Electrochemical device and electronic device
By introducing a thermal sensing unit into the electrode assembly of the electrochemical device, and utilizing the cooperation of the heat shrink layer and the resistance layer, the contact discharge of the electrode sheet in the overcharge state is realized, reducing heat accumulation, and improving the safety and safety of the electrochemical device. The heat-resistant performance solves the safety hazard problem of heat dissipation of electrochemical devices after charging.
Patent Information
- Application Number
- CN202011302539.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-11-19
AI Technical Summary
When existing electrochemical devices continue to charge after being fully charged, the heat generated inside the electrode assembly cannot be dissipated in time, resulting in safety hazards and the risk of burning or explosion.
An electrochemical device is designed. Its electrode assembly includes a first pole piece, an isolation film and a second pole piece. The thermal sensing unit is composed of a heat shrinkable layer and a resistance layer. The heat shrinkable layer shrinks when the temperature rises, driving the isolation film. Shrink, causing the first pole piece and the second pole piece to contact and discharge, reducing the capacity of the electrochemical device and improving safety.
Through the design of the thermal sensing unit, the electrochemical device can effectively reduce heat accumulation in the overcharged state, improve safety, avoid the risk of combustion or explosion, and enhance the heat resistance of the electrochemical device.
Smart Images

Figure CN114520303B_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present application relate to the technical field of electrochemical devices, and in particular, to an electrochemical device and an electronic device. Background Art
[0002] Electrochemical devices are devices that convert electrical energy into chemical energy, and when electrical energy is needed, they convert chemical energy back into electrical energy to power electronic devices. With the rapid growth of mobile electronic devices, the demand for electrochemical devices has increased rapidly, and the research and application of electrochemical devices has also increased.
[0003] In the process of implementing the embodiments of the present application, the inventors of the present application found that the electrode assemblies of current electrochemical devices do not have the function of overcharge protection. After the electrochemical device is fully charged, continuing to charge will cause a large amount of heat to be generated inside the electrode assembly. If the heat cannot be dissipated in time, the accumulated heat will cause the electrochemical device to burn or explode, posing a huge safety hazard. Therefore, it is urgently necessary to provide an electrochemical device that can provide overcharge protection. Summary of the invention
[0004] In view of the above problems, embodiments of the present application provide an electrochemical device and an electronic device, which overcome the above problems or at least partially solve the above problems.
[0005] According to one aspect of an embodiment of the present application, an electrochemical device is provided, comprising an electrode assembly, wherein the electrode assembly comprises a first pole piece, an isolation membrane and a second pole piece, wherein the first pole piece and the second pole piece have opposite polarities, and the isolation membrane is disposed between the first pole piece and the second pole piece, and wherein the electrode assembly comprises a thermal sensing unit, wherein the thermal sensing unit comprises at least one heat shrinkage layer, wherein the heat shrinkage layer can shrink during a process in which the temperature rises from 25 degrees Celsius to 200 degrees Celsius, and wherein the heat shrinkage layer is disposed on at least one surface of the isolation membrane, and wherein the heat shrinkage layer is located between the first pole piece and the isolation membrane.
[0006] In an optional manner, the heat shrinkable layer is also arranged between the second pole piece and the isolation film.
[0007] In an optional manner, the thermal sensing unit further includes at least one resistance layer, and the resistance layer is arranged between the first pole piece and the heat shrink layer.
[0008] In an optional manner, the heat shrink layer is further disposed between the second pole piece and the isolation film, and the resistance layer is further disposed between the second pole piece and the heat shrink layer.
[0009] In an optional manner, the first pole piece includes a first current collector, and the first current collector is in contact with the resistance layer.
[0010] In an optional manner, the second pole piece includes a second current collector, and the second current collector is in contact with the resistance layer.
[0011] In an optional manner, the electrode assembly is a winding structure, the side from which the electrode ear of the electrode assembly extends is the first edge area of the electrode assembly, the side opposite to the side from which the electrode ear of the electrode assembly extends is the second edge area of the electrode assembly, and the thermal sensing unit is arranged in the first edge area or the second edge area.
[0012] In an optional manner, taking the first pole piece as a reference, the thermal sensing unit is arranged on the outermost circle of the first pole piece.
[0013] In an optional manner, the heat shrinkable layer satisfies at least one of the following characteristics: (a) the heat shrinkable layer includes at least one of polyethylene wax, polyethylene, polypropylene, polypropylene wax or vaseline; (b) the thickness of the heat shrinkable layer is 20 μm to 100 μm; (c) the melting temperature of the heat shrinkable layer is 60 degrees Celsius to 110 degrees Celsius.
[0014] In an optional manner, the resistor layer satisfies at least one of the following characteristics: (a) the resistor layer includes an organic matter and a conductive agent, the organic matter includes at least one of polyethylene wax, polyethylene, polypropylene, polypropylene wax or vaseline, and the conductive agent includes at least one of copper particles, aluminum particles, graphite, carbon black or graphene; (b) the mass percentage of the conductive agent in the resistor layer is 8% to 20%; (c) the thickness of the resistor layer is 20μm to 100μm.
[0015] In an optional manner, the area of the heat shrinkable layer is 0.05 mm 2 Up to 8mm 2 .
[0016] In an optional manner, the electrochemical device satisfies the following formula:
[0017]
[0018] Wherein, U represents the full charge voltage of the electrochemical device, Cap represents the capacity of the electrochemical device, and R represents the resistance value of the resistance layer, wherein the unit of the full charge voltage is V, the unit of the capacity of the electrochemical device is Ah, and the unit of the resistance value of the resistance layer is Ω.
[0019] According to one aspect of an embodiment of the present application, an electronic device is provided, comprising the above-mentioned electrochemical device.
[0020] The beneficial effects of the embodiments of the present application are as follows: Different from the existing electrochemical devices, the electrochemical device provided by the embodiments of the present application includes an electrode assembly, the electrode assembly includes a first pole piece, a separator, a second pole piece and a thermal sensing unit, the first pole piece and the second pole piece have opposite polarities, and the separator is disposed between the first pole piece and the second pole piece. The thermal sensing unit includes at least one heat shrink layer, the heat shrink layer is disposed on at least one surface of the separator, the heat shrink layer is located between the first pole piece and the separator, and / or, the heat shrink layer is located between the second pole piece and the separator. After the electrochemical device is fully charged, the heat generated inside the electrode assembly continues to be charged, and the heat generated inside the electrode assembly will cause the heat shrink layer to shrink, thereby driving the separator to shrink, causing the first pole piece and the second pole piece to contact and discharge, thereby reducing the capacity of the electrochemical device and improving the safety of the electrochemical device in an overcharged state. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] One or more embodiments are exemplarily described by pictures in the corresponding drawings, and these exemplified descriptions do not constitute limitations on the embodiments. Elements with the same reference numerals in the drawings represent similar elements, and unless otherwise stated, the figures in the drawings do not constitute proportional limitations.
[0022] Figure 1 is a schematic diagram of an electrochemical device provided in an embodiment of the present application;
[0023] Figure 2 is a schematic diagram of an implementation method of an electrode assembly provided in an embodiment of the present application;
[0024] Figure 3 The embodiment of this application provides Figure 2 A magnified schematic diagram of the middle A area;
[0025] Figure 4 It is a schematic diagram of an electrode assembly provided in an embodiment of the present application, in which a resistance layer is disposed on a first active material or a second active material;
[0026] Figure 5 is a schematic diagram of another implementation of the electrode assembly provided in an embodiment of the present application;
[0027] Figure 6 The embodiment of this application provides Figure 5 A magnified schematic diagram of the middle B area;
[0028] Figure 7 is a schematic diagram of an electrochemical device in the prior art. DETAILED DESCRIPTION
[0029] In order to facilitate the understanding of the present application, the present application is described in more detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that when an element is described as "fixed to" another element, it can be directly on the other element, or there can be one or more centered elements therebetween. When an element is described as "connected to" another element, it can be directly connected to the other element, or there can be one or more centered elements therebetween. The terms "vertical", "horizontal", "left", "right", "inside", "outside" and similar expressions used in this specification are for illustrative purposes only.
[0030] Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this specification includes any and all combinations of one or more of the related listed items.
[0031] See also Figure 1 The electrochemical device 200 includes an electrode assembly 100, the electrode assembly 100 includes a first pole piece 10, a separator 20, a second pole piece 30 and a thermal sensing unit 40, the first pole piece 10 and the second pole piece 30 have opposite polarities, and the separator 20 is disposed between the first pole piece 10 and the second pole piece 30. The thermal sensing unit 40 includes at least one heat shrinkable layer 401, which can shrink during the process of the temperature rising from 25 degrees Celsius to 200 degrees Celsius, and the heat shrinkable layer 401 is disposed on at least one surface of the separator 20, the heat shrinkable layer 401 is located between the first pole piece 10 and the separator 20, and / or, the heat shrinkable layer 401 is located between the second pole piece 30 and the separator 20, and the heat shrinkable layer 401 is used to shrink the separator 20 when the temperature of the electrode assembly 100 is greater than a preset threshold value, so as to make the first pole piece 10 and the second pole piece 30 contact discharge. After the electrochemical device 200 is fully charged, it continues to charge, and a large amount of heat will be generated inside the electrode assembly 100, causing the heat shrinkage layer 401 to shrink, thereby driving the isolation membrane 20 to shrink, resulting in contact discharge between the first electrode plate 10 and the second electrode plate 30, thereby reducing the capacity of the electrochemical device and improving the safety of the electrochemical device 200 in an overcharged state.
[0032] For the above-mentioned thermal sensing unit 40, please refer to Figure 1-Figure 3 The thermal sensing unit 40 includes at least one heat shrinkable layer 401 and at least one resistor layer 402. The contacting heat shrinkable layer 401 and the resistor layer 402 satisfy the following relationship: the orthographic projection area of the resistor layer 402 in the thickness direction falls within the orthographic projection area of the heat shrinkable layer in the thickness direction.
[0033] For the above heat shrink layer 401, please refer to Figure 2 and Figure 3 There are two heat shrink layers 401 , one heat shrink layer 401 is located between the first pole piece 10 and the isolation film 20 , and the other heat shrink layer 401 is located between the second pole piece 30 and the isolation film 20 .
[0034] It should be noted that when there are two heat shrink layers 401 , both heat shrink layers 401 may be located between the first pole piece 10 and the isolation film 20 , or both heat shrink layers 401 may be located between the second pole piece 30 and the isolation film 20 .
[0035] It should be noted that the number of heat shrink layer 401 can also be one, that is, the heat shrink layer 401 is disposed on one surface of the isolation film 20, and the heat shrink layer 401 is located between the first pole piece 10 and the isolation film 20, and / or, the heat shrink layer 401 is located between the second pole piece 30 and the isolation film 20. In other words, please refer to Figure 5 and Figure 6 The heat shrink layer 401 is located between the first pole piece 10 and the isolation film 20, or the heat shrink layer 401 is located between the second pole piece 30 and the isolation film 20, or one end of the heat shrink layer 401 is disposed on one surface of the isolation film 20, and the other end of the heat shrink layer 401 is disposed on the other surface of the isolation film 20.
[0036] It is worth noting that, in some embodiments, the heat shrink layer 401 satisfies at least one of the following characteristics: (a) the heat shrink layer 401 includes at least one of polyethylene wax, polyethylene, polypropylene, polypropylene wax or vaseline; (b) the thickness of the heat shrink layer 401 is 20 μm to 100 μm; (c) the melting temperature of the heat shrink layer 401 is 60 degrees Celsius to 110 degrees Celsius. By selecting or limiting the material, size and melting temperature of the heat shrink layer 401, the melting speed of the heat shrink layer 401 and the shrinking speed of the isolation film 20 can be controlled, thereby making the speed of contact discharge between the first pole piece 10 and the second pole piece 30 controllable.
[0037] It is worth noting that, in some embodiments, the area of the heat shrink layer 401 (referring to a single area on one surface of the pole piece) is 0.05 mm 2 Up to 8mm 2 By setting the area of the heat shrink layer 401, on the one hand, the shrinking speed of the isolation film 20 can be controlled, and then the speed of contact discharge between the first pole piece 10 and the second pole piece 30 can be controlled. On the other hand, selecting a suitable area of the heat shrink layer 401 will not have a significant impact on the charging / discharging performance of the electrochemical device 200, and will not affect the energy density of the electrochemical device.
[0038] For the above-mentioned resistance layer 402, see Figure 2 and Figure 3 There are two resistor layers 402 , one resistor layer 402 is disposed between the first pole piece 10 and the heat shrink layer 401 , and the other resistor layer 402 is disposed between the second pole piece 30 and the heat shrink layer 401 .
[0039] It should be noted that the number of the resistor layer 402 may also be one, and the resistor layer 402 is disposed between the first pole piece 10 and the heat shrink layer 401, and / or, the resistor layer 402 is disposed between the second pole piece 30 and the heat shrink layer 401. The configuration of the resistor layer 402 may refer to the configuration of the heat shrink layer 401, and will not be described in detail here.
[0040] It should be noted that, in some embodiments, the resistor layer 402 satisfies at least one of the following characteristics: (a) the resistor layer 402 includes an organic matter and a conductive agent, the organic matter includes at least one of polyethylene wax, polyethylene, polypropylene, polypropylene wax or vaseline, and the conductive agent includes at least one of copper particles, aluminum particles, graphite, carbon black or graphene; (b) the mass percentage of the conductive agent in the resistor layer 402 is 8% to 20%; (c) the thickness of the resistor layer 402 is 20μm to 100μm.
[0041] It should be noted that, in some embodiments, the electrochemical device 200 satisfies the following formula:
[0042]
[0043] Among them, U represents the full charge voltage of the electrochemical device 200, Cap represents the capacity of the electrochemical device 200, and R represents the resistance value of the resistance layer 402. Among them, the unit of the full charge voltage is V, the unit of the capacity of the electrochemical device 200 is mAh, and the unit of the resistance value of the resistance layer 402 is Ω.
[0044] It can be understood that the limitation of the above formula can ensure that the electrochemical device 200 can release 2% to 5% of the electricity within 5 minutes, thereby releasing a suitable amount of electricity in a short time and avoiding thermal runaway of the electrochemical device.
[0045] It should be noted that by setting the resistance layer 402, the resistance layer 402 is opposite to the heat shrink layer 401, and the heat shrink layer 401 shrinks and drives the isolation membrane 20 to shrink, so that the first pole piece 10 and the second pole piece 30 will contact each other through the resistance layer 402, and the discharge speed of the electrochemical device 200 can be adjusted by adjusting the thickness of the resistance layer 402, the conductive agent and the conductive agent content.
[0046] For the first pole piece 10 and the second pole piece 30, please refer to Figure 2 and Figure 3The first pole piece 10 includes a first current collector 101 and a first active material layer 102, and the first active material layer 102 is disposed on the first current collector 101. The second pole piece 30 includes a second current collector 301 and a second active material layer 302, and the second active material layer 302 is disposed on the second current collector 301. Figure 2 and Figure 3 In the embodiment, the number of the resistance layers 402 is two, one resistance layer 402 is disposed on the first current collector 101 , and the other resistance layer 402 is disposed on the second current collector 301 .
[0047] It can be understood that, if the number of the resistance layer 402 is one, then one resistance layer 402 is disposed on the first current collector 101 , and / or one resistance layer 402 is disposed on the second current collector 301 .
[0048] As a preferred embodiment, the resistance layer 402 is disposed on the edge of the first current collector 101 , and / or the resistance layer 402 is disposed on the edge of the second current collector 301 .
[0049] It should be noted that, in some embodiments, please refer to Figure 4 The first active material layer 102 covers the first current collector 101 , the second active material layer 302 covers the second current collector 301 , the resistor layer 402 is disposed on the first active material layer 102 , and / or the resistor layer 402 is disposed on the second active material layer 302 .
[0050] In some embodiments, the electrode assembly 100 is a wound structure, see Figure 1 , the electrode assembly 100 is connected with a pole ear 50, the pole ear 50 is located in a direction perpendicular to the winding direction of the electrode assembly 100, the side from which the pole ear 50 extends is the first edge area of the electrode assembly 100, and the side opposite to the side from which the pole ear 50 of the electrode assembly 100 extends is the second edge area of the electrode assembly 100, and the thermal sensing unit 40 is arranged in the first edge area or the second edge area. Preferably, the thermal sensing unit 40 is arranged in the first edge area. Since the space on the side from which the pole ear 50 extends is relatively large, the heat generated by the electrode assembly 100 here is easily released, and the thermal sensing unit 40 is located in the first edge area, the electrochemical device 200 is safer when charging.
[0051] It should be noted that, in some embodiments, the first edge area is an area within 20 mm from the edge of the electrode assembly 100 toward the electrode assembly 100 , and the second edge area is an area within 20 mm from the edge of the electrode assembly 100 toward the electrode assembly 100 .
[0052] It should be noted that the electrode assembly 100 is a winding structure, see Figure 2, the first pole piece 10, the isolation film 20, the second pole piece 30, the heat shrinkable layer 401 and the resistance layer 402 are all wound structures. In some embodiments, please refer to Figure 3 , with the first pole piece 10 as a reference, the thermal sensing unit 40 is disposed at the outermost circle of the first pole piece 10. In other words, the thermal sensing unit 40 is disposed at the outermost circle of the first pole piece 10, and the shrinkage of the heat shrinkable film brings the isolation film 20 to shrink, thereby achieving contact discharge between the first pole piece 10 and the second pole piece 30, and the energy density of the electrode assembly 100 is high.
[0053] It is understandable that the electrode assembly 100 may also be other structures, not limited to the winding structure. Regardless of the structure of the electrode assembly 100, after the electrochemical device 200 is fully charged, if charging continues, the first pole piece 10 and the second pole piece 30 will contact discharge, thereby ensuring the safety of the electrochemical device 200 in an overcharged state.
[0054] For the electrode assembly 100 having a winding structure, see Figure 2 and Figure 3 , an optimal arrangement of the first pole piece 10, the isolation film 20, the second pole piece 30, the heat shrink layer 401 and the resistor layer 402 of the electrode assembly 100 is that the number of heat shrink layers 401 is two, and the number of resistor layers 402 is two. The first active material layer 102 is arranged on the first current collector 101, one resistor layer 402 is arranged on the outermost circle of the first current collector 101, one resistor layer 402 is arranged on the first current collector 101 at a position opposite to the heat shrink layer 401, and one resistor layer 402 is located in the first edge region. The second active material layer 302 is arranged on the second current collector 301, another resistor layer 402 is arranged on the outermost circle of the second current collector 301, another resistor layer 402 is arranged on the second current collector 301 at a position opposite to the heat shrink layer 401, and another resistor layer 402 is located in the first edge region. The two heat shrink layers 401 are respectively located on the two surfaces of the isolation film 20, and the two heat shrink layers 401 are opposite to the resistor layer 402.
[0055] In order to facilitate readers to more intuitively and better understand the performance and effect of the electrochemical device of the present application, 9 electrochemical devices of the present application and 1 electrochemical device of the prior art were selected for comparative experiments, wherein the 9 electrochemical devices of the present application are specifically as follows:
[0056] Electrochemical device 1
[0057] <1-1. Preparation of positive electrode sheet>
[0058] The positive electrode active materials lithium cobalt oxide, acetylene black, and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3, and then N-methylpyrrolidone (NMP) is added as a solvent to prepare a slurry with a solid content of 75%, and stirred evenly. The slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, dried at 90°C, and cold pressed to obtain a positive electrode sheet with a positive electrode active material layer thickness of 100μm, and then the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet coated with a positive electrode active material layer on both sides. The positive electrode sheet is cut into a specification of 74mm×867mm and welded to the pole ear for standby use.
[0059] according to Figure 1 A resistor layer is coated on the corresponding position of the positive electrode sheet. The thickness of the resistor layer is 20 μm and the area of the resistor layer is 8 mm 2 The organic matter in the resistance layer is polyethylene, the conductive agent is carbon black, the mass percentage of carbon black is 8%, and the binder is sodium carboxymethyl cellulose. The actual measured resistance value of the resistance layer is 1.46Ω.
[0060] <1-2. Preparation of negative electrode sheet>
[0061] The negative electrode active material artificial graphite, acetylene black, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in a mass ratio of 96:1:1.5:1.5, and then deionized water is added as a solvent to prepare a slurry with a solid content of 70%, and stirred evenly. The slurry is evenly coated on one surface of a copper foil with a thickness of 8 μm, dried at 110°C, and cold pressed to obtain a negative electrode sheet with a negative electrode active material layer coated on one side with a thickness of 150 μm, and then the above coating steps are repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet with a negative electrode active material layer coated on both sides. The negative electrode sheet is cut into a specification of 74 mm × 867 mm and welded to the pole ear for standby use.
[0062] according to Figure 1 A resistor layer is coated on the corresponding position of the negative electrode sheet. The thickness of the resistor layer is 20 μm and the area of the resistor layer is 8 mm 2 The organic matter in the resistance layer is polyethylene, the conductive agent is carbon black, the binder is sodium carboxymethyl cellulose, the mass percentage of carbon black is 8%, and the actual measured resistance value of the resistance layer is 1.46Ω.
[0063] <1-3. Preparation of isolation film>
[0064] A polyethylene separator with a thickness of 9 μm was selected. Figure 1 A heat shrink layer is coated on the corresponding position of the isolation film. The heat shrink layer is composed of polyethylene and also includes a binder, sodium carboxymethyl cellulose. The thickness of the heat shrink layer is 20 μm and the area of the heat shrink layer is 8 mm.2 , the melting temperature of the heat shrinkable layer is 80 degrees Celsius.
[0065] <1-4. Preparation of electrolyte>
[0066] In an environment with a water content of less than 10ppm, non-aqueous organic solvents of ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), propyl propionate (PP), and vinylene carbonate (VC) are mixed in a mass ratio of 20:30:20:28:2, and then lithium hexafluorophosphate (LiPF6) is added to the non-aqueous organic solvent to dissolve and mix evenly to obtain an electrolyte, wherein the mass ratio of LiPF6 to the non-aqueous organic solvent is 8:92.
[0067] <1-5. Preparation of lithium-ion batteries>
[0068] The positive electrode sheet, the separator, and the negative electrode sheet prepared above are stacked in order, so that the separator is placed between the positive and negative electrode sheets to play a role of isolation. Figure 1 The electrode assembly is wound and then placed in a packaging film, dehydrated at 80°C, injected with a prepared electrolyte, and subjected to vacuum packaging, standing, formation, hot pressing and shaping to obtain a lithium-ion battery.
[0069] Electrochemical device 2,
[0070] The preparation process of the electrochemical device 2 is the same as that of the electrochemical device 1, except that the mass percentage of carbon black is 14%, and the resistance value of the resistance layer actually measured is 1.25Ω.
[0071] Electrochemical device 3,
[0072] The preparation process of the electrochemical device 3 is the same as that of the electrochemical device 1, except that the mass percentage of carbon black is 20%, and the resistance value of the resistance layer actually measured is 0.85Ω.
[0073] Electrochemical device 4,
[0074] The preparation process of electrochemical device 4 is the same as that of electrochemical device 1, except that the thickness of the heat shrink layer is 60 μm and the area of the heat shrink layer is 5 mm 2 The thickness of the resistor layer is 60 μm and the area of the resistor layer is 5 mm 2 The actual measured resistance value of the resistor layer is 1.67Ω.
[0075] Electrochemical device 5,
[0076] The preparation process of electrochemical device 5 is the same as that of electrochemical device 1, except that the thickness of the heat shrink layer is 60 μm and the area of the heat shrink layer is 5 mm2 The thickness of the resistor layer is 60 μm and the area of the resistor layer is 5 mm 2 The mass percentage of carbon black is 14%, and the resistance value of the resistance layer actually measured is 1.43Ω.
[0077] Electrochemical device 6,
[0078] The preparation process of electrochemical device 6 is the same as that of electrochemical device 1, except that the thickness of the heat shrink layer is 60 μm and the area of the heat shrink layer is 5 mm 2 The thickness of the resistor layer is 60 μm and the area of the resistor layer is 5 mm 2 The mass percentage of carbon black is 20%, and the resistance value of the resistance layer actually measured is 0.97Ω.
[0079] Electrochemical device 7,
[0080] The preparation process of electrochemical device 7 is the same as that of electrochemical device 1, except that the thickness of the heat shrink layer is 100 μm and the area of the heat shrink layer is 2 mm. 2 , the thickness of the resistance layer is 100μm, and the area of the resistance layer is 2mm 2 The actual measured resistance value of the resistance layer is 1.83Ω.
[0081] Electrochemical device 8,
[0082] The preparation process of electrochemical device 8 is the same as that of electrochemical device 1, except that the thickness of the heat shrink layer is 100 μm and the area of the heat shrink layer is 2 mm. 2 , the thickness of the resistance layer is 100μm, and the area of the resistance layer is 2mm 2 The mass percentage of carbon black is 14%, and the resistance value of the resistance layer actually measured is 1.58Ω.
[0083] Electrochemical device 9,
[0084] The preparation process of electrochemical device 9 is the same as that of electrochemical device 1, except that the thickness of the heat shrink layer is 100 μm and the area of the heat shrink layer is 2 mm. 2 , the thickness of the resistance layer is 100μm, and the area of the resistance layer is 2mm 2 The mass percentage of carbon black is 20%, and the resistance value of the resistance layer actually measured is 1.23Ω.
[0085] The electrochemical device of the prior art is:
[0086] The electrochemical device 10 has a full charge voltage of 4.45 V and a capacity of 5 Ah. Figure 7, the electrode assembly of the electrochemical device 10 includes a first pole piece 10', a separator 20', a second pole piece 30' and a pole tab 50'. The first pole piece 10', the separator 20', the second pole piece 30' and the pole tab 50' of the electrochemical device 10 are respectively the same as the first pole piece 10, the separator 20, the second pole piece 30 and the pole tab 50 of the present application. However, the electrochemical device 10 does not include a thermal sensing unit.
[0087] For each of the 10 electrochemical devices mentioned above, 10 devices were taken and placed in a hot box for hot box performance test. The hot box was heated from room temperature to a preset temperature, such as 125°C or 130°C, at a rate of 5°C / min, and the temperature was maintained for 60 minutes. Each electrochemical device was observed to see whether it burned. If there was no combustion, it was considered to have passed. The number of each electrochemical device that passed the test was counted and recorded in the following Table 1.
[0088] Table 1 Hot box performance test results
[0089]
[0090]
[0091] From Table 1, the heat resistance of the electrochemical device provided in the embodiment of the present application is 5°C higher than the heat resistance temperature of the electrochemical device 10 of the prior art. If the resistance value of the resistance layer of the electrochemical device provided in the embodiment of the present application is different, the combustion conditions in the 130°C hot box are different, that is, if the resistance value of the resistance layer is different, the discharge speed of the electrochemical device is different, so that the heat resistance of the electrochemical device is different. Therefore, the experimental results in Table 1 prove that the electrochemical device provided in the embodiment of the present application adds a resistance layer, so that the resistance value of the resistance layer can be adjusted, and then the discharge rate of the electrochemical device can be adjusted, so that the heat resistance of the electrochemical device can be adjusted by adjusting the resistance value of the resistance layer.
[0092] In the embodiment of the present application, the electrochemical device 200 includes an electrode assembly 100, the electrode assembly 100 includes a first pole piece 10, a separator 20, a second pole piece 30 and a thermal sensing unit 40, the first pole piece 10 and the second pole piece 30 have opposite polarities, and the separator 20 is disposed between the first pole piece 10 and the second pole piece 30. The thermal sensing unit 40 includes at least one heat shrink layer 401, the heat shrink layer 401 is disposed on at least one surface of the separator 20, the heat shrink layer 401 is located between the first pole piece 10 and the separator 20, and / or, the heat shrink layer 401 is located between the second pole piece 30 and the separator 20, and the heat shrink layer 401 is used to shrink the separator 20 when the temperature of the electrode assembly 100 is greater than a preset threshold value, so as to make the first pole piece 10 and the second pole piece 30 contact discharge. After the electrochemical device 200 is fully charged, it continues to charge, and a large amount of heat will be generated inside the electrode assembly 100, causing the heat shrink layer 401 to shrink, thereby driving the isolation film 20 to shrink, resulting in the first pole piece 10 and the second pole piece 30 to contact discharge, thereby reducing the capacity of the electrochemical device and improving the safety of the electrochemical device 200 in an overcharged state. When the thermal sensing unit 40 of the electrode assembly 100 includes at least one resistance layer 402, the resistance layer 402 is arranged between the first pole piece 10 and the heat shrink layer 401, and / or, the resistance layer 402 is arranged between the second pole piece 30 and the heat shrink layer 401, and the rate of contact discharge between the first pole piece 10 and the second pole piece 30 can be adjusted by adjusting the resistance value of the resistance layer 402, so that the application range of the electrochemical device 200 is wide.
[0093] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Under the concept of the present application, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present application as above, which are not provided in detail for the sake of simplicity. Although the present application has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features can be replaced by equivalents. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.
Claims
1. An electrochemical device, comprising an electrode assembly, wherein the electrode assembly comprises a first pole piece, a separator and a second pole piece, wherein the first pole piece and the second pole piece have opposite polarities, and the separator is disposed between the first pole piece and the second pole piece, wherein: The electrode assembly includes a thermal sensing unit, Wherein, the thermal sensing unit includes at least one heat shrink layer, which can shrink when the temperature rises from 25 degrees Celsius to 200 degrees Celsius, thereby driving the isolation membrane to shrink, causing the first pole piece and the second pole piece to contact and discharge, and the heat shrink layer is arranged on at least one surface of the isolation membrane, and the heat shrink layer is located between the first pole piece and the isolation membrane.
2. The electrochemical device according to claim 1, characterized in that The heat shrinkable layer is also arranged between the second pole piece and the isolation film.
3. The electrochemical device according to claim 1, characterized in that The thermal sensing unit further includes at least one resistance layer, and the resistance layer is arranged between the first pole piece and the heat shrink layer.
4. The electrochemical device according to claim 3, characterized in that The heat shrink layer is further arranged between the second pole piece and the isolation film, and the resistance layer is further arranged between the second pole piece and the heat shrink layer.
5. The electrochemical device according to claim 3, characterized in that The first pole piece includes a first current collector, and the first current collector is in contact with the resistance layer.
6. The electrochemical device according to claim 4, characterized in that The second pole piece includes a second current collector, and the second current collector is in contact with the resistance layer.
7. The electrochemical device according to any one of claims 1 to 6, characterized in that: The electrode assembly is a winding structure, the side from which the electrode ear of the electrode assembly extends is the first edge area of the electrode assembly, the side opposite to the side from which the electrode ear of the electrode assembly extends is the second edge area of the electrode assembly, and the thermal sensing unit is arranged in the first edge area or the second edge area.
8. The electrochemical device according to claim 7, characterized in that Taking the first pole piece as a reference, the thermal sensing unit is arranged at the outermost circle of the first pole piece.
9. The electrochemical device according to claim 1, characterized in that The heat shrinkable layer satisfies at least one of the following characteristics: (a) the heat shrinkable layer comprises at least one of polyethylene wax, polyethylene, polypropylene, polypropylene wax or vaseline; (b) the thickness of the heat shrinkable layer is 20 μm to 100 μm; (c) The melting temperature of the heat shrinkable layer is 60 degrees Celsius to 110 degrees Celsius.
10. The electrochemical device according to claim 3 or 4, characterized in that: The resistance layer satisfies at least one of the following characteristics: (a) the resistance layer comprises an organic substance and a conductive agent, the organic substance comprises at least one of polyethylene wax, polyethylene, polypropylene, polypropylene wax or vaseline, and the conductive agent comprises at least one of copper particles, aluminum particles, graphite, carbon black or graphene; (b) the mass percentage of the conductive agent in the resistance layer is 8% to 20%; (c) The thickness of the resistance layer is 20 μm to 100 μm.
11. The electrochemical device according to claim 1, characterized in that The area of the heat shrinkable layer is 0.05 mm 2 Up to 8mm 2 .
12. The electrochemical device according to claim 3 or 4, characterized in that: The electrochemical device satisfies the following formula: Wherein, U represents the full charge voltage of the electrochemical device, Cap represents the capacity of the electrochemical device, and R represents the resistance value of the resistance layer, wherein the unit of the full charge voltage is V, the unit of the capacity of the electrochemical device is Ah, and the unit of the resistance value of the resistance layer is Ω.
13. An electronic device, characterized in that: It comprises the electrochemical device according to any one of claims 1 to 12.
Citation Information
Patent Citations
Multilayer polyolefin battery diaphragm and preparation method thereof
CN102544416A
Pole piece, battery cell and battery
CN109524606A