Core-sheath composite fibers and multifilaments

By designing the multi-leaf shape of more than three convex parts and the interfiber gap structure of specific fibers in the cross-section of the fiber, the problem that synthetic fibers are difficult to show the texture of natural silk in the clothing material is solved, and the advanced luster, lightness and retraction of multi-filament is achieved The balance of elasticity.

CN114521216BActive Publication Date: 2024-11-19TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080066545.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-28
Filing Date
2020-10-02
Publication Date
2024-11-19
Estimated Expiration
2040-10-02

AI Technical Summary

Technical Problem

The prior art is difficult to achieve the advanced luster, lightness and rebound feeling of synthetic fibers in clothing materials at the same time, and there are constraints on the design of the gap structure between the fibers, making it difficult to balance the texture of natural silk.

Method used

The core sheath composite fiber formed of two or more polymers is used, and the fiber cross-section has a multi-leaf shape with more than three convex portions. The maximum thickness to the minimum thickness ratio of the sheath component is 5.0 or more, forming a large inter-fiber gap of more than 10 μm. The specific structure of the interfiber gap of less than 5 μm is formed by dissolution of the sheath component.

Benefits of technology

The microfiber gaps less than 5 μm and coarse fiber gaps above 10 μm are uniformly mixed in the multifilament, showing a natural silk-like high-quality luster, light and soft texture, and improving the rebound feeling of the fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114521216B_ABST
    Figure CN114521216B_ABST
Patent Text Reader

Abstract

In the fiber cross section of the core-sheath composite fiber formed of two or more polymers, the sheath component completely covers the multi-lobed core component having three or more convex portions, and the maximum thickness S of the sheath component is max With minimum thickness S min Ratio S max / S min A core-sheath composite fiber having a sheath-like filament ratio of 5.0 or more and a multifilament formed of a core component of the core-sheath composite fiber are provided. A core-sheath composite fiber and a multifilament suitable for obtaining a good textile close to natural silk are provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a core-sheath composite fiber and a multifilament which are suitable for obtaining a textile product having a high-quality luster like natural silk and being light, soft and having a resilient feel. Background Art

[0002] Synthetic fibers made of polyester, polyamide, etc. have excellent mechanical properties and dimensional stability, and are therefore widely used in clothing and non-clothing applications. However, as people's lives become more diverse and they pursue a better life, many applications, such as clothing, require a high level of texture and functionality that traditional synthetic fibers do not have.

[0003] If we link the changes in the technological development of synthetic fibers, we can say that the motivation for imitating the characteristics of natural raw materials has promoted the evolution of various element technologies. This is because natural fibers such as hemp, wool, cotton, and silk have excellent texture and functions, and people feel that the complex luster and texture woven from these materials are attractive and high-end.

[0004] In the history of synthetic fibers that imitate natural raw materials, especially in the case of silk-like raw materials that aim to achieve the characteristics of silk, the most advanced variety of natural raw materials (hereinafter referred to as natural silk), a wide range of fiber technologies have been proposed, ranging from polymer technology to yarn making technology such as designing fiber cross-sectional shapes or blending different fibers.

[0005] For example, it is known that if the cross-sectional shape of a polyester fiber that highly reflects light is set to a multi-lobed irregular cross-section, the reflection of light is amplified by the concavoconvexity of the multi-lobed shape, and a fiber with high brightness and soft luster such as natural silk is produced in large quantities as a representative example of silk-like raw materials. However, it is sometimes difficult to satisfy the texture of natural silk other than luster (dryness, lightness, softness, resilience, etc.) by only forming a simple irregular cross-section, and various fiber technologies related to composite fibers that seek the texture of natural silk by further complicating the cross-sectional shape are disclosed.

[0006] Patent Document 1 proposes a composite fiber having a multi-lobed shape in the fiber cross section, and in which an easily soluble component is arranged in a tapered shape toward the inside of the fiber at the apex of the multi-lobed shape. In this composite fiber, when the easily soluble component is subjected to elution treatment, grooves are arranged at the apex of the multi-lobed shape, thereby reproducing the high-quality gloss and dry touch of natural silk by the reflection of light based on the multi-lobed shape and the increase in friction based on the grooves, and further reproducing the silky sound that is a characteristic of textiles formed of natural silk.

[0007] Patent Document 2 proposes a composite fiber in which an easily soluble component divides a poorly soluble component into a plurality of components in the fiber cross section. In this composite fiber, one composite fiber is divided into a plurality of fibers with irregular cross sections when the easily soluble component is subjected to elution treatment, thereby combining the effect of the thinned fiber diameter with the effect of the irregular cross section, and in addition to having a high-grade luster like natural silk and a dry touch, a soft texture can be imparted.

[0008] In addition, it is known that a silk-like woven knitted fabric is obtained by using a multifilament formed by mixing fibers having a shrinkage difference, and Patent Document 3 proposes a shrinkage difference mixed fiber multifilament formed by at least two fiber groups with different heat shrinkage rates produced by a spinning mixed fiber method. In this shrinkage difference mixed fiber multifilament, one of the fibers is made of a copolyester, and when heated, a difference in yarn length between the fiber groups is generated due to the shrinkage difference, and the cloth is given a rich ridge, etc., so that it can be made into a silk-like raw material.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 57-5912

[0012] Patent Document 2: Japanese Patent Application Publication No. 2010-222771

[0013] Patent Document 3: Japanese Patent Application Laid-Open No. 2-19528 Summary of the invention

[0014] Problems to be solved by the invention

[0015] As in Patent Document 1, by forming a special cross-sectional shape using eluted components, light reflection and friction are controlled, thereby reproducing the high-quality luster, dry touch, and unique silk sound that are unique to natural silk to a certain extent. However, in Patent Document 1, the inter-fiber spaces are sometimes insufficient, and single fibers are formed in a dense form in the cloth. Therefore, when worn as clothing, there is a case where the comfortable lightness and soft texture are insufficient.

[0016] On the other hand, as in Patent Document 2, the method of reducing the bending rigidity of individual single fibers by thinning the fiber diameter by dissolution splitting, etc., thereby imparting flexibility to the fabric is effective from the viewpoint of imparting flexibility. However, in Patent Document 2, the gaps formed in the multifilament are sometimes limited, and by further thinning the yarn diameter, it is easy to become a fabric with the most densely packed single fibers depending on the fabric structure. Therefore, in order to obtain the light texture unique to natural silk, it is necessary to design the fabric precisely, etc., and there are restrictions on the expansion of raw materials.

[0017] In addition, as in Patent Document 3, the method of providing ridges to fabrics by mixing fibers with different shrinkage is effective from the viewpoint of obtaining lightness due to the ridges, but since different fibers are mixed during drawing or yarn processing, fiber distribution may be uneven. In this way, when fiber distribution is uneven, for example, clogging may occur at the portion where the fibers on the high shrinkage side are unevenly distributed, and the soft texture may be impaired.

[0018] As described above, various technologies have been proposed so far as silk-like raw materials that effectively utilize synthetic fibers, but it is difficult to say that there is a technology that has a high-grade luster like natural silk and a light, soft and resilient texture with good balance. Therefore, the object of the present invention is to solve the problems of the above-mentioned prior art and provide a core-sheath composite fiber and multifilament suitable for obtaining a good textile close to natural silk.

[0019] Means for solving problems

[0020] The object of the present invention is achieved by the following means.

[0021] A core-sheath composite fiber, wherein in a fiber cross section of the core-sheath composite fiber formed of two or more polymers, the sheath component is completely covered with a multi-lobed core component having three or more convex portions, and the maximum thickness S of the sheath component is max With minimum thickness S min Ratio S max / S min 5.0 or above;

[0022] A multifilament yarn formed from the core component of the core-sheath composite fiber described above;

[0023] A multifilament having an average inter-fiber gap distance of 5 to 30 μm, wherein the inter-fiber gap distance is less than 5 μm in a ratio of 10 to 50%;

[0024] A fiber product, a part of which contains the core-sheath composite fiber or multifilament described above.

[0025] Effects of the Invention

[0026] If the core-sheath composite fiber or multifilament of the present invention is used, a unique void structure can be formed in the multifilament, in which fine fiber voids less than 5 μm and coarse fiber voids greater than 10 μm are uniformly mixed between individual fibers, like natural silk. This can result in a textile product having a high-quality luster like natural silk, which is light, soft, and has a resilient feel. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] [ Figure 1] is a schematic diagram of the cross-sectional structure of raw silk obtained from silkworm cocoons which are the raw material of natural silk.

[0028] [ Figure 2 ] (a) and (b) are examples of schematic diagrams of the cross-sectional structure of the core-sheath composite fiber of the present invention.

[0029] [ Figure 3 ] (a), (b), and (c) are examples of schematic diagrams of cross-sectional structures of composite fibers in the prior art.

[0030] [ Figure 4 ] (a), (b), and (c) are examples of schematic diagrams of the cross-sectional structure of the core-sheath composite fiber of the present invention.

[0031] [ Figure 5 ] (a) and (b) are examples of schematic diagrams of the cross-sectional structure of the core-sheath composite fiber of the present invention.

[0032] [ Figure 6 ] (a) and (b) are examples of schematic diagrams of the cross-sectional structure of composite fibers in the prior art.

[0033] [ Figure 7 ] is an example of the curling morphology of the curled fibers constituting the multifilament of the present invention.

[0034] [ Figure 8 ] are examples of schematic diagrams of the cross-sectional structure of the multifilament of the present invention; (a) is a diagram for understanding "uniformly mixed existence", and (b) is a diagram for understanding the method of measuring the average inter-fiber void distance.

[0035] [ Fig. 9 ] (a) and (b) are examples of schematic diagrams of the cross-sectional structure of the crimped fibers constituting the multifilament of the present invention.

[0036] [ Fig.10 ] (a) and (b) are schematic diagrams of the cross-sectional structure of an example of a core-sheath composite fiber that can be produced from the multifilament of the present invention.

[0037] [ Fig.11 ] is a schematic diagram of the cross-sectional structure of an example of a composite fiber that can be produced by multifilament yarn according to the prior art.

[0038] [ Fig.12 ] is a cross-sectional view of a composite spinneret for illustrating the method for producing the core-sheath composite fiber and multifilament of the present invention. DETAILED DESCRIPTION

[0039] Hereinafter, the present invention will be described in detail together with preferred embodiments thereof.

[0040] In the process of pursuing the principle of the appearance of the texture of natural silk, if we re-examine the yarn-making process of natural silk, we can find that when raw silk is obtained from silkworm cocoons, which are the raw materials of natural silk, its fiber cross-sectional shape is a silk protein ( Figure 1 a) contains sericin with easily soluble components ( Figure 1 b) Covering. In natural silk, there is a unique yarn-making process in which sericin is dissolved from the raw silk. It is believed that the light and soft texture unique to natural silk can be formed by the appearance of inter-fiber spaces caused by the dissolution of sericin.

[0041] In previous silk-like raw materials, a method of forming inter-fiber gaps by thinning the fibers with alkali or other agents was often used. However, the inventors of the present application focused on the formation process of the inter-fiber gaps and, based on detailed observations of natural silk woven fabrics and silk-like raw materials based on prior art, found that there were significant differences in the size and distribution of the inter-fiber gaps formed between natural silk and previous raw materials.

[0042] That is, it was discovered that in the case of natural silk, fine inter-fiber spaces smaller than 5 μm and coarse inter-fiber spaces larger than 10 μm are uniformly mixed between individual fibers. In contrast, in previous raw materials, only inter-fiber spaces smaller than 5 μm or larger than 10 μm could be formed, and the difference in the formation of these spaces would have a significant impact on the properties of woven knitted fabrics.

[0043] This is because when the size of the inter-fiber gap is 10 μm or more, the fibers fixed at the bundle point of the woven knitted fabric can be moved, resulting in softness and lightness due to the reduction of the apparent density of the high void ratio. However, when the size of the inter-fiber gap is 5 μm or more, the bending rigidity is reduced, thereby reducing the rebound feeling. Therefore, in the conventional raw materials with inter-fiber gaps that are biased towards one of less than 5 μm or more than 10 μm, there is a trade-off relationship in terms of lightness, softness and rebound feeling. On the other hand, in natural silk in which coarse inter-fiber gaps of 10 μm or more that are responsible for lightness and softness and fine inter-fiber gaps of less than 5 μm that are responsible for rebound feeling are uniformly mixed, this trade-off relationship is eliminated, and a light, soft and rebounding texture can be presented in a well-balanced manner.

[0044] The present invention is formed based on the above-mentioned understanding. The purpose of the present invention is to form the specific inter-fiber gaps achieved by the above-mentioned natural silk. In the composite fiber of the present invention, in the fiber cross-section of the core-sheath composite fiber formed by more than two polymers, it is important that the sheath component completely covers the multi-lobed core component with more than three convex parts, which becomes the first requirement of the present invention.

[0045] The core-sheath composite fiber referred to in the present invention refers to a fiber composed of two or more polymers and having a cross-sectional shape in which a core component is covered by a sheath component in a cross section perpendicular to the fiber axis.

[0046] As the core component and sheath component constituting the core-sheath composite fiber of the present invention, since the thermoplastic polymers have excellent processability, as the polymer group constituting the fiber, for example, polyester, polyethylene, polypropylene, polystyrene, polyamide, polycarbonate, polymethyl methacrylate, polyphenylene sulfide and other polymer groups and copolymers thereof are preferred. From the viewpoint of being able to impart particularly high interfacial affinity and obtaining fibers without composite cross-section anomalies, the thermoplastic polymers used in the core-sheath composite fiber are preferably all the same polymer group and copolymers thereof. Furthermore, from the viewpoint of not only being able to form a bending rigidity close to that of natural silk, but also being able to obtain good color development during dyeing, a polyester combination can be cited as a particularly preferred range. In addition, the polymer may also contain various additives such as inorganic substances such as titanium oxide, silicon dioxide, and barium oxide, colorants such as carbon black, dyes, and pigments, flame retardants, fluorescent whitening agents, antioxidants, or ultraviolet absorbers.

[0047] In addition, in the process of paying attention to environmental issues, in the present invention, it is also preferred to use biopolymers and recycled polymers derived from plants from the viewpoint of reducing environmental load, and the polymer used in the present invention can be a recycled polymer that has been recycled by any method of chemical recycling, material recycling, and thermal recycling. Even when using biopolymers and recycled polymers, polyester resins can make the characteristics of the present invention significant by their polymer properties. As described above, recycled polyester can be preferably used in the present invention from the viewpoint of obtaining bending rigidity close to natural silk and good color development.

[0048] Here, the purpose of the core-sheath composite fiber of the present invention is to dissolve the sheath component after high-level processing such as weaving and knitting to obtain a multifilament formed by the core component. Therefore, relative to the solvent used in the dissolution of the sheath component, it is preferred that the core component is difficult to dissolve and the sheath component is easy to dissolve. It is appropriate to pre-select the core component according to the purpose, and select the sheath component from the above-mentioned polymers in consideration of the solvent that can be used. At this time, the greater the dissolution rate ratio of the difficult-to-dissolve component (core component) to the easy-to-dissolve component (sheath component) relative to the solvent, the more preferred combination it can be said, and the polymer can be selected based on the range of the dissolution rate ratio of up to 3000 times.

[0049] As the sheath component, for example, it is preferably selected from polymers such as polyester and its copolymers, polylactic acid, polyamide, polystyrene and its copolymers, polyethylene, polyvinyl alcohol, etc. that can be melt-molded and are more soluble than other components. In addition, from the viewpoint of simplifying the dissolution process of the sheath component, the sheath component is preferably a copolyester, polylactic acid, polyvinyl alcohol, etc. that is easily soluble in an aqueous solvent or hot water, etc., and in particular, since it is easily soluble in an aqueous solvent such as an alkaline aqueous solution while maintaining crystallinity, it does not cause melting between the composite fibers even in false twisting processing with friction under heating, etc. From the viewpoint of high-order processing passability, particularly preferred polymers include polyesters copolymerized with 5 mol% to 15 mol% of 5-sodium sulfoisophthalic acid and polyesters copolymerized with 5 wt% to 15 wt% of polyethylene glycol having a weight average molecular weight of 500 to 3000 in addition to the above-mentioned 5-sodium sulfoisophthalic acid.

[0050] Generally, if the size of the inter-fiber voids increases, the softness due to the mobility of the fibers fixed at the bundling point of the woven knitted fabric and the lightness improvement due to the reduction of the apparent density at a high void ratio can be obtained, but on the other hand, the reduction of the bending rigidity as described above also causes a reduction in the sense of resilience. In order to eliminate this trade-off relationship, it is important that the coarse inter-fiber voids of 10 μm or more, which have the effect of improving the lightness, and the fine inter-fiber voids of less than 5 μm, which have both softness and a sense of resilience, exist in combination. In order to achieve this, in the core-sheath composite fiber of the present invention, it is necessary that the sheath component completely covers the multi-lobed core component having three or more convex portions.

[0051] If the sheath component completely covers the core component of the multi-lobed shape having more than three convex parts, the sheath can be dissolved to form coarse inter-fiber gaps of 10 μm or more in the concave parts of the multi-lobed shape where the sheath thickness is larger, and fine inter-fiber gaps of less than 5 μm can be formed in the convex parts where the sheath thickness is smaller, thereby achieving the light and soft texture unique to natural silk and a texture with a resilient feel. Furthermore, by forming concave-convex parts on the fiber surface, a reflection amplification effect of light can be obtained, thereby not only showing a high-grade luster such as the high brightness and soft luster of natural silk, but also forming concave-convex parts on the fiber surface and obtaining a dry touch. From this point of view, the more convex parts there are, the higher the inter-fiber gap formation, the gloss effect, and the dry feeling will be, so it is preferred as Figure 2 A three-lobed shape having three convex parts as shown in (a) of FIG. Figure 2 The 4-lobed shape with 4 convex parts as shown in (b). If the number of concave and convex parts is too large, the intervals between the concave and convex parts will become thinner, and the effect will gradually become similar to a circular cross-section. Therefore, the actual upper limit of the convex parts of the multi-lobed shape of the core component in the present invention is 6.

[0052] In the composite fiber of the present invention, from the viewpoint that only movable inter-fiber gaps of less than 5 μm are formed between adjacent single fibers due to the dissolution of the sheath component, the minimum thickness S of the sheath component is preferably 0.1 μm. min Ratio S to fiber diameter D min A composite fiber in which / D is 0.01 or more.

[0053] In the present invention, the fiber diameter D refers to the multifilament formed by the core-sheath composite fiber of the present invention embedded with an embedding agent such as epoxy resin, and the image of the fiber cross section perpendicular to the fiber axis is taken with a transmission electron microscope (TEM) at a magnification that can observe more than 10 fibers. At this time, if metal staining is implemented, the contrast of the junction of the core component and the sheath component can be clearly seen by using the staining difference between the polymers. The diameter of the fiber randomly extracted from each image taken in the same image is measured in μm units, measured to the first decimal place, and the simple average of the results of this operation for 10 randomly extracted fibers is calculated, and the value obtained by rounding off the first decimal place is set as the fiber diameter D (μm). Here, when the fiber cross section perpendicular to the fiber axis is not a perfect circle, its area is measured, and the value obtained by circle conversion is used.

[0054] In addition, the minimum thickness S of the sheath component referred to in the present invention is min It means, for example Figure 2 (a) Figure 5 As shown in (a), a straight line is drawn from the center of gravity G1 of the core component 1 existing on the fiber cross section to an arbitrary fiber surface, and the distance between the intersection S1 of the outer periphery of the core component 1 and the straight line and the intersection F of the fiber surface and the straight line, i.e., S1-F, is obtained by measuring the value to the first decimal place, and the minimum value among the obtained values ​​is calculated, and the simple average of the results obtained by performing this operation on 10 randomly selected fibers is obtained, and the value obtained by rounding off to the first decimal place is set as the minimum thickness S of the sheath component. min (μm). Here, for example Figure 4 (a) Figure 5 As shown in (b), when there is a core component 2 different from the core component 1 whose center of gravity is taken on a straight line drawn from the center of gravity G1 of the core component 1 to an arbitrary fiber surface, the distance between the intersection S1 of the periphery of the core component 1 and the straight line and the intersection S2 closest to S1 among the intersections of the periphery of the core component 2 and the straight line, i.e., S1-S2, is used. It should be noted that regarding the symbols in the figure, for example, G1 is the center of gravity of the core component 1, G2 is the center of gravity of the core component 2, and G is their general name, and the same is true for other symbols.

[0055] Furthermore, for the obtained fiber diameter D and the minimum thickness S of the sheath component min , calculate the ratio (S min / D) and round off the third decimal place to the nearest integer, and set the value S min / D.

[0056] If the configuration is the minimum thickness S of the sheath component min Ratio S to fiber diameter D min In the case where the sheath component has a S / D of 0.01 or more, the sheath dissolves out in the obtained woven knitted fabric, and fine inter-fiber spaces of less than 5 μm in which the fibers fixed at the bundling point of the woven knitted fabric can only move are revealed, which can give a soft texture, and is therefore preferred. From this point of view, S min The higher the S / D, the larger the size of the gaps between the fine fibers less than 5 μm, and the easier it is for the fibers to move. min When / D is set to 0.03 or more, the softness is further increased, and the high drapability unique to natural silk can be exhibited, which can be cited as a more preferred range. On the other hand, if the size of the inter-fiber space is too large, the bending recovery is also reduced, and the rebound feeling, which is one of the textures of natural silk, is impaired. Therefore, the actual upper limit in the present invention is 0.1.

[0057] As described above, in order to eliminate the trade-off between increased softness and lightness and decreased resilience due to the increase in the size of the inter-fiber spaces, it is important to set the core component to a multi-lobed shape, form coarse inter-fiber spaces of 10 μm or more by dissolving the sheath in the concave parts of the multi-lobed shape where the sheath thickness is larger, and form fine inter-fiber spaces of less than 5 μm in the convex parts where the sheath thickness is smaller, and it is further important to control the size of the maximum and minimum inter-fiber spaces. Therefore, the inventors of the present application conducted in-depth research and found that by setting the ratio of the maximum to the minimum inter-fiber spaces to be above a certain range, a sufficient difference is generated in the two inter-fiber spaces, so that the light, soft and resilient texture unique to natural silk can be highlighted. That is, the maximum thickness S of the sheath component is 1.34mm / s. max With minimum thickness S min Ratio S max / S min The second requirement is 5.0 or above.

[0058] In the present invention, the maximum thickness S of the sheath component max This means, for example, Figure 2 (a) Figure 5As shown in (a), a straight line is drawn from the center of gravity G1 of the core component 1 existing in the fiber cross section to an arbitrary fiber surface, and the distance between the intersection point S1 of the outer periphery of the core component 1 and the straight line and the intersection point F of the fiber surface and the straight line is obtained by measuring the value to the first decimal place, that is, S1-F, and the maximum value among the obtained values ​​is calculated. The simple average of the results obtained by performing this operation on 10 randomly selected fibers is obtained, and the value obtained by rounding off to the first decimal place is set as the minimum thickness S of the sheath component. max (μm). Here, for example Figure 4 (a) Figure 5 As shown in (b), when there is a core component 2 different from the core component 1 whose center of gravity is taken on a straight line drawn from the center of gravity G1 of the core component 1 to any fiber surface, the distance between the intersection S1 of the periphery of the core component 1 and the straight line and the intersection S2 closest to S1 among the intersections of the periphery of the core component 2 and the straight line, i.e., S1-S2, is used to obtain the value obtained by measuring the distance.

[0059] Furthermore, for the maximum thickness S of the sheath component obtained, max Minimum thickness S of the sheath component min , calculate the ratio (S max / S min ) and round off the second decimal place to the nearest integer, and set the value obtained by rounding off to S max / S min .

[0060] In the core-sheath composite fiber of the present invention, if the maximum thickness S of the sheath component corresponding to the coarse inter-fiber gap of 10 μm or more is max The minimum thickness S of the gap between fine fibers is equivalent to less than 5 μm min Ratio S max / S min If S is 5.0 or more, the lightness, softness and resilience of natural silk can be fully highlighted. max / S min When the value is set to 10.0 or more, the inter-fiber space size close to that of natural silk can be formed, and the lightness closer to that of natural silk can be obtained, so it can be cited as a more preferred range. max / S min The higher the better, but if S max / S min If the S is high, the degree of irregularity of the irregular cross-section fiber obtained after the sheath component is dissolved becomes high, and there are cases where high-order problems such as sparkling and stripes occur when the fabric is made. max / S min The actual upper limit is 30.0.

[0061] The area ratio of the sheath component in the core-sheath composite fiber of the present invention is preferably set to 10% to 50%. If the area occupied by the sheath component is increased, the effect of forming inter-fiber voids due to the dissolution of the sheath component is improved, so it is preferably 10% or more, and more preferably 20% or more. In addition, the higher the area ratio of the sheath component, the more preferred it is from the viewpoint of inter-fiber voids, but on the other hand, there is a decrease in strength due to excessive dissolution of the sheath component and a long dissolution treatment time, so the actual upper limit is 50%.

[0062] In the core-sheath composite fiber of the present invention, it is preferred that the fiber cross section is a perfect circle or an ellipse, and the inscribed circle diameter R of the fiber is A ( Figure 4 (a) The diameter of A) and the diameter of the circumscribed circle R B ( Figure 4 The relationship between (a) and (b) is preferably 1.0 ≤ R B / R A ≤2.5. Here, R B / R A Indicates the degree of fiber shape.

[0063] In the core-sheath composite fiber of the present invention, it is important to allow different inter-fiber spaces to coexist when the multi-lobal shape is formed by sheath dissolution. Figure 3 The core-sheath composite fibers (a) and (b) change similarly before and after the elution of the sheath component. Figure 2 (a), (b), Figure 4 (b), (c), Figure 5 (a) such a perfect circle, or Figure 4 (a) Figure 5 In the case of (b) a multi-lobed core component is formed in the elliptical core-sheath composite fiber, it is possible to mix the inter-fiber voids of 10 μm or more and the inter-fiber voids of less than 5 μm, which is preferred. B / R A 1.0≤R B / R A ≤2.5, the core-sheath composite fiber of the present invention is likely to be most densely packed when present as a multifilament, and thus the inter-fiber voids obtained after the sheath component is eluted can be made uniform without unevenness, which is preferred from the viewpoint of quality control.

[0064] In the core-sheath composite fiber of the present invention, from the viewpoint of enhancing the dry touch after the dissolution of the sheath component, the multi-lobed core component preferably has a groove at the front end of the convex portion toward the center of gravity of the core component, and the ratio of the distance from the center of gravity G of the core component to the bottom M of the groove, i.e., GM, to the distance GN from the center of gravity G of the core component to the front end N of the convex portion, i.e., GN / GM, is preferably 1.1 to 1.5.

[0065] The distance GM from the center of gravity G of the core component to the groove bottom M in the present invention refers to, for example, Figure 5 As shown in (a), the distance between the intersection of two arbitrary straight lines that divide the area of ​​the core component into 1 / 2, that is, the center of gravity G1 of the core component, and the point on the groove surface closest to the center of gravity G1 of the core component, that is, the groove bottom M1, is calculated. At this time, when there are more than two core components, the largest value among the values ​​obtained for each core component is used. The simple average of the results obtained by performing this operation on 10 randomly selected fibers is obtained, and the value obtained by rounding off the first decimal place is set as the distance from the center of gravity G of the core component to the groove bottom M, that is, GM (μm).

[0066] In addition, the distance from the center of gravity G of the core component to the front end N of the convex portion, that is, GN, referred to in the present invention means, for example Figure 5 As shown in (a), the distance between the center of gravity of the core component, i.e., G1, and the front end of the convex portion, i.e., N1, which is the farthest point on the groove surface from the center of gravity of the core component, G1, is calculated. At this time, when there are two or more core components, the largest value among the values ​​obtained for each core component is used. The simple average of the results obtained by performing this operation on 10 randomly selected fibers is obtained, and the value obtained by rounding off the first decimal place is set as the distance from the center of gravity of the core component G to the front end of the convex portion N, i.e., GN (μm).

[0067] Furthermore, the simple average of the ratio (GN / GM) of the distance from the center of gravity G of the core component to the groove bottom M, i.e., GM, and the distance from the center of gravity G of the core component to the front end N of the convex portion, i.e., GN, is calculated, and the value obtained by rounding off to the third decimal place is defined as GN / GM. At this time, when there is no groove at the front end of the convex portion in the core component, GN / GM=1.0.

[0068] In the present invention, after the sheath component is dissolved, a groove having a depth of GN / GM of 1.1 or more is formed at the front end of the convex portion along the center of gravity direction of the core component, and the friction force is increased by point contacting the skin with the groove surface, thereby enhancing the dry touch feeling, which is preferred. Furthermore, if the groove depth is formed to be GN / GM or more than 1.3, in addition to the dry feeling, light is diffusely reflected, not only with a softer luster, but also white blurring caused by regular reflection of light can be suppressed, and color rendering can be improved during dyeing, so it can be cited as a more preferred range. Among them, if the groove depth is deepened, the friction force will become too high and there is a possibility of deterioration of wear resistance such as fibrillation, so the actual upper limit of GN / GM is 1.5.

[0069] From the viewpoint of pursuing the texture of natural silk by reproducing the interfiber spaces unique to natural silk in more detail, in the core-sheath composite fiber of the present invention, the core component is preferably divided into two or more by the sheath component, and each of the divided core components has the above-mentioned multilobal shape.

[0070] When raw silk is extracted from silkworm cocoons, which are the raw materials of natural silk, silk protein ( Figure 1 a) is formed by sericin ( Figure 1 b) The cross-sectional shape of the covered fibers. That is, the spaces between the separated adjacent fibers are independent of the arrangement of the single fibers in the multifilament and are usually controlled only by the proportion of sericin dissolved. This can be understood as a state in which micro-fiber spaces of less than 5 μm stably exist between the single fibers that are unique to natural silk. In the core-sheath composite fiber of the present invention, it is preferred that the core component is divided into two or more sheath components, and each of the divided core components has a multi-lobed shape. There is no particular limitation on the number of divisions as long as it is two or more, for example Figure 4 As shown in (c), it can also be divided into 6 core components, but as the number of divisions increases, the inter-fiber gaps obtained will become smaller and precise control of the cross-section will become difficult, so the actual upper limit of the number of divisions is 10.

[0071] In the present invention, in order to further enlarge the inter-fiber spaces, it is preferred to arrange polymers with different melting points adjacent to each other in the fiber cross section, so that the core-sheath composite fiber has a curled shape according to the difference in shrinkage during heat treatment caused by the difference in melting points, or the sheath component of the core-sheath composite fiber is dissolved to show a difference in yarn length. If the inter-fiber spaces are enlarged, not only can a high-grade gloss and high color rendering be obtained by increasing the diffuse reflection of light, but also the lightness brought about by the increase in the void ratio and the decrease in the apparent density can be further enhanced.

[0072] That is, in the core-sheath composite fiber of the present invention, among the core components separated by the sheath components, it is preferred that the adjacent core components 1 (for example Figure 4(a), (b), (c) c1) and core component 2 (e.g. Figure 4 (a), (b), (c) and (c2) are formed of polymers with different melting points.

[0073] In the present invention, polymers with different melting points refer to a combination of polymers with a melting point difference of more than 10° C. among melt-moldable polymer groups such as polyester, polyethylene, polypropylene, polystyrene, polyamide, polycarbonate, polymethyl methacrylate, and polyphenylene sulfide, and their copolymers. In addition, in the core-sheath composite fiber of the present invention, since the purpose is to utilize the shrinkage difference of the core component to show the curled shape in the core-sheath composite fiber, or to make the sheath component of the core-sheath composite fiber dissolve to show the difference in yarn length, it is preferred that the core component 1 is a low-melting point polymer with high shrinkage, and the core component 2 is a high-melting point polymer with low shrinkage. As a combination of such a low-melting point polymer and a high-melting point polymer, for example, as a polyester system, copolymerized polyethylene terephthalate / polyethylene terephthalate, polybutylene terephthalate / polyethylene terephthalate, polypropylene terephthalate / polyethylene terephthalate, thermoplastic polyurethane / polypropylene terephthalate, As the core-sheath composite fiber of the present invention, from the viewpoint of not only being able to approach the bending rigidity of natural silk but also being able to obtain good color development when dyed, a particularly preferred range is a combination in which the divided core component is preferably a polyester-based one. In addition, examples of copolymer components in the copolymerized polyethylene terephthalate include succinic acid, adipic acid, azelaic acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, maleic acid, phthalic acid, isophthalic acid, and 5-sodium sulfonate of isophthalic acid. From the viewpoint of maximizing the shrinkage difference with polyethylene terephthalate, polyethylene terephthalate copolymerized with 5 mol % to 15 mol % of isophthalic acid is preferred.

[0074] As the area ratio of the core component 1 of the low melting point polymer to the core component 2 of the high melting point polymer in the core-sheath composite fiber of the present invention, it is preferred that the core component 1 / core component 2 is in the range of 70% / 30% to 30% / 70%. If it is in this range, it will not be affected by the hardening of the texture caused by the clogging of the mesh when the low melting point polymer is highly shrunk due to heat treatment, and the curling morphology can be fully manifested in the core-sheath composite fiber based on the shrinkage difference, or the yarn length difference can be fully manifested after the sheath component of the core-sheath composite fiber is dissolved, and a coarser inter-fiber space can be obtained.

[0075] The core-sheath composite fiber of the present invention is temporarily formed into various sheet-like fiber structures such as woven knitted fabrics, nonwoven fabrics, and papermaking, and then the sheath component is dissolved to obtain a multifilament composed of the core component. The multifilament can obtain a high-grade luster and a dry touch due to its unique fiber cross-sectional shape and inter-fiber spaces, and can obtain a natural silk texture such as a light, soft, and resilient texture.

[0076] In order to maximize the texture of natural silk with the above-mentioned high-grade luster, light, soft and resilient texture, it is important to form a void structure in which fine inter-fiber voids of less than 5 μm and coarse inter-fiber voids of 10 μm or more are uniformly mixed between individual fibers, as achieved by natural silk. Therefore, it is important for the multifilament of the present invention to have a void structure in which the average inter-fiber void distance is 5 to 30 μm, and the proportion of the inter-fiber void distance less than 5 μm is 10 to 50%.

[0077] Here, the inter-fiber gap distance referred to in the present invention refers to the image of a cross section of a multifilament-formed fabric taken perpendicular to the longitudinal direction of the fabric and perpendicular to the fiber axis of the multifilament using a scanning electron microscope (SEM) at a magnification that enables observation of 10 or more fibers. Figure 8 As shown in (b), a perfect circle that can enclose 10 fibers is drawn for each captured image. Among the 10 fibers existing inside the perfect circle, any one fiber is selected, and the intersection of the straight line connecting the center of gravity of the fiber and the adjacent fiber and the surface of each fiber is determined. The distance between the intersections is measured in μm units to the first decimal place. Furthermore, the value obtained by rounding off the first decimal place after the determined value is set as the inter-fiber gap distance (μm). The "adjacent" mentioned here means that there are no other fibers on the straight line connecting the center of gravity of any two fibers. Among the 10 fibers existing inside the perfect circle, as Figure 8 As shown in (b), this operation is performed for all adjacent fibers, the simple average of the results is calculated, and the value obtained by rounding off to the first decimal place is set as the average inter-fiber gap distance (μm). In addition, the proportion of inter-fiber gap distances less than 5 μm is also calculated.

[0078] The longer the average inter-fiber gap distance is, the more space is generated in which the fibers fixed at the bundle point of the woven knitted fabric can only move, and the effect of improving softness is obtained, so the average inter-fiber gap distance needs to be 5 μm or more. Furthermore, if the average inter-fiber gap distance is set to 10 μm or more, the apparent density is reduced when the cloth is made by showing fluffyness, and the lightness is improved, so that a light and soft texture close to natural silk can be shown, so it can be cited as a preferred range. From this point of view, lightness and softness are improved, but on the other hand, the bending rigidity reduction suppression effect in the inter-fiber gaps less than 5 μm uniformly mixed in the multifilament becomes smaller, and there is a tendency to reduce the sense of rebound, so the average inter-fiber gap distance is substantially upper limit 30 μm.

[0079] In addition to the above, in order to suppress the reduction in bending rigidity caused by the increase in the average inter-slot distance and maintain the sense of resilience, the proportion of the inter-fiber space distance less than 5 μm is required to be 10% or more. In addition, if the proportion of the inter-fiber space distance less than 5 μm is set to more than 20%, the relationship between lightness, softness and resilience is eliminated, and a light, soft and resilient texture can be well balanced, so it is cited as a preferred range. From this point of view, if the proportion of the inter-fiber space distance less than 5 μm is increased, the sense of resilience is improved, but on the other hand, there is a tendency for lightness and softness to decrease, so the proportion of the inter-fiber space distance less than 5 μm is substantially upper limit 50%.

[0080] The multifilament yarn of the present invention preferably has a void structure with a void ratio of 30 to 80%.

[0081] Here, the porosity referred to in the present invention refers to the image of a cross section of a multifilament-formed fabric taken perpendicular to the longitudinal direction of the fabric and perpendicular to the fiber axis of the multifilament using a scanning electron microscope (SEM) at a magnification that enables observation of 10 or more fibers. Figure 8 As shown in (b), a perfect circle that can enclose 10 fibers is drawn for each image taken, and the value of the total cross-sectional area of ​​the 10 fibers existing inside the perfect circle is calculated from the cross-sectional area of ​​the perfect circle. At this time, if the fibers contained inside the perfect circle are more than 1 / 2, it is recorded as 1 fiber, and the value is expressed in μm. 2 The cross-sectional area was measured to the first decimal place. The value obtained by dividing the obtained value by the cross-sectional area of ​​a perfect circle was multiplied by 100 and the value was rounded off to the first decimal place to be calculated as the porosity (%).

[0082] If the multifilament has a void structure with a void ratio of 30% or more, a space is created in which the fibers fixed at the bundling points of the woven knitted fabric can move, thereby obtaining an effect of improving the flexibility, which is preferred.

[0083] In addition, if the void structure has a void ratio of 50% or more, the apparent density is reduced when the fabric is made due to the high void ratio, and the lightness is improved, so that a light and soft texture close to natural silk can be shown, so it is cited as a more preferred range. From this point of view, the higher the average inter-fiber void distance and the void ratio, the higher the lightness and softness, but on the other hand, the bending rigidity reduction suppression effect in the inter-fiber voids less than 5 μm uniformly mixed in the multifilament becomes smaller, and there is a tendency to reduce the rebound feeling, so the void structure with a void ratio of 80% is the actual upper limit.

[0084] The multifilament of the present invention preferably contains two or more crimped fibers composed of polymers having different melting points, and the crimped fibers are preferably uniformly mixed. Figure 7 The fibers shown have a twisted, curled morphology.

[0085] In addition, the term "the crimped fibers are uniformly mixed" as used in the present invention means that Figure 8 As shown in (a), for any crimped fiber X in the multifilament, there is at least one crimped fiber Y composed of a polymer different from that of the crimped fiber X among all the crimped fibers adjacent to the crimped fiber X. In addition, the term "adjacent" as used in the present invention means that there is no other crimped fiber on the straight line connecting the centroid of the crimped fiber X and the centroid of any crimped fiber. As a method for obtaining the void structure of the multifilament of the present invention, there is a method of Figure 2 (a) Figure 5 (a) a method of eluting the sheath component after bundling a plurality of core-sheath composite fibers, Figure 4 From the viewpoint of making the interstices between fine fibers smaller than 5 μm and the interstices between coarse fibers larger than 10 μm more uniformly mixed in the multifilament, it is preferred to use the following method: Fig.10 As shown in (a) and (b), a plurality of core-sheath composite fibers in which the fiber cross section is divided into two by the sheath component d and the core components c1 and c2 are formed by polymers with different melting points are bundled and then heat-treated to develop a curled shape. Thereafter, the sheath component is dissolved out and the fibers are divided according to each polymer, thereby allowing the curled fibers composed of different polymers to be evenly mixed.

[0086] If the above method is used, the core-sheath composite fiber is subjected to heat treatment to develop a curled morphology, thereby forming a coarse inter-fiber space of 10 μm or more. In addition, because the sheath component exists between the core components, after the sheath component is dissolved, the inter-fiber space of less than 5 μm can be more stably formed between the adjacent curly fibers formed by polymers with different melting points, so that the inter-fine fiber space of less than 5 μm and the coarse inter-fiber space of more than 10 μm can be more uniformly mixed in the multifilament. That is, in the multifilament of the present invention, it is preferred that two or more curly fibers composed of polymers with different melting points are included, and the curly fibers are uniformly mixed, thereby making the texture of natural silk such as the high-grade luster, dry touch, light, soft and resilient texture based on the specific fiber cross-sectional shape and the void structure more prominent.

[0087] In the multifilament of the present invention, the crimped fiber preferably has a crimp peak number of 5 peaks / cm or more.

[0088] If it is within this range, the volume exclusion effect between fibers can be fully exerted, and a coarse inter-fiber space of tens of μm can be formed. Furthermore, if it is 10 peaks / cm or more, the volume exclusion effect between fibers is further improved, so that the size of the inter-fiber space can be further coarsened, and a light and soft texture close to natural silk can be shown, so it is listed as a more preferred range. On the other hand, if the number of curling peaks increases, there is a situation where the steric hindrance effect brought by the curling morphology is greater than the volume exclusion effect, thereby causing entanglement between fibers and impairing softness, so the upper limit of the number of curling peaks is 100 peaks / cm.

[0089] In the multifilament of the present invention, the difference in yarn length between two or more crimped fibers composed of different polymers is preferably 3% or more. By setting the difference in yarn length to 3% or more, the number of crimp peaks of the crimped fibers composed of polymers with different melting points showing a crimped morphology can be set to 10 peaks / cm or more. However, if the difference in yarn length is too large, the number of crimp peaks also increases, and the steric hindrance effect caused by the crimp morphology is greater than the volume exclusion effect, resulting in entanglement between fibers and impairing flexibility. Therefore, the upper limit of the difference in yarn length is 20%.

[0090] In the multifilament of the present invention, the crimped fiber is preferably composed of a homopolymer. If the crimped fiber is composed of a homopolymer, the core-sheath composite fiber composed of adjacent polymers with different melting points shows a more crimped morphology by heat treatment, so the crimp phases in the adjacent crimped fibers are consistent, and micro-fiber gaps less than 5 μm can be formed. On the other hand, when composed of two or more different polymers, the center of gravity of the polymer on the cross section is different depending on the composite cross section. Therefore, for the fiber composed of adjacent polymers with different melting points, the sheath component is dissolved to become a crimped fiber with a different crimp morphology, so the crimp phases are inconsistent, and it is difficult to stably form micro-fiber gaps less than 5 μm.

[0091] The fiber constituting the multifilament of the present invention preferably has a multilobal shape having three or more convex portions in the fiber cross section.

[0092] In the fiber cross section, if a multi-lobed shape with more than three convex parts is formed, the effect of light reflection amplification can be obtained by forming concavoconvex parts on the fiber surface, and combined with the complex reflection of light brought by the existence of the inter-fiber spaces of the above-mentioned size, a high-grade luster such as natural silk with high brightness and soft luster can be shown. In addition, by forming concavoconvex parts on the fiber surface to increase friction, a dry touch can also be obtained. From this point of view, the more convex parts, the higher the gloss effect and dry feeling, but when the number of concavoconvex parts is too much, the interval between the concavoconvex parts becomes thinner, and its effect will gradually be similar to a circular cross section, so the actual upper limit of the convex parts of the fiber constituting the multifilament of the present invention is 6.

[0093] In the fibers constituting the multifilament of the present invention, the inscribed circle diameter R C ( Fig. 9 (a) The diameter of C) and the circumscribed circle diameter R D ( Fig. 9 The relationship between the diameter of (a) D and (d) is preferably 1.5≤R D / R C ≤2.0. Here, R D / R C Indicates the degree of irregularity of the fiber. If it is within the above range, the light reflected and amplified by the multi-lobed concavo-convex parts can be reflected uniformly without glare, which is preferable from the viewpoint of quality control.

[0094] In the fiber constituting the multifilament of the present invention, from the viewpoint of enhancing the dry touch, in the fiber cross section, a groove is present at the tip of the convex portion, and the ratio of the distance MN from the groove bottom M to the tip N of the convex portion to the fiber diameter D (MN / D) is preferably 0.04 to 0.20.

[0095] The ratio of the distance MN from the groove bottom M to the convex tip N to the fiber diameter D (MN / D) mentioned in the present invention can be obtained as follows: the multifilament of the present invention is embedded with an embedding agent such as epoxy resin, and an image of the fiber cross section along the direction perpendicular to the fiber axis is taken with a scanning electron microscope (SEM) at a magnification that allows observation of 10 or more fibers. From each of the images taken, for example, fibers randomly extracted from the same image are imaged. Fig. 9 As shown, the distance MN between the groove bottom M as the point closest to the groove surface and the convex tip N as the farthest point is calculated from the intersection point of any two straight lines that make the cross-sectional integral of the fiber cross section of the crimped fiber 1 / 2, i.e., the center of gravity G.

[0096] In addition, the fiber diameter is measured in μm to the first decimal place. At this time, when the fiber cross section perpendicular to the fiber axis is not a perfect circle, its area is measured and the value obtained by converting it to a circle is used as the fiber diameter.

[0097] In addition, the ratio (MN / D) of the distance from the groove bottom M to the front end N of the protrusion obtained, that is, MN, and the fiber diameter D is calculated to the fourth decimal place, and the simple average of the results of this operation is obtained for 10 randomly selected fibers, and the value obtained by rounding off to the third decimal place is defined as MN / D. At this time, when the groove at the front end of the protrusion does not exist in the crimped fiber, MN / D=0.

[0098] In the fiber constituting the multifilament of the present invention, it is preferred to have grooves with a depth of MN / D of 0.04 or more, thereby increasing the frictional force by making point contact with the skin using the groove surface, thereby enhancing the dry touch. Furthermore, if the groove depth is formed to be MN / D of 0.10 or more, in addition to the dry feeling, light is diffusely reflected, not only having a softer luster, but also suppressing the white blur caused by the regular reflection of light, and improving the color rendering during dyeing, so it can be cited as a more preferred range. Among them, if the groove depth is deepened, the frictional force becomes too high, and there is a situation where the wear resistance is deteriorated due to fibrillation, so the actual upper limit of MN / D is 0.20.

[0099] In the fiber constituting the multifilament of the present invention, from the viewpoint of making the texture softer, the fiber diameter is preferably set to 15 μm or less. Furthermore, by setting the fiber diameter to 12 μm or less, it is possible to approach the single yarn fineness of natural silk, which is about 10 μm, and obtain a skin touch closer to natural silk, so that it becomes a range suitable for general clothing uses such as underwear, shirts, and blouses that come into contact with the skin. However, if the fiber diameter is too thin, the bending recovery is reduced, not only the rebound feeling, which is one of the textures of natural silk, is impaired, but also the color rendering property may be reduced, so the fiber diameter is preferably 8 μm or more.

[0100] In the core-sheath composite fiber and multifilament of the present invention, as realized by natural silk, a specific gap structure can be formed in which fine inter-fiber gaps of less than 5 μm and coarse inter-fiber gaps of tens of μm are uniformly mixed and exist between individual fibers. Therefore, if a fiber product is made of at least a part of the core-sheath composite fiber or multifilament of the present invention, various textures unique to natural silk can be reproduced, so it is of course suitable for suits and kimonos that were previously mainly made of natural silk, and it also has the ease of operation that only synthetic fibers have, so it can be preferably suitable for general clothing such as jackets, skirts, shorts, underwear, sportswear, clothing materials, carpets, sofas, curtains and other indoor products, car seats and other vehicle interior products, cosmetics, cosmetic masks, rags, health products and other daily uses, etc., involving a wide range of fiber products.

[0101] Hereinafter, an example of a method for producing the core-sheath composite fiber and the multifilament of the present invention will be described in detail.

[0102] As a method for spinning the core-sheath composite fiber of the present invention formed of two or more polymers, it can be produced by melt spinning for the purpose of producing long fibers, solution spinning such as wet and dry-wet spinning, melt blowing and spunbonding suitable for obtaining sheet-like fiber structures, etc. From the perspective of improving productivity, melt spinning is preferred. In addition, in the melt spinning method, it can be produced by using a composite spinneret described later, and the spinning temperature at this time is set to a temperature at which the high melting point and high viscosity polymers mainly show fluidity among the types of polymers used. The temperature at which fluidity is shown varies depending on the molecular weight, but if it is set between the melting point of the polymer and the melting point + 60°C, it can be stably produced.

[0103] The spinning speed can be set to about 500 to 6000 m / min, and can be changed according to the physical properties of the polymer and the purpose of use of the fiber. In particular, from the perspective of setting a high orientation and improving mechanical properties, it is preferred to set the spinning speed to 500 to 4000 m / min and then stretch it, because this can promote the uniaxial orientation of the fiber. During stretching, it is preferred to set the preheating temperature appropriately based on a temperature at which the polymer can soften, such as the glass transition temperature. As the upper limit of the preheating temperature, it is preferred to set the temperature at which the yarn path is not disturbed due to the spontaneous elongation of the fiber during the preheating process. For example, in the case of PET having a glass transition temperature of around 70°C, the preheating temperature is usually set to about 80 to 95°C.

[0104] In addition, when the discharge amount per single hole of the spinneret of the core-sheath composite fiber of the present invention is set to about 0.1 to 10 g / min / hole, stable production can be achieved. The discharged polymer flow is given an oil agent after cooling and solidification, and is pulled by a roller reaching a predetermined peripheral speed. Thereafter, it is stretched by a heated roller to obtain the desired core-sheath composite fiber.

[0105] In addition, in the core-sheath composite fiber of the present invention formed by two or more polymers, by setting the melt viscosity ratio of the polymers used to less than 5.0 and the difference in solubility parameter values ​​to less than 2.0, a composite polymer flow can be stably formed and a fiber with a good composite cross-section can be obtained, which is preferred.

[0106] As a composite spinneret used when producing the core-sheath composite fiber of the present invention formed of two or more polymers, it is preferable to use a composite spinneret described in Japanese Patent Application Laid-Open No. 2011-208313. Fig.12 The composite spinneret shown in FIG. 1 is assembled in a spinning unit in a state where three components, namely, a metering plate 1, a distribution plate 2, and a discharge plate 3, are stacked from the top and provided for spinning. Fig.12 This is an example of using three polymers, polymer A, polymer B, and polymer C. In the conventional composite spinneret, it is difficult to composite more than three polymers, and it is still preferred to use Fig.12 The composite spinneret illustrated utilizes a fine flow path.

[0107] for Fig.12 For the spinneret components illustrated, the following functions are performed, namely, the metering plate 1 meters the amount of polymer in each discharge hole and each distribution hole and allows it to flow in, the distribution plate 2 is used to control the composite cross-section and its cross-sectional shape in the cross-section of the single fiber, and the discharge plate 3 is used to compress and discharge the composite polymer flow formed in the distribution plate 2.

[0108] In order to avoid complicating the description of the composite spinneret, it is not shown in the figure, but for the components stacked upstream compared to the metering plate 1, it is sufficient to use components that form a flow path in conjunction with the spinning machine and the spinning assembly. By designing the metering plate 1 in conjunction with the existing flow path components, the existing spinning assembly and its components can be directly and effectively utilized. Therefore, there is no need to specialize the spinning machine specifically for the spinneret. In addition, in fact, multiple flow path plates can be stacked between the flow path-metering plate or between the metering plate 1 and the distribution plate 2. The purpose is to form the following structure, that is, to set a flow path that effectively transfers the polymer along the cross-sectional direction of the spinneret and the cross-sectional direction of the single fiber, and to introduce it into the distribution plate 2. The composite polymer flow discharged from the discharge plate 3 is cooled and solidified according to the above-mentioned manufacturing method, and then given an oil agent, and is pulled with a roller that reaches a specified peripheral speed. After that, a stretching process is performed with a heated roller to form the desired core-sheath composite fiber.

[0109] In the case of removing the sheath component from the core-sheath composite fiber of the present invention and manufacturing a multifilament formed by the core component, it is necessary to dissolve the sheath component to obtain a fiber formed by the core component, so the core-sheath composite fiber can be immersed in a solvent in which the easily soluble component is soluble to remove the sheath component. In the case where the easily soluble component is a copolymerized polyethylene terephthalate, polylactic acid, etc., which is copolymerized by sodium 5-sulfonate of isophthalic acid, polyethylene glycol, etc., an alkaline aqueous solution such as an aqueous sodium hydroxide solution can be used. At this time, if the alkaline aqueous solution is heated to more than 50°C, the hydrolysis can be accelerated, so it is preferred. In addition, if a fluid dyeing machine is used, it can be processed in large quantities at one time, so it is preferred from an industrial point of view.

[0110] Example

[0111] The core-sheath composite fiber and multifilament of the present invention will be specifically described with reference to the following examples.

[0112] The following evaluations were performed on Examples and Comparative Examples.

[0113] A. Melt viscosity of polymer

[0114] The moisture content of the polymer in the form of chips was reduced to 200 ppm or less by a vacuum dryer, and the melt viscosity was measured by a capillary rheometer manufactured by Toyo Seiki Co., Ltd. by changing the strain rate in stages. It should be noted that, as for the measurement temperature, the time from the time the sample was put into the heating furnace under a nitrogen atmosphere to the start of the measurement was set to 5 minutes, and the shear rate was set to 1216 s- 1 The value was evaluated as the melt viscosity of the polymer.

[0115] B. Melting point of polymer

[0116] The moisture content of the flaky polymer was made to be less than 200 ppm by a vacuum dryer, and about 5 mg was weighed. A differential scanning calorimeter (DSC) Q2000 made by TA Instruments was used. After heating from 0°C to 300°C at a heating rate of 16°C / min, the DSC measurement was performed at 300°C for 5 minutes. The melting point was calculated using the melting peak observed during the heating process. Three measurements were performed for each sample, and the average value was set as the melting point. It should be noted that when multiple melting peaks were observed, the melting peak vertex on the highest temperature side was set as the melting point.

[0117] C. Fineness

[0118] The weight of 100 m of the multifilament was measured and calculated by multiplying the weight by 100. This operation was repeated 10 times, and the average value was rounded off to the second decimal place and was defined as the fineness (dtex) of the multifilament.

[0119] D. Section parameters (R B / R A )

[0120] The core-sheath composite fiber was embedded with an embedding agent such as epoxy resin, and an image of the fiber cross section perpendicular to the fiber axis was taken using a scanning electron microscope (SEM) manufactured by HITACHI at a magnification that enables observation of more than 10 fibers. The obtained image was analyzed using WinROOF computer software manufactured by Mitani Shoji to calculate the circumscribed circle diameter R of the fiber. B (For example Figure 4 (a) The diameter of B) and the diameter of the inscribed circle of the fiber R A (For example Figure 4 The ratio of (a) to the diameter of A, that is, R B / R A In the present invention, the measurement is performed three times per filament, and the simple average of the results of the measurement for 10 filaments is calculated, and the value obtained by rounding off to the third decimal place is defined as R. B / R A .

[0121] E. Section parameters (S min / D, S max / S min )

[0122] The core-sheath composite fiber is embedded with an embedding agent such as epoxy resin, and an image of the fiber cross section perpendicular to the fiber axis is taken using a transmission electron microscope (TEM) at a magnification that allows observation of more than 10 fibers. At this time, if metal staining is performed, the contrast of the junction of the composite components can be clearly seen by using the staining difference between the polymers. In the captured image, the minimum thickness S of the sheath component is min The ratio of fiber diameter D, i.e. S min / D, the maximum thickness of the sheath component S max Minimum thickness S of the sheath component min The ratio of S max / S min Perform calculations.

[0123] In the present invention, the diameter of the fiber randomly extracted from each image taken is measured in μm units, and the measurement is performed to the first decimal place. The simple average of the results of the operation is performed on 10 randomly extracted fibers, and the value obtained by rounding off the first decimal place is set as the fiber diameter D (μm). Here, when the cross section of the fiber in the direction perpendicular to the fiber axis is not a perfect circle, its area is measured, and the value obtained by converting the circle is used.

[0124] In addition, the minimum thickness S of the sheath component in the present invention ismin It means, for example Figure 2 (a) Figure 5 As shown in (a), from each image taken, a straight line is drawn from the center of gravity G1 of the core component 1 existing on the cross section of the fiber randomly extracted in the same image to the surface of any fiber, and the distance between the intersection point S1 of the outer periphery of the core component 1 and the straight line and the intersection point F of the fiber surface and the straight line, i.e., S1-F, is measured, and the value measured to the first decimal place is obtained, and the minimum value of the obtained values ​​is calculated. The simple average of the results obtained by performing this operation on 10 randomly extracted fibers is obtained, and the value obtained by rounding off to the first decimal place is set as the minimum thickness S of the sheath component. min (μm). Here, for example Figure 4 (a) Figure 5 As shown in (b), when there is a core component 2 different from the core component 1 whose center of gravity is taken on a straight line drawn from the center of gravity G1 of the core component 1 to any fiber surface, the value obtained by measuring the distance S1-S2 between the intersection S1 of the periphery of the core component 1 and the straight line and the intersection S2 of the periphery of the core component 2 and the straight line that is closest to S1 is used.

[0125] For the obtained fiber diameter D and the minimum thickness S of the sheath component min , calculate the ratio (S min / D) and round off the third decimal place to the nearest integer, and set the value S min / D.

[0126] In addition, the minimum thickness S of the sheath component in the present invention is max It means, for example Figure 2 (a) Figure 5 As shown in (a), from each image taken, a straight line is drawn from the center of gravity G1 of the core component 1 existing on the cross section of the fiber randomly extracted in the same image to the arbitrary fiber surface, and the distance S1-F between the intersection S1 of the outer periphery of the core component 1 and the straight line and the intersection F of the fiber surface and the straight line is measured, and the value measured to the first decimal place is obtained, and the maximum value of the obtained values ​​is calculated. The simple average of the results obtained by performing this operation on 10 randomly extracted fibers is obtained, and the value obtained by rounding off to the first decimal place is set as the minimum thickness S of the sheath component. max (μm). Here, for example Figure 4 (a) Figure 5 As shown in (b), when there is a core component 2 different from the core component 1 whose center of gravity is taken on a straight line drawn from the center of gravity G1 of the core component 1 to any fiber surface, the distance between the intersection S1 of the periphery of the core component 1 and the straight line and the intersection S2 of the periphery of the core component 2 and the straight line closest to S1, that is, the value obtained by measuring S1-S2, is used.

[0127] The maximum thickness S of the sheath component is obtained max Minimum thickness S of the sheath component min , calculate the ratio (S max / S min ) and round off the second decimal place to the nearest integer, and set the value obtained by rounding off to S max / S min .

[0128] F. Section parameters (GN / GM)

[0129] For the core-sheath composite fiber observed in the item E., in the case where the multi-lobed core component has a groove at the tip of the convex portion facing the center of gravity of the core component, the ratio of the distance GM from the center of gravity G of the core component to the groove bottom M to the distance GN from the center of gravity G of the core component to the tip N of the convex portion, i.e., GN / GM, is calculated. At this time, when there is no groove at the tip of the convex portion in the core component, GN / GM=1.0.

[0130] The distance GM from the center of gravity G of the core component to the groove bottom M in the present invention means, for example Figure 5 As shown in (a), the value obtained by calculating the distance between the intersection of any two straight lines that divide the area of ​​the core component into 1 / 2, that is, the center of gravity G1 of the core component, and the point closest to the center of gravity G1 of the core component in the groove surface, that is, the groove bottom M1. At this time, when there are more than two core components, the largest value among the values ​​obtained for each core component is used. The simple average of the results obtained by performing this operation on 10 randomly selected fibers is obtained, and the value obtained by rounding off the first decimal place is set as the distance from the center of gravity G of the core component to the groove bottom M, that is, GM (μm).

[0131] In addition, the distance from the center of gravity G of the core component to the front end N of the convex portion, that is, GN in the present invention means, for example Figure 5 As shown in (a), the value obtained by calculating the distance between the center of gravity G1 of the core component and the point on the groove surface farthest from the center of gravity G1 of the core component, that is, the front end N1 of the convex portion. At this time, when there are two or more core components, the largest value among the values ​​obtained in each core component is adopted. The simple average of the results obtained by performing this operation on 10 randomly selected fibers is obtained, and the value obtained by rounding off the first decimal place is set as the distance from the center of gravity G of the core component to the front end N of the convex portion, that is, GN (μm).

[0132] For the distance from the center of gravity G of the core component to the groove bottom M, i.e. GM, and the distance from the center of gravity G of the core component to the front end N of the convex part, i.e. GN, the simple average of their ratio (GN / GM) is calculated, and the value rounded to the third decimal place is set as GN / GM.

[0133] G. Mixed existence of fibers in multifilament

[0134] The scanning electron microscope (SEM) manufactured by HITACHI was used to take images of a cross section of the multifilament fabric perpendicular to the longitudinal direction of the fabric and perpendicular to the fiber axis in the multifilament at a magnification that enables observation of 10 or more fibers. The images were analyzed using WinROOF computer software manufactured by Mitani Shoji. Figure 8 As shown in (a), in any fiber X in the multifilament, among all the fibers in a state where no other fiber exists on a straight line connecting the center of gravity of the fiber X and the center of gravity of any fiber, the number of fibers Y composed of a polymer different from that of the fiber X is evaluated. The simple average of the results of the evaluation for 10 fibers randomly selected from one multifilament is calculated, and the value is rounded off to the first decimal place, and the mixed state is judged in two levels based on the following criteria.

[0135] A: Uniformly mixed (the number of fibers Y made of a polymer different from that of fibers X is one or more)

[0136] C: Predominantly mixed (the fiber Y composed of a polymer different from that of the fiber X is less than one fiber).

[0137] H. Number of curl peaks (peaks / cm)

[0138] In a fabric formed of multifilaments, the multifilaments are extracted from the fabric in a manner that does not plastically deform, one end of the multifilaments is fixed, a load of 1 mg / dtex is applied to the other end, and after more than 30 seconds, a mark is applied at an arbitrary position where the distance between two points in the fiber axis of the multifilaments becomes 1 cm. After that, the fibers are separated from the multifilaments in a manner that does not plastically deform, and the pre-attached marks are adjusted to be the initial 1 cm and fixed on a glass slide. The sample is imaged at a magnification that allows the 1 cm mark to be observed using a VHX-2000 digital microscope manufactured by Keyence. The number of curling peaks between the marks is obtained in the image taken. The simple average of the results of this operation for 10 fibers composed of the same polymer is obtained, and the value obtained by rounding off the first decimal place is set as the number of curling peaks (peaks / cm). When fibers formed by different polymers are mixed, the number of curling peaks is obtained for the fibers formed by each polymer, and the number of curling peaks of the fiber formed by the polymer with the largest number of curling peaks is used.

[0139] I. Yarn length difference

[0140] In a fabric formed of multifilaments, a multifilament is extracted from the fabric in a manner that does not plastically deform, one end of the multifilament is fixed, a load of 1 mg / dtex is applied to the other end, and after 30 seconds or more, a mark is applied at an arbitrary position where the distance between two points in the fiber axis direction of the multifilament becomes 1 cm. Thereafter, the fibers are separated from the multifilament in a manner that does not plastically deform, and the fibers are fixed on a glass slide in such a manner that the distance between the previously attached marks becomes the initial 1 cm. The sample is imaged at a magnification that enables observation of the 1 cm mark using a VHX-2000 digital microscope manufactured by Keyence. The obtained image is analyzed using WinROOF computer software manufactured by Mitani Shoji, thereby measuring the actual fiber length between the marks. This operation is performed on 10 fibers formed of different polymers, and the simple average of the results is calculated, and (the largest actual fiber length - the smallest actual fiber length) / (the smallest actual fiber length)×100 is calculated from the obtained results, and the value obtained by rounding off to the first decimal place is set as the yarn length difference (%).

[0141] J. Inter-fiber gap distance

[0142] In the case of a fabric formed of multifilaments, an image of a cross section of the fabric perpendicular to the longitudinal direction of the fabric and perpendicular to the fiber axis of the multifilaments was taken using a scanning electron microscope (SEM) manufactured by HITACHI at a magnification that enables observation of 10 or more fibers. The taken image was analyzed using WinROOF computer software manufactured by Mitani Shoji, as shown in FIG. Figure 8 As shown in (b), a perfect circle that can enclose 10 fibers is drawn, and any one fiber is selected from the 10 fibers existing inside the perfect circle, and the intersection of the straight line connecting the center of gravity of the fiber and the adjacent fiber and the surface of each fiber is determined, and the distance between the intersections is measured in μm units to the first decimal place. Furthermore, the value obtained by rounding off the first decimal place after the obtained value is set as the inter-fiber gap distance (μm). The "adjacent" mentioned here means that there are no other fibers on the straight line connecting the center of gravity of any two fibers. Among the 10 fibers existing inside the perfect circle, as Figure 8 As shown in (b), this operation is performed for all adjacent fibers, the simple average of the results is calculated, and the value obtained by rounding off to the first decimal place is set as the average inter-fiber gap distance (μm). In addition, the proportion of inter-fiber gap distances less than 5 μm is calculated.

[0143] K.Porosity

[0144] In the case of a fabric formed of multifilaments, an image of a cross section of the fabric perpendicular to the longitudinal direction of the fabric and perpendicular to the fiber axis of the multifilaments was taken using a scanning electron microscope (SEM) manufactured by HITACHI at a magnification that enables observation of 10 or more fibers. The taken image was analyzed using WinROOF computer software manufactured by Mitani Shoji, as shown in FIG. Figure 8 As shown in (b), a perfect circle that can enclose 10 fibers is drawn, and the value of the total cross-sectional area of ​​the 10 fibers existing inside the perfect circle is calculated by deducting the cross-sectional area of ​​the perfect circle. In this case, if more than 1 / 2 of the fibers are included inside the perfect circle, it is recorded as 1 fiber, and the value is expressed in μm. 2 The cross-sectional area is measured to the first decimal place, and the value obtained by dividing the obtained value by the cross-sectional area of ​​a perfect circle is calculated, and the value obtained by rounding off to the first decimal place after multiplying by 100 is defined as the porosity (%).

[0145] L. Fiber diameter of special-shaped cross-section fibers

[0146] Using the image captured by item K., the diameter of the fiber randomly extracted from the same image is measured in μm units, and the diameter is measured to the first decimal place. For the largest fiber diameter among the results of this operation for 10 randomly extracted fibers, the value obtained by rounding off the first decimal place is set as the fiber diameter D (μm). Here, when the fiber cross section perpendicular to the fiber axis is not a perfect circle, its area is measured, and the value obtained by converting the circle is used.

[0147] M. Section parameters (R D / R C )

[0148] The image captured by item K was analyzed using WinROOF computer software manufactured by Mitani Shoji, and the circumscribed circle diameter R of the fiber was calculated. D (For example Fig. 9 (a) The diameter of C) and the inscribed circle diameter R of the fiber C (For example Fig. 9 The ratio of (a) to the diameter of C) is R D / R C In the present invention, the measurement is performed three times per filament, and the simple average of the results of the measurement for 10 filaments is calculated, and the value obtained by rounding off the second decimal place is defined as R. D / R C .

[0149] N. Section parameters (MN / D)

[0150] For the fiber observed in item K., when there is a groove at the tip of the convex portion, calculate the ratio of the distance MN from the groove bottom M to the tip N of the convex portion to the fiber diameter D, that is, MN / D. At this time, when there is no groove at the tip of the convex portion in the fiber, MN / D=0.

[0151] The ratio of the distance MN from the groove bottom M to the front end N of the convex portion to the fiber diameter D (MN / D) mentioned in the present invention is obtained by embedding the multifilament with an embedding agent such as epoxy resin, and taking an image of the fiber cross section perpendicular to the fiber axis with a scanning electron microscope (SEM) manufactured by HITACHI at a magnification that enables observation of 10 or more fibers. The fibers randomly extracted from the same image in the captured image are analyzed using WinROOF computer software manufactured by Mitani Shoji, for example. Fig. 9 As shown in (b), calculate the distance MN from the intersection of any two straight lines that make the cross-sectional integral of the fiber cross section of the fiber equal to 1 / 2, i.e., the center of gravity G, to the nearest point on the groove surface (i.e., the groove bottom M) and the farthest point (i.e., the front end N of the convex portion).

[0152] The fiber diameter D is measured in μm to the first decimal place. When the cross section of the fiber perpendicular to the fiber axis is not a perfect circle, the area is measured and the value obtained by converting the circle is used as the fiber diameter D.

[0153] For the distance MN from the bottom of the groove M to the front end of the convex part N and the fiber diameter D, their ratio (MN / D) is calculated to the fourth decimal place, and the simple average of the results of performing this operation on 10 randomly selected fibers is obtained. The value rounded to the third decimal place is set as MN / D.

[0154] O. Texture evaluation (gloss, lightness, softness, resilience, dryness)

[0155] The number of fibers was adjusted so that the cover factor (CFA) in the warp direction was 800 and the cover factor (CFB) in the weft direction was 1200, and 8 satin fabrics were made. The CFA and CFB mentioned here refer to the warp density and weft density of the woven fabric measured in the interval of 2.54 cm according to JIS-L-1096:20108.6.1, and CFA=warp density×(fineness of warp yarn) 1 / 2 , CFB = weft density × (fineness of weft yarn) 1 / 2 The obtained woven fabric was evaluated for five textures, namely, glossiness, lightness, softness, rebound feeling, and dry feeling, using the following method.

[0156] As for the glossiness, an automatic variable angle photometer (GONIOPHOTOMETER GP-200) manufactured by Murakami Color Research Institute was used to inject light into each sample at an incident angle of 60°. The light intensity at the receiving angle of 0° to 90° was determined by measuring the secondary reflected light distribution every 0.1°. The maximum light intensity (specular reflection) near the receiving angle of 60° was divided by the minimum light intensity (diffuse reflection) near the receiving angle of 0°. This operation was performed three times for each part, and the simple average of the results of the operation for a total of 10 parts was obtained. The value obtained by rounding off the second decimal place was set as the comparative glossiness. Based on the obtained comparative glossiness, the glossiness was judged in three levels based on the following standards.

[0157] S: Excellent gloss (comparative gloss <1.6)

[0158] A: Good gloss (1.6≤contrast gloss<1.9)

[0159] C: Poor gloss (1.9 ≤ comparative gloss).

[0160] Lightness The thickness (cm) of a 20 cm × 20 cm woven fabric was measured using a constant pressure thickness gauge (PG-14J) manufactured by Teletech, and the volume of the woven fabric was calculated. The value obtained by dividing the weight (g) of the woven fabric by the obtained volume was set as the apparent density (g / cm 3 ). Based on the obtained apparent density, the lightness was evaluated into three levels according to the following criteria.

[0161] S: Excellent lightness (apparent density ≤ 0.33)

[0162] A: Good lightness (0.34<apparent density≤0.39)

[0163] C: Poor lightness (0.4 < apparent density).

[0164] The flexibility was calculated by using a pure bending tester (KES-FB2) manufactured by KATO Tech, with an effective sample length of 20 cm × 1 cm and holding a 20 cm × 20 cm woven fabric, and calculating the maximum curvature in the weft direction to ± 2.5 cm -1 When bent under the conditions of , the curvature is 0.5cm -1 and 1.5cm -1 The difference in bending moment per unit width (gf cm / cm) divided by the difference in curvature 1cm -1 The value obtained is the same as the curvature -0.5cm -1 and -1.5cm -1 The difference in bending moment per unit width (gf cm / cm) divided by the difference in curvature 1cm -1This operation was performed three times for each part, and the simple average of the results of the operation for a total of 10 parts was calculated. The value obtained by rounding off to the fourth decimal place and dividing by 100 was set as the bending hardness B×10 -2 (gf cm 2 / cm). According to the bending hardness B×10 -2 The softness was evaluated into three grades based on the following criteria.

[0165] S: Excellent flexibility (bending hardness B×10 -2 ≤1.0)

[0166] A: Good flexibility (1.0 < bending hardness B × 10 -2 ≤1.9)

[0167] C: Poor flexibility (1.9 < bending hardness B × 10 -2 ).

[0168] For the rebound feeling, a pure bending tester (KES-FB2) manufactured by KATO Tech was used to hold a 20 cm × 20 cm woven fabric with an effective sample length of 20 cm × 1 cm, and the curvature when bent in the weft direction was calculated to ±1.0 cm. -1 This operation was performed three times for each part, and the simple average of the results of the operation for a total of 10 parts was calculated. The value obtained by rounding off to the fourth decimal place and dividing by 100 was set as the bending recovery 2HB×10 -2 (gf·cm / cm). According to the obtained bending recovery 2HB×10 -2 The rebound feeling was evaluated into three levels based on the following criteria.

[0169] S: Excellent rebound feeling (bending recovery 2HB×10 -2 ≤1.0)

[0170] A: Good rebound feeling (1.0<bending recovery 2HB×10 -2 ≤1.9)

[0171] C: Poor rebound feeling (1.9<bending recovery 2HB×10 -2 ).

[0172] For the dry feeling, the KATO Tech automated surface tester (KES-FB4) was used to apply a load of 50 g to a terminal that was wound with piano wire to form a 1 cm × 1 cm area of ​​a 20 cm × 20 cm woven fabric, and the terminal was slid at a speed of 1.0 mm / sec to obtain the average friction coefficient MIU. This operation was performed three times for each location, and the simple average of the results of the operation for a total of 10 locations was obtained, and the value rounded off to the second decimal place was set as the friction coefficient. Based on the obtained friction coefficient, the dry feeling was judged in three levels based on the following standards.

[0173] S: Excellent dry feeling (0.7 ≤ friction coefficient)

[0174] A: Good dry feeling (0.3≤friction coefficient<0.7)

[0175] C: Poor dry feeling (friction coefficient < 0.3).

[0176] P. Color rendering

[0177] The number of fibers was adjusted so that the cover factor (CFA) in the warp direction was 800 and the cover factor (CFB) in the weft direction was 1200, and 8 satin fabrics were made. The obtained woven fabric was dyed black using the disperse dye Sumikaron BlackS-3B (10% owf). The dyed woven fabric was evaluated for the L value based on the reflection measurement of the woven fabric using CM-3700A manufactured by Konica Minolta. The operation was measured 3 times for each part, and the simple average of the results of the operation for a total of 10 parts was calculated. The value obtained by rounding off the first decimal place was set as the black dyeing L value. Based on the obtained black dyeing L value, the color rendering was judged in 3 levels based on the following standards.

[0178] S: Excellent color development (black dyeing L value <15)

[0179] A: Good color rendering (15≤black dyeing L value<18)

[0180] C: Poor color rendering (18 ≤ black dyeing L value).

[0181] Q. Wear resistance

[0182] The number of fibers was adjusted so that the cover factor (CFA) in the warp direction was 1100 and the cover factor (CFB) in the weft direction was 1100, and a plain woven fabric was prepared. The obtained woven fabric was dyed black using disperse dye Sumikaron Black S-3B (10% owf). The dyed woven fabric was cut into a circle with a diameter of 10 cm, moistened with distilled water and mounted on a disk. Furthermore, the woven fabric cut into a 30 cm square was fixed on a horizontal plate in a dry state. The disk mounted with the woven fabric moistened with distilled water was brought into horizontal contact with the woven fabric fixed on the horizontal plate, and the disk was subjected to a circular motion of 420 g and a speed of 50 rpm for 10 minutes in a manner such that a circle with a diameter of 10 cm was drawn at the center of the disk, so that the two woven fabrics were rubbed. After the rubbing was completed, the woven fabric was left for 4 hours, and the degree of fading of the woven fabric mounted on the disk was judged on a scale of 1 to 5 using a gray scale for fading, with a scale of 0.5. From the obtained grade determination results, wear resistance was determined into three grades based on the following criteria.

[0183] S: Excellent wear resistance (level judgment: 4 or above)

[0184] A: Good wear resistance (level judgment: level 3 or level 3-4)

[0185] C: Poor abrasion resistance (grade determination: less than grade 3).

[0186] [Example 1]

[0187] As polymer 1, polyethylene terephthalate copolymerized with 8 mol % of 5-sodium sulfonate isophthalic acid and 9 wt % of polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa·s, melting point: 233°C) was prepared, and as polymer 2, polyethylene terephthalate (PET, melt viscosity: 130 Pa·s, 254°C) was prepared.

[0188] These polymers were melted at 290°C, respectively, and weighed in a weight ratio of 30 / 70 for polymer 1 / polymer 2, and poured into a Fig.12 The spinning assembly of the composite spinneret shown in FIG. Figure 5 The inflowing polymer is discharged from the discharge hole in the form of a core-sheath composite fiber of a perfect circular shape as shown in (a), and a composite structure in which the sheath component completely covers the core component having a groove at the front end of the convex part of the trilobal cross section. At this time, the sheath component is polymer 1 and the core component is polymer 2.

[0189] The discharged composite polymer stream was cooled and solidified, and then provided with an oil agent, and was taken up at a spinning speed of 1500 m / min and stretched between rolls heated to 90°C and 130°C to produce a core-sheath composite fiber of 56 dtex-36 filaments.

[0190] The ratio of the minimum thickness of the sheath component to the fiber diameter (S min / D) is 0.03, and the ratio of the maximum thickness to the minimum thickness of the sheath component (S max / S min ) was 16. In addition, the ratio of the distance from the center of gravity G of the core component to the groove bottom M, i.e. GM, to the distance from the center of gravity G of the core component to the front end N of the convex portion, i.e. GN (GN / GM) was 1.42, which confirmed that it was the core-sheath composite fiber of the present invention.

[0191] In addition, the inscribed circle diameter R of the core-sheath composite fiber is A The diameter of the circumscribed circle R B The ratio is 1.0, which facilitates the densest packing in the case of multifilaments, so that the inter-fiber spaces obtained after the sheath component is dissolved can be uniform without deviation.

[0192] The woven fabric made of the core-sheath composite fiber was treated in a 1 wt% sodium hydroxide aqueous solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, thereby obtaining a woven fabric composed of multifilaments (fiber diameter 10 μm) formed by the core component of the core-sheath composite fiber.

[0193] In the woven fabric composed of the multifilament, the sheath component completely covering the multi-leaf core component is dissolved, and thus, in the multifilament, there is a void structure in which fine inter-fiber voids of less than 5 μm and coarse inter-fiber voids of 10 μm or more are uniformly present between individual fibers, as in natural silk, resulting in a good gloss (contrast gloss: 1.7) with no viewing angle dependence, a good rebound feeling (bending recovery 2HB: 0.6×10 -2 gf·cm / cm) dry feeling (friction coefficient: 0.7), and good lightness (apparent density: 0.40g / cm 3 ) and softness (bending hardness B: 0.7×10 -2 gf cm 2 / cm) with a texture close to natural silk.

[0194] Furthermore, it was found that when the woven fabric was dyed black, it exhibited excellent color development (black dyeing L value: 14) by utilizing the diffuse reflection of light from the inter-fiber spaces uniformly existing between the single fibers and the grooves at the front ends of the convex parts of the special-shaped cross-section fibers, and also had good abrasion resistance (grade 3-4) without discoloration due to fibrillation in the grooves. The results are shown in Table 1-1.

[0195] [Examples 2 and 3]

[0196] The same procedures as in Example 1 were followed except that the weight ratio of polymer 1 / polymer 2 was changed to 20 / 80 (Example 2) and 10 / 90 (Example 3).

[0197] In Examples 2 and 3, the less the sheath component, the greater the bending hardness, and the characteristic woven fabric has an elastic touch while retaining the texture of natural silk. In addition, since the groove at the front end of the convex part of the fiber in the multifilament is shallow, the wear resistance is also excellent. The results are shown in Table 1-1.

[0198] [Example 4]

[0199] The composite structure of the core-sheath composite fiber is changed to Figure 2 (a), and all other aspects are implemented according to Example 1.

[0200] In Example 4, there is no groove at the tip of the convex part of the fiber in the multifilament, so the diffuse reflection of light is reduced and the reflection intensity is increased, and the visual recognition of the gloss is increased. In addition, the wear resistance is also excellent. The results are shown in Table 1-1.

[0201] [Comparative Example 1]

[0202] As polymer 1, polyethylene terephthalate copolymerized with 8 mol % of 5-sodium sulfonate isophthalic acid and 9 wt % of polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa·s, melting point: 233°C) was prepared, and as polymer 2, polyethylene terephthalate (PET, melt viscosity: 130 Pa·s, 254°C) was prepared.

[0203] After these polymers were melted at 290°C, they were weighed in a weight ratio of 30 / 70 for polymer 1 / polymer 2 and poured into a Fig.12 The spinning assembly of the composite spinneret shown in FIG. Figure 3 The inflowing polymer is discharged from the discharge hole in a simple composite structure in which the sheath component covers the core component of a circular cross section as shown in (a). At this time, the sheath component is polymer 1 and the core component is polymer 2.

[0204] The discharged composite polymer stream was cooled and solidified, and then provided with an oil agent, and was taken up at a spinning speed of 1500 m / min and stretched between rolls heated to 90°C and 130°C to produce a core-sheath composite fiber of 56 dtex-36 filaments.

[0205] The woven fabric made of the woven core-sheath composite fiber is treated in a 1 wt% sodium hydroxide aqueous solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, thereby obtaining a woven fabric composed of multifilaments (fiber diameter 10 μm) formed by the core component of the core-sheath composite fiber.

[0206] The obtained woven fabric had coarse inter-fiber spaces of 10 μm or more between each fiber in the multifilament, but no inter-fiber spaces of less than 5 μm, and the spaces collapsed when the woven fabric was touched, so it lacked lightness and resilience. In addition, since there were no convex parts or grooves in the core component, it also lacked a dry feeling. The results are shown in Table 1-1.

[0207] [Comparative Example 2]

[0208] The composite structure of the core-sheath composite fiber is changed to Figure 3 (b), and all other aspects were implemented according to Comparative Example 1.

[0209] In Comparative Example 2, the dry feeling was slightly improved due to the core component of the trilobal cross section, but after the sheath component was eluted, there were no fine inter-fiber spaces of less than 5 μm between individual fibers, and the lightness and resilience were lacking. The results are shown in Table 1-1.

[0210] [Comparative Example 3]

[0211] As polymer 1, polyethylene terephthalate copolymerized with 8 mol % of 5-sodium sulfonate isophthalic acid and 9 wt % of polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa·s, melting point: 233°C) was prepared, and as polymer 2, polyethylene terephthalate (PET, melt viscosity: 130 Pa·s, 254°C) was prepared.

[0212] These polymers were melted at 290°C, respectively, and weighed so that the weight ratio of polymer 1 to polymer 2 was 5 / 95, and poured into a Fig.12 The spinning assembly of the composite spinneret shown in FIG. Figure 6 As shown in (a), the polymer is discharged from the discharge hole in the form of a composite structure in which the easily soluble component is arranged in a tapered shape along the fiber inner direction at the front end of the convex part of the difficult soluble component in a trilobal shape as described in Japanese Patent Publication No. 57-5912. At this time, the easily soluble component is polymer 1 and the difficult soluble component is polymer 2.

[0213] The discharged composite polymer stream was cooled and solidified, and then oil was applied, and the yarn was taken up at a spinning speed of 1500 m / min and stretched between rolls heated to 90°C and 130°C to produce composite fibers of 56 dtex-36 filaments.

[0214] The woven fabric made of the composite fiber was treated in a 1 wt% sodium hydroxide aqueous solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, thereby obtaining a woven fabric composed of multifilaments (fiber diameter 12 μm) formed by the difficultly soluble components of the composite fiber.

[0215] In Comparative Example 3, there are deep grooves tapering along the fiber interior direction at the front end of the convex part of the trilobal-shaped special-shaped cross-section fiber, so the friction coefficient is increased, and although the dry feeling is excellent, the wear resistance is poor. In addition, after the dissolution of the sheath component, there are no coarse inter-fiber gaps of 10 μm or more between the individual fibers, and the glaring luster lacks a sense of luxury. In addition, it also lacks lightness, softness, and resilience. The results are shown in Table 1-2.

[0216] [Examples 5 and 6]

[0217] The same procedures as in Example 4 were followed except that the discharge rate was changed so that the fiber diameter of the modified cross-section fiber consisting only of the core component of the core-sheath composite fiber was 14 μm (Example 5) or 17 μm (Example 6).

[0218] In Examples 5 and 6, the fiber cross section of the multifilament obtained after the sheath was dissolved was increased by increasing the fiber diameter, and the unevenness caused by the three-leaf cross section was strengthened, the reflection intensity was further increased, and the visual recognition of the gloss of the obtained woven fabric was further increased. In addition, since the bending hardness was increased, while retaining the natural silk-like texture, a characteristic elastic touch was obtained. The results are shown in Table 1-2.

[0219] [Example 7]

[0220] The composite structure of the core-sheath composite fiber is changed to Figure 2 (b), and all other aspects are implemented according to Example 4.

[0221] In Example 7, the fiber cross section of the fibers in the multifilament yarn was changed from a trilobal cross section to a quadlobal cross section, so that diffuse reflection of light at the convex portion increased, and a woven fabric having a texture that not only had a more luxurious luster but also had improved friction and a dry touch was obtained. The results are shown in Table 1-2.

[0222] [Comparative Example 4]

[0223] As polymer 1, polyethylene terephthalate copolymerized with 8 mol % of 5-sodium sulfonate isophthalic acid and 9 wt % of polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa·s, melting point: 233°C) was prepared, and as polymer 2, polyethylene terephthalate (PET, melt viscosity: 130 Pa·s, 254°C) was prepared.

[0224] These polymers were melted at 290°C, respectively, and weighed so that the weight ratio of polymer 1 to polymer 2 was 20 / 80, and poured into a pre-assembled Fig.12 The spinning assembly of the composite spinneret shown, such as Figure 3 As shown in (c), the polymer is discharged from the discharge hole in a composite structure in which the easily soluble component is divided into a plurality of poorly soluble components as described in Japanese Patent Publication No. 2010-222771. At this time, the easily soluble component is polymer 1 and the poorly soluble component is polymer 2.

[0225] The discharged composite polymer stream was cooled and solidified, and then oil was applied, and the yarn was taken up at a spinning speed of 1500 m / min and stretched between rolls heated to 90°C and 130°C to produce composite fibers of 56 dtex-18 filaments.

[0226] The woven fabric made of the composite fiber was treated in a 1 wt% sodium hydroxide aqueous solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, thereby obtaining a woven fabric composed of multifilaments (fiber diameter 6 μm) formed by the difficultly soluble components of the composite fiber.

[0227] In Comparative Example 4, the fibers in the multifilament yarn have a fine fiber diameter, so the gloss and softness are excellent, but the fine fiber gaps less than 5 μm and the coarse fiber gaps of 10 μm or more are not uniformly present between the individual fibers, and the lightness and resilience are lacking. In addition, due to the fine fiber diameter, dyeing is difficult, and the color development is also lacking. The results are shown in Table 1-2.

[0228] [Example 8]

[0229] As polymer 1, polyethylene terephthalate copolymerized with 8 mol % of 5-sodium sulfonate of isophthalic acid and 9 wt % of polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa·s, melting point: 233°C) was prepared, as polymer 2, polyethylene terephthalate copolymerized with 7 mol % of isophthalic acid (IPA copolymerized PET, melt viscosity: 140 Pa·s, melting point: 232°C) was prepared, and as polymer 3, polyethylene terephthalate (PET, melt viscosity: 130 Pa·s, melting point: 254°C) was prepared.

[0230] After these polymers were melted at 290°C, they were weighed so that the weight ratio of polymer 1 / polymer 2 / polymer 3 was 30 / 35 / 35, and poured into a pre-assembled Fig.12 The spinning assembly of the composite spinneret shown in FIG. Figure 5 The core-sheath composite fiber is an elliptical fiber as shown in (b), wherein the sheath component completely covers the core component, the core component is divided into two by the sheath component, and the divided core component 1 and core component 2 are respectively formed into a composite structure having a groove at the front end of the convex part of the trilobal cross section, and the inflowing polymer is discharged from the discharge hole. At this time, the sheath component is polymer 1, the core component 1 is polymer 2, and the core component 2 is polymer 3.

[0231] The discharged composite polymer stream was cooled and solidified, and then provided with an oil agent, and was taken up at a spinning speed of 1500 m / min and stretched between rolls heated to 90°C and 130°C to produce a core-sheath composite fiber of 56 dtex-18 filaments.

[0232] The ratio of the minimum thickness of the sheath component to the fiber diameter (S min / D) is 0.03, and the ratio of the maximum thickness to the minimum thickness of the sheath component (S max / S min ) was 12. In addition, the ratio of the distance GM from the center of gravity G of the core component to the groove bottom M to the distance GN from the center of gravity G of the core component to the front end N of the convex portion (GN / GM) was 1.38, which confirmed that it was the core-sheath composite fiber of the present invention.

[0233] In addition, the inscribed circle diameter R of the core-sheath composite fiber is A The diameter of the circumscribed circle R B The ratio is 1.8, which facilitates the densest packing in the presence of multifilaments, so that the inter-fiber spaces obtained after the sheath component is dissolved can be uniform without deviation.

[0234] The woven fabric of the core-sheath composite fiber is treated in a 1 wt% sodium hydroxide aqueous solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, and then heat-treated with wet heat at 130°C to obtain a woven fabric composed of multifilaments (fiber diameter 10 μm) formed by the core component of the core-sheath composite fiber.

[0235] For the woven fabric composed of the multifilament, the sheath component completely covering the multi-leaf core component is dissolved, and a void structure is shown in which fine inter-fiber voids of less than 5 μm and coarse inter-fiber voids of 10 μm or more are uniformly present between individual fibers, as in natural silk. In addition, since core component 1 and core component 2 have different shrinkage differences, the difference in yarn length is shown by heat treatment after the sheath component is dissolved. Compared with Example 1, the inter-fiber voids of 10 μm or more become coarser, thereby having a void structure that is more similar to the inter-fiber voids of natural silk. In addition, its texture has a high-grade gloss that is not dependent on viewing angle (comparative gloss: 1.4) and an excellent rebound feeling (bending recovery 2HB: 0.8×10 -2 gf·cm / cm) dry feeling (friction coefficient: 0.8), and very light (apparent density: 0.32g / cm 3 ) and excellent flexibility (bending hardness B: 0.9×10 -2 gf cm 2 / cm), a woven fabric with a texture like natural silk.

[0236] Furthermore, it can be seen that when the woven fabric is dyed black, the diffuse reflection of light is further enhanced, showing excellent color rendering (black dyeing L value: 13), and also having good abrasion resistance (grade 3-4) without discoloration due to fibrillation in the groove portion. The results are shown in Table 2-1.

[0237] [Examples 9 and 10]

[0238] The same procedures as in Example 8 were followed except that the polymer 2 was changed to polytrimethylene terephthalate (PPT) (Example 9) or polyethylene terephthalate (PET) (Example 10).

[0239] In Example 9, the rubber elasticity of PPT is combined to provide a woven fabric that not only has a softer texture but also has a unique stretching function that natural silk does not have. In addition, since PPT has a lower refractive index than PET, the color rendering of the obtained woven fabric is also excellent.

[0240] In Example 10, although there was no difference in yarn length, the natural silk-like texture was fully exhibited, and the core component was divided into two, so compared with Example 1, the fine fiber gaps less than 5 μm and the coarse fiber gaps of 10 μm or more existed more evenly, and the texture of the obtained woven fabric was improved in lightness, softness, and resilience. The results are shown in Table 2-1.

[0241] [Example 11]

[0242] The composite structure of the core-sheath composite fiber is changed to Figure 4 (a), and all other aspects are implemented according to Example 8.

[0243] In Example 11, the front end of the convex part of the special-shaped cross-section fiber has no groove part, so the diffuse reflection of light is reduced, the reflection intensity is increased, and the visual recognition of the gloss is improved. In addition, the wear resistance is also excellent. The results are shown in Table 2-1.

[0244] [Examples 12 and 13]

[0245] The composite structure of the core-sheath composite fiber is set as Figure 4 The above steps were carried out in the same manner as in Example 8 except that the weight ratio of polymer 2 / polymer 3 was changed to 50 / 20 (Example 12) and 20 / 50 (Example 13).

[0246] In Examples 12 and 13, as the ratio of polymer 2 as a high shrinkage component increases, the yarn length difference becomes stronger, and the lightness of the obtained woven fabric increases. In addition, as the ratio of polymer 3 as a low shrinkage component increases, the diffuse reflection of light decreases and the reflection intensity increases, the visual recognition of the gloss increases, and not only that, the clogging of the mesh caused by the high shrinkage rate of the high shrinkage component in the wet heat treatment can be suppressed, and the softness and resilience are also excellent. The results are shown in Table 2-1 and Table 2-2.

[0247] [Example 14]

[0248] The composite structure of the core-sheath composite fiber is set as Figure 4 (a), the degree of irregularity (R B / R A ) is changed to 3.0, and all other aspects are implemented according to Example 8.

[0249] Since the greater the profile of the core-sheath composite fiber, the greater the profile of the core component, the unevenness of the fiber cross section of the fiber in the multifilament obtained after the sheath is dissolved is enhanced by the trilobal cross section, the reflection intensity is further increased, and the visual recognition of the gloss of the obtained woven fabric is further increased. The results are shown in Table 2-2.

[0250] [Example 15]

[0251] The composite structure of the core-sheath composite fiber is changed to Figure 4 (b), irregularity (R B / R A =1.0), and all other aspects were carried out in accordance with Example 8.

[0252] The smaller the degree of irregularity of the core-sheath composite fiber, the easier it is to pack densely when it exists as a multifilament, so that the inter-fiber gaps obtained after the sheath component is eluted can be uniform and uniform, and the quality of the obtained woven fabric can be improved. The results are shown in Table 2-2.

[0253] [Example 16]

[0254] The composite structure of the core-sheath composite fiber is changed to Figure 4 (c), irregularity (R B / R A =1.0), and all other aspects were carried out in accordance with Example 8.

[0255] In Example 16, the core component was divided into six parts by the sheath component, and the fiber diameter of the modified cross-section fiber obtained after the sheath component was removed became thinner, so that a woven fabric having not only a softer and more luxurious luster but also excellent softness was obtained. The results are shown in Table 2-2.

[0256] [Comparative Example 5]

[0257] As polymer 1, polyethylene terephthalate copolymerized with 8 mol % of 5-sodium sulfonate of isophthalic acid and 9 wt % of polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa·s, melting point: 233°C) was prepared, as polymer 2, polyethylene terephthalate copolymerized with 7 mol % of isophthalic acid (IPA copolymerized PET, melt viscosity: 140 Pa·s, melting point: 232°C) was prepared, and as polymer 3, polyethylene terephthalate (PET, melt viscosity: 130 Pa·s, melting point: 254°C) was prepared.

[0258] After these polymers were melted at 290°C, they were weighed so that the weight ratio of polymer 1 / polymer 2 / polymer 3 was 5 / 42.5 / 42.5, and poured into a pre-assembled Fig.12 The spinning assembly of the composite spinneret shown, such as Figure 6 As shown in (b), the composite structure is formed by arranging the easily soluble component in a tapered shape along the fiber inner direction at the front end of the convex part of the difficult-to-dissolve component described in Japanese Patent Laid-Open No. 2-145825, and the difficult-to-dissolve component is formed of two polymers, a high shrinkage component and a low shrinkage component, and the inflowing polymer is discharged from the discharge hole. At this time, the easily soluble component is polymer 1, the high shrinkage component among the difficult-to-dissolve components is polymer 2, and the low shrinkage component is polymer 3.

[0259] The discharged composite polymer flow is cooled and solidified, and then given an oil agent, and is wound up at a spinning speed of 1500 m / min and stretched between rollers heated to 90°C and 130°C, thereby producing composite fibers of 56dtex-36 filaments (high shrinkage: 28dtex-18 filaments, low shrinkage: 28dtex-18 filaments).

[0260] The woven fabric made of the woven composite fiber was treated in a 1 wt% sodium hydroxide aqueous solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, and then heat-treated with wet heat at 130°C to obtain a woven fabric composed of multifilaments (fiber diameter 12 μm) formed by the difficult-to-dissolve components of the composite fiber.

[0261] In Comparative Example 5, there is a deep groove tapering along the fiber inner direction at the front end of the convex part of the trilobal shaped fiber, so the friction coefficient is increased, and although the dry feeling is excellent, the wear resistance is poor. In addition, although lightness is obtained by showing the curling shape caused by the difference in thermal shrinkage between the high shrinkage component and the low shrinkage component, the fine fiber gaps less than 5μm and the coarse fiber gaps of 10μm or more are not uniformly present between each fiber, and the shrinkage rate of the high shrinkage component is high, so the mesh is clogged, lacking softness and resilience. The results are shown in Table 2-2.

[0262] [Example 17]

[0263] As polymer 1, polyethylene terephthalate copolymerized with 8 mol % of 5-sodium sulfonate of isophthalic acid and 9 wt % of polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa·s, melting point: 233°C) was prepared, as polymer 2, polyethylene terephthalate copolymerized with 7 mol % of isophthalic acid (IPA copolymerized PET, melt viscosity: 140 Pa·s, melting point: 232°C) was prepared, and as polymer 3, polyethylene terephthalate (PET, melt viscosity: 130 Pa·s, melting point: 254°C) was prepared.

[0264] After these polymers were melted at 290°C, they were weighed so that the weight ratio of polymer 1 / polymer 2 / polymer 3 was 30 / 35 / 35, and poured into a pre-assembled Fig.12 The spinning assembly of the composite spinneret shown, such as Fig.10 As shown in (b), it is a core-sheath composite fiber, in which the sheath component completely covers the core component, the core component is divided into two by the sheath component, and the divided core component 1 and core component 2 are respectively formed into a composite structure with a groove at the front end of the convex part of the three-leaf cross section, and the inflow polymer is discharged from the discharge hole. At this time, the sheath component is polymer 1, the core component 1 is polymer 2, and the core component 2 is polymer 3.

[0265] The discharged composite polymer stream was cooled and solidified, and then provided with an oil agent, and was taken up at a spinning speed of 1500 m / min and stretched between rolls heated to 90°C and 130°C to produce a core-sheath composite fiber of 56 dtex-18 filaments.

[0266] The ratio of the minimum thickness of the sheath component to the fiber diameter (S min / D) is 0.03, and the ratio of the maximum thickness to the minimum thickness of the sheath component (S max / S min ) was 12. In addition, the ratio of the distance GM from the center of gravity G of the core component to the groove bottom M to the distance GN from the center of gravity G of the core component to the front end N of the convex portion (GN / GM) was 1.38, which confirmed that it was the core-sheath composite fiber of the present invention.

[0267] In addition, the inscribed circle diameter R of the core-sheath composite fiber is A The diameter of the circumscribed circle R B The ratio is 1.8, which facilitates the densest packing in the presence of multifilaments, so that the inter-fiber spaces obtained after the sheath component is dissolved can be uniform without deviation.

[0268] The woven fabric of the core-sheath composite fiber obtained by weaving was heat-treated at 130°C with wet heat, and then treated in a 1 wt% sodium hydroxide aqueous solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, thereby obtaining a woven fabric composed of multifilaments in which crimped fibers composed of different polymers were uniformly mixed. The crimped fibers obtained had a composite structure (profile: 1.6) with grooves (MN / D: 0.13) at the front end of the convex part of the trilobal cross section, a fiber diameter of 10 μm, a crimp peak number of 14 peaks / cm, and a yarn length difference of 7% for the crimped fibers composed of polymers with different melting points.

[0269] For the woven fabric formed by the multifilament, the volume exclusion effect between fibers due to the curling morphology caused by the difference in thermal shrinkage of polymers with different melting points during wet heat treatment not only forms coarse inter-fiber gaps of 10 μm or more between individual fibers, but also forms inter-fiber gaps of less than 5 μm between adjacent crimped fibers formed by polymers with different melting points. In the multifilament, fine inter-fiber gaps of less than 5 μm and coarse inter-fiber gaps of more than 10 μm are more evenly mixed, and the inter-fiber gap structure is similar to the inter-fiber gaps of natural silk. The evaluation of the inter-fiber gap structure showed that the average inter-fiber gap distance was 10.5 μm, the proportion of inter-fiber gap distances less than 5 μm was 25%, and the void ratio was 65%.

[0270] In addition, the woven fabric has a high-quality luster that is not dependent on viewing angle (comparative glossiness: 1.4), is very light (apparent density: 0.32 g / cm 3 ) and a dry feel (friction coefficient: 0.8), and a more stable inter-fiber gap distance of less than 5 μm was formed compared with Example 8, thereby making the rebound feel (bending recovery 2HB: 0.7×10 -2 gf·cm / cm), flexibility (bending hardness B: 0.8×10 -2 gf cm 2 / cm) is even better, with a texture just like natural silk.

[0271] In addition, it can be seen that when the woven fabric is dyed black, the diffuse reflection of light is further enhanced by the coarse inter-fiber gaps of 10 μm or more uniformly existing between the fibers, showing excellent color rendering (black dyeing L value: 13), and also having good abrasion resistance (grade 3-4) without discoloration due to fibrillation in the groove portion. The results are shown in Table 3.

[0272] [Examples 18 and 19]

[0273] The same procedures as in Example 17 were followed except that the weight ratio of polymer 1 / polymer 2 / polymer 3 was changed to 20 / 40 / 40 (Example 18) and 10 / 45 / 45 (Example 19).

[0274] In Examples 18 and 19, as the sheath component is reduced, the ratio of the inter-fiber space distance of the multifilaments that is less than 5 μm increases, and the bending hardness associated with this increases, thereby obtaining a characteristic woven fabric having an elastic touch while retaining the texture of natural silk. In addition, since the groove at the front end of the convex part of the crimped fiber becomes shallow, the abrasion resistance is also excellent. The results are shown in Table 3.

[0275] [Example 20]

[0276] The entire process was carried out in the same manner as in Example 17 except that the polymer 2 was changed to polytrimethylene terephthalate (PPT, melt viscosity: 150 Pa·s, melting point: 233° C.).

[0277] In Example 20, the rubber elasticity of PPT is combined to provide a woven fabric that not only has a softer texture, but also has a unique stretching function that natural silk does not have. In addition, since PPT has a lower refractive index than PET, the color rendering of the obtained woven fabric is also excellent. The results are shown in Table 3.

[0278] [Example 21]

[0279] The entire process was carried out in the same manner as in Example 17 except that the polymer 2 was changed to polyethylene terephthalate having a high melt viscosity (high viscosity PET, melt viscosity: 250 Pa·s, melting point: 254° C.).

[0280] In Example 5, the crimp is expressed by the difference in viscosity rather than the difference in melting point between polymer 3 and polymer 2, thereby reducing the number of crimp peaks of the crimped fibers constituting the multifilament, thereby suppressing the diffuse reflection of light caused by the void structure of the multifilament, and increasing the visual recognition of the gloss. Furthermore, the appearance of the crimp morphology during the wet heat treatment is reduced, thereby increasing the ratio of the void distance between fibers less than 5 μm, and also improving the resilience. The results are shown in Table 3.

[0281] [Comparative Example 6]

[0282] As polymer 1, polyethylene terephthalate copolymerized with 8 mol % of 5-sodium sulfonate of isophthalic acid and 9 wt % of polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa·s, melting point: 233°C) was prepared, as polymer 2, polyethylene terephthalate copolymerized with 7 mol % of isophthalic acid (IPA copolymerized PET, melt viscosity: 140 Pa·s, melting point: 232°C) was prepared, and as polymer 3, polyethylene terephthalate (PET, melt viscosity: 130 Pa·s, melting point: 254°C) was prepared.

[0283] After melting each of these polymers at 290°C, the polymers were weighed so that the weight ratio of polymer 1 to polymer 2 became 2.5 / 47.5 and the weight ratio of polymer 1 to polymer 3 became 2.5 / 47.5, and poured into the assembled Fig.12 The spinning assembly of the composite spinneret shown, such as Fig.11 As shown in FIG. 1 , the composite structure is formed by arranging the easily soluble component in a tapered shape along the fiber inner direction at the tip of the convex part of the trilobal shape of the difficult soluble component described in Japanese Patent Application Laid-Open No. 2-145825, and the inflowing polymer is discharged in such a manner that the composite fiber composed of two components, the high shrinkage component and the easily soluble component, and the composite fiber composed of two components, the low shrinkage component and the easily soluble component, are discharged from the respective discharge holes. At this time, the easily soluble component is polymer 1, the high shrinkage component is polymer 2, and the low shrinkage component is polymer 3.

[0284] The discharged composite polymer flow is cooled and solidified, and then given an oil agent, and is wound up at a spinning speed of 1500 m / min and stretched between rollers heated to 90°C and 130°C, thereby producing composite fibers of 56dtex-36 filaments (high shrinkage: 28dtex-18 filaments, low shrinkage: 28dtex-18 filaments).

[0285] The woven fabric made of the woven composite fiber was heat-treated with wet heat at 130°C, and then treated in a 1 wt% sodium hydroxide aqueous solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, thereby obtaining a woven fabric composed of multifilaments (fiber diameter 12 μm) formed by the difficult-to-dissolve components of the composite fiber.

[0286] In Comparative Example 6, there is a deep groove tapering along the fiber inner direction at the front end of the convex part of the trilobal shaped cross-section fiber, so the friction coefficient is increased, and although the dry feeling is excellent, the wear resistance is poor. In addition, lightness can be obtained by using the difference in yarn length between the high shrinkage component and the low shrinkage component, but on the other hand, due to the spinning mixed fiber method, the fibers formed by different polymers are mixed unevenly, the proportion of the inter-fiber gap distance less than 5μm is small, and the rebound feeling is lacking. The results are shown in Table 3.

[0287] [Example 22]

[0288] The composite structure of the core-sheath composite fiber is changed to Fig.10 (a), and all other aspects are implemented according to Example 17.

[0289] In Example 22, the crimped fibers in the multifilament yarn have no grooves at the front ends of the convex portions, so diffuse reflection of light is reduced and reflection intensity is increased, and the visual recognition of gloss is increased. In addition, abrasion resistance is also excellent. The results are shown in Table 4.

[0290] [Examples 23 and 24]

[0291] The same procedures as in Example 17 were followed except that the weight ratio of polymer 2 / polymer 3 was changed to 50 / 20 (Example 23) and 20 / 50 (Example 24).

[0292] In Examples 23 and 24, as the ratio of polymer 2 as a high shrinkage component increases, the number of crimp peaks and yarn length difference of the crimped fibers in the multifilament yarn become more apparent, the average inter-fiber void distance in the void structure of the multifilament yarn becomes higher, and the lightness of the obtained woven fabric increases. In addition, as the ratio of polymer 3 as a low shrinkage component increases, the number of crimp peaks of the crimped fibers in the multifilament yarn also decreases, so that the diffuse reflection of light caused by the void structure of the multifilament yarn is suppressed, and not only the visual recognition of the gloss increases, but also the appearance of the crimp morphology in the wet heat treatment becomes smaller, so the ratio of the inter-fiber void distance of less than 5 μm also increases, and the rebound feeling is also excellent. The results are shown in Table 4.

[0293] [Examples 25 and 26]

[0294] The same procedures as in Example 17 were followed except that the discharge rate was changed so that the fiber diameter of the crimped fibers in the multifilament yarn was 14 μm (Example 25) or 17 μm (Example 26).

[0295] In Examples 25 and 26, by increasing the fiber diameter, the unevenness caused by the crimped fiber in the multifilament having a trilobal cross section is enhanced, the reflection intensity is further increased, and the visual recognition of the gloss of the obtained woven fabric is further increased. In addition, since the bending hardness is increased, while retaining the natural silk-like texture, a characteristic elastic touch is obtained. The results are shown in Table 4.

[0296] Industrial Applicability

[0297] For the multifilament of the present invention, two or more crimped fibers composed of different polymers are uniformly mixed in the multifilament, so that a unique inter-fiber interspace of less than 5 μm and a coarse inter-fiber interspace of 10 μm or more can be formed in the multifilament, like natural silk. Therefore, the fiber products formed by the multifilament of the present invention can reproduce various textures unique to natural silk, and are of course suitable for suits and kimonos that were previously mainly made of natural silk, and also have the ease of handling that only synthetic fibers have, so they can be preferably suitable for fiber products involving various aspects, such as general clothing materials such as jackets, skirts, shorts, and underwear, sports clothing, clothing materials, indoor products such as carpets, sofas, curtains, vehicle interior products such as car seats, cosmetics, cosmetic masks, rags, health products, and other daily uses.

[0298] [Table 1-1]

[0299]

[0300] [Table 1-2]

[0301]

[0302] [Table 2-1]

[0303]

[0304] [Table 2-2]

[0305]

[0306] [Table 3]

[0307]

[0308] [Table 4]

[0309]

[0310] Description of Reference Numerals

[0311] a Silk protein formed by the insoluble components in the raw silk of natural silk

[0312] b Sericin formed from easily soluble components in raw silk of natural silk

[0313] c Poorly soluble ingredients

[0314] d. Easily soluble ingredients

[0315] A A perfect circle inscribed at two or more points in the composite fiber cross section (inscribed circle)

[0316] B A perfect circle circumscribed at two or more points in the composite fiber cross section (circumscribed circle)

[0317] C A perfect circle inscribed at two or more points in the fiber cross section (inscribed circle)

[0318] D A perfect circle circumscribed by two or more points in the fiber cross section (circumscribed circle)

[0319] F The intersection of the fiber surface and a straight line drawn from the intersection point (center of gravity) of any two straight lines that divide the area of ​​the fiber cross section into two equal parts.

[0320] G The intersection point (center of gravity) of any two straight lines that divide the area of ​​the fiber cross section into two equal parts

[0321] M The point on the groove surface at the tip of the convex portion closest to the intersection (center of gravity) of any two straight lines that divide the area of ​​the fiber cross section into two equal parts

[0322] N The point on the groove surface at the tip of the convex portion that is farthest from the intersection (center of gravity) of any two straight lines that divide the area of ​​the fiber cross section into two equal parts

[0323] S The intersection of a straight line drawn from the intersection of any two straight lines that divide the area of ​​the fiber cross section into two equal parts toward any fiber surface and the outer periphery of the core component

[0324] X Any fiber in multifilament

[0325] Y is a fiber in a multifilament yarn, in which no other fiber exists on a straight line connecting its center of gravity and the center of gravity of X, and is a fiber composed of a polymer different from that of X.

[0326] 1 Measuring plate

[0327] 2 Distribution board

[0328] 3 Discharge plate

Claims

1. Multifilament formed by the core component of a core-sheath composite fiber, in, In the fiber cross section of the core-sheath composite fiber formed of two or more polymers, the cross-sectional shape is a perfect circle or an ellipse, the sheath component completely covers the multi-lobed core component having three or more convex portions, and the maximum thickness S of the sheath component is max With minimum thickness S min Ratio S max / S min is 5.0 or above, The multifilament has a void structure in which the average inter-fiber void distance is 5 to 30 μm, and the proportion of the inter-fiber void distance less than 5 μm is 10 to 50%.

2. The multifilament according to claim 1, in, In the multi-leaf core component, there is a groove toward the center of gravity of the core component at the front end of the convex part, and the ratio GN / GM of the distance GM from the center of gravity G of the core component to the groove bottom M and the distance GN from the center of gravity G of the core component to the front end N of the convex part is 1.1 to 1.

5.

3. The multifilament according to claim 1 or 2, in, The core component is divided into two or more parts by the sheath component, and each of the divided core components has a multi-lobed shape.

4. The multifilament according to claim 3, in, In the core components divided by the sheath component, adjacent core components are formed of polymers having different melting points.

5. The multifilament according to claim 1 or 2, which has a void structure with a void ratio of 30 to 80%.

6. The multifilament according to claim 1 or 2, comprising two or more crimped fibers composed of polymers having different melting points, wherein the crimped fibers are uniformly mixed.

7. The multifilament according to claim 1 or 2, which is composed of fibers having a groove at the front end of the protrusion in the fiber cross section, and the ratio of the distance MN from the groove bottom M to the front end N of the protrusion to the fiber diameter D (MN / D) is 0.04 to 0.

20.

8. A fiber product, a part of which contains the multifilament according to any one of claims 1 to 7.