 5% by weight. In order to further improve the dyeing efficiency, iodine compounds can also be added to the dyeing treatment liquid as needed. Iodine compounds are compounds containing iodine and elements other than iodine in the molecule, and examples thereof include potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, titanium iodide, etc.
[0084] <Cross-linking treatment tank>
[0085] The cross-linking treatment tank is a treatment tank containing a cross-linking treatment liquid. The cross-linking treatment liquid cross-links the roll film F0 after dyeing. As the cross-linking treatment liquid, a solution containing a boron compound as an active ingredient can be used. For example, as the cross-linking treatment liquid, a solution obtained by dissolving a boron compound in a solvent can be used. As a solvent, water is usually used, but an organic solvent that is compatible with water can also be further added. As boron compounds, boric acid, borax, etc. can be listed. As the concentration of the boron compound in the cross-linking treatment liquid, it is not particularly limited, preferably 1% to 10% by weight, more preferably 2% to 7% by weight, and further preferably 2% to 6% by weight. In addition, from the perspective of obtaining a polarizer with uniform optical properties, an iodine compound can also be added to the cross-linking treatment liquid as needed.
[0086] <Stretching treatment tank>
[0087] The stretching treatment tank is a treatment tank that contains a stretching treatment liquid.
[0088] The stretching treatment liquid is not particularly limited, and for example, a solution containing a boron compound as an effective ingredient can be used. As the stretching treatment liquid, for example, a solution obtained by dissolving a boron compound and various metal salts, zinc compounds, etc. used as needed in a solvent can be used. As a solvent, water is usually used, but an organic solvent that is compatible with water can also be further added. The concentration of the boron compound in the stretching treatment liquid is not particularly limited, but is preferably 1% to 10% by weight, more preferably 2% to 7% by weight. From the viewpoint of suppressing the dissolution of iodine adsorbed on the film, an iodine compound can also be added to the stretching treatment liquid as needed.
[0089] <Washing tank>
[0090] The cleaning treatment tank is a treatment tank containing a cleaning treatment liquid. The cleaning treatment liquid cleans the stretched roll film F0. The cleaning treatment liquid is a treatment liquid for cleaning treatment liquids such as dyeing treatment liquid and cross-linking treatment liquid attached to the roll film F0. As the cleaning treatment liquid, water such as ion exchange water, distilled water, and pure water is typically used.
[0091] The oven 3 is installed on the downstream side of the cleaning treatment tank constituting the treatment tank 2 described above. The oven 3 is installed to dry the film after the treatment.
[0092] It should be noted that the treatment tank 2 of the present embodiment has a swelling treatment tank, a dyeing treatment tank, a cross-linking treatment tank, a stretching treatment tank and a cleaning treatment tank, but one or two treatment tanks thereof may be omitted. On the other hand, the treatment tank 2 may further have an adjustment treatment tank (not shown). The adjustment treatment tank is a treatment tank that accommodates an adjustment treatment solution. The adjustment treatment tank is arranged between the cross-linking treatment tank and the stretching treatment tank, or between the stretching treatment tank and the cleaning treatment tank. The whole treatment solution is a solution for adjusting the hue of the film, and a solution containing an iodine compound as an effective ingredient may be used.
[0093] The film obtained by drying the washed roll film F0 in the oven 3 is the polarizer F1.
[0094] The thickness of the polarizer F1 at the exit side of the oven 3 is not particularly limited, but for example, when it is 20 μm or less, the production method of this embodiment can be appropriately used.
[0095] The moisture content of the polarizer F1 on the exit side of the oven 3 is not particularly limited, but the manufacturing method of this embodiment can be appropriately used when it is 15% or less. For example, when the drying temperature in the oven 3 is 60° C. or more and the drying time is 30 seconds or more, the moisture content of the polarizer F1 on the exit side of the oven 3 is likely to be 15% or less.
[0096] The polarizer F1 to which the present invention can be preferably applied is not limited to a polarizer obtained by stretching a single-layer film, and may be a polarizer obtained by stretching a laminated film obtained by coating a PVA-based resin on a substrate.
[0097] As the above-mentioned polarizer, representative examples include thin polarizing films described in Japanese Patent Publication No. 51-069644, Japanese Patent Publication No. 2000-338329, International Publication No. 2010 / 100917, Japanese Patent Publication No. 2014-059328, and Japanese Patent Publication No. 2012-73563. These thin polarizing films can be obtained by a manufacturing method including a step of stretching a PVA-based resin layer and a stretching resin substrate in a laminated state and a step of dyeing. According to this manufacturing method, even if the PVA-based resin layer is thin, it can be stretched in a manner without undesirable conditions such as breakage caused by stretching because it is supported by the stretching resin substrate.
[0098] Next, if Figure 1 As shown, the active energy ray curing adhesive is applied to both sides of the polarizer F1 by the coater 6. In this embodiment, a gravure coater is used as the coater 6. In addition, the active energy ray curing adhesive is applied to one side of the protective film F2 drawn out from the drawing roller 5 by the coater 6. Then, the protective film F2 coated with the adhesive is bonded to both sides of the polarizer F1 coated with the adhesive by the bonding roller 7.
[0099] As the adhesive applied by the coater 6 , an active energy ray-curable adhesive is used.
[0100] As the active energy ray-curable adhesive, a conventionally known active energy ray-curable adhesive can be used. The active energy ray-curable adhesive generally contains an active energy ray-curable component and a polymerization initiator, and contains various additives as necessary.
[0101] Active energy ray-curable components can be roughly divided into electron beam curable, ultraviolet curable, and visible light curable. In addition, from the perspective of the curing mechanism, active energy ray-curable components can be roughly divided into radical polymerizable compounds and cation polymerizable compounds.
[0102] As free radical polymerizable compounds, compounds having free radical polymerizable functional groups of carbon-carbon double bonds such as (meth)acryloyl and vinyl groups can be cited. In addition, any free radical polymerizable compound among monofunctional free radical polymerizable compounds or polyfunctional free radical polymerizable compounds having more than two functions can be used. In addition, these free radical polymerizable compounds can be used alone or in combination of two or more. As free radical polymerizable compounds, compounds having (meth)acryloyl groups are preferred, and examples thereof include (meth)acrylamide derivatives having (meth)acrylamide groups, (meth)acrylates having (meth)acryloyloxy groups, and the like.
[0103] When a free radical polymerizable compound is used as the polymerization initiator of the active energy ray-curable adhesive, the polymerization initiator can be appropriately selected according to the active energy ray. When the adhesive is cured by ultraviolet light or visible light, a polymerization initiator that is cleaved by ultraviolet light or visible light is used. Examples of such polymerization initiators include benzophenone compounds, aromatic ketone compounds, acetophenone compounds, aromatic ketal compounds, aromatic sulfonyl chloride compounds, and thioxanthone compounds.
[0104] As the cationic polymerizable compound, a monofunctional cationic polymerizable compound having one cationic polymerizable functional group in the molecule, a polyfunctional cationic polymerizable compound having two or more cationic polymerizable functional groups in the molecule, etc. can be listed. As the cationic polymerizable functional group, an epoxy group, an oxetane group, a vinyl ether group, etc. can be listed. As the cationic polymerizable compound having an epoxy group, an aliphatic epoxy compound, an alicyclic epoxy compound, an aromatic epoxy compound, etc. can be listed. As the cationic polymerizable compound having an oxetane group, 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetane)methoxymethyl]benzene, 3-ethyl-3-(phenoxymethyl)oxetane, etc. can be listed. As the cationic polymerizable compound having a vinyl ether group, 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 4-hydroxybutyl vinyl ether, etc. can be listed.
[0105] When a cationic polymerizable compound is used as an active energy ray-curable adhesive, a cationic polymerization initiator is added. The cationic polymerization initiator generates cationic species or Lewis acid by irradiation with active energy rays such as visible light, ultraviolet rays, and electron beams, thereby initiating a polymerization reaction with an epoxy group of the cationic polymerizable compound. As the cationic polymerization initiator, a photoacid generator and a photobase generator can be used.
[0106] In the present invention, an active energy ray-curable adhesive that is cured by light including visible light of 380 nm to 450 nm may be used. In this case, an active energy ray-curable adhesive containing a radical polymerizable compound and a polymerization initiator is preferably used.
[0107] Such an active energy ray-curable adhesive is disclosed in, for example, Japanese Patent Publication No. 2018-092186, and as the active energy ray-curable adhesive of the present invention, the active energy ray-curable adhesive described in the above publication can be used. In this specification, due to space limitations, the transfer to the above publication is omitted, and the description related to the adhesive in the above publication is directly introduced into this specification.
[0108] The thickness of the adhesive coating is not particularly limited, but if it is too small, the bonding strength of the film decreases, and if it is too large, the thickness of the polarizing film F becomes relatively too large. From this viewpoint, the thickness of the adhesive coating formed on the polarizer F1 and the protective film F2 is preferably 0.1 μm to 5 μm respectively.
[0109] In addition, the viscosity of the adhesive at the start of coating is not particularly limited, but if it is too small or too large, the adhesiveness of the adhesive will decrease from the start of coating. From this viewpoint, the viscosity of the adhesive at 25° C. at the start of coating is preferably adjusted to 1 mPa·s to 100 mPa·s, more preferably 10 mPa·s to 50 mPa·s, and particularly preferably 15 mPa·s to 45 mPa·s.
[0110] The protective film F2 is in the form of a long strip. In addition, the protective film F2 is a film having lower hydrophilicity than the polarizer F1 (having hydrophobicity). As the protective film F2, it is preferred to have excellent transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, etc. Protective film F2 is preferably a protective film having excellent transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, etc. For example, polyester polymers such as polyethylene terephthalate and polyethylene naphthalate, cellulose polymers such as cellulose diacetate and cellulose triacetate, acrylic polymers such as polymethyl methacrylate, polystyrene, styrene polymers such as acrylonitrile-styrene copolymer (AS resin), polycarbonate polymers, etc. In addition, examples of polymers forming the protective film F2 include: polyethylene, polypropylene, polyolefins with a ring system or a norbornene structure, polyolefin polymers such as ethylene-propylene copolymers, vinyl chloride polymers, nylon, amide polymers such as aromatic polyamides, imide polymers, sulfone polymers, polyethersulfone polymers, polyetheretherketone polymers, polyphenylene sulfide polymers, vinyl alcohol polymers, vinylidene chloride polymers, vinyl butyral polymers, aromatic ester polymers, polyoxymethylene polymers, epoxy polymers, or blends of the above polymers. In the protective film F2, one or more appropriate additives may be included. As additives, for example, ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, anti-coloring agents, flame retardants, nucleating agents, antistatic agents, pigments, colorants, etc. The content of the thermoplastic resin in the protective film F2 is preferably 50 to 100% by weight, more preferably 50 to 99% by weight, further preferably 60 to 98% by weight, and particularly preferably 70 to 97% by weight. If the content of the thermoplastic resin in the protective film F2 is 50% by weight or less, there is a concern that the high transparency inherent in the thermoplastic resin may not be fully exhibited.
[0111] In addition, as the protective film F2, there can be cited the polymer film described in Japanese Patent Publication No. 2001-343529, for example (A) a thermoplastic resin having a substituted and / or unsubstituted imide group in the side chain, and a resin composition of a thermoplastic resin having a substituted and / or unsubstituted phenyl and nitrile group in the side chain. As a specific example, there can be cited a film of a resin composition containing an alternating copolymer formed by isobutylene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. As a film, a film formed by a mixed extrudate of a resin composition can be used. These films have a small phase difference and a small photoelastic coefficient, so that the unevenness caused by the strain of the polarizing film F can be eliminated. In addition, the moisture permeability is small, so the humidification durability is excellent.
[0112] Next, if Figure 1As shown, after the adhesive between the polarizer F1 and the protective film F2 is irradiated with active energy rays from the active energy ray irradiation device 8 and cured, it is dried in an oven 9. The active energy ray is appropriately selected according to the curability of the active energy ray curing adhesive. As active energy rays, electron beams, ultraviolet rays, visible light, etc. can be cited. Finally, the long strip-shaped surface protective film F3 extracted from the extraction roller 10 is laminated to one side of the polarizer F1 with the protective film F2 laminated on both sides by the laminating roller 11, thereby obtaining a long strip-shaped polarizing film F. The polarizing film F is rolled up with the winding roller 12.
[0113] It should be noted that in Figure 1 In the example shown, the active energy ray-curable adhesive is applied to both the polarizer F1 and the protective film F2, but the adhesive may be applied only to both sides of the polarizer F1. Figure 1 Of the total of 4 coating machines 6 shown, Figure 1 The two coating machines 6 are located on the lower side (downstream side of the polarizer F1 in the conveying direction). Alternatively, the adhesive may be applied only on one side of the protective film F2. In this case, there is no need Figure 1 Of the total of 4 coating machines 6 shown, Figure 1 2 coating machines 6 are arranged on the upper side (upstream side in the conveying direction of the polarizer F1). Figure 1 In the example shown, protective films F2 are attached to both sides of the polarizer F1, so that Figure 1 A pair of coaters 6 are arranged in the left and right directions, and a pair of active energy ray irradiation devices 8 are arranged in the left and right directions. However, in the case where the protective film F2 is attached to only one side of the polarizer F1, the coaters 6 and the active energy ray irradiation devices 8 may also be arranged in the left and right directions. Figure 1 Only one unit is configured in either the left or right direction.
[0114] Hereinafter, the operation of the control system 100 according to the present embodiment will be described.
[0115] The control device 40 of the control system 100 controls the peripheral speed of the first tension cutting roller 20 so that the tension measured by the tension meter 30 reaches a predetermined value (corresponding to the first control step of the present invention). Specifically, during the manufacture of the polarizing film F, the tension meter 30 always measures the tension of the polarizer F1 and outputs the measured value to the control device 40. Then, as shown in FIG. Figure 2As shown, the control device 40 controls the circumferential speed of the first tension cutting roller 20a in such a way that the tension Ta input from the tension meter 30a disposed on the most downstream side reaches a predetermined value (tension constant control). Specifically, when the input tension Ta is smaller than a value predetermined and stored in the control device 40, the control device 40 sends a control signal to the drive unit (motor etc. not shown) of the first tension cutting roller 20a in such a way that the circumferential speed of the first tension cutting roller 20a becomes a circumferential speed P1a larger than the current one. On the contrary, when the input tension Ta is larger than a value predetermined and stored in the control device 40, the control signal is sent to the drive unit of the first tension cutting roller 20a in such a way that the circumferential speed of the first tension cutting roller 20a becomes a small circumferential speed P1a.
[0116] Next, the control device 40 controls the circumferential speed of the first tension cutting roller 20b in such a manner that the tension Tb input from the tension meter 30b disposed on the upstream side closest to the tension meter 30a reaches a predetermined value (tension constant control). Specifically, when the input tension Tb is smaller than the value predetermined and stored in the control device 40, the control device 40 sends a control signal to the drive unit (motor etc. not shown) of the first tension cutting roller 20b in such a manner that the circumferential speed of the first tension cutting roller 20b becomes a circumferential speed P1b larger than the current one. On the contrary, when the input tension Tb is larger than the value predetermined and stored in the control device 40, the control signal is sent to the drive unit of the first tension cutting roller 20b in such a manner that the circumferential speed of the first tension cutting roller 20b becomes a small circumferential speed P1b.
[0117] Finally, the control device 40 controls the circumferential speed of the first tension cutting roller 20c arranged on the outlet side of the processing tank 2 in such a manner that the tension Tc input from the tension meter 30c arranged on the most upstream side reaches a predetermined value (tension constant control). Specifically, when the input tension Tc is smaller than the value predetermined and stored in the control device 40, the control device 40 sends a control signal to the drive unit (motor etc. not shown) of the first tension cutting roller 20c in such a manner that the circumferential speed of the first tension cutting roller 20c becomes a circumferential speed P1c larger than the current one. On the contrary, when the input tension Tc is larger than the value predetermined and stored in the control device 40, the control signal is sent to the drive unit of the first tension cutting roller 20c in such a manner that the circumferential speed of the first tension cutting roller 20c becomes a small circumferential speed P1c.
[0118] As described above, the control system 100 of the present embodiment controls the peripheral speed of the first tension cutting roller 20 in the first control process so that the tension measured by the tension meter 30 disposed on the downstream side of the first tension cutting roller 20 reaches a predetermined value. That is, the peripheral speed of the first tension cutting roller 20 is controlled so that the actually measured tension becomes a predetermined value, so that even if the moisture content of the polarizer F1 on the outlet side of the oven 3 is low, the variation of the tension actually generated in the polarizer F1 becomes small, and the transportation of the polarizer F1 can be stabilized.
[0119] In addition, the control system 100 of the present embodiment controls the circumferential speed P1a by the combination of the tension meter 30a and the first tension cutting roller 20a arranged on the most downstream side in the first control process, and then controls the circumferential speed of the combination arranged on the upstream side until the circumferential speed P1c is controlled by the combination of the tension meter 30c and the first tension cutting roller 20c arranged on the most upstream side. Therefore, the control does not diverge, and stable circumferential speed control can be achieved.
[0120] After executing the first control process described above, the control system 100 of the present embodiment measures the circumferential speed of the first tension cutting roller 20c arranged on the exit side of the processing tank 2, and controls the circumferential speed of the second tension cutting roller 60 in such a way that the ratio of the measured circumferential speed P1c' of the first tension cutting roller to the circumferential speed of the second tension cutting roller 60 reaches a predetermined value (equivalent to the second control process of the present invention). Specifically, during the manufacture of the polarizing film F, the encoder 70 always measures the rotation speed of the first tension cutting roller 20c and outputs it to the control device 40. The control device 40 calculates the circumferential speed P1c' of the first tension cutting roller 20c based on the input rotation speed of the first tension cutting roller 20c and the pre-stored outer diameter of the first tension cutting roller 20c. Then, as Figure 2As shown, the control device 40 controls the circumferential speed of the second tension cutting roller 60 in such a way that the ratio of the circumferential speed P1c' of the first tension cutting roller 20c to the circumferential speed of the second tension cutting roller 60 reaches a predetermined value (ratio constant control). Specifically, when the circumferential speed of the second tension cutting roller 60a is set to P2a, the circumferential speed of the second tension cutting roller 60b is set to P2b, the circumferential speed of the second tension cutting roller 60c is set to P2c, the circumferential speed of the second tension cutting roller 60d is set to P2d, and the circumferential speed of the second tension cutting roller 60e is set to P2e, the control device 40 sets P2a / P1c'=β1, P2b / P1c'=β2, P2c / P The circumferential speeds P2a, P2b, P2c, P2d and P2e are determined in the manner of P1c'=β3, P2d / P1c'=β4, P2e / P1c'=β5 (β1, β2, β3, β4, β5 are given constants), so that the second tension cutting rollers 60a~60e are rotated at the respective circumferential speeds P2a~P2e, and a control signal is sent to a driving part (motor etc. not shown in the figure) of the second tension cutting rollers 60a~60e.
[0121] The control system 100 of this embodiment controls the circumferential speed of the first tension cutting roller 20c in a tension constant control manner in the first control process. Therefore, the circumferential speed of the first tension cutting roller 20c arranged on the outlet side of the processing tank 2 is different from the existing situation in which it is controlled in a ratio constant control manner, and it changes instead of being constant.
[0122] Furthermore, the control system 100 of the present embodiment controls the circumferential speed of the second tension cutting roller 60 in the second control process basically so that the ratio of the measured circumferential speed P1c' of the first tension cutting roller 20c disposed on the outlet side of the processing tank 2 to the circumferential speed of the second tension cutting roller 60 reaches a predetermined value, that is, performs ratio constant control. However, the circumferential speed of the first tension cutting roller 20c disposed on the outlet side of the processing tank 2, which serves as a reference for the ratio, uses the actually measured circumferential speed P1c', so as described above, even if the circumferential speed P1c' of the first tension cutting roller 20c disposed on the outlet side of the processing tank 2 changes, the ratio constant control can be appropriately performed to stretch the roll film F0 at a predetermined given stretch ratio.
[0123] Example
[0124] Hereinafter, the present invention will be described in more detail by way of examples and comparative examples, but the present invention is not limited to the following examples.
[0125] <Example>
[0126] As the roll film F0, a polyvinyl alcohol film (VF-PS-4500 manufactured by Kuraray Co., Ltd.) with an average degree of polymerization of 2400 and a saponification degree of 99.9 mol% and a thickness of 45 μm was used, and treatment was carried out in the treatment tank 2. Specifically, in the treatment tank 2, it was immersed in warm water at 30°C for 60 seconds to make it swell. Then, it was immersed in an aqueous solution of iodine / potassium iodide (weight ratio = 0.5 / 8) with a concentration of 0.3%, and the film was dyed while being stretched to 3.5 times. Then, it was stretched in a borate aqueous solution at 65°C so that the total stretch ratio became 6 times. After the above treatment in the treatment tank 2, it was dried at a drying temperature of 40°C for 3 minutes in the oven 3 to obtain a PVA-type polarizer F1 with a thickness of 18 μm.
[0127] The moisture content of the polarizer F1 at the exit side of the oven 3 was measured and found to be 14%.
[0128] The water content of the polarizer F1 was measured as follows.
[0129] About 60 minutes after the device was put into operation, the polarizer F1 just taken out of the oven 3 was cut into a square shape at an arbitrary position to obtain a sample piece. The weight of the cut sample piece was quickly measured under the standard state. Then, the sample piece was forced to dry at 120°C for 2 hours in a heating oven, and the weight of the sample piece was quickly measured under the standard state. It should be noted that it is believed that the moisture contained in the sample piece is almost completely eliminated by this forced drying.
[0130] The moisture content of the polarizer F1 was determined by substituting the weight of the sample piece before forced drying (the weight of the polarizer F1 after drying) and the weight of the sample piece after forced drying (the weight of the polarizer F1 after complete drying) into the following formula.
[0131] Moisture content of polarizer F1 = (weight of polarizer F1 after drying - weight of polarizer F1 after complete drying) / weight of polarizer F1 after drying × 100
[0132] In an embodiment, Figure 1 and Figure 2 As shown in FIG. 1 , when the polarizer F1 is transported, a constant tension control is performed, that is, the circumferential speed of the first tension cutting roller 20 is controlled so that the tension measured by the tension meter 30 disposed between the processing tank 2 and the laminating roller 7 and located on the downstream side of the first tension cutting roller 20 reaches a predetermined value, and the presence or absence of breakage of the polarizer F1 is investigated. Figure 2 The variation of the tension measured by the tension meter 30a shown in FIG. It should be noted that even when the variation of the tension is measured using the tension meters 30b and 30c, the variation amount is the same as that when the tension is measured using the tension meter 30a.
[0133] <Comparative Example>
[0134] In the comparative example, when the polarizer F1 is transported, constant ratio control is performed, that is, the circumferential speed of the first tension cutting roller 20 is controlled in such a way that the ratio of the circumferential speed of the bonding roller 7 to the circumferential speed of the first tension cutting roller 20 arranged between the processing tank 2 and the bonding roller 7 reaches a predetermined value. In addition, the presence or absence of breakage of the polarizer F1 and the change in tension measured by the tension meter 30a are investigated under the same conditions as those in the embodiment.
[0135] Table 1 shows the results of the above test.
[0136] As shown in Table 1, in the comparative example, the tension fluctuation was extremely large, and the polarizer F1 broke within 1 hour from the start of transportation.
[0137] On the other hand, in the example, the tension variation was small and the polarizer F1 did not break.
[0138] [Table 1]
[0139]
Claims
1. A method for producing a polarizing film, wherein a roll film is dyed with a dichroic substance while being uniaxially stretched in a treatment tank, then dried in an oven to produce a polarizer, and the polarizer is laminated to a protective film with a laminating roller to produce a polarizing film, in, A plurality of first tension cutting rollers and a tension meter for conveying the polarizer are alternately arranged between the processing tank and the laminating roller, and the tension meter is located between the processing tank and the laminating roller and on the downstream side of the first tension cutting roller. The method includes a first control step of controlling the peripheral speed of the first tension cutting roller so that the tension measured by the tension meter becomes a predetermined value. In the first control process, after the circumferential speed is controlled using the combination of the tension meter and the first tension cutting roller arranged on the most downstream side, the circumferential speed is controlled sequentially toward the upstream side using the combination of the tension meter and the first tension cutting roller arranged closer to the upstream side than the combination arranged on the most downstream side.
2. The method for producing a polarizing film according to claim 1, in, The first tension cutting roller is arranged at the outlet side of the processing tank, and the second tension cutting roller for conveying the roll film is arranged in the processing tank, The method includes the following second control step: after executing the first control step, the circumferential speed of the first tension cutting roller arranged on the exit side of the processing tank is measured, and the circumferential speed of the second tension cutting roller is controlled in such a way that the ratio of the measured circumferential speed of the first tension cutting roller to the circumferential speed of the second tension cutting roller becomes a predetermined value.
3. The method for producing a polarizing film according to claim 1, in, The moisture content of the polarizer at the exit side of the oven is less than 15%.
4. The method for producing a polarizing film according to claim 1, in, The thickness of the polarizer at the exit side of the oven is less than 20 μm.
5. A polarizing film manufacturing device, comprising: a treatment tank for dyeing a roll film with a dichroic substance while uniaxially stretching it, an oven for drying the roll film treated in the treatment tank to produce a polarizer, a laminating roller for laminating the polarizer to a protective film, and a first tension cutting roller disposed between the treatment tank and the laminating roller and conveying the polarizer, The manufacturing device comprises: a tension meter disposed between the treatment tank and the laminating roller and located downstream of the first tension cutting roller, and Control device, The first tension cutting rollers and the tension meters are arranged alternately in plurality. The control device controls the peripheral speed of the first tension cutting roller so that the tension measured by the tension meter becomes a predetermined value. After the control device performs control of the circumferential speed using the combination of the tension meter and the first tension cutting roller arranged on the most downstream side, it sequentially performs control of the circumferential speed toward the upstream side using the combination of the tension meter and the first tension cutting roller arranged closer to the upstream side than the combination arranged on the most downstream side.
6. A control system used in the manufacturing device of the polarizing film according to claim 5, the control system comprising: The tensiometer, and The control device.