A cardanol-modified phenolic amide curing agent and preparation method thereof

Through the preparation of the phenolamide curing agent modified by cashew phenol, the problem of dark and unstable color of the phenolamide curing agent and insufficient low-temperature curing ability of polyamide is solved, and the low-temperature rapid curing, good adhesion and anti-corrosion performance are achieved. It is suitable for many type of coatings.

CN114524750BActive Publication Date: 2024-11-19ZHEJIANG WANSHENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210151438.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-18
Publication Date
2024-11-19
Estimated Expiration
2042-02-18

AI Technical Summary

Technical Problem

The existing phenoamine curing agents are darker in color and unstable, and have poor mechanical properties, while the polyamide curing agent cannot cure under low temperature environments, resulting in limited usability in winter.

Method used

The preparation method of a phenolamide curing agent modified by cashew phenol includes an ene reaction in pyrrolidone, followed by a Mannich reaction with fatty amines and paraformaldehyde, combined with maleic anhydride and MXDA, and using specific catalysts and conditions, A phenolamide curing agent with low temperature curing properties, long service life, good adhesion and anti-corrosion properties are obtained.

Benefits of technology

It achieves rapid curing in low-temperature environments, improves hardness, improves impact resistance, improves adhesion and toughness, and has good anti-corrosion properties. It is suitable for electronic potting materials and epoxy anti-corrosion coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003510726680000021
    Figure BDA0003510726680000021
  • Figure BDA0003510726680000031
    Figure BDA0003510726680000031
  • Figure BDA0003510726680000071
    Figure BDA0003510726680000071
Patent Text Reader

Abstract

The invention discloses a cardanol-modified phenolic amide curing agent and a preparation method thereof. The high-purity cardanol shown in formula (4) is used as a raw material, and the ene reaction is carried out with maleic anhydride, the obtained product is subjected to condensation reaction with a fatty amine, and the condensation product is subjected to Mannich reaction with polyformaldehyde and a fatty amine to obtain a target product; or the high-purity cardanol shown in formula (4) is used as a raw material, and the ene reaction is carried out with maleic anhydride, the obtained product is subjected to condensation reaction with a fatty amine, and the obtained product is subjected to Mannich reaction with polyformaldehyde and MXDA to obtain a compound of formula (5); the product has both the low-temperature curing performance of phenolic amide and the good adhesion, toughness, corrosion resistance and insulation performance of polyamide, and can be used in the fields of electronic potting materials, anti-corrosion coatings and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of epoxy resin anticorrosive coatings, and particularly relates to a cardanol-modified phenolic amide curing agent and a preparation method thereof. Background Art

[0002] Cardanol is a natural phenolic substance with a phenolic hydroxyl functional group and an unsaturated 15-C long-chain hydrocarbon. It can be used as a bio-based substitute for petrochemical raw materials and is widely used in coatings and adhesives. Because of its abundant source, renewable nature and low price, it has become a research hotspot in recent years.

[0003] Phenolic amine is made of phenols, aldehydes and polyamines through the Mannich reaction. It contains phenolic hydroxyl groups, has low-temperature curing properties, has a 15-carbon long carbon chain, can provide the product with good toughness, has a benzene ring structure, and has high temperature resistance. However, it also has some disadvantages, such as darker color, instability, and mechanical properties that are slightly different from polyamide.

[0004] Polyamide curing agent is synthesized from vegetable oil dimer and ethyleneamine, and has many excellent properties, such as long operation cycle, low toxicity, good adhesion, good room temperature curing performance, and is widely used in epoxy primer or mid-coat, epoxy anti-corrosion coating, electronic potting materials and other fields. Because it cannot be cured in low temperature environment, its use in winter is limited. Summary of the invention

[0005] In view of the above problems existing in the prior art, the object of the present invention is to provide a cardanol-modified phenolic amide curing agent and a preparation method thereof. The curing agent obtained by the method has both the low-temperature curing performance of phenolic amine and the characteristics of polyamide such as long service life, good adhesion, good toughness and good anti-corrosion performance, and can be used in the fields of electronic potting materials, anti-corrosion coatings, etc.

[0006] The present invention provides a cardanol-modified phenolic amide curing agent, characterized in that its structural formula is as shown in formula (1) or formula (5):

[0007]

[0008] Where n is 1-10.

[0009] Furthermore, the present invention also provides a method for preparing the cardanol-modified phenolic amide curing agent, which is characterized by comprising the following steps:

[0010] 1) adding high-purity cardanol represented by formula (4) and maleic anhydride to pyrrolidone, carrying out ene reaction under the action of a catalyst, and obtaining a compound of formula (3) after post-treatment;

[0011] 2) the compound of formula (3) obtained in step 1) is subjected to a condensation reaction with a fatty amine to obtain a compound of formula (2);

[0012] 3) the compound obtained in step 2) is subjected to a Mannich reaction with paraformaldehyde and a fatty amine to obtain the target compound represented by formula (1);

[0013] 4) The compound obtained in step 2) is subjected to a Mannich reaction with paraformaldehyde and MXDA to obtain the target compound represented by formula (5).

[0014]

[0015] Furthermore, the present invention also defines that the catalyst in step 1) is cobalt isooctanoate or cobalt cyclohexaneate, and the amount of the catalyst is 0.2%-5%, preferably 0.2%-3% of the total mass of the raw materials.

[0016] Furthermore, the present invention also defines the molar ratio of cardanol to maleic anhydride in step 1) as 0.5-1:1-3; preferably 0.5-1:1-2.

[0017] Furthermore, the present invention also defines the post-treatment process in step 1) as adding water and a solvent, standing to separate the layers, and removing the solvent under reduced pressure from the organic layer to obtain a product, wherein the solvent is xylene, ethyl acetate, toluene, ethyl ether, n-butanol, isopropanol, methanol or acetonitrile; preferably xylene, toluene or ethyl acetate.

[0018] Furthermore, the present invention also defines the temperature of the ene reaction in step 1) as 80-200°C, preferably 130-200°C, and more preferably 130-190°C.

[0019] Furthermore, the present invention also defines the condensation reaction temperature in step 2) as 80-200°C, preferably 100-200°C, more preferably 130-200°C; the molar ratio of the compound of formula (3) to the fatty amine is 0.5-1:1-2.5, preferably 0.5-1:1-2.

[0020] Furthermore, the present invention also defines that the fatty amines in step 2) and step 3) are each independently a compound of at least one primary amine or secondary amine, preferably one or a mixture of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethylenepolyamine, dimethyldipropylenetriamine, meta-xylylenediamine, mixed amine (E-100), N-aminoethylpiperazine, trimethylhexamethylenediamine, 1-3-pentanediamine, 1,2-cyclohexanediamine; the molar ratio of the compound represented by formula (2) to paraformaldehyde and the fatty amine is 1:1-2.5:1-2.5, preferably 1:1-2.0:1-2.0.

[0021] Furthermore, the present invention also limits the temperature of the mannich reaction in step 3) to 50-150°C, preferably 70-150°C.

[0022] The present invention adopts the above technology to obtain a cardanol-modified phenolic amide curing agent, which has both the low-temperature curing performance of phenolic amine and the characteristics of polyamide such as long service life, good adhesion, good toughness and anti-corrosion performance, and can be used in the fields of electronic potting materials, anti-corrosion coatings, etc. DETAILED DESCRIPTION

[0023] The present invention is further described below in conjunction with embodiments, but the protection scope of the present invention is not limited thereto:

[0024] Example 1: Preparation of the compound of formula (3)

[0025] 150 g of cardanol, 53.9 g of maleic anhydride, 0.75 g of catalyst cobalt isooctanoate and 9 g of pyrrolidone were added to the reaction flask, and the temperature was raised to 150-190 ° C for reaction after nitrogen replacement, and the temperature was kept for 4-5 hours, and the temperature was lowered, 90 g of xylene and 90 g of water were added, and the layers were allowed to stand and separated. The organic layer was decompressed and desolvated at 100-120 ° C to obtain the compound shown in formula (3); analysis results: the acid value is 230 mgKOH / g, and the iodine value is 110 g / 100 g.

[0026] Example 1a: Preparation of the compound of formula (3)

[0027] 150 g of cardanol, 63.7 g of maleic anhydride, 1.0 g of catalyst cobalt cyclohexane and 10 g of solvent pyrrolidone were added to the reaction flask, and the temperature was raised to 150-190 ° C for reaction after nitrogen replacement, and the temperature was kept for 5-7 hours. The temperature was lowered, 100 g of ethyl acetate and 100 g of water were added, and the layers were allowed to stand, and the liquids were separated. The solvent was removed under reduced pressure at 100-120 ° C to obtain the compound shown in formula (3); analysis results: the acid value is 236 mgKOH / g, and the iodine value is 105 g / 100 g.

[0028] Example 2: Preparation of the compound represented by formula (2)

[0029] 100 g of the compound represented by formula (3) and 42.2 g of diethylenetriamine (DETA) were added to the reaction flask, the temperature was raised to 150-160°C for reaction, the temperature was kept for 4-5 hours, and the temperature was lowered to obtain the compound represented by formula (2). The analysis results showed that the amine value was 510 mgKOH / g and the viscosity was 22000 cp@25°C.

[0030] Example 2a: Preparation of the compound represented by formula (2)

[0031] 100 g of the compound represented by formula (3) and 59.9 g of tetraethylenepentamine were added to the reaction flask, the temperature was raised to 160-170°C for reaction, the temperature was kept for 4-5 hours, and the temperature was lowered to obtain the compound represented by formula (2). The analysis results showed that the amine value was 603 mgKOH / g and the viscosity was 24000 cp@25°C.

[0032] Example 2b: Preparation of the compound represented by formula (2)

[0033] 100 g of the compound represented by formula (3) and 89 g of mixed amine E-100 were added to the reaction bottle, the temperature was raised to 170-180°C for reaction, the temperature was kept for 4-5 hours, and the temperature was lowered to obtain the compound represented by formula (2). The analysis results showed that the amine value was 680 mgKOH / g and the viscosity was 27300 cp@25°C.

[0034] Example 3: Preparation of the target compound represented by formula (1)

[0035] 100 g of the compound of formula (2) obtained in Example 2, 21.1 g of diethylenetriamine (DETA), and 7.3 g of polyformaldehyde were added to a reaction flask, and the temperature was raised to 100-130°C for reaction. The temperature was kept for 3-5 hours, and vacuum dehydration was performed to prepare the target compound of formula (1). The analysis results showed that the amine value was 310 mgKOH / g and the viscosity was 33000 cp@25°C.

[0036] Example 3a: Preparation of the target compound represented by formula (1)

[0037] 100 g of the compound of formula (2) obtained in Example 2a, 20 g of diethylenetriamine, and 8.4 g of polyformaldehyde were added to a reaction flask, and the temperature was raised to 100-130°C for reaction. The temperature was kept for 3-5 hours, and vacuum dehydration was performed to prepare the target compound of formula (1). The analysis results showed that the amine value was 305 mgKOH / g and the viscosity was 35100 cp@25°C.

[0038] Example 3b: Preparation of the target compound represented by formula (1)

[0039] 100 g of the compound of formula (2) obtained in Example 2b, 43.51 g of mixed amine (E-100), and 6.8 g of polyformaldehyde were added to a reaction flask. The temperature was raised to 130-150°C for reaction. The temperature was kept for 3-5 hours and vacuum-dried to prepare the target compound of formula (1). The analysis results showed that the amine value was 359 mgKOH / g and the viscosity was 36420 cp@25°C.

[0040] Example 4: Preparation of the compound represented by formula (5)

[0041] 100 g of the compound of formula (2) obtained in Example 2, 27.8 g of MXDA, and 7.3 g of polyformaldehyde were added to a reaction flask, and the temperature was raised to 100-130° C. for reaction. The temperature was kept for 3-5 hours, and vacuum-dried to prepare a compound of formula 5. The analysis results showed that the amine value was 295 mgKOH / g and the viscosity was 36000 cp@25° C.

[0042] Example 4a: Preparation of the compound represented by formula (5)

[0043] 100 g of the compound of formula (2) obtained in Example 2a, 26 g of MXDA, and 8.4 g of polyformaldehyde were added to a reaction flask, and the temperature was raised to 130-150° C. for reaction. The temperature was kept for 3-5 hours, and vacuum-dried to prepare a compound of formula 5. The analysis results showed that the amine value was 280 mgKOH / g and the viscosity was 38000 cp@25° C.

[0044] Performance test data comparison

[0045] The epoxy resin E-51 was mixed and cured with the compound sample represented by formula (1) obtained in Example 3, the compound sample represented by formula (5) obtained in Example 4, the commercially available phenolic amine curing agent WSCM-1101, and the polyamide curing agent WSCM-4115 in a stoichiometric ratio, and the low-temperature curing performance, physical and mechanical properties, and anti-corrosion performance were compared. The results are shown in Table 1:

[0046] Table 1 Performance comparison of the product obtained by the present invention and the existing product

[0047]

[0048] It can be concluded from the above table that the product of the present invention has a faster curing speed than the polyamide curing agent (WSCM-4115), can be cured within 48 hours at 5°C, has improved hardness, and has better impact resistance than the phenolic amine curing agent (WSCM-1101). It has both the low-temperature curing performance of phenolic amine and the good adhesion and flexibility of polyamide.

[0049] Salt spray resistance test (paint): salt spray chamber test method

[0050] According to the American ASTM B117-1997 "Determination of Salt Spray Resistance of Paint Film", the experiment was conducted by mixing the resin component A and the curing agent and spraying them on the steel plate, drying them, and the dry film thickness was 100um. The steel plate was scratched and placed in a salt spray box (test conditions: temperature: 35℃ 5% sodium chloride aqueous solution). The corrosion and damage conditions on the sample were checked regularly, and the time (hours) was recorded. The results are shown in Table 2:

[0051] Table 2 Salt spray resistance performance of the product of the present invention and the existing product

[0052]

[0053] According to the above test data, the new type of phenolic amide curing agent modified by cardanol of the present invention not only retains the low-temperature curing performance of phenolic amine, but also has the good adhesion and toughness of polyamide, as well as the salt spray corrosion resistance, and can be used for epoxy resin anti-corrosion coatings.

Claims

1. A method for preparing a cardanol-modified phenolic amide curing agent, characterized in that The steps include: 1) adding high-purity cardanol represented by formula (4) and maleic anhydride to pyrrolidone, carrying out ene reaction under the action of a catalyst, and obtaining a compound of formula (3) after post-treatment; 2) the compound of formula (3) obtained in step 1) is subjected to condensation reaction with mixed amine E-100 to obtain the corresponding compound; 3) The compound obtained in step 2) is subjected to a Mannich reaction with paraformaldehyde and mixed amine E-100 to obtain the target compound.

2. The method for preparing the cardanol-modified phenolic amide curing agent according to claim 1, characterized in that The amount of catalyst used in step 1) is 0.2%-3% of the total mass of the raw materials.

3. The method for preparing the cardanol-modified phenolic amide curing agent according to claim 1, characterized in that The post-treatment process in step 1) is to add water and a solvent, stand for stratification, and remove the solvent under reduced pressure from the organic layer to obtain a product, wherein the solvent is xylene, ethyl acetate, toluene, ether, n-butanol, isopropanol, methanol or acetonitrile.

4. The method for preparing the cardanol-modified phenolic amide curing agent according to claim 3, characterized in that The solvent for the post-treatment process in step 1) is xylene, toluene or ethyl acetate.

5. The method for preparing the cardanol-modified phenolic amide curing agent according to claim 1, characterized in that The temperature of the ene reaction in step 1) is 130-200°C.

6. The method for preparing the cardanol-modified phenolic amide curing agent according to claim 5, characterized in that The temperature of the ene reaction in step 1) is 130-190°C.

7. The method for preparing the cardanol-modified phenolic amide curing agent according to claim 1, characterized in that The condensation reaction temperature in step 2) is 170-180°C.

8. The method for preparing the cardanol-modified phenolic amide curing agent according to claim 1, characterized in that The temperature of the mannich reaction in step 3) is 130-150°C.

9. The method for preparing the cardanol-modified phenolic amide curing agent according to claim 1, characterized in that The catalyst in step 1) is cobalt isooctanoate or cobalt cyclohexaneate, and the amount of the catalyst is 0.2%-5% of the total mass of the raw materials.